Next Article in Journal
Method for an Effective Selection of Tools and Cutting Conditions during Precise Turning of Non-Alloy Quality Steel C45
Next Article in Special Issue
A Data-Driven Approach for Studying the Influence of Carbides on Work Hardening of Steel
Previous Article in Journal
Organic Nanoparticles Based on D-A-D Small Molecule: Self-Assembly, Photophysical Properties, and Synergistic Photodynamic/Photothermal Effects
Previous Article in Special Issue
The Positive Role of Nanometric Molybdenum–Vanadium Carbides in Mitigating Hydrogen Embrittlement in Structural Steels
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Substantial Improvement of High Temperature Strength of New-Generation Nano-Oxide-Strengthened Alloys by Addition of Metallic Yttrium

1
Institute of Physics of Materials, Czech Academy of Sciences, Žižkova 22, 616 62 Brno, Czech Republic
2
Faculty of Electrical Engineering, University of West Bohemia, Univerzitni 8, 306 14 Pilsen, Czech Republic
*
Author to whom correspondence should be addressed.
Materials 2022, 15(2), 504; https://doi.org/10.3390/ma15020504
Submission received: 9 December 2021 / Revised: 5 January 2022 / Accepted: 5 January 2022 / Published: 10 January 2022

Abstract

:
Oxide-dispersion-strengthened (ODS) Fe-Al-Y2O3-based alloys (denoted as FeAlOY) containing 5 vol. % of nano-oxides have a potential to become top oxidation and creep-resistant alloys for applications at temperatures of 1100–1300 °C. Oxide dispersoids cause nearly perfect strengthening of grains; thus, grain boundaries with limited cohesive strength become the weak link in FeAlOY in this temperature range. One of the possibilities for significantly improving the strength of FeAlOY is alloying with appropriate elements and increasing the cohesive strength of grain boundaries. Nearly 20 metallic elements have been tested with the aim to increase cohesive strength in the frame of preliminary tests. A positive influence is revealed for Al, Cr, and Y, whereby the influence of Y is enormous (addition of 1% of metallic Y increases strength by a factor of 2), as it is presented in this paper.

1. Introduction

The application of advanced materials with excellent oxidation and high-temperature creep resistance enables an increase in operating temperature of heat engines and, thus, an increase in efficiency with a positive impact on the environment. Top-level metallic materials with the best creep performance are represented by Ni-based superalloy single crystals [1] that are applicable up to 1100 °C and by oxide-dispersion-strengthened (ODS) ferritic alloys [2,3] applicable up to 1300 °C. In both cases, excellent creep resistance is achieved by the Orowan mechanism due to the dispersion of particles effectively prohibiting dislocation motion at high temperatures.
Classical ferritic ODS alloys are strengthened by 0.5% volume fraction of very stable Y-based nano-oxides typically of 5–20 nm in size [4]. The ferritic matrix of classical ODS alloys allows dissolving a rather high amount of Al (up to 10%, note: wt. % is used in all notation), which stabilizes bcc lattice and excludes transformation of ferrite to austenite.
Classical ODS alloys are usually produced in two steps. In the first step, a homogeneous powder consisting of a matrix with dispersed nano-sized Y2O3 is produced by mechanical alloying (MA). In the second step, the powder is consolidated via hot extrusion, hot isostatic pressing, spark plasma sintering, or via their combinations [5,6,7,8,9,10,11]. Auger et al. [12] applied hot cross rolling to improve the resistance of 14YWT ODS alloys against radiation. Zhang et al. [13] used hot rolling to improve the strength of Fe–9Cr-0.06C-1.5W-0.5Ti-0.18Si-0.35Y2O3 ODS alloys after hot consolidation. Kumar et al. [14] investigated mechanical properties of Fe-18Cr-2W-0.2Ti-xY2O3 alloys consolidated from MA powder by forging. Zhou et al. [15] applied combinations of forging, cold rolling, hot rolling, and annealing to ODS310 alloys. However, incomplete secondary recrystallization results in inhomogeneous bimodal grain size distribution causing brittle cracking along grain boundaries in ODS alloys [16]. All these methods of consolidation and subsequent thermomechanical treatment are complicated and expensive.
A new-generation of ODS Fe-Al-Y2O3-based alloys (denoted as FeAlOY) containing a high-volume fraction of oxides of about 5%, which is one order of magnitude higher than in classical ODS alloys [3,17], has been developed by the authors. The consolidation by hot rolling results in ultra-fine-grained (UFG) microstructure due to dynamic recrystallization. Such a material is hard and brittle at room temperature and soft and ductile at 1100–1300 °C. The coarse-grained microstructure obtained by full secondary recrystallization is the key factor for acquiring excellent creep strength. However, several ODS alloys studied in the available literature do not meet this requirement (see, e.g., [16]). Our recent experiments clearly indicate that UFG microstructure after unsuccessful secondary recrystallization or incomplete secondary recrystallization in ODS alloys causes its creep strength to reach only a fraction of the creep strength of completely recrystallized ODS alloys. Furthermore, expensive ODS alloys are often studied and applied at loading conditions for which much cheaper and better substitutes exist. One could recommend limiting studies and applications of ODS alloys to temperatures and loading conditions at which the properties of ODS alloys are really exceptional.
Recent tensile testing at low strain rates (10−6 s−1) and creep tests at 1100 °C have revealed that strengthening the matrix by nano-oxide dispersion is very effective due to the Orowan mechanism. Under loading corresponding to 60–70% of the strength determined by the tensile test, the creep strain rate is practically unmeasurable (<10−9 s−1), and the time to fracture reaches several thousands of hours. Then, the grain boundaries with limited cohesive strength become weak links in FeAlOY at 1100–1300 °C. One of the possibilities for significantly improving the strength of the FeAlOY is alloying appropriate elements and, thus, increasing the cohesive strength of grain boundaries. Nearly 20 metallic elements have been tested with the aim to increase cohesive strength within the preliminary study (unpublished results). The study reveals that the cohesive strength of grain boundaries increases with the content of Al and, thus, the content of Al in FeAlOY is fixed to 10%, which is the solubility limit of Al in ferrite at low temperatures. Such a high content of Al ensures excellent oxidation resistance [18] as well as a significant decrease in density to 6.5 g/cm3. The role of alloying with Cr seems to be at least neutral and may open quite interesting possibilities. Thus, it must be investigated in combination with other alloying elements in more detail in the near future.
Originally, the addition of metallic Y to FeAlOY has been motivated by an improvement in the stability of oxide dispersion against coarsening because pure Y2O3 oxide is chemically more stable than mixed (Al,Y)2O3 oxides; therefore, it is more resistant against coarsening [3]. As a certain amount of O is introduced into FeAlOY by using powders naturally oxidized at the surface for FeAlOY production, it is necessary to compensate O by the addition of metallic Y to gain pure Y2O3 nanodispersoid. This is why a series of experiments on FeAlOY with different amounts of added metallic Y is performed. These tests also include tensile tests at strain rates 10−6 s−1 and 1100 °C. The study provides unprecedented results, which are presented in this paper.

2. Materials and Methods

Chemically homogeneous Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 powders with variable amounts of added metallic Y in the range of 0 to 1.75% are prepared by MA from Fe, Al, and Y2O3 powders and from Cr and Y granulates of 99.9% purity. A vacuum-tight milling container has the volume of 22 dm3 and a diameter of 400 mm; it is made from low alloyed steel and is filled with 100 martensitic bearing balls (Fe-1Cr-1C) of 40 mm diameter. A total of 1.5 kg of the powder is mechanically alloyed in a vacuum by rotation of the milling container along the horizontal axis (70 rpm). After two weeks of MA, the homogeneous powder particles consist of a solid solution with a large amount of defects, such as dislocations and vacancies [3]. More detailed powder characterization can be found in [19]. The MA powder is subsequently hot consolidated by rolling. The powder is canned in an evacuated 20/1 mm steel tube and hot consolidated by rolling in three steps to a thickness of 8 mm at 870 °C, to a thickness of 5 mm at 900 °C, and to a thickness of 3.25 mm at 900 °C. Then, the hot rolled sheet is stripped from the can and annealed at 1200 °C/4 h to provoke secondary recrystallization. The oxides nucleate and grow during hot rolling up to a size of 5 nm; then, they coarsen to 20–30 nm during annealing, provoking secondary recrystallization [20].
Flat specimens with a gauge length of 25 mm and cross section of 2.5 mm × 3.5 mm are cut by a precise electrical discharge machine from rolled sheets and grinded to P400. Tensile tests are performed by using the Zwick/Roell KAPPA DS 50 kN creep test system (Zwick/Roell, Fürstenfeld, Austria) with a furnace up to 1200 °C. Microstructures are observed by using SEM (scanning electron microscope/microscopy) Tescan Lyra 3 XMU FEG/SEMxFIB (Tescan, Brno, Czech Republic) equipped with a X-Max80 EDS detector for X-ray microanalysis and a symmetry electron backscatter diffraction (EBSD) detector with an Aztec control system (Oxford Instruments, Abingdon, UK). The X-ray diffraction (XRD) measurement is performed on a PanAnalytical Empyrean automated diffractometer in Bragg–Brentano configuration (Malvern Pananalytical Ltd., Malvern, United Kingdom), which uses a 1D detector and a cobalt lamp (λ-Kα1,2 = 1.788965, 1.792850 Å, acceleration voltage of 30 kV and current of 20 mA) with a β filter. The specimens are measured in continuous mode with steps of 0.04 2θ° from 10 to 130 degree range while they rotate. Quality and quantity are interpreted by the HighScorePlus 4.0 software, utilizing the Rietveld method and the ICSD database (2017).

3. Tensile Testing

Four specimens of each of the Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 ODS alloys with additions of 0, 0.25, 0.5, 0.75, 1, 1.25, 1.5, and 1.75% Y are prepared and mechanically tested. Tensile tests at a strain rate of 10−6 s−1 and a temperature of 1100 °C are performed on all 64 prepared specimens. The typical stress strain curves are presented in Figure 1, and the results of all tensile tests are summarized in Figure 2. From Figure 1 and Figure 2, it is evident that strength increases with increasing Y content in both Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 ODS alloys up to a certain limit; it then drops to much lower values. In the case of high strength, low ductility is observed, which indicates the existence of a significant portion of intergranular brittle fracture, and this can be explained by grain boundary decohesion. Thus, the cohesion strength of grain boundaries seems to be the weakest link in the specimens, and the strength of the specimens can be considered as a measure of the cohesive strength of the grain boundaries, provided that the grain microstructure of the specimens is similar. In order to judge this assumption, a relevant microstructure characterization by SEM is performed.

4. Microstructure Characterization

Grain microstructures are characterized by EBSD for Fe-10Al-4Y2O3 ODS alloys with 0, 1, and 1.75% Y and for Fe-10Al-4Cr-4Y2O3 ODS alloys with 0, 1.25, and 1.75% Y, and the results are presented in Figure 3. Generally, the grains after secondary recrystallization are pancake-shaped and lay on the rolling plane. The Euler color EBSD maps in Figure 3 are taken from the body of the specimen; they cover its entire thickness, while the x-axis of the map is parallel to the rolling direction, and the y-axis is normal to the rolling plane. Figure 3a–c correspond to 0%, 1%, and 1.75% of Y in Fe-10Al-4Y2O3 ODS alloys, and Figure 3d–h correspond to 0%, 1.25%, and 1.75% of Y in Fe-10Al-4Cr-4Y2O3 ODS alloys. The grain microstructures for 0% of Y (Figure 3a,d) consist of grains of a mean size of about 200 µm elongated in the rolling direction with an aspect ratio of about 2. Figure 3b,e correspond to 1% Y in Fe-10Al-4Y2O3 and 1.25% Y in Fe-10Al-4Cr-4Y2O3 ODS alloys, respectively, and they consist of very large grains of sizes that are over 1 mm elongated in the rolling direction with an aspect ratio over 2. One can also realize that the grains near the surface of the specimen are significantly finer, and there are sporadic regions without secondary recrystallization (see Figure 3e for 1.25% Y in the Fe-10Al-4Cr-4Y2O3 ODS alloy). Figure 3c depicts the Euler color EBSD map of the specimen with 1.75% Y in Fe-10Al-4Y2O3 in which no secondary recrystallization occurs during annealing and the grains are equiaxed with a mean size of about 500 nm. The Euler color EBSD map in Figure 3f corresponds to the specimen with 1.75% Y in Fe-10Al-4Cr-4Y2O3, in which the grains are not fully recrystallized and exhibit prevailing coarse-grained microstructure of sizes between 0.2 and 2 mm with islands of fine equiaxed grains with a mean size of about 500 nm (see Figure 3f,g). Moreover, the phase map reveals precipitation of Al2Y shown in Figure 3h, which is due to the excess of Y, which cannot be dissolved in the matrix. Histograms of grain areas for Fe-10Al-4Y2O3 ODS alloys with (a) 0, (b) 1, and (c) 1.75% Y and for Fe-10Al-4Cr-4Y2O3 ODS alloys with (d) 0, (e) 1.25, and (f) 1.75% Y and the values of mean aspect ratios of the grains are presented in Figure 4. It is necessary to note that although the ultra-fine-grained microstructure is equiaxed after hot rolling, it changes to rather large pancaked grains oriented in the rolling plane due to secondary recrystallization (see Figure 3a,b,d,e) and remains as slightly coarsened and equiaxed in unrecrystallized regions (see Figure 3c,g).
X-ray diffraction data are acquired in order to elucidate phase composition and lattice parameters of compounds present in the head of Fe-10Al-4Cr-4Y2O3 ODS specimen alloys with 1.25% of Y after the tensile test in the air atmosphere. The diffractogram displayed in Figure 5 shows labeled peaks of four phases (with space groups) corresponding to the bcc matrix (Im-3m) with Y2O3 (Ia-3) nanoprecipitates and to surface oxidized layer consisting of Al2O3 (R-3c) with precipitates of Y3Al5O12 YAG (Ia-d). It must be noted that the detected thin surface oxide layer ensures excellent long-term protection of the specimen against further oxidation. It must be noted that although Y2O3 nano-oxides are detected by X-ray diffraction, the evaluation of their volume fraction does not result in realistic values (5–6% as it follows from the inputs). In order to perform a significantly more precise analysis, methods based on transmission electron microscopy (TEM) must be utilized. In the case of the Fe-10Al-4Cr-4Y2O3 ODS alloy with 1.75% added Y, Al2Y (Fd-3m) precipitates are detected (see Figure 3h). In the case of Fe-10Al-4Y2O3 or Fe-10Al-4Cr-4Y2O3 ODS alloys with no or small amounts of added Y, one can expect precipitation of three types of nano-oxides—YAlO3 (YAP-Pnma), Y4Al2O9 (YAM-P21/c), and Y2O3—which deserves a separate TEM study.
An example of typical nano-oxide dispersion (practically independent of Y and Cr content) and its size distribution histogram in recrystallized grains is presented in Figure 6. The fracture mechanism of the Fe-10Al-4Cr-4Y2O3 ODS specimen alloy with 1.25 Y (with the highest strength) can be deduced from Figure 7. Here, it is clearly shown that the fracture is initiated in an unrecrystallized and much softer region in the central part of the specimen (some other unrecrystallized regions are also revealed in Figure 3e). This region can be considered as a defect, and one can expect that it could be removed by annealing at 1200 °C for a longer time than 4 h to fully complete secondary recrystallization.

5. Discussion

Y2O3 nano-oxides are extremely stable against coarsening and play a decisive role in strengthening FeAlOY up to temperatures of 1300 °C. Strengthening can be described by the Orowan theory, which allows the calculation of an increase of shear stress τ due to the presence of precipitates as τ = G b / Δ , where G is the shear modulus, b is the length of the Burgers vector, and Δ is the mean distance between precipitates. By using the values of G 40 GPa corresponding to 1100 °C (see [21] for the estimation of the temperature dependence of the elastic constants), b = a 3 / 2 0.25 nm with lattice constant a 0.29 nm and Δ 50 nm estimated from Figure 6 provide a value of τ 200 MPa , which is well above the measured strengths presented in Figure 1. This supports our hypothesis that the strength of FeAlOY is determined by the cohesive strength of grain boundaries.
The present study clearly revealed that achieving an excellent tensile and creep strength at 1100 °C and higher temperatures is conditioned by complete secondary recrystallization resulting in very coarse grains. The results shown in Figure 2 and Figure 3 clearly indicate that the strengths of specimens exhibiting no or incomplete secondary recrystallization is significantly lower than that with complete or nearly complete secondary recrystallization. In the case of unrecrystallized grain microstructure, the strength is several times lower and ductility is very high at 1100 °C (see stress-strain curve for the highest amount of Y in Figure 1a). In the case of incomplete secondary recrystallization, both tensile strength and ductility are low (see stress-strain curve for highest amount of Y in Figure 1b), which indicates that the fracture is easily initialized in soft unrecrystallized regions, as demonstrated in Figure 5.
It is still not clear why an increase of Y content behind a certain limit blocks secondary recrystallization in the Fe-10Al-4Y2O3 ODS alloy and why it only slows down secondary recrystallization in the Fe-10Al-4Cr-4Y2O3 ODS alloy. Moreover, alloying with Cr increases the tendency of ODS alloys to complete secondary recrystallization. This is a promising finding that opens the door for further significant optimization of high temperature strength of the FeAlOY by varying the chemical composition.
The results in Figure 1 and Figure 2 show an unprecedented result: alloying by about 1% of a substitutional element (Y) increases the strength by a factor of 2 at 1100 °C. The increase in strength can be attributed to the following reasons:
i.
Significant change of the grain microstructure and its morphology;
ii.
Increase in cohesive strength of the grain boundary due to a change in its chemical composition (e.g., Y segregates grain boundaries and strengthens interatomic bonds);
iii.
Change of chemical composition of the nano-oxides from mixed Al-Y oxides to pure Y oxides, which exhibit a improved wetting of the matrix; thus, the nano-oxides act as stronger clamps holding the grains together.
In any case, reason (i) is approved by this study; however, one cannot exclude that it is the only one. Reason (ii), which involves the segregation of elements at grain boundaries, can be identified by energy dispersive spectroscopy mapping in TEM. In order to test reason (iii), it is necessary to find appropriate hot consolidation conditions that provide similar grain structures in two FeAlOYs with different amounts of Y and, thus, possess different ratios of mixed Al-Y and pure Y oxides, which must be accurately characterized by TEM. The detailed analysis of this problem is a challenge for our team in the near future.

6. Conclusions

The conclusions can be summarized in the following items:
  • Two batches of Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 ODS alloys with variable amounts of added metallic Y in the range of 0 to 1.75% are prepared by mechanical alloying, hot consolidation by rolling, and annealing to provoke secondary recrystallization.
  • The amount of added metallic Y substantially influences the strength of ODS alloys determined by tensile tests at 1100 °C and a strain rate of 10−6 s−1.
  • Alloying by Y linearly increases the strength of ODS alloys up to a limit of about 1%, for which the strength increases by a factor of 2 compared to ODS alloys with no added Y. Beyond the limit, the strength drops by a factor of 6 in the case of the Fe-10Al-4Y2O3 ODS alloy and by a factor of 2 in the case of the Fe-10Al-4Cr-4Y2O3 ODS alloy.
  • Three reasons are considered for explaining the increase in strength of ODS alloys by Y alloying: (i) by significant change of the grain microstructure and its morphology, (ii) by an increase in cohesive strength of the grain boundary due to change its chemical composition, and (iii) by a change of chemical composition of nano-oxides from mixed Al-Y oxides to pure Y oxides, which exhibit improved wetting of the matrix.
  • Reason (i) (alloying by Y significantly influences the grain microstructure after annealing) explains qualitatively the behavior of the strength of ODS alloys. This, however, does not exclude the fact that reasons (ii) and (iii) do not play significant roles. Reasons (ii) and (iii) will be investigated in detail by our team in the near future.

Author Contributions

J.S., conceptualization, methodology, and writing; P.B., investigation; J.H., conceptualization, and investigation; N.L., data curation and editing; M.J., investigation; B.M., writing—review and editing, data curation, supervision, project administration; P.D., methodology. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Czech Science Foundation in the frame of Project 21-02203X.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Acknowledgments

The authors gratefully acknowledge the financial support from the Czech Science Foundation in the frame of Project 21-02203X.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Pollock, T.M.; Argon, A.S. Directional coarsening in nickel-base superalloy single crystals with high volume fraction of coherent precipitates. Acta Metall. Mater. 1994, 42, 1859–1874. [Google Scholar] [CrossRef]
  2. Oksiuta, Z. High-temperature oxidation resistance of ultrafine-grained 14% Cr ODS ferritic steel. J. Mater. Sci. 2013, 48, 4801–4805. [Google Scholar] [CrossRef] [Green Version]
  3. Material Data Sheet, INCOLOY, Alloy MA 956, INCOLOY, Alloy MA 957; Inco Alloys Limitted: Hereford, UK, 2004.
  4. Karak, S.K.; Majumdar, J.D.; Witczak, Z.; Lojkowski, W.; Ciupiński, Ł.; Kurzydłowski, K.J.; Manna, I. Evaluation of Microstructure and Mechanical Properties of Nano-Y2O3-Dispersed Ferritic Alloy Synthesized by Mechanical Alloying and Consolidated by High-Pressure Sintering. Met. Mater. Trans. A 2013, 44, 2884–2894. [Google Scholar] [CrossRef]
  5. Byun, T.S.; Yoon, J.H.; Wee, S.H.; Hoelzer, D.T.; Maloy, S.A. Fracture behavior of 9Cr nanostructured ferritic alloy with improved fracture toughness. J. Nucl. Mater. 2014, 449, 39–48. [Google Scholar] [CrossRef]
  6. Kim, J.H.; Byun, T.S.; Hoelzer, D.T.; Kim, S.W.; Lee, B.H. Temperature dependence of strengthening mechanisms in the nanostructured ferritic alloy 14YWT: Part I—Mechanical and microstructural observations. Mater. Sci. Eng. A 2013, 559, 101–110. [Google Scholar] [CrossRef]
  7. Fu, J.; Brouwer, J.C.; Richardson, I.M.; Hermans, M.J.M. Effect of mechanical alloying and spark plasma sintering on the microstructure and mechanical properties of ODS Eurofer. Mater. Des. 2019, 177, 107849. [Google Scholar] [CrossRef]
  8. Massey, C.P.; Dryepondt, S.N.; Edmondson, P.D.; Terrani, K.A.; Zinkle, S.J. Influence of mechanical alloying and extrusion conditions on the microstructure and tensile properties of Low-Cr ODS FeCrAl alloys. J. Nucl. Mater. 2018, 512, 227–238. [Google Scholar] [CrossRef]
  9. Li, J.; Wu, S.; Ma, P.; Yang, Y.; Wu, E.; Xiong, L.; Liu, S. Microstructure evolution and mechanical properties of ODS FeCrAl alloys fabricated by an internal oxidation process. Mater. Sci. Eng. A 2019, 757, 42–51. [Google Scholar] [CrossRef]
  10. Li, Z.; Lu, Z.; Xie, R.; Lu, C.; Shi, Y.; Liu, C. Effects of Y2O3, La2O3 and CeO2 additions on microstructure and mechanical properties of 14Cr-ODS ferrite alloys produced by spark plasma sintering. Fusion Eng. Des. 2017, 121, 159–166. [Google Scholar] [CrossRef]
  11. Montes, J.M.; Cuevas, F.G.; Cintas, J.; Urban, P. A One-Dimensional Model of the Electrical Resistance Sintering Process. Met. Mater. Trans. A 2015, 46, 963–980. [Google Scholar] [CrossRef]
  12. Auger, M.A.; Hoelzer, D.T.; Field, K.G.; Moody, M.P. Nanoscale analysis of ion irradiated ODS 14YWT ferritic alloy. J. Nucl. Mater. 2020, 528, 151852. [Google Scholar] [CrossRef]
  13. Zhang, G.; Zhou, Z.; Mo, K.; Miao, Y.; Xu, S.; Jia, H.; Liu, X.; Stubbins, J.F. The effect of thermal-aging on the microstructure and mechanical properties of 9Cr ferritic/martensitic ODS alloy. J. Nucl. Mater. 2019, 522, 212–219. [Google Scholar] [CrossRef]
  14. Kumar, D.; Prakash, U.; Dabhade, V.V.; Laha, K.; Sakthivel, Z. Development of Oxide Dispersion Strengthened (ODS) Ferritic Steel Through Powder Forging. J. Mater. Eng. Perform. 2017, 26, 1817–1824. [Google Scholar] [CrossRef]
  15. Zhou, Z.; Sun, S.; Zou, L.; Schneider, Y.; Schmauder, S.; Wang, M. Enhanced strength and high temperature resistance of 25Cr20Ni ODS austenitic alloy through thermo-mechanical treatment and addition of Mo. Fusion Eng. Des. 2019, 138, 175–182. [Google Scholar] [CrossRef]
  16. Pal, S.; Alam, M.E.; Maloy, S.A.; Hoelzer, D.T.; Odette, R.G. Texture evolution and microcracking mechanisms in as-extruded and cross-rolled conditions of a 14YWT nanostructured ferritic alloy. Acta Mater. 2018, 152, 338–357. [Google Scholar] [CrossRef]
  17. Bártková, D.; Šmíd, M.; Mašek, B.; Svoboda, J.; Šiška, F. Kinetic study of static recrystallization in an Fe–Al–O ultra-fine-grained nanocomposite. Phil. Mag. Lett. 2017, 97, 379–385. [Google Scholar] [CrossRef]
  18. Stratil, L.; Horník, V.; Dymáček, P.; Roupcová, P.; Svoboda, J. The influence of aluminium content on oxidation resistance of new-generation ODS alloy at 1200 °C. Metals 2020, 10, 1478. [Google Scholar] [CrossRef]
  19. Svoboda, J.; Kunčická, L.; Luptáková, N.; Weiser, A.; Dymáček, P. Fundamental Improvement of Creep Resistance of New-Generation Nano-Oxide Strengthened Alloys via Hot Rotary Swaging Consolidation. Materials 2020, 13, 5217. [Google Scholar] [CrossRef] [PubMed]
  20. Svoboda, J.; Luptáková, N.; Jarý, M.; Dymáček, P. Influence of hot consolidation conditions and Cr-alloying on microstructure and creep in new-generation ODS alloy at 1100 °C. Metals 2020, 10, 5070. [Google Scholar] [CrossRef] [PubMed]
  21. Chlupová, A.; Šulák, I.; Kunčická, L.; Kocich, R.; Svoboda, J. Microstructural aspects of new grade ODS alloy consolidated by rotary swaging. Mater. Character 2021, 181, 111477. [Google Scholar] [CrossRef]
Figure 1. The typical stress-strain curves of (a) Fe-10Al-4Y2O3 and (b) Fe-10Al-4Cr-4Y2O3 ODS alloys with addition of different amounts of Y.
Figure 1. The typical stress-strain curves of (a) Fe-10Al-4Y2O3 and (b) Fe-10Al-4Cr-4Y2O3 ODS alloys with addition of different amounts of Y.
Materials 15 00504 g001
Figure 2. Measured tensile strengths of all specimens of Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 ODS alloys with addition of different amounts of Y. Several values coincide, and they are not visible.
Figure 2. Measured tensile strengths of all specimens of Fe-10Al-4Y2O3 and Fe-10Al-4Cr-4Y2O3 ODS alloys with addition of different amounts of Y. Several values coincide, and they are not visible.
Materials 15 00504 g002
Figure 3. Euler color EBSD maps of grain microstructure for Fe-10Al-4Y2O3 ODS alloys with (a) 0, (b) 1, and (c) 1.75% Y and for Fe-10Al-4Cr-4Y2O3 ODS alloys with (d) 0, (e) 1.25, and (f,g) 1.75% Y. (h) is the phase map corresponding to (g) indicating precipitation of Al2Y (blue phase). The (g) and (h) maps correspond to a yellow rectangle in map (f).
Figure 3. Euler color EBSD maps of grain microstructure for Fe-10Al-4Y2O3 ODS alloys with (a) 0, (b) 1, and (c) 1.75% Y and for Fe-10Al-4Cr-4Y2O3 ODS alloys with (d) 0, (e) 1.25, and (f,g) 1.75% Y. (h) is the phase map corresponding to (g) indicating precipitation of Al2Y (blue phase). The (g) and (h) maps correspond to a yellow rectangle in map (f).
Materials 15 00504 g003aMaterials 15 00504 g003b
Figure 4. Histograms of grain areas for Fe-10Al-4Y2O3 ODS alloys and aspect ratios (numbers in brackets) with (a) 0% Y (2.7), (b) 1% Y (5.7), and (c) 1.75% Y (1.7) and for Fe-10Al-4Cr-4Y2O3 ODS alloys with (d) 0% Y (3.6), (e) 1.25% Y (6.7), and (f) 1.75% Y (2.5).
Figure 4. Histograms of grain areas for Fe-10Al-4Y2O3 ODS alloys and aspect ratios (numbers in brackets) with (a) 0% Y (2.7), (b) 1% Y (5.7), and (c) 1.75% Y (1.7) and for Fe-10Al-4Cr-4Y2O3 ODS alloys with (d) 0% Y (3.6), (e) 1.25% Y (6.7), and (f) 1.75% Y (2.5).
Materials 15 00504 g004aMaterials 15 00504 g004b
Figure 5. X-ray diffraction data measured on specimens’ surface after the tensile test in air atmosphere.
Figure 5. X-ray diffraction data measured on specimens’ surface after the tensile test in air atmosphere.
Materials 15 00504 g005
Figure 6. (a) The secondary electron SEM image of oxide dispersion in the section of the specimen in the grain interior of the recrystallized Fe-10Al-4Cr-4Y2O3 ODS alloy with 1.25% Y after final etching by the Vilella–Bain etchant and (b) its size distribution histogram.
Figure 6. (a) The secondary electron SEM image of oxide dispersion in the section of the specimen in the grain interior of the recrystallized Fe-10Al-4Cr-4Y2O3 ODS alloy with 1.25% Y after final etching by the Vilella–Bain etchant and (b) its size distribution histogram.
Materials 15 00504 g006
Figure 7. An Euler color EBSD map of Fe-10Al-4Cr-4Y2O3 ODS specimen with 1.25 Y showing coarse-grained microstructure and mixed trans/inter-crystalline fracture initiated in the soft unrecrystallized region.
Figure 7. An Euler color EBSD map of Fe-10Al-4Cr-4Y2O3 ODS specimen with 1.25 Y showing coarse-grained microstructure and mixed trans/inter-crystalline fracture initiated in the soft unrecrystallized region.
Materials 15 00504 g007
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Svoboda, J.; Bořil, P.; Holzer, J.; Luptáková, N.; Jarý, M.; Mašek, B.; Dymáček, P. Substantial Improvement of High Temperature Strength of New-Generation Nano-Oxide-Strengthened Alloys by Addition of Metallic Yttrium. Materials 2022, 15, 504. https://doi.org/10.3390/ma15020504

AMA Style

Svoboda J, Bořil P, Holzer J, Luptáková N, Jarý M, Mašek B, Dymáček P. Substantial Improvement of High Temperature Strength of New-Generation Nano-Oxide-Strengthened Alloys by Addition of Metallic Yttrium. Materials. 2022; 15(2):504. https://doi.org/10.3390/ma15020504

Chicago/Turabian Style

Svoboda, Jiří, Petr Bořil, Jakub Holzer, Natália Luptáková, Milan Jarý, Bohuslav Mašek, and Petr Dymáček. 2022. "Substantial Improvement of High Temperature Strength of New-Generation Nano-Oxide-Strengthened Alloys by Addition of Metallic Yttrium" Materials 15, no. 2: 504. https://doi.org/10.3390/ma15020504

APA Style

Svoboda, J., Bořil, P., Holzer, J., Luptáková, N., Jarý, M., Mašek, B., & Dymáček, P. (2022). Substantial Improvement of High Temperature Strength of New-Generation Nano-Oxide-Strengthened Alloys by Addition of Metallic Yttrium. Materials, 15(2), 504. https://doi.org/10.3390/ma15020504

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop