Next Article in Journal
Controlled Atmosphere Brazing of 3003 Aluminum Alloy Using Low-Melting-Point Filler Metal Fabricated by Melt-Spinning Technology
Previous Article in Journal
Correlation between Nonlinear Optical Effects and Structural Features of Aurone-Based Methacrylic Polymeric Thin Films
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Transport and Electrochemical Properties of Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2 Composites

1
Institute of Solid State Chemistry and Mechanochemistry, SB RAS, Kutateladze Str. 18, 630128 Novosibirsk, Russia
2
Mechanical Engineering Department, Novosibirsk State Technical University, 630071 Novosibrsk, Russia
*
Author to whom correspondence should be addressed.
Materials 2022, 15(17), 6079; https://doi.org/10.3390/ma15176079
Submission received: 11 July 2022 / Revised: 25 August 2022 / Accepted: 29 August 2022 / Published: 1 September 2022
(This article belongs to the Section Energy Materials)

Abstract

:
The study demonstrates that the introduction of the electrochemically inactive dielectric additive Li2TiO3 to LTO results in a strong decrease in the grain boundary resistance of LTO-Li2TiO3 (LTC) composites at a low concentration of Li2TiO3. With the increase in the concentration of Li2TiO3 in LTC composites, the grain boundary resistance goes through a minimum and increases again due to the growth of the insulation layer of small Li2TiO3 particles around LTO grains. For LTO-TiO2 (LTT) composites, a similar effect was observed, albeit not as strong. It was found that LTC composites at low concentration of Li2TiO3 have unusually high charge–discharge capacity exceeding the theoretical value for pure LTO. This effect is likely to be caused by the occurrence of the electrochemical activity of Li2TiO3 in the vicinity of the interfaces between LTO and Li2TiO3. The increase in the capacity may be qualitatively described in terms of the model of two-phase composite in which there is the interface layer with a high capacity. Contrasting with LTC composites, in LTT composites, no capacity enhancement was observed, which was likely due to a noticeable difference in crystal structures of LTO and TiO2 preventing the formation of coherent interfaces.

1. Introduction

Lithium titanate batteries (LTBs), which use lithium titanate Li4Ti5O12 (LTO) as the anode material, open up new possibilities for the energy storage of lithium-ion batteries (LIBs) with a number of economical as well as ecological aspects. These batteries are characterized by relatively fast recharge, low internal resistance, high charge and discharge rates, long cycle life, high reliability and safety. At present, Toshiba, YABO and Altair Nanotechnologies produce LTBs for electric vehicles and energy storage. Research on LTO-based materials began about 30 years ago to replace graphite as the negative electrode in LIBs [1,2]. LTO is already known to be crystallized in cubic syngony (space group Fd-3m) and have AB2O4 spinel structure presented as Li[Li1/6Ti5/6]2O4. The volume change of the unit cell associated with insertion/extraction of lithium in/out Li4 + xTi5O12 (0 < x < 3) is very small (~0.2%). Therefore, Li4Ti5O12 is regarded as a zero-strain material for lithium insertion that offers high stability during cycling (up to 10,000 cycles) without significant loss of capacity [3,4,5]. High potential plateau around 1.55 V (vs. Li+/Li°), exceeds the reduction potential of most electrolyte solvents, and thus avoids the formation of lithium dendrites on the anode surface. This ensures the safety of LIB with an LTO anode, in contrast to LIB with a graphite anode [4,5,6,7]. However, the main limitation for the wide practical use of LTO is poor electronic and ionic conductivity, which, according to various reports, ranges from 10−13 to 10−7 S cm−1 [8,9,10].
Heterogeneous doping is one of the most promising approaches to materials modification. This approach makes it possible to obtain composite solid electrolytes with high ionic conductivity [11,12,13,14]. The introduction of heterogeneous additives can lead not only to improved charge-discharge characteristics, but also to an increase in the specific capacity of the electrode material. As Krajewski et al. (2016) reported, CV and EIS measurements show an increase in Li+ chemical diffusion coefficient values with increasing the amount of Ag nanoparticles in the LTO powder up to 3% wt. [15]. Galvanostatic charge/discharge studies (Krajewski et al., 2017) demonstrate the enhanced electrochemical properties of Li4Ti5O12 powder after its modification with Ag–Cu nanoparticles mixture, namely ca. 12.5% increase in specific capacity retention and ca. 19 mAh g−1 increases in specific capacity at a current rate of 10 C were observed [16]. The authors suggest the reason of improved electrochemical properties to be surface activation through contact with conductive nanoparticles, which leads to an increase in the electrochemically active electrode surface as well as in the reaction rate. Dielectric phases can also be used as heterogeneous additives for doping electrode materials. It was recently discovered that LTO-based composite electrode materials with additives of the electrochemically inert phase Li2TiO3 have better electrochemical characteristics compared to pure LTO-based anode material [17,18].
The phase β-Li2TiO3 with monoclinic structure (space group C2/c) is the most studied modification of Li2TiO3 [19,20]. The values of the specific discharge capacity of β-Li2TiO3 depend on the particle size or the discharge rate. For micrometer-sized Li2TiO3 particles, the discharge capacity is about 12–15 mAh g−1 for the first five discharge cycles [21,22]. The specific discharge capacity of nanofibers on the first cycle is 18.77 mAh g−1 [21]. Large capacity loss on the first cycle and less strong but continuous decrease in capacity on the next 10 cycles indicates that Li2TiO3 is electrochemically inactive, and its reversible capacity can be neglected.
Nevertheless, the addition of Li2TiO3 as a structurally compatible dopant to LTO [17,18] demonstrates not only a better rate capability but also higher specific discharge capacities (216 mAh g−1 at 0.1 C and 194 mAh g−1 at 0.5 C) as compared to LTO (175 mAh g−1) [23]. As Li2TiO3 is an electrochemically inert material, the authors (Li et al., 2017; Bhatti et al., 2016) suggest that Li2TiO3 inclusions could improve the lithium ion conductivity of the composite nanofibers and, in addition, enable intercalating of more lithium ions to the interfaces of the composite nanofibers which can be considered as additional lithium storage sites [23,24].
In this study, LTO-Li2TiO3 and LTO-TiO2 composites have been chosen as systems for studying the electrophysical and electrochemical properties. Both composites were obtained by solid-phase synthesis by changing the Li/Ti ratio. In the case of Li excess, the Li2TiO3 phase is formed as an additional phase, and in the case of Ti excess the composites contain TiO2 phase.

2. Materials and Methods

2.1. Synthesis

The samples of LTO, LTO-Li2TiO3 and LTO-TiO2 composites were synthesized by solid-state reaction. As the initial reagents, Li2CO3 (Chemical grade, Rare Metals Plant Inc., Novosibirsk, Russia) and TiO2 (rutile, Chemical grade, Interkhim Inc., Novosibirsk, Russia) powders were used. For the synthesis of LTO, LTO-TiO2 and LTO-Li2TiO3 composites the initial reagents were taken in amount corresponding to different atomic ratio to Li:Ti. The final products of synthesis obtained at the Li:Ti ratios equal to 2.8:5, 3.2:5, 3.6:5, 4:5, 4.2:5, 4.4:5, 4.6:5, 4.8:5 and 5.2:5 were denoted as LTT-3, LTT-2, LTT-1, LTO, LTC-05, LTC-1, LTC-15, LTC-2 and LTC-3, respectively. The initial reagents were preliminarily mixed in agate mortar and then mechanically treated in a high-energy planetary mill AGO-2 in steel jars by steel balls (diameter 8 mm) for 5 min at a rate of 400 rpm. Prior milling of a small portion of the mixture was milled in order to line surfaces of the jar and the balls with the treated material in order to avoid possible contamination of the treatment products by the wearing material from the jar and balls. After treatment, the mixtures were pressed into pellets and annealed at 950 °C for 5 h.

2.2. Characterization

Phase identification of the prepared samples was carried out by X-ray diffraction (XRD) using a D8 Advance powder diffractometer (Bruker) in Θ-Θ -geometry under Bragg–Brentano focusing with CuKα radiation source and a one-dimensional Lynx-Eye detector with a nickel filter. The ICDD-PDF2 database was used for phase identification. Quantitative phase analysis and refinement of the structure parameters were performed by the Rietveld method using the Topas 4.2 program.
The morphology of the LTC samples was studied by high-resolution transmission electron microscopy (HREM) on a dual-corrected transmission electron microscope Themis Z (Thermo Fisher Scientific) with an accelerating voltage of 200 kV and a limiting resolution of 0.07 nm and 0.06 nm.
To study the transport properties and ionic conductivity, the test samples were compressed into the pellets at 20 MPa and sintered at 950 °C for 5 h in air. Silver paste electrodes were deposited on the surfaces of the pellets. Electrical measurements were carried out in air in the temperature range from 35 to 250 °C in forevacuum in a stepwise isothermal mode using a HP-4284A Precision LCR Meter in the frequency range of 30 Hz–1 MHz.
To identify electrochemical properties, 80 wt.% of active material under study, 6 wt.% of carbon black, 4 wt.% of nanotubes, and 10 wt.% of PVDF binder were mixed and dispersed in N-methylpyrrolidone (NMP) to form slurry. Copper foil 15 μm in thickness was coated with the resulting slurry and dried in a vacuum oven at 120 °C overnight. The total loading of the film coating was approximately 1.5–2 mg cm−2. The coated foils were punched into 8 mm diameter disks to obtain the working electrode, and dried at 120 °C overnight under vacuum before being placed in the glovebox for cell assembling. The electrolyte used was a mixture (1:1 by mass) of1 M LiPF6 solution in ethylene carbonate (EC) and dimethylcarbonate (DMC). The electrodes were assembled inside a dry glovebox chamber into coin cell of the CR2032 type with the metallic lithium counter electrode. Charge/discharge curves were recorded on ACK 2.5.10.1 analyzer in the galvanostatic mode at various current densities between 1.0 and 2.5 V (vs. Li+/Li°).

3. Results

3.1. Structural Studies

Figure 1 shows the XRD patterns of LTO, LTC-2 and LTT-2 composites, corresponding to the two-phase systems Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2, respectively. The content of the impurity phases β-Li2TiO3 or TiO2 depends on the relative amount of lithium in the initial mixture. The excess Li content (atomic ratio of Li/Ti > 4/5) produces a two-phase system Li4Ti5O12-Li2TiO3 as shown in Figure 1 b whose patterns include overlapping XRD peaks of monoclinic β-Li2TiO3 (ICDD-33-0831) Figure 1 a and cubic Li4Ti5O12 (ICDD-49-0207) Figure 1 c. If lithium is deficient (atomic ratio of Li/Ti < 4/5), two-phase systems Li4Ti5O12-TiO2 as shown in Figure 1 d are formed when the impurity phase is rutile TiO2 with orthorhombic structure (ICDD-21-1276) (Figure 1e).
The Li2TiO3 and TiO2 phases concentrations in the composites determined from the XRD profiles were 4.6; 9.7; 16.4; 19.7 and 28.4 wt.% for LTC-05, LTC-1, LTC-15, LTC-2 and LTC-3 composites and 11.6 and 20.3 wt.% for LTT-1 and LTT-2 composites, respectively. These values correlate well with the calculated data presented in Table 1.
Thus, composites with a certain percentage of the additional phase can be obtained by changing the deviation from the stoichiometric ratio Li:Ti = 4:5. Figure 2 shows a detailed part of the XRD patterns in the 2θ range from 41 to 44°. It is clearly seen that by increasing or decreasing the Li content in the initial reagents, it is possible to obtain the final product with a given content of impurity phase of a certain type, which is confirmed by calculations performed by the Rietveld method.

3.2. Ionic Conductivity

The electrical properties of the synthesized materials were studied through the method of impedance spectroscopy. For the analysis of the impedance spectra at the temperature range from 35 to 250 °C the equivalent circuit was proposed as shown in Figure 3.
The circuit includes three impedances connected in series related to the impedance of the bulk material, Zb, the grain boundary impedance Zgb, and the electrode impedance Ze. Each element of the circuit corresponds to a different stage of ion transport or polarization in the material. Bulk impedance and grain boundary impedances include two elements: resistance (Rb and Rgb) and constant phase element (CPEb and CPEgb). The electrode impedance is described by the constant angle element CPEe, a special case of which is the Warburg impedance. The volume resistance of the sample is related to the value of the volume conductivity, σb, by the ratio σb = 1/Rb (d/S), where d is the pellet thickness and S is the electrode area. The value of the bulk conductivity is described by the Arrhenius equation:
σ b = A b T exp ( E b k T )
The grain boundary resistance Rgb can be represented as σgb = 1/Rgb·(d/S), where σgb is a parameter which has the dimension of conductivity and also obeys the Arrhenius dependence:
σ g b = A g b T exp ( E g b k T )
The CPEb, CPEgb, and CPEe values are defined by the equations
C P E b = Y b ( i ω ) α b
C P E g b = Y g b ( i ω ) α g b
C P E e = Y e ( i ω ) α e
where Yb, Ygb and Ye are constants; αb, αgb and αe are the exponents (0 < αb, αgb, αe < 1) and ω is the angular A.C. frequency. Empirically, it was found that the best agreement between theoretical and experimental data is observed assuming that CREb values depend on temperature according to the expression:
Y g b = Y g b T exp ( ( 1 α g b ) E g b k T )
The reasons for this dependence remain unclear and require additional theoretical analysis which is beyond the scope of this study. The expression for the Warburg impedance was used as the electrode impedance, i.e., it was assumed that in all cases αe = 0.5.
Thus, 11 independent parameters were used to fit the theoretical dependencies (1–6) to the experimental data in the temperature range 35–250 °C: Ab, Eb, εb, Yb, αb, Agb, Egb, εgb, Ygb, αgb, Ye. The data obtained at 30 different A.C. frequencies in the frequency range of 30 Hz–1 MHz at 20–30 temperatures, i.e., a total of 600–900 experimental points, were used for the analysis. Fitting was performed using Mathcad 11.0 and UTCMathcad 15.0 software.
Typical fitting results are demonstrated in Figure 4a,c,e for samples LTO, LTC-1 and LTT-1, respectively. Figure 4b,d,f show some Nyquist plots for these samples. The numerical values of the equivalent circuit parameters obtained by fitting are shown in Table 2. The first element of the equivalent circuit, Zb, describing the transport of ions through the volume of the material, is characterized by the volume conductivity with the activation energy Eb = 0.47–0.53 eV. This value of the activation energy agrees well with the calculated data presented in the papers [25,26]. The value of LTO bulk conductivity at room temperature determined in this work (1.8 × 10–8 S cm−1) is within the range reported in the literature: from 8 × 10–10 [27] to 7.6 × 10–8 S cm−1 [28]. The low conductivity values can be explained by the absence of vacancies in positions 8a and interstitial lithium ions in positions 16c of the spinel structure. The second element of the equivalent circuit, describing the process of ion transport across grains surfaces, is characterized by the grain boundary resistance Rgb with the activation energy Egb = 0.90–1.1 eV. This process is limited by the contribution of the grain boundary resistance to the total impedance of the sample. At a high temperature, the electrode polarization effect described by CPEe is observed, indicating a predominantly ionic character of conductivity.
The conductivity measured at direct current (assuming negligibly small electrode impedance contribution), σdc = (σb−1 + σgb−1)−1, at low temperatures is determined by the value σgb. This value, determined by the grain boundary resistance, depends on the particle size of the samples, the density of the pellet, and the presence of impurities adsorbed on the grain’s surfaces. The addition of a small amount of Li2TiO3 to the LTO leads to a decrease in grain boundary resistance and an increase in values σgb. Despite the difference in the symmetry of the crystal structures, LTO and Li2TiO3 compounds have similar chemical and physical characteristics, their densities at room temperature differ by 1.5%. Consequently, the adhesion between LTO and Li2TiO3 can be expected to be strong, and a good interface contact is formed between the components during sintering of their mixture. In this case, at the LTO/Li2TiO3 interface, additional point defects may form due to interface interaction accompanied by the transfer of cations from one phase to another. Similar processes are characteristic of composite solid electrolytes [12,13].
As a result, the concentration of charge carriers near the interface increases, which leads to a decrease in the grain boundary resistance (or to an increase in σgb values) for LTC-1, LTC-2 samples. When the concentration of Li2TiO3 increases, small particles of the dielectric phase Li2TiO3 accumulate around LTO particles leading to an increase in the resistance of the grain boundaries and a decrease in the values of σgb. A similar effect is observed in LTT composites, but the relative effect of intergrain resistance reduction in these composites is lower compared to LTC composites.

3.3. Electrochemical Properties

In order to investigate the influence of the Li2TiO3 and TiO2 additives on the electrochemical properties of LTC and LTT composites, charge-discharge experiments were carried out. Figure 5 shows the charge-discharge curves for the samples under study measured at different charge/discharge rates in the potential range 1.0–2.5 V (vs. Li+/Li°). Charge-discharge curves for LTO have a plateau at the potential range of 1.55–1.6 V, corresponding to the reversible electrochemical reaction [29]:
Li4Ti5O12 + 3Li+ + 3e↔ Li7Ti5O12
The theoretical value of the electrochemical capacity for this process is 175 mAh g−1. The experimental values of average voltage and specific discharge capacity for the LTO sample obtained in this work at a discharge rate of 0.1 C are 1.6 V and 166 mAh g−1, respectively. Such values are typical for anode materials based on LTO when measured in the voltage range above 1 V (vs. Li+/Li°).
The theoretical value of the change–discharge capacitance of the two-phase composite can be obtained for the case when the electrochemical reaction proceeds independently for each component. In this case one can use the sum rule and obtain a linear relationship for the specific capacity related to the mass of the composite, Qth measured in [mAh g−1]:
Q t h = ( 1 w ) Q 1 0 + w Q 2 0
where w is the mass fraction of the impurity phase, Q 1 0 and Q 2 0 are the values of the theoretical capacity of individual compounds, LTO and heterogeneous impurity, respectively, in the potential range under study.
The choice of the correct values for the theoretical capacity of Q 1 0 and Q 2 0 depends on the values of the voltage range in which the charge–discharge curves are obtained. When operating in a wider voltage range (below 1 V vs. Li+/Li°), the discharge curves for pure LTO show an additional plateau at 0.5 V, leading to higher theoretical capacitance values. In the present work, we do not extend the potential range beyond the voltages below 1 V (vs. Li+/Li°), so a value of 175 mAh g−1 was taken as the theoretical value of Q10. The charge-discharge curves for the Li2TiO3 compound also show a broad plateau in the voltage region of 0.2–1.5 V (vs. Li+/Li°), which is observed in the nanostructured samples and is characterized by the theoretical capacity value of 170–200 mAh g−1 [30]. However, in the region of voltages above 1 V (vs. Li+/Li°), used in the present study, the experimental values of Li2TiO3 specific capacity obtained at low charge/discharge rates do not exceed 15 mAh g−1 [17,18]. It suggests that pure Li2TiO3 should be electrochemically inert material. In respect to TiO2, the ordinary crystalline state of TiO2 is known to intercalate only a few amounts of Li. The theoretical value of the capacity of TiO2 rutile does not exceed 15 mAh g−1 [31,32,33], which is close to the corresponding value for Li2TiO3. Therefore, in further calculations it was assumed that the theoretical value of the specific capacity of heterogeneous impurity for both Li2TiO3 and TiO2 is approximately equal to Q 2 0 = 15 mAh g−1.
Figure 6a shows the variation of the capacity with the mass fraction of the additives in the LTC and LTT composites in comparison with the theoretical relationship, Equation (8). As seen, the capacitance of composites should monotonically decrease with increasing concentration of the additive, Li2TiO3 or TiO2. Nevertheless, at low concentrations of Li2TiO3 the capacity of LTO-Li2TiO3 (LTC) composites markedly increases, reaching a value of 187 mAh g−1 which exceeds the theoretical value of the capacity of pure LTO (175 mAh g−1). With further increase in the concentration of Li2TiO3 additive, the capacity of composites LTO-Li2TiO3 decreases to the values expected from Equation (8). In contrast to LTO-Li2TiO3 composites, the discharge capacity of LTO-TiO2 composites monotonically decreases with increasing TiO2 concentration in good agreement with the theoretical dependence (8).

4. Discussion

Thus, the effect of increasing the specific capacity reported earlier [23,24] is fully confirmed by the results of the present study. This effect is typical only for the LTO-Li2TiO3 system. The additional contribution of LTO/Li2TiO3 interfaces provides additional sites for the introduction of lithium cations during electrochemical cycling. The effect can only be explained by a sharp increase in the partial capacitance of Li2TiO3 in the composite, which is caused by the interface interaction between Li2TiO3 and LTO and leads to the formation of coherent interfaces (due to a structural similarity) and appearance of the electrochemical activity of Li2TiO3 in the composite. The grain size (more correctly, the size of the coherent regions) of LTO and Li2TiO3, determined using the Rietveld full-profile analysis, are 500 and 80 nm, respectively, large particles of LTO are surrounded by smaller Li2TiO3 grains. High-resolution electron microscopy study showed that in LTC composites Li2TiO3 phase is located near the surfaces of large LTO crystallites. Figure 7 shows electron microscopy image of the Li2TiO3/LTO interface. It is seen that crystal lattices of the adjacent phases coherently stacks without visible defects, pores and cracks.
Let us assume that the composite consists of cubic LTO particles with the size of L covered by a layer of the second phase Li2TiO3 with the thickness of l as shown in Figure 8. In the vicinity of the LTO/Li2TiO3 interfaces there is a layer of the electrochemically active Li2TiO3 phase having a higher specific capacity with a characteristic thickness of λ. In such approximation, the volume fraction of Li2TiO3 monotonically increases with the thickness of the Li2TiO3 phase. When the concentration of Li2TiO3 is small (at l ≤ λ) practically all volume of this phase gets into the interface region. At higher concentrations (at l > λ) only part of Li2TiO3 phase remains electrochemically active.
Then, the volume fractions of LTO, Li2TiO3 and the interface phase of Li2TiO3, f1, f2 and fS can be estimated using dimensionless parameters α = λ/L and β = λ/L, respectively, as follows:
f 1 = ( 1 2 α 1 + 2 α ) 3
f 2 = 1 ( 1 2 α 1 + 2 α ) 3
f S = f 2   ( at   α     β ) ;   f S = ( 1 + 2 β 1 + 2 α ) 3 ( 1 1 + 2 α ) 3   ( at   α   >   β )  
The volume fractions of all the phases can be calculated varying the thickness of the Li2TiO3 phase, l, (or the parameter α) from zero to infinity at the fixed value of the interface thickness λ (or the parameter β). Mass fractions of the phases can be calculated using relations:
w 1 = ρ 1 f 1 ρ 1 f 1 + ρ 2 f 2 ;   w = ρ 2 f 2 ρ 1 f 1 + ρ 2 f 2 ;   w S = ρ 2 f S ρ 1 f 1 + ρ 2 f 2
where p1 and p2 are densities of the LTO and Li2TiO3, respectively; the density of the interface phase is supposed to be similar to one for Li2TiO3 phase. The theoretical value of the charge-discharge capacity may be represented in the equation:
Q t h = ( 1 w ) Q 1 0 + ( w w S ) Q 2 0 + w S Q S 0
where Q S 0 is the theoretical value for pure interface phase of Li2TiO3. Equation (13) differs from Equation (8) by the presence of the additional term wS Q S 0 , corresponding to the contribution of the interfaces (formally regarded as the interface phase) to the overall capacity of the material. In first approximation as a highest limit for the Q S 0 value, one can assume that during charge/discharge this interface phase of Li2TiO3 may be converted into the limiting composition of Li3TiO3 corresponding to the specific charge/discharge capacity of 244 mAh g−1, remaining electrochemically inactive outside the interface region. From the values L = 500 nm or 60 nm, p1 = 3.4 g cm−3; p2 = 4.0 g cm−3 and assuming that λ = 6 nm and Q S 0 = 244 mAh g−1, one can obtain theoretical dependences Qth = f(w), Equation (13), for the LTC composites with maxima qualitatively describing experimental values. It is clear that at low concentrations both theoretical and experimental data exceed the values predicted by Equation (8) and correspond to an upper limit of capacitance for ordinary mixture of the components. Figure 6 also shows that decrease in the grain size of LTO should lead to an increase in the capacitance and the shift of the capacitance maximum to the higher concentration of Li2TiO3 in the composites. This is the tendency for the composites obtained earlier by electro-spinning method with the LTO grain size of 60 nm [23]. In general, the model provides a rather good fit at low concentrations of Li2TiO3, whereas at high w experimental capacity values decrease, possibly, due to diffusion limitations.
Besides high capacity, LTC composites at low concentration of Li2TiO3 have a better cycling rate and stability compared to LTO as shown in Figure 6a. This effect is caused by the higher ionic conductivity of the composites, as demonstrated in the impedance measurements above. Due to a strong difference in crystal structures of LTO and TiO2, no strong interface interaction takes place in LTT composites. As a result, no additional increase in the electrochemical capacity and much less decrease in the grain boundary resistance is observed in these composites. At high concentration of Li2TiO3 the grain boundary resistance becomes high again and it leads to the decrease in the capacity as mentioned above.
No effect of the capacity enhancement is observed in LTT composites even at low concentration of the TiO2 dopant. The reason appears to be negligible contribution of interfaces to the overall capacity of the composite. This fact may be explained by weak interface interaction between LTO and TiO2 due to a strong structure discrepancy between the phases.

5. Conclusions

Samples of pure Li4Ti5O12 (LTO) with stoichiometric ratio of Li:Ti = 4:5 and composites LTO-Li2TiO3 (LTC) and LTO-TiO2 (LTT) with excess amount of Li (Li:Ti > 4:5) and deficient in Li (Li:Ti > 4:5), respectively, can be prepared and investigated by X-ray diffraction, impedance spectroscopy and electrochemical charge-discharge techniques. This study shows that introduction of electrochemically inactive dielectric materials Li2TiO3 and TiO2 to lithium titanium oxide LTO results in two non-trivial interrelated effects:
(i)
A strong decrease in the grain boundary resistance of LTC composites at low concentration of Li2TiO3. The effect may be caused by easy formation of coherent interfaces between structurally similar phases Li2TiO3 and LTO leading to redistribution of lithium ions in the vicinity of the interfaces. With the increase of the concentration of Li2TiO3 in LTC composites, the grain boundary resistance goes through a minimum and increases again due to growth insulation layer of small Li2TiO3 particles around LTO grains. For LTT composites, a similar effect was observed, albeit not as strong.
(ii)
Unusually high charge–discharge capacity of LTC composites at a low concentration of electrochemically inactive phase Li2TiO3 exceeding the theoretical value for pure LTO. This effect is likely to be caused by the appearance of the electrochemical activity of Li2TiO3 in the composite. This effect results from the interface interaction between LTO and Li2TiO3 taking place due to formation of coherent interfaces between structurally similar phases. The increase in the capacity may be qualitatively described in terms of a two-phase composite model with the interface layer of a high capacity. In addition, LTC composites have a better cycling rate and stability compared to LTO. This effect is caused by a higher ionic conductivity of the composites, as demonstrated in the impedance measurements above. Due to a noticeable difference in crystal structures of LTO and TiO2, no strong interface interaction occurs in LTT composites.
Both effects are closely interrelated, and their primary reason seems to be the influence of interfaces on the physical properties of the components of the composite, namely, on its transport properties and the electrochemical capacitance. This should be common and may be observed in different composite electrode materials containing components with similar crystal structures.

Author Contributions

Conceptualization, N.U. and A.K.; experimental, A.K. and A.U.; writing-review and editing, N.U. and A.K. All authors have read and agreed to the published version of the manuscript.

Funding

This research was supported by the State Assignment of ISSCM SB RAS, (project 121032500065-5).

Informed Consent Statement

Informed consent was obtained from all subjects.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Lu, J.; Chen, Z.; Pan, F.; Cui, Y.; Amine, K. High-Performance Anode Materials for Rechargeable Lithium-Ion Batteries. Electrochem. Energy Rev. 2018, 1, 35–53. [Google Scholar] [CrossRef]
  2. Ferg, E.; Gummow, R.J.; Kock, A.; Thackeray, M. Spinel anode for lithium-ion batteries. J. Electrochem. Soc. 1994, 11, L147. [Google Scholar] [CrossRef]
  3. Colbow, M.; Dahn, J.R.; Haering, R.R. Structure and electrochemistry of the spinel oxides LiTi2O4 and Li4/3Ti5/3O4/K. J. Power Sources 1989, 26, 397–402. [Google Scholar] [CrossRef]
  4. Sun, Y.-K.; Jung, D.-J.; Lee, Y.S.; Nahm, K.S. Synthesis and electrochemical characterization of spinel Li[Li(1-x)/3CrxTi(5-2x)/3]O4 anode materials. J. Power Sources 2004, 125, 242–245. [Google Scholar] [CrossRef]
  5. Murphy, D.W.; Cava, R.J.; Zahurak, S.M.; Santoro, A. Ternary LixTiO2 phases from insertion reactions. Solid State Ion. 1983, 9, 413–418. [Google Scholar] [CrossRef]
  6. Shu, J. Electrochemical behavior and stability of Li4Ti5O12 in a broad voltage window. J. Solid State Electrochem. 2009, 13, 1535–1539. [Google Scholar] [CrossRef]
  7. Borghols, W.J.H.; Wagemaker, M.; Lafont, U.; Kelder, E.M.; Mulder, F.M. Size effects in the Li4+xTi5O12 spinel. J. Am. Chem. Soc. 2009, 131, 17786–17792. [Google Scholar] [CrossRef]
  8. Pelegov, D.V.; Slautin, B.N.; Gorshkov, V.S.; Zelenovskiy, P.S.; Kiselev, E.A.; Kholkin, A.L.; Shur, V.Y. Raman spectroscopy, «big data», and local heterogeneity of solid state synthesized lithium titanate. J. Power Sources 2017, 346, 143–150. [Google Scholar] [CrossRef]
  9. Shen, L.; Ding, B.; Nie, P.; Cao, G.; Zhang, X. Advanced Energy-Storage Architectures Composed of Spinel Lithium Metal Oxide Nanocrystal on Carbon Textiles. Adv. Energy Mater. 2013, 3, 1484–1489. [Google Scholar] [CrossRef]
  10. Wolfenstine, J.; Lee, U.; Allen, J.L. Electrical conductivity and rate-capability of Li4Ti5O12 as a function of heat-treatment atmosphere. J. Power Sources 2006, 154, 287–289. [Google Scholar] [CrossRef]
  11. Wagner, J.B., Jr. High Conductivity Conductors: Solid Ionic Conductors; Takahashi, T., Ed.; World Scientific: Singapore, 1989; p. 102. [Google Scholar]
  12. Maier, J. Ionic conduction in space charge regions. J. Prog. Solid State Chem. 1995, 23, 171–263. [Google Scholar] [CrossRef]
  13. Uvarov, N.F. Composite solid electrolytes: Recent advances and design strategies. J. Solid State Electrochem. 2011, 15, 367–389. [Google Scholar] [CrossRef]
  14. Liang, C.C. Conduction Characteristics of the Lithium Iodide-Aluminum Oxide Solid Electrolytes. J. Eleetrochem. Soc. Electrochem. Sci. Technol. 1973, 120, 1289–1292. [Google Scholar] [CrossRef]
  15. Krajewski, M.; Hamankiewicz, B.; Czerwinski, A. Voltammetric and impedance characterization of Li4Ti5O12/n-Ag composite for lithium-ion batteries. Electrochim. Acta. 2016, 219, 277–283. [Google Scholar] [CrossRef]
  16. Krajewski, M.; Hamankiewicz, B.; Michalska, M.; Andrzejczuk, M.; Lipinska, L.; Czerwinski, A. Electrochemical properties of lithium–titanium oxide, modified with Ag–Cu particles, as a negative electrode for lithium-ion batteries, J. RSC Adv. 2017, 7, 52151–52164. [Google Scholar] [CrossRef]
  17. Wang, Y.; Zhou, A.; Dai, X.; Feng, L.; Li, J. Solid-state synthesis of submicron-sized Li4Ti5O12/Li2TiO3 composites with rich grain boundaries for lithium ion batteries. J. Power Sources 2014, 266, 114–120. [Google Scholar] [CrossRef]
  18. Masoud, E.; Indrisb, S. Block-shaped pure and doped Li4Ti5O12 containing a high content of a Li2TiO3 dual phase: An anode with excellent cycle life for high rate performance lithium-ion batteries. RSC Adv. 2015, 5, 108058–108066. [Google Scholar] [CrossRef]
  19. Dorrian, J.F.; Newnham, R.E. Refinement of the structure of Li2TiO3. Mater. Res. Bull. 1969, 4, 179–183. [Google Scholar]
  20. Laumann, A.; Fehr, K.T.; Wachsmann, M.; Holzapfel, M.; Iversen, B.B. Metastable formation of low temperature cubic Li2TiO3 under hydrothermal conditions—Its stability and structural properties. Solid State Ion. 2010, 181, 1525–1529. [Google Scholar] [CrossRef]
  21. Lakshmi-Narayana, A.; Hussain, O.; Mauger, A.; Julien, C.M. Transport Properties of Nanostructured Li2TiO3 Anode Material Synthesized by Hydrothermal Method. Sci 2019, 1, 56. [Google Scholar] [CrossRef]
  22. Tabuchi, M.; Nakashima, A.; Shigemura, H.; Ado, K.; Kobayashi, H.; Sakaebe, H.; Tatsumi, K.; Kageyama, H.; Nakamurab, T.; Kanno, R. Fine Li(4-x)/3Ti (2-2x)/3FexO 2 (0.18 < x < 0.67) powder with cubic rock-salt structure as a positive electrode material for rechargeable lithium batteries. J. Mater. Chem. 2003, 13, 1747–1757. [Google Scholar] [CrossRef]
  23. Li, J.; Guo, J.; Ma, Q.; Yang, Y.; Dong, X.; Yang, M.; Yu, W.; Wang, J.; Liu, G. Electrospun Li4Ti5O12/Li2TiO3 composite nanofibers for enhanced high-rate lithium ion batteries. J. Solid State Electrochem. 2017, 21, 2779–2790. [Google Scholar] [CrossRef]
  24. Bhatti, H.; Anjum, D.; Ullah, S.; Ahmed, B.; Habib, A.; Karim, A.; Hasanain, S.K. Electrochemical Characteristics and Li+ Ion Intercalation Kinetics of Dual-Phase Li4Ti5O12/Li2TiO3 Composite in the Voltage Range 0−3 V. J. Phys. Chem. C. 2016, 120, 9553–9561. [Google Scholar] [CrossRef]
  25. Hayashi, S.; Hatano, H. Ionic Conduction of Li2Ti3O7 and Li4Ti5O12. J. Ceram. Soc. Jpn. 1994, 102, 378–382. [Google Scholar] [CrossRef]
  26. Leonidov, I.A.; Leonidova, O.N.; Perelyaeva, L.A.; Samigullina, R.F.; Kovyazina, S.A.; Patrakeyev, M.V. Structure, Ionic Conduction, and Phase Transformations in Lithium Titanate Li4Ti5O12. Phys. Solid State 2003, 45, 2079–2084. [Google Scholar] [CrossRef]
  27. Zhong, Z.; Ouyang, C.; Shi, S.; Lei, M. Ab initio Studies on Li4+xTi5O12 Compounds as Anode Materials for Lithium-Ion Batteries. J. ChemPhysChem. 2008, 9, 2104–2108. [Google Scholar] [CrossRef]
  28. Wilkening, M.; Amade, R.; Iwaniak, W.; Heitjans, P. Ultraslow Li diffusion in spinel-type structured Li4Ti5O12. Phys. Chem. Chem. Phys. 2007, 9, 1239–1246. [Google Scholar] [CrossRef]
  29. Wolfenstine, J.; Allen, J.L. Electrical conductivity and charge compensation in Ta doped Li4Ti5O12. J. Power Sources 2008, 180, 582–585. [Google Scholar] [CrossRef]
  30. Xiea, Y.; Wanga, Q.; Gua, F.; Daia, K.; Shuia, M.; Shua, J. The electrochemical properties and intercalation mechanism of low strain Li2TiO3 as a high-performance anode material for lithium-ion batteries. J. Alloys Compd. 2021, 893, 162348–162360. [Google Scholar] [CrossRef]
  31. Koudriachova, M.; Harrison, N.; Leeuw, S. Effect of Diffusion on Lithium Intercalation in Titanium Dioxide. Phys. Rev. Letters 2001, 86, 1275–1278. [Google Scholar] [CrossRef]
  32. Hu, Y.; Kienle, L.; Guo, Y.; Maier, J. High Lithium Electroactivity of Nanometer-Sized Rutile TiO2. Adv. Mater. 2006, 18, 1421–1426. [Google Scholar] [CrossRef]
  33. Baudrin, E.; Cassaignon, S.; Koelsch, M.; Jolivet, J.-P.; Dupont, L.; Tarascon, J.-M. Structural evolution during the reaction of Li with nano-sized rutile type TiO2 at room temperature. Electrochem. Commun. 2007, 337–342. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of samples synthesized at different ratios of Li:Ti in the initial mixtures: composite (b) LTC-2 (Li:Ti = 4.8:5), (c) single phase LTO (Li:Ti = 4.0:5) and (d) LTT-2 composite (Li:Ti = 3.2:5) in comparison with the patterns of pure phases (a) Li2TiO3 and (e) TiO2 (rutile).
Figure 1. XRD patterns of samples synthesized at different ratios of Li:Ti in the initial mixtures: composite (b) LTC-2 (Li:Ti = 4.8:5), (c) single phase LTO (Li:Ti = 4.0:5) and (d) LTT-2 composite (Li:Ti = 3.2:5) in comparison with the patterns of pure phases (a) Li2TiO3 and (e) TiO2 (rutile).
Materials 15 06079 g001
Figure 2. The sections of XRD patterns showing both the reflections of LTO and the impurity phase in the pure LTO sample and (a) in LTC-1, LTC-2, LTC-3 and (b) LTT-1, LTT-2, LTT-3 composites.
Figure 2. The sections of XRD patterns showing both the reflections of LTO and the impurity phase in the pure LTO sample and (a) in LTC-1, LTC-2, LTC-3 and (b) LTT-1, LTT-2, LTT-3 composites.
Materials 15 06079 g002
Figure 3. The equivalent circuit used to interpret the results of electrical measurements.
Figure 3. The equivalent circuit used to interpret the results of electrical measurements.
Materials 15 06079 g003
Figure 4. Temperature dependences of the real part of conductivity, measured at different frequencies (indicated in the plots) (a,c,e) and Nyquist plots (b,d,f) obtained at temperatures 188–190 °C for LTO, LTC-1 and LTT-1 samples. Dots are experimental values; lines are theoretical curves obtained as a result of fitting.
Figure 4. Temperature dependences of the real part of conductivity, measured at different frequencies (indicated in the plots) (a,c,e) and Nyquist plots (b,d,f) obtained at temperatures 188–190 °C for LTO, LTC-1 and LTT-1 samples. Dots are experimental values; lines are theoretical curves obtained as a result of fitting.
Materials 15 06079 g004aMaterials 15 06079 g004b
Figure 5. The charge-discharge curves obtained for the studied samples in the region of potentials 1.0–2.5 V (vs. Li+/Li°) at the 2-nd cycle at different charge/discharge rates. Corresponding dQ/dU vs. U curves are presented in the upper plot for (a) LTO, (b) LTC-1, (c) LTC-2 and (d) LTT-1 samples.
Figure 5. The charge-discharge curves obtained for the studied samples in the region of potentials 1.0–2.5 V (vs. Li+/Li°) at the 2-nd cycle at different charge/discharge rates. Corresponding dQ/dU vs. U curves are presented in the upper plot for (a) LTO, (b) LTC-1, (c) LTC-2 and (d) LTT-1 samples.
Materials 15 06079 g005
Figure 6. The variation of the discharge capacity as a function of the mass fraction of the additive (a) and the discharge rate (b) in LTC and LTT composites. Points are experimental values obtained at the rate of 0.1C in the present work (black, magenta and green points for LTO, LTC and LTT composites, respectively) as well as data (orange points) reported earlier for LTC composites in the paper [23]. Red and green lines are guides for eyes to visualise experimental data for LTC and LTT composites. Blue line corresponds to the theoretical dependences obtained from Equation (8) and magenta lines were obtained using Equation (13) for two values of the LTO grain size: L = 500 nm or 60 nm with parameters λ = 6 nm, Q 1 0 = 175 mAh g−1, Q 2 0 = 15 mAh g−1 and Q S 0 = 244 mAh g−1.
Figure 6. The variation of the discharge capacity as a function of the mass fraction of the additive (a) and the discharge rate (b) in LTC and LTT composites. Points are experimental values obtained at the rate of 0.1C in the present work (black, magenta and green points for LTO, LTC and LTT composites, respectively) as well as data (orange points) reported earlier for LTC composites in the paper [23]. Red and green lines are guides for eyes to visualise experimental data for LTC and LTT composites. Blue line corresponds to the theoretical dependences obtained from Equation (8) and magenta lines were obtained using Equation (13) for two values of the LTO grain size: L = 500 nm or 60 nm with parameters λ = 6 nm, Q 1 0 = 175 mAh g−1, Q 2 0 = 15 mAh g−1 and Q S 0 = 244 mAh g−1.
Materials 15 06079 g006
Figure 7. An HRTEM image obtained from the near-surface area of the LTC composite particle. Lines correspond to the crystallographic planes (200) of LTO and (400) or (−313) planes of Li2TiO3. The interface position is roughly indicated by a dotted line.
Figure 7. An HRTEM image obtained from the near-surface area of the LTC composite particle. Lines correspond to the crystallographic planes (200) of LTO and (400) or (−313) planes of Li2TiO3. The interface position is roughly indicated by a dotted line.
Materials 15 06079 g007
Figure 8. A simplified model of the LTO-Li2TiO3 composite.
Figure 8. A simplified model of the LTO-Li2TiO3 composite.
Materials 15 06079 g008
Table 1. The calculated values of relative concentrations of components in composites.
Table 1. The calculated values of relative concentrations of components in composites.
SampleAtomic Ratio Li:TiMass Fraction of TiO2 or Li2TiO3Volume Fraction of TiO2 or Li2TiO3
LTT-32.8:50.2720.235
LTT-23.2:50.1790.152
LTT-13.6:50.0880.074
LTO4:500
LTC-054.2:50.0400.032
LTC-14.4:50.0790.064
LTC-154.6:50.1170.097
LTC-24.8:50.1550.129
LTC-35.2:50.2300.194
Table 2. Numerical values of the equivalent circuit parameters obtained by fitting.
Table 2. Numerical values of the equivalent circuit parameters obtained by fitting.
ImpedanceParameters of the Equivalent CircuitSample
LTOLTC-1LTC-2LTC-3LTT-1LTT-3
ZbAb, S·K·cm−17 × 1022 × 1032 × 1036 × 1030.5 × 1031.2 × 103
Eb,eV0.470.480.480.530.480.48
CPEb, S·cm−1·(Hz)αb3 × 10−119 × 10−105 × 10−101 × 10−114 × 10−121.5 × 10−10
αb0.60.50.40.60.650.5
ZgbAgb, S·K·cm−12.0 × 1055.7 × 1065.6 × 1063.3 × 1071.6 × 1063.7 × 106
Egb, eV0.970.900.901.020.980.91
CPEgb, S·cm−1·(Hz)αgb3 × 10−61.2 × 10−42.4 × 10−49 × 10−72.2 × 10−58 × 10−4
αgb0.850.770.750.910.800.71
ZeCPEe, S·cm−1·(Hz)αgb4 × 10−88 × 10−78 × 10−73.5 × 10−71.1 × 10−75 × 10−7
αe0.50.50.50.50.50.5
σbat 25 °C, S·cm−13 × 10−85 × 10−85 × 10−82 × 10−84 × 10−81 × 10−8
σdc at 25 °C, S·cm−1 *2 × 10−131 × 10−111 × 10−111 × 10−136 × 10−125 × 10−13
* Calculated from the Arrhenius relation.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Kozlova, A.; Uvarov, N.; Ulihin, A. Transport and Electrochemical Properties of Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2 Composites. Materials 2022, 15, 6079. https://doi.org/10.3390/ma15176079

AMA Style

Kozlova A, Uvarov N, Ulihin A. Transport and Electrochemical Properties of Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2 Composites. Materials. 2022; 15(17):6079. https://doi.org/10.3390/ma15176079

Chicago/Turabian Style

Kozlova, Anna, Nikolai Uvarov, and Artem Ulihin. 2022. "Transport and Electrochemical Properties of Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2 Composites" Materials 15, no. 17: 6079. https://doi.org/10.3390/ma15176079

APA Style

Kozlova, A., Uvarov, N., & Ulihin, A. (2022). Transport and Electrochemical Properties of Li4Ti5O12-Li2TiO3 and Li4Ti5O12-TiO2 Composites. Materials, 15(17), 6079. https://doi.org/10.3390/ma15176079

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop