Next Article in Journal
Microstructure and Electrical Conductivity of Cement Paste Reinforced with Different Types of Carbon Nanotubes
Next Article in Special Issue
Corrosion Behavior of High-Strength C71500 Copper-Nickel Alloy in Simulated Seawater with High Concentration of Sulfide
Previous Article in Journal
Uncovering the Effect of Al Addition on the Hydrogen Storage Properties of the Ternary TiVNb Alloy
Previous Article in Special Issue
Effect of Air Storage on Stress Corrosion Cracking of ZK60 Alloy Induced by Preliminary Immersion in NaCl-Based Corrosion Solution
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Formation of Nanoscale Al2O3 Protective Layer by Preheating Treatment for Improving Corrosion Resistance of Dilute Fe-Al Alloys

1
Key Laboratory of Automobile Materials, Ministry of Education, School of Materials Science and Engineering, Jilin University, Changchun 130022, China
2
Otto Schott Institute of Materials Research, Friedrich Schiller University, 07743 Jena, Germany
*
Author to whom correspondence should be addressed.
Materials 2022, 15(22), 7978; https://doi.org/10.3390/ma15227978
Submission received: 1 October 2022 / Revised: 8 November 2022 / Accepted: 9 November 2022 / Published: 11 November 2022
(This article belongs to the Special Issue Corrosion and Mechanical Behavior of Metal Materials)

Abstract

:
In this work, an attempt was made to improve the corrosion resistance of dilute Fe-Al alloys (1.0 mass% Al) by preheating treatment at 1073 K in H2 atmosphere. In comparison with pure Fe and unpreheated Fe-Al alloys, the resistance to oxidation at 673 K in pure O2 and to electrochemical corrosion in 5 wt.% NaCl solution is significantly improved for preheated Fe-Al alloys. This improvement is attributed to the formation of a 20 nm thin, but dense Al2O3 protective layer on the surface of preheated Fe-Al alloys.

1. Introduction

As one of the most widely used structural materials, ferroalloys are widely utilized in vehicle engineering, the petrochemical industry, machinery manufacturing, aerospace and marine engineering [1]. In modern society, high-temperature oxidation in air and electrochemical corrosion in wet air or chemical solution are the most common ways to cause ferroalloy failure, leading to economic losses and potential security risks [2]. Consequently, the high-temperature oxidation resistance [3,4] and corrosion resistance [5,6,7,8] of ferroalloys must be considered.
For ferroalloys, the commonly used anticorrosion methods include alloying, surface coating and electroplating. Although all mentioned methods improve the oxidation resistance and the electrochemical corrosion resistance of ferroalloys, they require additional process steps that are costly, and all methods are known to cause pollution. Numerous reports on tons of pollutants caused by alloying [9,10], electroplating [11,12,13] and protective painting [14,15] that cause serious damage to the environment are available. Due to the lack of a better alternative (so far), most commonly, the resistance to the oxidation and electrochemical corrosion of Fe is increased by adding high ratios of Cr and Ni [5,6,16,17,18] which are expensive, and which also have a negative impact on the plasticity of ferroalloys [19].
In fact, Al as an alloying element has been reported to have a positive effect on the oxidation resistance and corrosion resistance of the metallic alloys including Fe [20,21,22,23,24,25,26,27]. In comparison with Cr and Ni, Al is cheap and widely available, which makes it an interesting candidate for industrial use. However, the amount of Al that can be added to Fe is limited. Contents higher than 20 wt.% seriously reduce the plasticity of ferroalloys [19]. In recent years, to address this issue, a low alloying technique combined with a preheating treatment in reducing the atmosphere has been developed for Cu-Al alloys with the additions of <3 mass% Al [20,28,29]. The increase of the oxidation resistance was attributed to the formation of a surface Al2O3 protective layer that prevents the outward diffusion of Cu as well as the inward diffusion of O. At the same time, the matrix is covered by an Al2O3 protective layer, and the matrix does not directly contact air or an aqueous solution, which greatly improves the corrosion resistance of the Cu-based alloy.
In this work, the low alloying technique combined with the preheating treatment is applied to Fe to investigate its effect on the corrosion resistance of ferroalloys. It is expected that an Al2O3 protective layer can be formed on the surface of preheated Fe-Al alloys to improve its corrosion resistance by preventing the outward diffusion of Fe and inward diffusion of O. The low Fe-Al alloy is prepared by adding 1.0 mass% Al into Fe, and the alloy is preheated in a high purity H2 atmosphere and subsequently oxidized in a pure oxygen atmosphere. The resistance of the preheated Fe-Al alloy to oxidation at 673 K in pure O2 and to electrochemical corrosion in 5 wt.% NaCl solution will be measured. Correspondingly, the surface morphology, structure and the composition of the protective layer formed on the preheated Fe-Al alloy will also be characterized.

2. Materials and Experimental Procedures

Fe-Al alloys with 1.0 mass% Al are made from pure Fe (99.999 mass%) and Al (99.9999 mass%) by repeated melting in a vacuum electric arc furnace (DHL-300, SKY Technology Development CO., Shenyang, China) with a nonconsumable electrode under a protective atmosphere (99.999% Ar). The composition is chosen below the solubility limit of Al in Fe [30]. That is, there is no intermetallic compound in the sample to ensure its processability. The sample ingots were cut and cold rolled into thin plates with a thickness of 0.5 mm, and then subjected to mechanical and electrolytic polishing, where the electrolytic polishing current is 0.5 A and the reaction time is 1 min. After that, the samples were preheated in a high purity H2 atmosphere (99.9999%) at 101,325 Pa and 1073 K for 1440 min, referred to as P-FeAl. The samples used for the oxidation experiment were stamped into a round piece with a diameter of 4 mm, and the sample used for the electrochemical corrosion experiment was cut into a rectangular piece with a length of 10 mm and a width of 20 mm. During this process, the surface of the sample is covered with high-quality sulfuric acid paper to prevent external pollution and damage to the sample.
The mass gain of the preheated sample and those control samples with pure Fe and unpreheated Fe-Al alloys (uP-FeAl) during oxidation was measured using a thermogravimetric method (METTLER 1100LF, Mettler Toledo, Switzerland). When a sample is heated to the required test temperature in the reaction gas, the increase in mass is recorded. A scanning electron microscope (SEM, JEOL, Tokyo, Japan) and Energy Dispersive X-ray Spectroscopy (EDS, JEOL, Tokyo, Japan) were used to analyze the surface. The detection of surface elements was carried out by X-ray photoelectron spectroscopy (XPS, ESCALAB 250Xi, Thermo Fisher Scientific Inc., Waltham, MA USA). Transmission electron microscopy (TEM, Jeol-NEOARM200F, Jeol, Tokyo, Japan) analysis operating at 200 kV was performed to observe the microstructure of the Al2O3 layer on the preheated Fe-Al alloy.
The corrosion resistance was assessed with an electrochemical impedance spectroscopy (EIS) and potentiodynamic polarization measurement operated by a CHI660E electrochemical workstation (SUMAT, Beijing, China). The sample was installed in an electrochemical cell and exposed to solutions of 5 wt.% NaCl for 30 min. EIS spectral were then recorded at the open circuit potential (OCP), and measured with a three-electrode configuration, consisting of the sample as the working electrode (surface area 1 cm2), a platinum gauze counter electrode and a saturated calomel electrode (SCE) as the reference electrode in a Faraday cage. The EIS experiments were conducted in the frequency range of 105 Hz to 10−2 Hz at OCP by applying 10 mV sinusoidal amplitude. Potentiodynamic polarizations were performed after 30 min exposure to solutions of 5 wt.% NaCl. The samples were polarized using a scanning rate of 10 mV/s and a scanning range of − 0.3 V (vs. OCP) ~ 0 V. The solution was open to air and not stirred during the measurement. All experiments were performed at room temperature.

3. Results and Discussion

To see the effects of the preheating treatment on the oxidation resistance of low Fe-Al alloys, the weight gain curves of pure Fe, uP-FeAl and P-FeAl recorded during oxidation at 673 K in 0.1 MPa O2 are given in Figure 1. The weight gain of pure Fe increases the fastest as the oxidation proceeds. In comparison, the weight gain of uP-FeAl is significantly lowered, but still visibly increases, meaning that uP-FeAl is also oxidized but slower than pure Fe. Interestingly, the weight gain of P-FeAl is the lowest and increases the slowest, showing that the oxidation resistance of Fe-Al alloys is significantly improved after the preheating treatment.
To further evaluate the oxidation resistance of low Fe-Al alloys after preheating, the SEM images of the surface morphology of pure Fe, uP-FeAl and P-FeAl oxidized at 673 K for 2880 min in 0.1 MPa O2 are shown in Figure 2. The micrographs of oxidized pure Fe in Figure 2a,b and uP-FeAl in Figure 2c,d show significantly rough surfaces in comparison with that of P-FeAl. Oxide whiskers grown during the oxidation fully cover the alloy surface of pure Fe and uP-FeAl. The whiskers are composed of Fe2O3 [17]. The surface of P-FeAl in Figure 2e,f is strikingly smooth without oxide grains or whiskers. The oxide morphology images support the previous results of the superior antioxidant ability of P-FeAl from the weight gain curve in Figure 1.
To evaluate the corrosion resistance of one metal or alloy, one efficient way is to provide its electrochemical corrosion diagram, where a high polarization impedance and low corrosion current mean excellent corrosion resistance [31,32,33,34,35,36,37]. In this work, the electrochemical corrosion diagram of pure Fe, uP-FeAl and P-FeAl measured in 5 wt.% NaCl solution is given in Figure 3, with the electrochemical impedance spectroscopy (EIS) diagram in (a), the potentiodynamic polarization curves in (b), and the bode and phase angle plots in (c). In Figure 3a, the EIS curve of P-FeAl has the largest diameter of the semicircle, indicating that it has the highest resistance among the three. With reference to previous studies [38], a two time-constant equivalent circuit model inserted in Figure 3a is constructed to illustrate the electrochemical impedance of a sample that is exposed to the solution of 5 wt.% NaCl. In this model, Rs represents the solution resistance between the reference electrode and working electrode, the first time-constant represents the resistance of the Al2O3 protective layer (Rc) and its capacitance (Qc), while the second one describes the electrochemical processes (corrosion) at the substrate in terms of the charge transfer resistance (Rct) and the double layer capacitance (Qdl). Using such an equivalent circuit model, the fitting result gives that the charge transfer resistance of P-FeAl (Rct = 4948 Ω) is significantly higher than those of pure Fe (Rct = 788 Ω) and uP-FeAl (Rct = 1906 Ω). In Figure 3b, the potentiodynamic polarization curve can be adopted to obtain the corrosion current by the extrapolation method. Due to this, one sees that the corrosion potential (Ecorr) of P-FeAl (Ecorr = −0.87 V) is lower than that of uP-FeAl (Ecorr = −0.81 V) and pure Fe (Ecorr = −0.86 V), and the corrosion current of P-FeAl (IP-FeAl = 9.8 µA cm−2) is significantly lower than those of pure Fe (Ipure Fe = 35.9 µA cm−2) and uP-FeAl (IuP-FeAl = 79.6 µA cm−2). Figure 3c shows the Bode and phase angle plots of P-FeAl, pure Fe and uP-FeAl. The phase angle plots show two time-constants; one is for the Al2O3 protective layer (high frequency range 103–105 Hz), the other is for the electrochemical activity at the matrix (middle frequency range 10−1–102 Hz). As for the Bode plot, it can provide the polarization resistance (Rp) from the difference in the real impedance at a lower and higher frequency [34]. In light of this, P-FeAl has the highest impedance modulus value after 30 min exposure to the 5 wt.% NaCl solution at a low frequency region. Interestingly, the Rp of P-FeAl (Rp = 6656 Ω) is considerably higher than those of pure Fe (Rp = 1157 Ω) and uP-FeAl (Rp = 2786 Ω). All these results show that P-FeAl possesses a high corrosion resistance.
In Figure 1, Figure 2 and Figure 3, the excellent corrosion resistance of P-FeAl alloys should be attributed to the preheating treatment prior to the oxidation or corrosion experiments, and a surface protective layer that be formed might be responsible for the improvement. This will be further investigated in the following.
Figure 4 shows the EDS concentration depth profiles of Fe, Al and O measured on P-FeAl. In the vicinity of the surface, the signals of Al and O are strong, but that of Fe is negligibly weak. As the distance increases, the signals of Al and O decline deeply to a low level, especially for Al, while that of Fe increases quickly up to the maximum level. The depth profiles suggest the accumulation of Al and O in the vicinity of the surface, showing that a thin protective Al2O3 layer about 20 nm thick is formed on the surface of FeAl during the preheating treatment. The aluminum oxide layer formation is originated from the outward segregation of Al to the surface vicinity. Note that the composition of the aluminum oxide layer is not exactly Al2O3 but higher in Al content. In addition to this, the profiles show further that oxygen is solved in the Fe-Al alloy, but the level is not in accordance with any stochiometric iron oxide.
To characterize the composition of the surface protective layer, Figure 5 gives the XPS pattern of the P-FeAl surface. The O 1s spectrum displayed three characteristic peaks of metal–oxygen bonds (529.7 eV for O1), defect sites with a low oxygen coordination (531.2 eV for O2), and hydroxyl groups (532.8 eV for O3), consistent with that reported in the literature [39]. A further characteristic peak appears near 74.3 eV, which comes from Al 2p, also consistent with those reported results [39,40]. These measurements suggest that an Al2O3 is formed on the surface of P-FeAl, which should be responsible for the improvement in the oxidation resistance and corrosion resistance of P-FeAl.
To observe the microstructure of the surface protective layer, a TEM cross section of P-FeAl with EDS mapping of Al, O and Fe are given in Figure 6. In the brightfield image of the surface region shown in Figure 6a, a dense aluminum oxide layer formed on the surface is visible. The mean thickness is 20 ± 5 nm. Figure 6b shows an enlarged view of (a), where the Al2O3 protective layer can be clearly observed. The Fast Fourier Transform (FFT) inset of the crystalline aluminum oxide layer in Figure 6b was indexed, using the singlecrystal® 4 software, as Al2O3 orthorhombic (SG 33) structure in [ 0   3 ¯   1 ] orientation. Undoubtedly, this Al2O3 surface layer is the key to the improvement of the corrosion resistance of P-FeAl. Figure 6d–g exhibit the EDS mapping of Fe, Al, O and Pt over the cross section of P-FeAl as (c). The accumulation of Al and O can be found in the vicinity of the surface of P-FeAl, corresponding to Figure 6. The elemental distributions confirm the formation of a thin protective Al2O3 layer on the surface of P-FeAl during the preheating treatment. It should be noted here that, in Figure 6d–g, the signals of Al and O can also be observed at the interior place of the Fe-Al base a little further away from the surface, suggesting the internal oxidation of Al in Fe during the preheating process. The internal oxidation is attributed to the solution of O in Fe as shown in Figure 4. Unfortunately, this will lead to a decrease in the actual concentration of Al in Fe, limiting further growth of the surface Al2O3 layer.

4. Conclusions

In summary, P-FeAl is prepared with dilute Fe-Al alloys (1.0 mass% Al) as a precursor through a preheating treatment in an H2 atmosphere. After the preheating treatment, P-FeAl shows excellent oxidation resistance. Compared to pure Fe and uP-FeAl, the mass gain of P-FeAl during the oxidation in 0.1 MPa O2 at 673 K for 2880 min is much lower, where almost no oxides can be observed on its surface. In the electrochemical corrosion test, P-FeAl also showed excellent electrochemical corrosion resistance with Rp = 6656 Ω and IP-FeAl = 9.8 µA cm−2, which is significantly better than pure Fe (Rp = 1157 Ω and Ipure Fe = 35.9 µA cm−2) and uP-FeAl (Rp = 2786 Ω and IuP-FeAl = 79.6 µA cm−2). These improvements are attributed to an Al2O3 protective layer about 20 nm thick, which is self-formed on the surface due to the reaction of Al outward diffusion from the inner part of the FeAl base with an O2 remnant in the annealing atmosphere during the preheating treatment. Such a thin protective Al2O3 layer can prevent the diffusion of atoms or ions through it during the corrosion process.

Author Contributions

Conceptualization, Y.Z. and C.L.; methodology, Y.Z.; software, C.L. and K.F.; validation, Y.Z., K.F. and C.L.; formal analysis, Y.Z., S.L. and C.L.; investigation, C.L.; resources, Y.Z.; data curation, C.L., K.F. and Y.T.; writing—original draft preparation, C.L. and K.F.; writing—review and editing, Y.Z., S.L. and C.L.; visualization, Y.Z. and C.L.; supervision, Y.Z. and S.L.; project administration, Y.Z. and S.L.; funding acquisition, Y.Z. and S.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China (Nos. 51871107, 52130101 and 51631004), the Natural Science Foundation of Jilin Province (No. 20200201019JC), the Top-notch Young Talent Program of China (W02070051), the Chang Jiang Scholar Program of China (Q2016064), Key scientific and technological research and development projects of Jilin Provincial Department of Science and Technology (20220201113GX), the Fundamental Research Funds for the Central Universities, the Program for Innovative Research Team (in Science and Technology) in University of Jilin Province, and the Program for JLU Science and Technology Innovative Research Team (2017TD-09). S. Lippmann acknowledges financial support of the German Research Foundation (Deutsche Forschungsgemeinschaft DFG) under Grant Nos. INST 275/3911.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

S. Lippmann thanks C. Ronning, FSU Jena for granting access to the FIB facility. The authors thank S.Y. Liu, X. Li and Z.Y. Yang for experimental work.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Qiao, Y.X.; Wang, X.Y.; Yang, L.L.; Wang, X.J.; Chen, J.; Wang, Z.B.; Zhou, H.L.; Zou, J.S.; Wang, F.H. Effect of aging treatment on microstructure and corrosion behavior of a Fe-18Cr-15Mn-0.66N stainless steel. J. Mater. Sci. Technol. 2022, 107, 197–206. [Google Scholar] [CrossRef]
  2. Liu, M.; Li, J.; Zhang, Y.X.; Xue, Y.N. Recent Advances in Corrosion Research of Biomedical NiTi Shape Memory Alloy. Rare Metal Mat. Eng. 2021, 50, 4165–4173. [Google Scholar]
  3. Raman, R.K.S. Mechanical Alloying of Elemental Powders into Nanocrystalline (NC) Fe-Cr Alloys: Remarkable Oxidation Resistance of NC Alloys. Metals 2021, 11, 695. [Google Scholar] [CrossRef]
  4. Backman, D.G.; Williams, J.C. Advanced materials for aircraft engine applications. Science 1992, 255, 1082–1087. [Google Scholar] [CrossRef] [PubMed]
  5. Aye, K.K.; Nguyen, T.D.; Zhang, J.; Young, D.J. Effect of silicon on corrosion of Fe-20Cr and Fe-20Cr-20Ni alloys in wet CO2 with and without HCl at 650 °C. Corros. Sci. 2021, 179, 109096. [Google Scholar] [CrossRef]
  6. Liu, M. Finite element analysis of pitting corrosion on mechanical behavior of E690 steel panel. Anti-Corros. Method M. 2022, 69, 351–361. [Google Scholar] [CrossRef]
  7. Gong, Y.; Young, D.J.; Kontis, P.; Chiu, Y.L.; Larsson, H.; Shin, A.; Pearson, J.M.; Moody, M.P.; Reed, R.C. On the breakaway oxidation of Fe9Cr1Mo steel in high pressure CO2. Acta Mater. 2017, 130, 361–374. [Google Scholar] [CrossRef]
  8. Liu, M. Effect of uniform corrosion on mechanical behavior of E690 high-strength steel lattice corrugated panel in marine environment: A finite element analysis. Mater. Res. Express 2021, 8, 066510. [Google Scholar] [CrossRef]
  9. Wang, F.; Shu, Y. Influence of Cr content on the corrosion of Fe-Cr alloys: The synergistic effect of NaCl and water vapor. Oxid. Met. 2003, 59, 201–214. [Google Scholar] [CrossRef]
  10. Jung, K.; Ahn, S.; Kim, Y.; Oh, S.; Ryu, W.H.; Kwon, H. Alloy design employing high Cr concentrations for Mo-free stainless steels with enhanced corrosion resistance. Corros Sci. 2018, 140, 61–72. [Google Scholar] [CrossRef]
  11. Huang, C.A.; Chang, J.H.; Chen, C.Y.; Liao, K.Y.; Mayer, J. Microstructure and electrochemical corrosion behavior of Cr-Ni-Fe alloy deposits electroplated in the presence of trivalent Cr ions. Thin Solid Films 2013, 544, 69–73. [Google Scholar] [CrossRef]
  12. Choi, Y.I.; Shin, E.S.; Kuroda, K.; Okido, M.; Park, C.J. Improved surface morphology and corrosion resistance for galvannealed coatings by pre-electroplating iron. Corros. Sci. 2012, 58, 152–158. [Google Scholar] [CrossRef]
  13. Hu, W.B.; Cai, H.L.; Yang, M.H.; Tong, X.L.; Zhou, C.M.; Chen, W. Fe-C-coated fibre Bragg grating sensor for steel corrosion monitoring. Corros Sci. 2011, 53, 1933–1938. [Google Scholar] [CrossRef]
  14. Kim, J.H.; Lee, M.H. A Study on Cavitation Erosion and Corrosion Behavior of Al-, Zn-, Cu-, and Fe-Based Coatings Prepared by Arc Spraying. J. Therm. Spray Technol. 2010, 19, 1224–1230. [Google Scholar] [CrossRef]
  15. Jeong, Y.S.; Kainuma, S.; Ahn, J.H. Structural response of orthotropic bridge deck depending on the corroded deck surface. Constr. Build Mater. 2013, 43, 87–97. [Google Scholar] [CrossRef]
  16. Yu, C.; Nguyen, T.D.; Zhang, J.; Young, D.J. Sulfur Effect on Corrosion Behavior of Fe-20Cr-(Mn, Si) and Fe-20Ni-20Cr-(Mn, Si) in CO2-H2O at 650 °C. J. Electrochem. Soc. 2015, 163, C106–C115. [Google Scholar] [CrossRef]
  17. Rao, V.S. The influence of temperature on the oxidation behaviour of Fe3AI-Fe3AlC0.69 and FeAl-Fe3AlC0.69 intermetallics. Intermetallics 2003, 11, 713–719. [Google Scholar] [CrossRef]
  18. Wei, W.; Geng, S.J.; Chen, G.; Wang, F.H. Growth mechanism of surface scales on Ni-Fe-Cr alloys at 960 degrees C in air. Corros. Sci. 2020, 173, 108737. [Google Scholar] [CrossRef]
  19. Zhang, C.-H.; Huang, S.; Shen, J.; Chen, N.-X. Structural and mechanical properties of Fe–Al compounds: An atomistic study by EAM simulation. Intermetallics 2014, 52, 86–91. [Google Scholar] [CrossRef]
  20. Hong, S.H.; Zhu, Y.F.; Mimura, K.; Isshiki, M. Role of Al2O3 layer in oxidation resistance of Cu-Al dilute alloys pre-annealed in H2 atmospheres. Corros. Sci. 2006, 48, 3692–3702. [Google Scholar] [CrossRef]
  21. Novak, P.; Nova, K. Oxidation Behavior of Fe-Al, Fe-Si and Fe-Al-Si Intermetallics. Materials 2019, 12, 1748. [Google Scholar] [CrossRef] [PubMed]
  22. Jang, P.; Shin, S.; Jung, C.S.; Kim, K.H.; Seomoon, K. Fabrication of Fe-Al nanoparticles by selective oxidation of Fe-Al thin films. Nanoscale Res. Lett. 2013, 8, 1–6. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  23. Li, H.; Zhang, J.Q.; Young, D.J. Oxidation of Fe-Si, Fe-Al and Fe-Si-Al alloys in CO2-H2O gas at 800 degrees C. Corros. Sci. 2012, 54, 127–138. [Google Scholar] [CrossRef]
  24. Xu, Y.F.; Jeurgens, L.P.H.; Bo, H.; Lin, L.C.; Zhu, S.L.; Huang, Y.; Liu, Y.C.; Qiao, J.W.; Wang, Z.M. On the competition between synchronous oxidation and preferential oxidation in Cu-Zr-Al metallic glasses. Corros. Sci. 2020, 177, 108996. [Google Scholar] [CrossRef]
  25. Pang, X.J.; Li, S.S.; Qin, L.; Pei, Y.L.; Gong, S.K. Effect of trace Ce on high-temperature oxidation behavior of an Al-Si-coated Ni-based single crystal superalloz. J. IronSteel Res. Int. 2019, 26, 78–83. [Google Scholar]
  26. Wang, X.H.; Li, F.Z.; Chen, J.X.; Zhou, Y.C. Insights into high temperature oxidation of Al2O3-forming Ti3AlC2. Corros Sci. 2012, 58, 95–103. [Google Scholar] [CrossRef]
  27. Lu, S.D.; Li, X.X.; Liang, X.Y.; Shao, W.T.; Yang, W.; Chen, J. Effect of Al content on the oxidation behavior of refractory high-entropy alloy AlMo0.5NbTa0.5TiZr at elevated temperatures. Int. J. Refract Met. H. 2022, 105, 105812. [Google Scholar] [CrossRef]
  28. Zhu, Y.F.; Mimura, K.; Isshiki, M. Oxidation mechanism of copper at 623–1073 K. Mater. Trans. 2002, 43, 2173–2176. [Google Scholar] [CrossRef] [Green Version]
  29. Ogbuji, L.U. The oxidation behavior of an ODS copper alloy Cu-Al2O3. Oxid. Met. 2004, 62, 141–151. [Google Scholar] [CrossRef]
  30. Liu, Y.X.; Yin, F.C.; Hu, J.X.; Li, Z.; Cheng, S.H. Phase equilibria of Al-Fe-Sn ternary system. T Nonferr. Metal. Soc. 2018, 28, 282–289. [Google Scholar] [CrossRef]
  31. Li, R.; Wang, S.; Zhou, D.; Pu, J.; Yu, M.; Guo, W. A new insight into the NaCl-induced hot corrosion mechanism of TiN coatings at 500 °C. Corros. Sci. 2020, 174, 108794. [Google Scholar] [CrossRef]
  32. Dafali, A.; Hammouti, B.; Mokhlisse, R.; Kertit, S. Substituted uracils as corrosion inhibitors for copper in 3% NaCl solution. Corros. Sci. 2003, 45, 1619–1630. [Google Scholar] [CrossRef]
  33. Ozcan, M.; Dehri, I.; Erbil, M. Organic sulphur-containing compounds as corrosion inhibitors for mild steel in acidic media: Correlation between inhibition efficiency and chemical structure. Appl. Surf. Sci. 2004, 236, 155–164. [Google Scholar] [CrossRef]
  34. Saha, S.K.; Banerjee, P. Introduction of newly synthesized Schiff base molecules as efficient corrosion inhibitors for mild steel in 1 M HCl medium: An experimental, density functional theory and molecular dynamics simulation study. Mater. Chem. Front. 2018, 2, 1674–1691. [Google Scholar] [CrossRef]
  35. Solmaz, R.; Kardas, G.; Culha, M.; Yazici, B.; Erbil, M. Investigation of adsorption and inhibitive effect of 2-mercaptothiazoline on corrosion of mild steel in hydrochloric acid media. Electrochim. Acta 2008, 53, 5941–5952. [Google Scholar] [CrossRef]
  36. Saha, S.K.; Dutta, A.; Ghosh, P.; Sukul, D.; Banerjee, P. Novel Schiff-base molecules as efficient corrosion inhibitors for mild steel surface in 1 M HCl medium: Experimental and theoretical approach, Phys. Chem. Chem. Phys. 2016, 18, 17898–17911. [Google Scholar] [CrossRef]
  37. Visser, P.; Terryn, H.; Mol, J.M.C. On the importance of irreversibility of corrosion inhibitors for active coating protection of AA2024-T3. Corros. Sci. 2018, 140, 272–285. [Google Scholar] [CrossRef]
  38. Xu, J.; Zhou, C.; Chen, Z.; Wang, Y.; Jiang, S. Corrosion behaviors of (Cr,Fe)3Si/Cr13Fe5Si2 composite coating under condition of synergistic effects of electrochemical corrosion and mechanical erosion. J. Alloys Compd. 2010, 496, 429–432. [Google Scholar] [CrossRef]
  39. Zhu, X.X.; Sun, M.Y.; Zhao, R.; Li, Y.Q.; Zhang, B.; Zhang, Y.L.; Lang, X.Y.; Zhu, Y.F.; Jiang, Q. 3D hierarchical self-supported NiO/Co3O4@C/CoS2 nanocomposites as electrode materials for high-performance supercapacitors. Nanoscale Adv. 2020, 2, 2785–2791. [Google Scholar] [CrossRef]
  40. van den Brand, J.; Sloof, W.G.; Terryn, H.; de Wit, J.H.W. Correlation between hydroxyl fraction and O/Al atomic ratio as determined from XPS spectra of aluminium oxide layers. Surf. Interface Anal. 2004, 36, 81–88. [Google Scholar] [CrossRef]
Figure 1. Weight gain curves of pure Fe, uP-FeAl and P-FeAl oxidized at 673 K in 0.1 MPa O2 for 120 min showing the superior oxidation resistance of preheated Fe-Al alloys.
Figure 1. Weight gain curves of pure Fe, uP-FeAl and P-FeAl oxidized at 673 K in 0.1 MPa O2 for 120 min showing the superior oxidation resistance of preheated Fe-Al alloys.
Materials 15 07978 g001
Figure 2. SEM images of surface (oxide) morphologies of pure Fe, uP-FeAl and P-FeAl after oxidation in hydrogen with residual oxygen content of 0.1 MPa at 673 K for 2880 min. (a,b) pure Fe and (c,d) uP-FeAl with oxide flakes and whiskers; (e,f) P-FeAl covered by a uniform and dense oxide layer.
Figure 2. SEM images of surface (oxide) morphologies of pure Fe, uP-FeAl and P-FeAl after oxidation in hydrogen with residual oxygen content of 0.1 MPa at 673 K for 2880 min. (a,b) pure Fe and (c,d) uP-FeAl with oxide flakes and whiskers; (e,f) P-FeAl covered by a uniform and dense oxide layer.
Materials 15 07978 g002
Figure 3. Electrochemical corrosion curves of pure Fe, uP-FeAl and P-FeAl tested in 5 wt.% NaCl solution, with (a) EIS diagram at Ecorr, (b) Potentiodynamic polarization curves and (c) Bode and phase angle plots. Inset of (a) shows equivalent circuit model for EIS in (a) with Rs: solution resistance, Rc: film resistance, Qc: film capacitance, Qdl: double layer capacitance, Rct: charge transfer resistance.
Figure 3. Electrochemical corrosion curves of pure Fe, uP-FeAl and P-FeAl tested in 5 wt.% NaCl solution, with (a) EIS diagram at Ecorr, (b) Potentiodynamic polarization curves and (c) Bode and phase angle plots. Inset of (a) shows equivalent circuit model for EIS in (a) with Rs: solution resistance, Rc: film resistance, Qc: film capacitance, Qdl: double layer capacitance, Rct: charge transfer resistance.
Materials 15 07978 g003
Figure 4. EDS concentration depth profiles of Fe, Al and O measured on P-FeAl.
Figure 4. EDS concentration depth profiles of Fe, Al and O measured on P-FeAl.
Materials 15 07978 g004
Figure 5. The XPS pattern of the P-FeAl surface confirm the formation of Al2O3 oxide layer with the characteristic peak positions for (a) O 1s and (b) Al 2p.
Figure 5. The XPS pattern of the P-FeAl surface confirm the formation of Al2O3 oxide layer with the characteristic peak positions for (a) O 1s and (b) Al 2p.
Materials 15 07978 g005
Figure 6. (a) BF TEM image of P-FeAl cross section. (b) BF TEM image of P-FeAl cross section, where the inset gives FFT image Al2O3 phase with overlay fit of single crystal®. Fitted orientation [ 0   3 ¯   1 ] of orthorhombic Al2O3 (blue). (c) BF TEM image of P-FeAl cross section with corresponding EDS image of (d) Fe, (e) Al, (f) O and (g) Pt.
Figure 6. (a) BF TEM image of P-FeAl cross section. (b) BF TEM image of P-FeAl cross section, where the inset gives FFT image Al2O3 phase with overlay fit of single crystal®. Fitted orientation [ 0   3 ¯   1 ] of orthorhombic Al2O3 (blue). (c) BF TEM image of P-FeAl cross section with corresponding EDS image of (d) Fe, (e) Al, (f) O and (g) Pt.
Materials 15 07978 g006
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Li, C.; Freiberg, K.; Tang, Y.; Lippmann, S.; Zhu, Y. Formation of Nanoscale Al2O3 Protective Layer by Preheating Treatment for Improving Corrosion Resistance of Dilute Fe-Al Alloys. Materials 2022, 15, 7978. https://doi.org/10.3390/ma15227978

AMA Style

Li C, Freiberg K, Tang Y, Lippmann S, Zhu Y. Formation of Nanoscale Al2O3 Protective Layer by Preheating Treatment for Improving Corrosion Resistance of Dilute Fe-Al Alloys. Materials. 2022; 15(22):7978. https://doi.org/10.3390/ma15227978

Chicago/Turabian Style

Li, Chenglong, Katharina Freiberg, Yuntong Tang, Stephanie Lippmann, and Yongfu Zhu. 2022. "Formation of Nanoscale Al2O3 Protective Layer by Preheating Treatment for Improving Corrosion Resistance of Dilute Fe-Al Alloys" Materials 15, no. 22: 7978. https://doi.org/10.3390/ma15227978

APA Style

Li, C., Freiberg, K., Tang, Y., Lippmann, S., & Zhu, Y. (2022). Formation of Nanoscale Al2O3 Protective Layer by Preheating Treatment for Improving Corrosion Resistance of Dilute Fe-Al Alloys. Materials, 15(22), 7978. https://doi.org/10.3390/ma15227978

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.