Next Article in Journal
In Situ Recrystallization of Mesoporous Carbon–Silica Composite for the Synthesis of Hierarchically Porous Zeolites
Next Article in Special Issue
Structural Characterization of Al65Cu20Fe15 Melt-Spun Alloy by X-ray, Neutron Diffraction, High-Resolution Electron Microscopy and Mössbauer Spectroscopy
Previous Article in Journal
Microstructure Evolution of Ti-45Al-8.5Nb-0.2W-0.2B-0.02Y Alloy during Long-Term Thermal Exposure
Previous Article in Special Issue
Influence of Cu Content on Structure and Magnetic Properties in Fe86-xCuxB14 Alloys
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Fe-Co-B Soft Magnetic Ribbons: Crystallization Process, Microstructure and Coercivity

1
Institute of Metallurgy and Materials Science, Polish Academy of Sciences, 25 Reymonta Str., 30-059 Krakow, Poland
2
Faculty of Materials Science and Engineering, Warsaw University of Technology, 141 Woloska Str., 02-507 Warsaw, Poland
3
Lukasiewicz Research Network—Institute of Non-Ferrous Metals, 5 Sowinskiego Str., 44-100 Gliwice, Poland
*
Author to whom correspondence should be addressed.
Materials 2020, 13(7), 1639; https://doi.org/10.3390/ma13071639
Submission received: 13 March 2020 / Revised: 24 March 2020 / Accepted: 30 March 2020 / Published: 2 April 2020
(This article belongs to the Special Issue Structure and Properties of Crystalline and Amorphous Alloys)

Abstract

:
In this work, a detailed microstructural investigation of as-melt-spun and heat-treated Fe67Co20B13 ribbons was performed. The as-melt-spun ribbon was predominantly amorphous at room temperature. Subsequent heating demonstrated an amorphous to crystalline α-(Fe,Co) phase transition at 403 °C. In situ transmission electron microscopy observations, carried out at the temperature range of 25–500 °C and with the heating rate of 200 °C/min, showed that the first crystallized nuclei appeared at a temperature close to 370 °C. With a further increase of temperature, the volume of α-(Fe,Co) crystallites considerably increased. Moreover, the results showed that a heating rate of 200 °C/min provides for a fine and homogenous microstructure with the α-(Fe,Co) crystallites size three times smaller than when the ribbon is heated at 20 °C/min. The next step of this research concerned the influence of both the annealing time and temperature on the microstructure and coercivity of the ribbons. It was shown that annealing at 485 °C for a shorter time (2 s) led to materials with homogenous distribution of α-(Fe,Co) crystallites with a mean size of 30 nm dispersed in the residual amorphous matrix. This was reflected in the coercivity (20.5 A/m), which significantly depended on the volume fraction of crystallites, their size, and distribution.

1. Introduction

Among several groups of soft magnetic materials, Fe-based amorphous and nanocrystalline alloys are extremely interesting from both a scientific and an application point of view [1,2,3,4,5,6,7,8,9,10,11,12,13,14,15,16,17]. They exhibit not only optimal soft magnetic properties (e.g., low coercivity (Hc) and high permeability (µ’)) but also are characterized by relatively low magnetic core losses (Ps) in comparison with other materials. For this reason, they find various applications in motors, transformers, actuators, sensors, and electronic communication devices [3]. However, soft magnetic properties are sensitive to chemical composition as well as microstructural features of materials [18]. It was reported that nanocomposites consisting of α-Fe crystallites with sizes smaller than 35 nm and surrounded by an amorphous matrix showed low coercivity and high permeability [1,18]. This behavior, explained by Herzer [18] in 1989, is based on a random anisotropy model in which the averaging of magnetocrystalline anisotropy plays a key role. Thus, for this reason, α-Fe crystallites have to be smaller than the natural exchange length, which equals 35 nm for Fe. Customarily, nanomaterials are fabricated in a multistage process, which typically is realized in two steps: (1) production of amorphous ribbons by rapid quenching techniques and (2) crystallization of α-Fe nanocrystals involved by heat treatment [1,19]. The most important conditions, which allow for obtaining a fine and homogenous microstructure, are (i) large nucleation rates and (ii) small crystallite growth rates. Moreover, the crystallization process is also dependent on chemical composition. For systems containing Cu, heterogeneous nucleation of the α-Fe phase on Cu-clusters occurs, while the addition of other elements inhibits the crystallite’s growth [20]. In Cu-free alloys, homogenous nucleation takes place, while nucleation density is very sensitive to annealing temperature and heating rate [21].
Despite the work that has been done on Fe-Co-B ribbons, [22,23] including both structural and magnetic properties in the function of chemical composition and heat treatment conditions, there are still not that many detailed studies on the complex microstructural investigation of Fe-Co-B in the context of ultrarapid annealing (URA). Recently authors presented the analysis of the Fe80−xCo20Bx (x = 12–15 at.%) ribbons and discussed the effect of the chemical composition (boron content) and subsequent conventional heat treatment conditions on the structure, microstructure, and magnetic properties of these materials. It was shown that with the increase of boron content, the crystal structure of ribbons changes as follows: fully crystalline (12 at.% of B) → amorphous +crystalline (13 at.% of B) → fully amorphous (14 and 15 at.% of B). Moreover, magnetic properties such as the saturation magnetic flux density (Bs) value as well as coercivity were examined. The highest value of Bs was found to be for both as-spun and annealed Fe67Co20B13 ribbons, while Fe67Co19B14 ribbon exhibited the narrowest coercivity [22]. Thus, based on the aforementioned reports, we selected the optimal composition of Fe67Co20B13 to be promising for further investigation.
In this work, an attempt is made to study the crystallization process, structure, microstructure, and magnetic properties of as-spun and annealed Fe67Co20B13 ribbons. The in situ TEM observations during heating with two heating rates of 20 and 200 °C/min were carried out with the aim to understand the evolution of the crystallization process in both heating conditions. High-energy synchrotron measurements allowed one to estimate the amount of crystalline phase with respect to the amorphous ones. Microstructural observations, especially using high-resolution TEM, gave substantial information about the size and distribution of crystallites in an amorphous matrix as well as the microstructural details on an atomic scale. Furthermore, the correlation of structural–microstructural features and the effect on the crystallization process with magnetic properties was also discussed.

2. Materials and Methods

Fe67Co20B13 master alloy was prepared by induction melting from chemical elements Fe (99.85%), Co (99.9%), and binary compound FeB18 in an argon atmosphere. Then, the as-cast ingot was induction melted in an argon atmosphere and ejected with 26 kPa overpressure onto a copper wheel rotating with a linear speed of 34 m/s. The obtained ribbon (termed Ribbon 0) had 10 mm in width and 16 µm in thickness. Subsequent annealing at three temperatures for various times was performed at (i) 370 °C/60 s, (ii) 410 °C/30 s, and (iii) 485 °C/2 s, in a specially designed block heating system for the ultrarapid annealing technique, hereafter referred to as Ribbon 1, Ribbon 2, and Ribbon 3, respectively. The main parts of the heating system are two bulky copper blocks, heated up to the appropriate temperature. The temperature is stabilized by the PID controller, in terms of the thermocouple’s signal, situated in one of the blocks close to the sample’s surface. The microstructure of ribbons was examined using a Tecnai G2 Transmission Electron Microscope (TEM) (FEI, Eindhoven, The Netherlands) equipped with an energy-dispersive X-ray microanalyzer (EDX) (EDAX, Mahwah, NJ, USA) and a High Angle Annular Dark Field (HAADF) detector (Fischione, Pennsylvania, Pittsburgh, PA, USA). The Gatan 628 heating holder was used for the in situ experiments. Thin foils for TEM observations were prepared with TenuPol-5 double jet electropolished using an electrolyte of perchloric acid (20 vol.%) and methanol (80 vol.%) at a temperature of about −20 °C. Room temperature high-energy, wide-angle X-ray diffraction measurements were carried out at DESY synchrotron in Germany, Hamburg using the beamline P07 (87.1 keV, λ = 0.0142342 nm). The samples were rotated 180° around the ω axis in order to obtain diffraction with good grain statistics [24]. The amount of crystalline phase was calculated using Origin 2018 Academic software, from the integrated area of each peak using the following equation: area of crystalline peaks/(area of crystalline peaks+amorphous peaks). The background correction was performed using HighScore Plus software. Thermoanalysis was performed by a differential scanning calorimetry (DSC) using a thermal analyzer (Netzsch DSC 404C Pegasus, Netzsch-Gerätebau GmbH, Selb, Germany)) instrument with a heating rate of 20 °C/min. Magnetic measurements were performed in a hysteresis loop tracer, specially designed for soft magnetic materials in the ribbon shape attachment. Properties of extremely soft magnetic materials were measured with the high sensitivity in the magnetic field with a range of ±660 A/m. The measuring unit was based on the idea described by Kulik et al. [25].

3. Results and Discussion

3.1. Characterization of the as Spun Fe67Co20B13 Ribbon

Figure 1a shows the integrated high-energy synchrotron radiation diffraction patterns for the as-spun ribbon. According to the synchrotron diffraction patterns, the as-spun ribbon is almost fully amorphous with a characteristic broad diffused diffraction halo. Only a trace amount of crystallites (about 2%) in the amorphous matrix is detected. Very low peaks are observed at the 2Theta angles (~4.0, 5.6, and 7.0 degrees) that indicate the presence of a negligible amount in the primary α-(Fe,Co) phase. Han et al. investigated the influence of boron addition on the structure of ribbons and showed the two-phase structure of Fe67Co20B13 as-spun ribbon [22]. The differential scanning calorimetry (DSC) curve (Figure 2b) recorded on heating for Fe67Co20B13 as-spun ribbon showed the two-stage crystallization process. The first exothermic peak (Tp1), with the minimum at 403 °C, corresponds to the crystallization of the α-(Fe,Co) phase. The second peak (Tp2) occurring at 522 °C is related to the crystallization processes of iron and/or cobalt borides. Based on DSC curves, the temperatures for the heat treatment process have been selected, i.e., below and above the Tp1 value.
Figure 2 demonstrates bright-field (BF) images and the corresponding selected area electron diffraction patterns (SADPs) taken from different areas of the as-spun Fe67Co20B13 ribbon. Besides the amorphous phase (Figure 2a,b) with a characteristic amorphous halo ring (marked by white arrow), preliminary nanocrystalline regions have been found (Figure 2c,d). The SADP has been indexed in accordance with the bcc α-(Fe,Co) crystal structure. The size of crystalline regions was estimated to be between 100 and 200 nm. Moreover, the high-resolution transmission electron microscopy (HRTEM) micrograph, fast Fourier transform (FFT), and inverse fast Fourier transform (IFFT) images taken from (1) crystalline and (2) amorphous regions, marked with squares, are presented in Figure 3. The FFT obtained from the HRTEM image pointed by square 1 can be well indexed based on the α-(Fe,Co) structure confirming SADPs results. Additionally, the lattice fringes of the observed crystallite correspond to the (110) planes of the bcc α-(Fe,Co) phase. The area of square 2 reveals the existence of local atomic ordered regions with a size of about 1–2 nm, called “nanocrystalline (atomic) clusters” randomly dispersed in the amorphous matrix (highlighted by yellow ovals). Furthermore, onion-like contrasts are marked by blue arrows. This kind of local microstructure was already reported and described in Fe-Si-B-P-Cu systems [19].

3.2. In Situ TEM Heating Observations

The in situ TEM experiments were performed with two heating rates of 20 and 200 °C/min to compare and recreate conditions typically employed during the experimental heat treatment. During the in situ TEM experiments, carried out with a heating rate of 200 °C/min, the evolution of microstructure was observed (Figure 4a). At 375 °C, in consistence with the DSC scan, the crystallization nuclei were revealed, followed by the dendritic growth of crystals (430 °C). The same phenomenon was reported in [23] for Fe85-xCoxB15 alloys for x within the range of 12 < x < 25 at.%. The presence of the crystallized nuclei at this low temperature was associated with a phase separation taking place within the amorphous matrix. This led to the formation of a dendritic α-(Fe,Co) structure, whereas the majority of the sample volume remained in its amorphous state.
More significant differences were observed in the electron diffraction patterns (SADP) with the increase of temperature (Figure 5). The SADP taken at room temperature showed two typical diffused halo rings corresponding to the most intense reflections of the α phase, i.e., (111) and (211). At 400 and 450 °C, diffused spots appeared on the first ring (counting from the center of the diffraction pattern) and also on an additional diffraction ring that appeared between the first and the second halo ring. At 500 °C, all the diffraction rings are well-developed, and they correspond with high accuracy to the crystallographic planes of the α-(Fe,Co) phase. In addition, one can see individual reflections marked by arrows, which are characteristic of the Fe2B phase. In order to compare the microstructural changes with respect to the heating rate applied (20 and 200 °C/min), the BF image analysis was supplemented with measurements of crystallite sizes (dendrite arms cross-sections) at various temperatures.
Figure 6 shows a set of microstructures in the BF mode recorded for different temperatures during in situ heating at 20 and 200 °C/min. Histograms of crystallite size distribution and their average values are attached to individual images of microstructures. The histograms have been fitted by a lognormal function similarly, like in the case of rapid annealed Fe-Si-Nb-B-Cu soft magnetic amorphous alloys [13]. From Figure 6, one can see that in both cases, the same crystallization mechanism occurs, including nucleation and dendritic growth. However, the crystallite size for samples heated at 20 °C/min is three times larger than the crystal size of samples heated at 200 °C/min for the same measurement temperatures. In addition, by analyzing the nature of the histograms, it can be concluded that in the first case (20 °C/min), a bimodal crystallite size distribution occurs at all temperatures. In contrast, for the second case at temperatures of 410 °C and 480 °C, unimodal normal type distribution occurs. In summary, it can be stated that the crystallization process of amorphous Fe67Co20B13 ribbons at 20 and 200 °C/min heating rates carried out by in situ TEM leads to visibly different microstructures in respect of the particular size and distribution of the crystalline phase, which in turn leads to various magnetic properties.
Figure 7 shows the HREM image together with the corresponding FFT and IFFT images of the sample heated in situ to a temperature of 500 °C with a heating rate of 200 °C/min. Reflections corresponding to interplanar distances such as 2.51 and 2.03 Å, as well as diffusion rings corresponding to the amorphous phase, are well visible on the FFT image taken from the marked area (white square). According to the angle’s measurement, the presence of α-(Fe,Co) and (Fe,Co)2B phases with the [111] and [012] zone axes may be confirmed, respectively. Accordingly, the IFFT’s two nano regions corresponding to the α-(Fe,Co) and Fe2B phases separated by the amorphous phase can be distinguished (Figure 7 right image).

3.3. Characterization of Heat Treated Fe67co20B13 Ribbons

Figure 8 presents the synchrotron X-ray diffraction patterns of heat-treated ribbons. Samples after annealing show a two-phase structure consisting of both amorphous and α-(Fe,Co) crystalline phases. Moreover, the amount of crystalline α-(Fe,Co) phase calculated from X-ray diffraction patterns is found to be 6.5%, 38.7%, and 91.6% for ribbons annealed at 370, 410, and 485 °C, respectively. It is therefore clear that the higher the heat treatment temperature is, the greater the crystalline to amorphous phase ratio.
Figure 9 shows the set of BF micrographs (a, c, e) and SADPs (b, d, f) for Fe67Co20B13 ribbons after heat treatment performed under various conditions (370 °C/60 s, 410 °C/30 s, and 485 °C/2 s). Ribbon 1 has α-(Fe,Co) crystallites with an average crystal size of 53 ± 13 nm, randomly placed in the amorphous matrix. Both the BF image and SADP indicate that the content of the crystalline phase is much smaller than the amorphous phase. Ribbon 2 contains much more α-(Fe,Co) crystal grains compared to Ribbon 1, while the crystallites’ size decreases to 37 ± 8 nm. Ribbon 3 annealed at the highest temperature, within the investigated temperature range at almost fully crystalline, with the small amorphous regions surrounding α-(Fe,Co) crystallites with an average size of 30 ± 8 nm. By the increase of annealing temperature, extra spots appear. The new phase was identified to be iron and/or cobalt borides (Fe,Co)2B. The distinction between both phases cannot be made due to the same crystallites structure (I4/mcm) and similar lattice parameters (for Fe2B and for Co2B). In this case, the amount of borides was almost negligible. However, it is well known that the presence of borides in greater amounts has a negative impact on soft magnetic behavior leading, e.g., to the increase of coercive fields.
HRTEM micrograph for Ribbon 3 is shown in Figure 10. It proves that α-(Fe,Co) crystallites with a mean size of 30 nm are spread in the amorphous matrix. The aforementioned ribbons, due to their unique microstructure, are called “nanocomposite materials”, where the α-Fe crystallites are embedded in an amorphous matrix, which is beneficial from a magnetic properties point of view.

3.4. Magnetic Properties

Figure 11 presents B-H (where B is induction and H is a magnetic field) loops of heat-treated Fe67Co20B13 ribbons in the correlation with microstructural features apparent in BF images. The coercivity (Hc) considerably diminishes with the increase of heat treatment temperature from 49.8 A/m for Ribbon 1 to 20.5 A/m for Ribbon 3. This behavior is a consequence of microstructure evolution, including both α-(Fe,Co) crystallite sizes and their volume fraction as well as the distribution in the amorphous matrix. In the case of the ribbon annealed at a temperature of 370 °C for 60 s, slightly below the onset of α-(Fe,Co) phase crystallization peak (Figure 1b), the crystallites are the largest (53 nm), unevenly embedded in the matrix. Here, the α-(Fe,Co) crystallites grow from Fe-rich regions (well observed in HRTEM—Figure 4) while the annealing time (60 s) is sufficient for crystal growth. As a consequence of the existence of larger, heterogeneously distributed α-(Fe,Co) crystallites, the coercive field value is the largest. However, Ribbon 3 annealed at 485 °C for two s is characterized by a fine microstructure, where the crystallites with an average crystallite size of 30 nm are uniformly distributed in the amorphous matrix. In this case, α-(Fe,Co) crystallites are connected with both preexisting nuclei as well as newly formed ones. Short annealing times and a large number of nuclei inhibit crystallites growth. Thus, a low coercive field (20.5 A/m) in this alloy can be explained by the fact that the exchange correlation length is larger than the crystallite’s size. Additionally, it can be noticed that the saturation magnetic induction (Bs) was estimated to increase subtly with the annealing temperature.

4. Conclusions

Based on the in situ TEM experiments and the nano- and microstructure observations, the following conclusions can be drawn: (i) independently of the heating rate, the crystallization process of amorphous Fe67Co20B13 melt-spun ribbons is realized by the nucleation and dendritic growth of α-(FeCo) phase, while the first crystallization effects are manifested at a temperature close to 370 °C; (ii) finer and more homogeneous microstructures are observed in the case of sample heated with the heating rate of 200 °C/min than in the one heated with 20 °C/min; (iii) formation of Fe2B phase at 500 °C during heating with the 200 °C/min heating rate is confirmed by the HREM investigations. The aforementioned results prelude the ultrarapid annealing process for Fe-based soft magnetic ribbons being interesting and prospective from the scientific and application point of view. Moreover, we have examined the microstructure of Fe67Co20B13 ribbons after heat treatment performed under various conditions: (1) 370 °C/60 s, (2) 410 °C/30 s, and (3) 485 °C/2 s. These results were then correlated with the coercivity values. It was found that the annealing at the higher temperature (485 °C) for a very short time (2 s) provides a fine, homogenous microstructure resulting in lower coercivity Hc = 20.5 A/m and magnetic induction of B > 1.5 T. Further tests, including structural and magnetic studies, are needed to optimize the ultrarapid annealing process of this material.

Author Contributions

Conceptualization, A.K.-B., M.K., and W.M.; investigation, A.W., W.M., R.C., P.C., M.K., L.H., M.S.; P.Z., and P.W.; writing—original draft preparation, A.W., W.M.; writing—review and editing, W.M.; supervision, A.K.-B. All authors have read and agreed to the published version of the manuscript.

Funding

This research was founded by National Centre for Research and Development (POLAND) within the frame of project no TECHMATSTRATEG/347200/11/NCBR/2017.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Hou, Y.; Sellmyer, D.J. Magnetic Nanomaterials: Fundamentals, Synthesis and Applications; John Wiley & Sons: Hoboken, NJ, USA, 2017; ISBN 978-3-527-34134-4. [Google Scholar]
  2. Gavrila, H.; Ionita, V. Crystalline and amorphous soft magnetic materials and their applications—Status of art and challenges. J. Optoelectron. Adv. Mater. 2002, 4, 173–192. [Google Scholar]
  3. Herzer, G. Modern soft magnets: Amorphous and nanocrystalline materials. Acta Mater. 2013, 61, 718–734. [Google Scholar] [CrossRef]
  4. Inoue, A.; Shen, B.; Koshiba, H.; Kato, H.; Yavari, A.R. Cobalt-based bulk glassy alloy with ultrahigh strength and soft magnetic properties. Nat. Mater. 2003, 2, 661–663. [Google Scholar] [CrossRef] [PubMed]
  5. Yoshizawa, Y.; Oguma, S.; Yamanchi, K. New Febased soft magnetic alloys composed of ultrafine grain structure. J. Appl. Phys. 1998, 64, 6044–6046. [Google Scholar] [CrossRef]
  6. Kong, F.; Shen, B.; Mahino, A.; Inoue, A. Enhancement of soft magnetic properties of FeCoNbB nanocrystalline alloys with Cu and Ni additions. Thin Solid Films 2011, 519, 8280–8282. [Google Scholar] [CrossRef]
  7. Dong, C.; Inoue, A.; Wang, X.H.; Kong, F.L.; Zanaeva, E.N.; Wang, F.; Bazlov, A.I.; Zhu, S.L.; Li, Q. Soft magnetic properties of Fe82-83B14-15Si2C0.5-1 amorphous alloys with high saturation magnetization above 1.7 T. J. Non-Cryst. Solids 2018, 500, 173–180. [Google Scholar] [CrossRef]
  8. Sharma, P.; Zhang, X.; Zhang, Y.; Makino, A. Atomic packing and diffusion in Fe85Si2B9P4 amorphous alloy analyzed by ab initio molecular dynamics simulation. J. Appl. Phys. 2015, 117, 17B705. [Google Scholar]
  9. Akase, Z.; Aizawa, S.; Shindo, D.; Sharma, P.; Makino, A. In-situ Lorentz microscopy of Fe85Si2B8P4Cu1 nanocrystalline soft magnetic alloys. J. Magn. Magn. Mater. 2015, 375, 10–14. [Google Scholar] [CrossRef]
  10. Herzer, G. Soft magnetic nanocrystalline materials. Scr. Metall. Mater. 1995, 33, 1741–1756. [Google Scholar] [CrossRef]
  11. Herzer, G. Nanocrystalline Soft Magnetic Materials. Phys. Scr. 1993, 1993, 307. [Google Scholar] [CrossRef]
  12. Hsiao, A.; McHenry, M.E.; Laughlin, D.E.; Kramer, M.J.; Ashe, C.; Ohkubo, T. The Thermal, Magnetic, and Structural Characterization of the Crystallization Kinetics of Fe88Zr7B4Cu1, an Amorphous Soft Magnetic Ribbon. IEEE Trans. Magn. 2002, 38, 3039–3044. [Google Scholar] [CrossRef]
  13. Pradeep, K.G.; Herzer, G.; Choi, P.; Raabe, D. Atom probe tomography study of ultrahigh nanocrystallization rates in FeSiNbBCu soft magnetic amorphous alloys on rapid annealing. Acta Mater. 2014, 68, 295–299. [Google Scholar] [CrossRef]
  14. Zhang, Z.; Sharma, P.; Makino, A. Role of Si in high Bs and low core-loss Fe85.2B10−XP4Cu0.8SiX nano-crystalline alloys. J. Appl. Phys. 2012, 112, 103902. [Google Scholar] [CrossRef]
  15. Suzuki, K.; Makino, A.; Inoue, A.; Masumoto, T. Low core losses of nanocrystalline Fe–M–B (M = Zr, Hf, or Nb) alloys. J. Appl. Phys. 1993, 74, 3316–3322. [Google Scholar] [CrossRef]
  16. Cao, C.C.; Zhu, L.; Meng, Y.; Zhai, X.B.; Wang, Y.G. Atomic level structural modulation during the structural relaxation and its effect on magnetic properties of Fe81Si4B10P4Cu1 nanocrystalline alloy. J. Magn. Magn. Mater. 2018, 456, 274–280. [Google Scholar] [CrossRef]
  17. Ohta, M.; Yoshizawa, Y. Effect of Heating Rate on Soft Magnetic Properties in Nanocrystalline Fe80.5Cu1.5Si4B14 and Fe82Cu1Nb1Si4B12 Alloys. Appl. Phys. Express 2009, 2, 023005. [Google Scholar] [CrossRef]
  18. Herzer, G. Grain structure and magnetism of nanocrystalline ferromagnets. IEEE Trans. Magn. 1989, 25, 3327–3329. [Google Scholar] [CrossRef]
  19. Zhang, Y.; Sharma, P.; Makino, A. Sintered magnetic cores of high Bs Fe84.3Si4B8P3Cu0.7 nano-crystalline alloy with a lamellar microstructure. J. Appl. Phys. 2014, 115, 17A322. [Google Scholar] [CrossRef]
  20. Sato, K.; Takenaka, K.; Makino, A.; Hirotsu, Y. Direct imaging of structural heterogeneity of the melt-spun Fe85.2Si2B8P4Cu0.8 alloy. AIP Adv. 2015, 5, 067166. [Google Scholar] [CrossRef] [Green Version]
  21. Sharma, P.; Zhang, X.; Zhang, Y.; Makino, A. Competition driven nanocrystallization in high Bs and low coreloss Fe–Si–B–P–Cu soft magnetic alloys. Scr. Mater. 2015, 95, 3–6. [Google Scholar] [CrossRef]
  22. Han, Y.; Inoue, A.; Kong, F.L.; Chang, C.T.; Shu, S.L.; Shalaan, E.; Al-Marzouki, F. Softening and good ductility for nanocrystal-dispersed amorphous Fe–Co–B alloys with high saturation magnetization above 1.7 T. J. Alloys Compd. 2016, 657, 237–245. [Google Scholar] [CrossRef]
  23. Stergioudis, G.; Ivanov, G.; Polychroniadis, E.K. Evolution of Crystallization of the FeCoB Amorphous Alloys. Phys. Status Solidi 1991, 124, 393–399. [Google Scholar] [CrossRef]
  24. Chulist, R.; Straka, L.; Seiner, H.; Sozinov, A.; Schell, N.; Tokarski, T. Branching of {110) twin boundaries in five-layered Ni-Mn-Ga bent single crystals. Mater. Des. 2019, 171, 107703. [Google Scholar] [CrossRef]
  25. Kulik, T.; Sevage, H.T.; Hernando, A. A high-performance hysteresis loop tracer. J. Appl. Phys. 1993, 73, 6855–6857. [Google Scholar] [CrossRef]
Figure 1. (a) High-energy X-ray diffraction pattern and (b) differential scanning calorimetry curve recorded during heating for as-spun Fe67Co20B13 ribbon.
Figure 1. (a) High-energy X-ray diffraction pattern and (b) differential scanning calorimetry curve recorded during heating for as-spun Fe67Co20B13 ribbon.
Materials 13 01639 g001
Figure 2. Bright-field (BF) images (a,c) and selected area diffraction patterns (SADPs) (b,d) for as-spun Fe67Co20B13 ribbon.
Figure 2. Bright-field (BF) images (a,c) and selected area diffraction patterns (SADPs) (b,d) for as-spun Fe67Co20B13 ribbon.
Materials 13 01639 g002
Figure 3. High-resolution transmission electron microscopy (HRTEM) image and fast Fourier transform (FFT), and an inverse fast Fourier transform (IFFT) taken from crystalline (1) as well as amorphous (2) regions of as-spun Fe67Co20B13 ribbon.
Figure 3. High-resolution transmission electron microscopy (HRTEM) image and fast Fourier transform (FFT), and an inverse fast Fourier transform (IFFT) taken from crystalline (1) as well as amorphous (2) regions of as-spun Fe67Co20B13 ribbon.
Materials 13 01639 g003
Figure 4. Set of BF microstructures recorded for the samples in-situ heated at 200 °C/min.
Figure 4. Set of BF microstructures recorded for the samples in-situ heated at 200 °C/min.
Materials 13 01639 g004
Figure 5. Electron diffractions patterns obtained at different temperatures for samples heated in situ with a heating rate of 200 °C/min.
Figure 5. Electron diffractions patterns obtained at different temperatures for samples heated in situ with a heating rate of 200 °C/min.
Materials 13 01639 g005
Figure 6. Set of BF microstructures recorded at different temperatures during in situ heating at 20 and 200 °C/min and the corresponding histograms of crystallite size distribution.
Figure 6. Set of BF microstructures recorded at different temperatures during in situ heating at 20 and 200 °C/min and the corresponding histograms of crystallite size distribution.
Materials 13 01639 g006
Figure 7. HREM, FFT, and IFFT images of the sample in situ heated up to a temperature of 500 °C with a heating rate of 200 °C/min.
Figure 7. HREM, FFT, and IFFT images of the sample in situ heated up to a temperature of 500 °C with a heating rate of 200 °C/min.
Materials 13 01639 g007
Figure 8. High-energy X-ray diffraction patterns of heat treated Fe67Co20B13 ribbons.
Figure 8. High-energy X-ray diffraction patterns of heat treated Fe67Co20B13 ribbons.
Materials 13 01639 g008
Figure 9. Set of BF images and corresponding SADPs for Fe67Co20B13 ribbons heat-treated under various conditions: 370 °C/60 s (a), (b), (c), 410 °C/30 s (d), I, (f), and 485 °C/2 s (g), (h), (i).
Figure 9. Set of BF images and corresponding SADPs for Fe67Co20B13 ribbons heat-treated under various conditions: 370 °C/60 s (a), (b), (c), 410 °C/30 s (d), I, (f), and 485 °C/2 s (g), (h), (i).
Materials 13 01639 g009
Figure 10. HRTEM image, FFT, and IFFT images taken from the (1) amorphous region and (2) α-(Fe,Co) crystallite for Fe67Co20B13 heat-treated at 485 °C/2 s.
Figure 10. HRTEM image, FFT, and IFFT images taken from the (1) amorphous region and (2) α-(Fe,Co) crystallite for Fe67Co20B13 heat-treated at 485 °C/2 s.
Materials 13 01639 g010
Figure 11. Microstructure (BF images) and B-H curves for Fe67Co20B13 ribbons heat-treated at 370 °C/60 s (a), 410 °C/30 s (b), and 485 °C/2 s (c), show the change of hysteresis loops with the microstructural evolution of ribbons.
Figure 11. Microstructure (BF images) and B-H curves for Fe67Co20B13 ribbons heat-treated at 370 °C/60 s (a), 410 °C/30 s (b), and 485 °C/2 s (c), show the change of hysteresis loops with the microstructural evolution of ribbons.
Materials 13 01639 g011

Share and Cite

MDPI and ACS Style

Wojcik, A.; Maziarz, W.; Kowalczyk, M.; Chulist, R.; Szlezynger, M.; Czaja, P.; Hawelek, L.; Zackiewicz, P.; Wlodarczyk, P.; Kolano-Burian, A. Fe-Co-B Soft Magnetic Ribbons: Crystallization Process, Microstructure and Coercivity. Materials 2020, 13, 1639. https://doi.org/10.3390/ma13071639

AMA Style

Wojcik A, Maziarz W, Kowalczyk M, Chulist R, Szlezynger M, Czaja P, Hawelek L, Zackiewicz P, Wlodarczyk P, Kolano-Burian A. Fe-Co-B Soft Magnetic Ribbons: Crystallization Process, Microstructure and Coercivity. Materials. 2020; 13(7):1639. https://doi.org/10.3390/ma13071639

Chicago/Turabian Style

Wojcik, Anna, Wojciech Maziarz, Maciej Kowalczyk, Robert Chulist, Maciej Szlezynger, Pawel Czaja, Lukasz Hawelek, Przemyslaw Zackiewicz, Patryk Wlodarczyk, and Aleksandra Kolano-Burian. 2020. "Fe-Co-B Soft Magnetic Ribbons: Crystallization Process, Microstructure and Coercivity" Materials 13, no. 7: 1639. https://doi.org/10.3390/ma13071639

APA Style

Wojcik, A., Maziarz, W., Kowalczyk, M., Chulist, R., Szlezynger, M., Czaja, P., Hawelek, L., Zackiewicz, P., Wlodarczyk, P., & Kolano-Burian, A. (2020). Fe-Co-B Soft Magnetic Ribbons: Crystallization Process, Microstructure and Coercivity. Materials, 13(7), 1639. https://doi.org/10.3390/ma13071639

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop