Next Article in Journal
Recycling Local Waste Glass Bottles into Cement Paste: Effect on Hydration, Microstructure, and CO2 Emission
Previous Article in Journal
Effects of Alloying Elements and Mechanical Alloying on Characteristics of WVTaTiCr Refractory High-Entropy Alloys
Previous Article in Special Issue
Effect of Er, Si, Hf and Nb Additives on the Thermal Stability of Microstructure, Electrical Resistivity and Microhardness of Fine-Grained Aluminum Alloys of Al-0.25%Zr
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Hot Deformation Behavior of Hastelloy C276 Alloy: Microstructural Variation and Constitutive Models

1
School of Mechanical and Electrical Engineering, Central South University, Changsha 410083, China
2
State Key Laboratory of Precision Manufacturing for Extreme Service Performance, Changsha 410083, China
*
Authors to whom correspondence should be addressed.
Materials 2023, 16(18), 6192; https://doi.org/10.3390/ma16186192
Submission received: 7 August 2023 / Revised: 2 September 2023 / Accepted: 5 September 2023 / Published: 13 September 2023
(This article belongs to the Special Issue Plasticity, Damage, and Fracture for Lightweight High-Strength Metals)

Abstract

:
Isothermal deformation experiments of the Hastelloy C276 alloy were executed using the Gleeble-3500 hot simulator at a temperature range of 1000–1150 °C and a strain rate range of 0.01–10 s−1. Microstructural evolution mechanisms were analyzed via transmission electron microscope (TEM) and electron backscatter diffraction (EBSD). Results reveal that the influences of hot compression parameters on the microstructure variation features and flow behaviors of the Hastelloy C276 alloy were significant. The intense strain hardening (SH) effects caused by the accumulation of substructures were promoted when the strain rates were increased, and true stresses exhibited a notable increasing tendency. However, the apparent DRV effects caused by the annihilation of substructures and the increasingly dynamic recrystallization (DRX) behaviors occurred at high compressed temperature, inducing the reduction in true stresses. In addition, a physical-based (PB) constitutive model and a long short-term memory (LSTM) model optimized using the particle swarm optimization (PSO) algorithm were established to predict the flow behavior of Hastelloy C276 alloy. The smaller average absolute relative error and greater relation coefficient suggest that the LSTM model possesses a higher forecasting accuracy than the PB model.

1. Introduction

Because of the outstanding erosion resistance, antioxidant properties and high-temperature intensity, Ni-based superalloys are extensively employed in the marine industry and energy fields [1,2,3,4,5]. Hastelloy C276 alloy, a typical Ni-based superalloy, is widely used in petrochemical industries and the shielding jackets of nuclear reactors [6,7,8]. Generally, the components of Hastelloy superalloys are machined using hot deformation processes [9,10,11]. During hot deformation of Hastelloy C276 alloy, the features of flow behaviors and microstructure changes become complicated [12,13]. Therefore, investigation of the hot deformation behaviors and microstructure evolution of Hastelloy C276 alloy is crucial to precisely control the microstructures and improve the service properties [14,15].
Recently, some studies investigated the microstructure changes in alloys during hot deformation [16,17,18,19]. For example, the nucleation and coarsening features of dynamic recrystallization (DRX) were explored in numerous investigations [20,21], and multiple kinetic models were proposed for describing the DRX features of Ni-based superalloys, i.e., Hastelloy C276 alloy [22] and GH4169 alloy [23]. Moreover, the evolution mechanisms of substructures, including the dislocation clusters/loops and subgrains were explored, which impacted the DRX behaviors of Ni-based superalloys [24,25,26]. Additionally, the interaction of the precipitate phase, substructures and DRX grains in Ni-based superalloys during hot deformation [27] was revealed.
Normally, the hot flow behaviors of alloys exhibited nonlinear features and were intimately connected with the deformation parameters [28,29,30,31,32,33]. Precisely modeling of the flow behaviors was confirmed as a promising method for identifying the hot deformation features and optimizing the formation process of alloys [34,35]. Recently, multiple phenomenological models [36,37] were set up to reconstitute hot deformation behaviors of Ni-based superalloys [38]. Moreover, Chen et al. [39] developed a physically based (PB) mechanism model to accurately predict the true stresses and microstructural evolution characteristics of a nickel-based alloy in hot-working. Taking into account the combined impact of dynamic recovery (DRV) and dimples, Wen et al. [40] modeled the high-temperature tensile characteristics of an ultra-high strength steel utilizing a PB equation. Similarly, multiple PB equations were established or modified for reconstituting the hot deformation features of alloys, i.e., Hastelloy C276 alloy [41], steel [42] and Mg-9%Al-1%Zn [43]. Additionally, various artificial neural network algorithms [44,45], containing support vector regression (SVR) [46], long short-term memory (LSTM) [47] and back propagation (BP) combined with the particle swarm optimization (PSO) algorithm [48], were employed to model the hot deformation characteristics of alloys.
Previously, research was conducted to analyze microstructural changes and to model high-temperature working behaviors of Ni-based superalloys. Nevertheless, a comprehensive analysis of the evolving microstructural features and hot deformation mechanisms of the Hastelloy C276 alloy remain limited. In this present paper, the high-temperature compression features of Hastelloy C276 alloy are researched. The changes in substructures (dislocation cells, subgrain, etc.) and interaction with DRX grains are revealed. Moreover, to reproduce the flow characteristics, the PB model and the PSO-LSTM model are developed.

2. Materials and Methodology

The experimental material is a forged commercial Hastelloy C276 alloy and its chemical composition is shown in Table 1. The size of the experimental cylinder sample is Φ8 mm × 12 mm. Hot compression experiments with a constant strain rate are performed using the Gleeble-3500 thermomechanical simulator which is prepared by the DSI company (Nashville, TN, USA). The samples are heated to the tested temperature at a rate of 10 K/s, and held for 5 min to counterpoise the temperature gradient. Here, four compressed temperatures (1000 °C, 1050 °C, 1100 °C and 1150 °C) are selected. Then, the tested samples are hot-compressed at strain rates of 0.01 s−1, 0.1 s−1, 1 s−1, and 10 s−1, respectively. The final height reduction in the hot-compressed sample is chosen as 60%. The deformed samples are rapidly water-cooled to room temperature (T0) to maintain the microstructure after hot compression, and are analyzed using TEM and EBSD.
For TEM and EBSD analysis, the hot-compressed specimens are sectioned along the central axis and cut into slices. Then, the slice is ground with SiC grinding papers and etched using a solution of 30 mL HClO4 and 270 mL CH3CH2OH. The experimental data are analyzed via the OIM software Version 6.0. The initial microstructure of the researched alloy is shown in Figure 1a, and its local misorientation is indicated in Figure 1b. The prominent grain structures are characterized as equiaxed grain and twinning grain. Moreover, few substructures can be detected.

3. Results and Discussion

3.1. High-Temperature Flow Behaviors of the Hastelloy C276 Alloy

Figure 2 shows the typical true stress–true strain curves of the tested alloy at different temperatures ( T ) and strain rates ( ε ˙ ). It can be distinctly seen that a rapid increase in flow stress appears at the primary strain stage of all curves. This is because of the significant work hardening effect induced by the rapid accumulation and proliferation of dislocations in this period. As the hot deformation process continues, the DRX behavior is activated, and the annihilation of substructures is accelerated. Next, the flow stress gradually reduces.
From Figure 2a, it is seen that the flow stress decreases as the T increases. The predominant cause for this is that the annihilation of dislocation loops/clusters and subgrains rotation is promoted at high T , inducing the intense DRV mechanism [49]. Moreover, the extension rate of grain boundaries is increased with increasing T , which prominently strengthens the coarsening of subgrains and the DRX grains. Additionally, the true stress exhibits an increasing tendency with the increase in ε ˙ (Figure 2b). This occurs because the progression of DRV and DRX mechanisms can be promoted at low ε ˙ .

3.2. Microstructure Evolution

Normally, the microstructural changes in the Hastelloy C276 alloy are abruptly affected by formation parameters. Moreover, the microstructure evolution mechanism has a direct effect on the service performance of the Hastelloy C276 alloy components. Therefore, investigation of the microstructural change in the Hastelloy C276 alloy during hot working is a dire necessity.

3.2.1. Effects of Compressed Temperature

Figure 3 shows the typical KAM maps of the tested Hastelloy C276 alloy at various temperatures. Accordingly, the strain rate is selected as 0.01 s−1. Here, the KAM angle between adjacent substructures changes from 0° to 5°, with the color changing from blue to red. For the compressed temperature (T) at 1000 °C, fewer areas with the blue color can be detected, suggesting the appearance of intense nucleation and interaction of substructures (Figure 3a). This is because the massive dislocation clusters, indicated by black lines, around grain boundaries or within grains are generated under complicated hot-stress conditions, as revealed in the TEM image of Figure 4a. Meanwhile, many fine DRX nucleus and subgrains are formed. With T increasing to 1050 °C, the areas covered in blue color experience the prominent extension, which implies the sufficient annihilation of substructures (Figure 3b). This is attributed to the abrupt increase in the DRX and DRV behaviors at high compressed temperatures, resulting in the heavy annihilation of substructures. When T ascends to 1150 °C, most areas are marked with blue, indicating the full development of substructures (Figure 3c). In the TEM image at 1150 °C (Figure 4b), it is discovered that the number of black lines around the grain boundaries/inside the grains tends to become significantly less, suggesting that numerous dislocations arrays/clusters are consumed through annihilation of dislocation and interaction. Concurrently, the DRX nucleus and subgrains display prominent coarsening features, which also can sweep the substructures near the grain boundaries. Hence, the elimination of substructures becomes intense with increasing T.
The typical evolution characteristics of grain structure over various compression temperatures are displayed in Figure 5. Accordingly, the ε ˙ is set as 0.01 s−1. It is seen that most of the original grains exhibit a flattened state, and the grain boundaries display bulging, which is characteristic of the researched alloys at 1000 °C (Figure 5a). Moreover, numerous fine DRX grains are generated around the bulging regions of the original grain boundaries, which forms a necklace morphology, implying the occurrence of discontinuous dynamic recrystallization (DDRX). Through statistical calculations, the mean size of grains ( d ¯ a v g ) at T of 1000 °C is computed as 4.36 µm (Figure 5b). With increasing T , almost all fine DRX grains exhibit a dominant coarsening behavior, as revealed in Figure 5c. Simultaneously, it is discovered that low-angle grains boundaries (LAGBs) form and interact, which then gradually transforms into high-angle grain boundaries (HAGBs), indicating the tendency of continuous dynamic recrystallization (CDRX). Correspondingly, the d ¯ a v g for the tested Hastelloy C276 alloy at 1050 °C reaches 5.18 µm (Figure 5d). When T gradually ascends to 1150 °C, almost all deformed original grains are replaced with DRX grains, and a dominant growth of DRX grains can be observed (Figure 5e). Concurrently, the value of d ¯ a v g ascends to 8.69 μm for the researched Hastelloy C276 alloy at 1150 °C, as shown in Figure 5f. This is because the migration rate of alloying elements and dislocations are boosted at higher T , which is beneficial for the increase in grain boundary migration ability. Additionally, the annihilation of substructures is enhanced with increasing T , thereby reducing the resistance for the mobility of DRX grain boundaries. Thus, the coarsening behaviors of grains become outstanding as T ascends.

3.2.2. Effects of Strain Rate

For T at 1150 °C, the typical KAM pictures at various ε ˙ are shown in Figure 3c and Figure 6. It is seen that the zone covered in red/yellow colors is relatively expanded at ε ˙ of 0.1 s−1 (Figure 6a), compared to that at 0.01 s−1 (Figure 3c). With the further increase in ε ˙ , the zones covered in red/yellow colors are continuously extended, as shown in Figure 6b,c. This implies that the progression of LAGBs is sensibly promoted with increasing ε ˙ . It is primarily caused by the formation of substructures and interaction with DRX grains. As seen in TEM pictures of Figure 4b and Figure 7, the formation of fine substructures, including the dislocation clusters/arrays and subgrains, is prominently increased at higher ε ˙ . Moreover, it is also discovered that the coarsening behavior of twins and DRX grains becomes loose with increasing ε ˙ . This induces the suppression of the annihilation of substructures. Additionally, the compression deformation time for the consumption of substructures through effective DRV as well as DRX mechanisms is decreased. Hence, the nucleation and interaction of LAGBs is enhanced with increasing ε ˙ .
The EBSD pictures highlighting the evolution of grain structure over ε ˙ are shown in Figure 8. Here, T is selected as 1150 °C. At a relatively low ε ˙ of 0.1 s−1 (Figure 8a), the morphology of DRX grains becomes finer compared to that at 0.01 s−1 (Figure 5e). Accordingly, the d ¯ a v g at the ε ˙ of 0.1 s−1 reaches 5.81 μm (Figure 8b). This implies that the growth behaviors of DRX grains exhibit a weakening tendency at higher ε ˙ . With a substantial increase in ε ˙ , the flattened original grains prominently increase, as displayed in Figure 8c,e. Simultaneously, the d ¯ a v g at the ε ˙ of 1 s−1 and 10 s−1 are statistically computed as 6.07 μm and 6.97 μm, respectively, as seen in Figure 8d,f. The primary cause for this result is that the nucleated density of substructures (as displayed in Figure 6 and Figure 7) is increased at higher ε ˙ , inducing the increase in resistance to the migration of the DRX grain boundary. Additionally, the compression deformation time for the nucleation/growth of DRX grain becomes shorter with increasing ε ˙ , and the remaining original grains with relatively large size are increased. Therefore, the value of d ¯ a v g is increased with the increase in ε ˙ .

3.3. Physically Based Constitutive Model

During hot deformation, the flow stress is intimately correlated with microstructural evolution mechanism, and can be expressed as [1,39]
σ = σ y + σ i + σ g
where σ is the flow stress, and σ y , σ i and σ g are the short-range stress, the stress affected by the interaction of dislocation and the stress affected by the grain size evolution, respectively.
Normally, the σ y is often computed as [50]
σ y = A y ( α y ε ˙ exp ( Q y / R T ) ) n y
where A y , α y   Q y and n y represent material factors.
In hot deformation, the rapid movement and proliferation of dislocations lead to a continuous increase in internal stress. Meanwhile, the occurrence of dynamic softening mechanisms (DRV and DRX) enhances the annihilation and rearrangement of dislocations. Hence, the correlation between the dislocation density and true stress can be identified as [29]
σ i = M α μ b ρ i
where M is a Taylor coefficient (3.06) [39], α is an interaction constant, μ is the shear modulus ( μ = 85.89 0.0207 T ), b is the Burger vector, ρ i is the dislocation density and its evolution rate ( ρ ˙ i ) is defined as [39]
ρ ˙ i = ρ ˙ i + ρ ˙ i ( drv ) ρ ˙ i ( drx )
where ρ ˙ i + , ρ ˙ i ( drv ) and ρ ˙ i ( drx ) are the evolution rate of ρ i connected with work hardening (WH), DRV and DRX mechanisms, respectively.
Normally, the value of ρ ˙ i + can be computed as [51]
ρ ˙ i + = M b 1 Λ ε ˙
where Λ is the mean free path, and can be determined as [39]
Λ = 1 s i + 1 d i
where d i is the average grain size. s i is the size of substructure and can be expressed as [39]
s i = f w / ρ i
where f w illustrates the coefficient of work hardening, and can be expressed as
f w = A w ε ˙ n w exp ( Q w / R T )
where A w , Q w and n w are the material constants.
Normally, the d i can be identified as [1]
d i = X drx d drx + ( 1 X drx ) d 0
where d 0 and d drx are the original grain size and the average grain size of DRX, respectively, and the X drx indicates the DRX fraction.
For the researched Hastelloy C276 alloy in hot compression with constant strain rates, the X drx can be defined as [22]
{ X drx = 1 exp [ 0.693 ( ε ε c ε 0 . 5 ε c ) n ] ( ε ε c ) { ε c = 0.0012239 Z 0.11739 ( ε ˙ = 0.1   s 1 10   s 1 ) ε c = 0.001543 Z 0.11366 ( ε ˙ = 0.01   s 1 0.1   s 1 ) { ε 0 . 5 = 0.000815 Z 0.17507 ( ε ˙ = 0.1   s 1 10   s 1 ) ε 0 . 5 = 0.000582 Z 0.19245 ( ε ˙ = 0.01   s 1 0.1   s 1 ) n = { 1.512 ( ε ˙ = 0.1   s 1 10   s 1 ) 1.610 ( ε ˙ = 0.01   s 1 0.1   s 1 ) Z = ε ˙ exp ( 467710.9 R T )
where ε c and ε 0.5 are the critical strain and the strain when the X drx reaches 50%, respectively; Z is the Zener–Hollomon parameter; R expresses a gas constant (8.314 Jmol−1 K−1).
Moreover, the d drx for the researched Hastelloy C276 alloy can be identified as [22]
d drx = 431.54 ε ˙ 0.10222 exp ( 46293.77 R T )
Furthermore, the ρ ˙ i ( drv ) is usually determined as [52]
ρ ˙ i ( drv ) = f v ρ i ε ˙
where f v is the work hardening coefficient, and can be identified as
f v = A v ε ˙ n v exp ( Q v / R T )
where A v , Q v and n v represent the material constants.
Meanwhile, the ρ ˙ i ( drx ) can be defined as [39]
ρ ˙ i ( drx ) = f X ( ρ i ρ i 0 ) ( 1 X ) X ˙ ε ˙
where ρ i 0 is the initial dislocation density. f x is the material coefficient, and can be identified as [39],
f x = A x ε ˙ n x exp ( Q x / R T )
where A x , Q x and n x are the material constants.
During hot deformation, the σ g is normally defined as [52]
σ g = X i f g d i 0 . 5
where f g is the material coefficient, and can be expressed as [39]
f g = A g ε ˙ n g exp ( Q g / R T )
where A g , Q g and n g are the material constants.
The above formulas are programmed into MATLAB software (Version R2021b), and the material constants in the formulas are calculated using the algorithms in the MATLAB optimization toolbox. Here, the Genetic Algorithm is employed to obtain these constants. The optimum results are listed in Table 2.
Based on the above-established PB constitutive model, the forecasted hot compression curves are shown in Figure 9. Clearly, most of the tested true stresses at the ε ˙ of 10 s−1 and 1 s−1 surpassingly fit with the forecasted results of the PB model (Figure 9a,b). On the other hand, the disparity in the experimental true stresses and the ones evaluated with the PB model at a relatively low ε ˙ of 0.1 s−1 and 0.01 s−1 can be detected. This is attributed to the fact that the microstructural evolution mechanisms of the researched alloy, especially the DRX kinetic behaviors, exhibit a prominent difference as the ε ˙ is less than 0.1 s−1 or larger than 0.1 s−1. With changes in the compression conditions, the complex microstructure features also evolves, leading to the occurrence of complicated hot compression characteristics, which are hard to be ideally reconstituted using the PB model.

3.4. PSO-LSTM Model

Based on its excellent ability to model nonlinear data, the LSTM is adopted to reveal the hot compression behaviors of the researched Hastelloy C276 alloy. The typical structure of the LSTM model is shown in Figure 10. Here, the input layers are chosen as the T , ε and ε ˙ . Correspondingly, the output layer is defined as σ . Owing to the intricacy of the stress–strain data, the value of hidden layer is set as 2 [47].
Normally, the LSTM model searches for a global optimal solution through gradient descent. The typical data transmission process of the LSTM unit is depicted in Figure 11. The forgetting gate, inputting gate and outputting gate are used to protect and control the cell state, so as to achieve the purpose of learning or forgetting information from time series data. The input data will be fed into the outputting gate, the forgetting gate, the inputting gate and the candidate gate, respectively. Then, the four gates will output different data for subsequent computation; the detailed procedures can be interpreted as follows.
Firstly, the forgetting gate ( f t ) cleans up the useless input data x t from the last cell status, which can be expressed as [53]
f t = σ 1 ( W 1 [ h t 1 , x t ] + b 1 )
where σ 1 is the activation function; [ h t 1 , x t ] is the inputting data; W 1 and b 1 represent the weight and bias of the forgetting gate, respectively.
Then, the storage status of information for the individual cell is determined. Here, the sigmoid function ( σ 2 ) of the inputting gate ( i t ), as the activation function, decides which kind of message will be delivered to the hyperbolic tangent activation function ( tan h ). The formulas of i t and C ˜ t can be determined as [47]
i t = σ 2 ( W 2 [ h t 1 , x t ] + b 2 )
C ˜ t = tanh ( W 3 [ h t 1 , x t ] + b 3 )
where C ˜ t represents the unit state; W 2 and b 2 represent the weight and bias of the inputting gate, respectively. W 3 and b 3 represent the weight and bias of the cell status, respectively.
Next, the inputting gate is combined with the forgetting gate, and the cell status is refreshed from C t 1 to C t . The refreshed equation of C t can be expresses as [47]
C t = f t C t 1 + i t C ˜ t
Therefore, the data counted in the outputting gate o t can be renovated and calculated using [47]
o t = σ 3 ( W 4 [ h t 1 , x t ] + b 4 )
where σ 3 represents the activation function of outputting gate; W 4 and b 4 represent the weight and bias of the outputting gate, respectively.
Eventually, with the introduction of the activation function ( tan h ), the next hidden status ( h t ) can be expressed as [47]
h t = o t tanh ( c t )
Normally, the LSTM model can effectively overcome the defects of vanishing gradients and exploding gradient. However, several problems including the susceptible to fall into local minima and the relatively limited convergence rate significantly affect the applicability of the LSTM model. In order to improve convergence speed and forecasting accuracy of the LSTM model, the coupling of the PSO algorithm with the LSTM model (PSO-LSTM) is proposed to reconstruct the hot compression behaviors of the researched alloy. Commonly, the PSO algorithm is characterized as an evolutionary computing technology based on swarm intelligence. The individual positions of a PSO algorithm can be updated by tracking the individual extreme value ( p b e s t ) and the group extreme value ( g b e s t ). The velocity and position equation of particle can be, respectively, expressed as [53]
v i = W × v i + c 1 × r a n d ( ) × ( p b e s t i x i ) + c 2 × r a n d ( ) × ( g b e s t i x i )
x i = x i + v i
where v i is the speed of the particles, w illustrates the inertia factor, the r a n d ( ) indicates a random number from 0 to 1, x i is the current position of the particles, and c 1 and c 2 are the learning factors.
Figure 12 displays the flowchart of the established PSO-LSTM model. First, the parameters of the LSTM network and the parameters (population size, evolution times, individual update range, and speed update range) of the PSO algorithm can be defined. Then, the fitness function, which is the root mean square error ( R M S E ) of the predicted and experimental value, can be determined. Concurrently, the p b e s t and g b e s t are updated according to the fitness. Finally, the optimal results are assigned to the LSTM model, and then the training result of the LSTM model is obtained.
Seventy-five percent of the experimental data are used for training. Correspondingly, the other twenty-five percent of the tested data are used for validating the model. According to the developed LSTM network, the length of the PSO particle matrix is set as 4. The population size is 10, and the learning factor is 2. The maximum iteration step is 100.
The total iterations of the LSTM model are set as 1500 and the min-batch size is set as 128. Concurrently, the gradient threshold is set as 1. The training method adopts Adaptive Moment Estimation (Adam). In order to ensure smooth training of the model, all experimental data are normalized as
X i = X X min X max X min
where X is the input value. X max and X min are the maximum and minimum value, respectively.
After inputting the data, the PSO-LSTM model performs iterative calculations to achieve its own convergence. Usually, the fitness function is utilized to assess the convergence, as shown in Figure 13. A better convergence occurs as the fitness value is small. When the PSO algorithm iterates to the 10th generation, the fitness value of the best particle reaches the lowest point (6.266). Therefore, the optimal LSTM parameters are obtained from the PSO algorithm at the 10th generation. Here, the hidden layer 1 node is 150 and the hidden layer 2 node is 100. Accordingly, the fully connected layer node is 162, and the learning rate is 0.048. The predicted value of flow stress can be obtained by integrating the parameters into the LSTM model.
The forecasting capacity of the established PSO-LSTM model is shown in Figure 14. Through contrastive analysis, it is seen that the experimental true and predicted stresses generated by the PSO-LSTM model exhibit the outstanding consistency. It implies that the PSO-LSTM model can be employed to achieve accurate reconstitution of the hot compression features of the tested alloy.

3.5. Verification

The correlation coefficients ( R ) and average absolute relative errors ( A A R E ) are often used to assess the fit of tested and forecasted data. Accordingly, the values of R and A A R E are evaluated as
R = i = 1 N ( E i E ¯ ) ( P i P ¯ ) i = 1 N ( E i E ¯ ) 2 ( P i P ¯ ) 2
A A R E = 1 N i = 1 N | E i P i E i |
where E i and P i are the experimental and predicted data, respectively. E ¯ and P ¯ are the mean value of the experimental data and the predicted data, respectively. N is the volume of total data.
The values of R and A A R E are shown in Figure 15. It is observed that the values of R for the proposed PB model and PSO-LSTM model are computed as 0.984 and 0.99, respectively. This implies that a good correlation between the tested stresses and forecasted results via the two models can be achieved (Figure 15a,b). Additionally, the value of A A R E for the PB model is computed as 9.29%, which is relatively larger than that of the PSO-LSTM model (3.84%). It suggests that the established PSO-LSTM model has better forecasting capacity for hot compression behaviors of the tested Hastelloy C276 alloy compared with that of the PB model.

4. Conclusions

The microstructural evolution and high-temperature compressed features of the Hastelloy C276 alloy are investigated in this paper. Several important conclusions from our analyses can be drawn:
  • Wehn the strain rate is increased, the WH effect induced by the formation of high-density dislocation clusters/arrays and subgrains is enhanced, and consequently, the true stress increases. Nevertheless, the dislocation rearrangement, caused by the promising DRV effect and the nucleation/coarsening of DRX grains, are enhanced at higher compression temperatures, thereby inducing a prominent decrease in true stress.
  • Both the PB model and the PSO-LSTM model are proposed for reconstituting the hot compression behaviors of the tested Hastelloy C276 alloy. A reasonably larger R and a smaller A A R E of the PSO-LSTM model can be acquired, which suggest its higher forecasting accuracy than the PB model.

Author Contributions

Conceptualization, S.C.; Methodology, D.H., Y.L., X.Y. and G.L.; Validation, Y.L., X.Y. and G.L.; Writing—original draft, D.H. and S.C.; Writing—review & editing, D.H.; Project administration, Y.L. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the National Natural Science Foundation of China (Grant No. 52005519), the National Key Research and Development Program of China (No. 2022YFB3706902), Hunan Provincial Natural Science Foundation of China (Grant No. 2021JJ40738, 2023JJ20065), Changsha Municipal Natural Science Foundation (No. kq2007024), State Key Laboratory of Featured Metal Materials and Life-cycle Safety for Composite Structures (2022GXYSOF04, 2022GXYSOF24), and Postgraduate Scientific Research Innovation Project of Hunan Province (No. 1053320216356).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The raw/processed data acquired in present investigation cannot be shared at this time because the data also forms part of an ongoing research.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. He, D.G.; Yan, X.T.; Lin, Y.C.; Xia, Y.C. Microstructural evolution and kinetic characteristics during metadynamic recrystallization in a Ni-Cr-Mo alloy. J. Alloys Compd. 2022, 926, 166830. [Google Scholar] [CrossRef]
  2. Xiao, J.F.; Cui, H.T.; Zhang, H.J.; Wen, W.D.; Zhou, J. A physical-based constitutive model considering the motion of dislocation for Ni3Al-base superalloy. Mater. Sci. Eng. A 2020, 772, 138631. [Google Scholar] [CrossRef]
  3. Ning, Y.Q.; Wang, T.; Fu, M.W.; Li, M.Z.; Wang, L.; Zhao, C.D. Competition between work-hardening effect and dynamic-softening behavior for processing as-cast GH4720Li superalloys with original dendrite microstructure during moderate-speed hot compression. Mater. Sci. Eng. A 2015, 642, 187–193. [Google Scholar] [CrossRef]
  4. Wang, G.Q.; Chen, M.S.; Li, H.B.; Lin, Y.C.; Zeng, W.D.; Ma, Y.Y. Methods and mechanisms for uniformly refining deformed mixed and coarse grains inside a solution-treated Ni-based superalloy by two-stage heat treatment. J. Mater. Sci. Technol. 2021, 77, 47–57. [Google Scholar] [CrossRef]
  5. Long, J.C.; Zhu, N.Y.; Xia, Q.X.; Cheng, X.Q. A Study of the Dynamic Recrystallization Behavior of Ni-Based Superalloy during Hot Power Spinning Based on Cellular Automaton. Adv. Eng. Mater. 2019, 21, 1801022. [Google Scholar] [CrossRef]
  6. Zhang, C.; Zhang, L.W.; Shen, W.F.; Liu, C.R.; Xia, Y.N. The Kinetics of Metadynamic Recrystallization in a Ni-Cr-Mo-Based Superalloy Hastelloy C-276. J. Mater. Eng. Perform. 2016, 25, 545–552. [Google Scholar] [CrossRef]
  7. Chen, J.; Wang, J.Z.; Yan, F.Y.; Zhang, Q.; Li, Q.A. Corrosion wear synergistic behavior of Hastelloy C276 alloy in artificial seawater. Trans. Nonferrous Met. Soc. China 2015, 25, 661–668. [Google Scholar] [CrossRef]
  8. Lin, Y.C.; Qian, S.S.; Chen, X.M.; Li, X.H.; Yang, H. Staggered spinning of thin-walled Hastelloy C-276 cylindrical parts: Numerical simulation and experimental investigation. Thin. Wall. Struct. 2019, 140, 466–476. [Google Scholar] [CrossRef]
  9. Xia, Q.X.; Long, J.C.; Zhu, N.Y.; Xiao, G.F. Research on the microstructure evolution of Ni-based superalloy cylindrical parts during hot power spinning. Adv. Manuf. 2019, 7, 52–63. [Google Scholar] [CrossRef]
  10. Dhananchezian, M. Study the machinability characteristics of Nicked based Hastelloy C-276 under cryogenic cooling. Measurement 2019, 136, 694–702. [Google Scholar] [CrossRef]
  11. Wang, X.K.; Xia, Q.X.; Cheng, X.Q. Deformation behavior of haynes230 superalloy during backward flow forming. Int. J. Precis. Eng. Manuf. 2017, 18, 77–83. [Google Scholar] [CrossRef]
  12. Zhang, C.; Tang, X.L.; Zhang, L.W.; Cui, Y. Cellular automaton modeling of dynamic recrystallization of Ni–Cr–Mo-based C276 superalloy during hot compression. J. Mater. Res. 2019, 34, 3093–3103. [Google Scholar] [CrossRef]
  13. Zhang, X.Y.; Guo, S.L.; Zhong, J. Microevolution of grain boundary character distribution in Hastelloy C-276 during the annealing process. J. Mater. Res. Technol. 2022, 18, 1534–1541. [Google Scholar] [CrossRef]
  14. Jaladurgam, N.R.; Kanjarla, A.K. Hot deformation characteristics and microstructure evolution of Hastelloy C-276. Mater. Sci. Eng. A 2018, 712, 240–254. [Google Scholar] [CrossRef]
  15. Kong, Y.H.; Chang, P.P.; Li, Q.; Xie, L.X.; Zhu, S.G. Hot deformation characteristics and processing map of nickel-based C276 superalloy. J. Alloys Compd. 2015, 622, 738–744. [Google Scholar] [CrossRef]
  16. Xing, J.; Liu, C.Z.; Li, A.M.; Wang, S.M.; Zhang, X.J.; Shi, Y.X. Microstructural evolution and stability of coarse-grained S31254 super austenitic stainless steel during hot deformation. Metals 2022, 12, 1319. [Google Scholar] [CrossRef]
  17. Sun, B.; Zhang, T.B.; Song, L.; Zhang, L. Microstructural evolution and dynamic recrystallization of a nickel-based superalloy PMEP962NP during hot deformation at 1150 °C. J. Mater. Res. Technol. 2022, 18, 1436–1449. [Google Scholar] [CrossRef]
  18. Zhao, H.T.; Zhi, H.R.; Wang, S.W.; Wang, Y.L. The hot deformation behavior and microstructural evolution of TP2 pure Copper. Trans. Indian Inst. Met. 2023, 76, 1467–1474. [Google Scholar] [CrossRef]
  19. Luo, Y.M.; Shi, C.B.; Xu, H.C. Microstructure evolution and hot deformation characteristics of 15Cr-22Ni iron-base superalloy. J. Alloys Compd. 2022, 938, 168628. [Google Scholar] [CrossRef]
  20. Li, Q.; Bu, H.Y.; Han, J.Y.; Li, M.N. Dynamic recrystallization behavior and processing maps of 5CrNiMoV steel during hot deformation. Mater. Res. Express 2023, 10, 046519. [Google Scholar] [CrossRef]
  21. Cai, Y.Q.; Xiang, S.; Tan, Y.B. Insight into the dynamic recrystallization behavior and microstructure evolution of MP159 superalloy during hot deformation. Met. Mater. Int. 2022, 28, 2381–2394. [Google Scholar] [CrossRef]
  22. Yan, X.T.; Xia, Y.C.; He, D.G.; Lin, Y.C. Microstructural Evolution and an Improved Dynamic Recrystallization Kinetic Model of a Ni-Cr-Mo Alloy in Hot Deformation. Materials 2022, 15, 3161. [Google Scholar] [CrossRef] [PubMed]
  23. Chen, X.M.; Lin, Y.C.; Li, X.H.; Chen, M.S.; Yuan, W.Q. Investigation on strain dependence of metadynamic recrystallization behaviors of GH4169 superalloy. Vacuum 2018, 149, 1–11. [Google Scholar] [CrossRef]
  24. Li, B.; Du, Y.; Chu, Z.J.; Zhou, W.; Yang, X.L. Research on dynamic recrystallization behavior of Ni-Fe-Cr based alloy. Mater. Charact. 2020, 169, 110653. [Google Scholar] [CrossRef]
  25. Chen, F.L.; Li, K.D.; Tang, B.; Liu, D.G.; Zhong, H.; Li, J.S. Deformation behavior and microstructural evolution of Inconel 625 superalloy during the hot compression process. Metals 2021, 11, 824. [Google Scholar] [CrossRef]
  26. Guo, S.L.; Liu, J.C.; Du, B.; Liu, S.P.; Zhang, X.Y.; Li, D.F. An Investigation on Constitutive Relation and Dynamic Recrystallization of Hastelloy C-276 Alloy During Hot Deformation. J. Mater. Eng. Perform. 2020, 29, 5902–5912. [Google Scholar] [CrossRef]
  27. Zhang, C.; Zhang, L.W.; Cui, Y.; Feng, Q.Y.; Cheng, C.Q. Effects of High-Temperature Aging on Precipitation and Corrosion Behavior of a Ni-Cr-Mo-Based Hastelloy C276 Superalloy. J. Mater. Eng. Perform. 2020, 29, 2026–2034. [Google Scholar] [CrossRef]
  28. Kotkunde, N.; Krishnamurthy, H.N.; Singh, S.K.; Jella, G. Experimental and Numerical Investigations on Hot Deformation Behavior and Processing Maps for ASS 304 and ASS 316. High Temp. Mater. Process. 2018, 37, 873–888. [Google Scholar] [CrossRef]
  29. Wen, D.X.; Gao, C.X.; Zheng, Z.Z.; Wang, K.; Xiong, Y.B.; Wang, J.K.; Li, J.J. Hot tensile behavior of a low-alloyed ultrahigh strength steel: Fracture mechanism and physically-based constitutive model. J. Mater. Res. Technol. 2021, 13, 1684–1697. [Google Scholar] [CrossRef]
  30. Savaedi, Z.; Motallebi, R.; Mirzadeh, H. A review of hot deformation behavior and constitutive models to predict flow stress of high-entropy alloys. J. Alloys Compd. 2022, 903, 163964. [Google Scholar] [CrossRef]
  31. Fan, X.G.; Yang, H.; Gao, P.F. Prediction of constitutive behavior and microstructure evolution in hot deformation of TA15 titanium alloy. Mater. Des. 2013, 51, 34–42. [Google Scholar] [CrossRef]
  32. Xu, W.C.; Jin, X.Z.; Xiong, W.D.; Zeng, X.Q.; Shan, D.B. Study on hot deformation behavior and workability of squeeze-cast 20 vol% SiCw/6061Al composites using processing map. Mater. Charact. 2018, 135, 154–166. [Google Scholar] [CrossRef]
  33. Tang, C.P.; Liu, W.H.; Chen, Y.Q.; Liu, X.; Deng, Y.L. Hot Deformation Behavior of a Differential Pressure Casting Mg–8Gd–4Y–Nd–Zr Alloy. J. Mater. Eng. Perform. 2017, 26, 383–391. [Google Scholar] [CrossRef]
  34. Mirzadeh, H. Constitutive Description of 7075 Aluminum Alloy During Hot Deformation by Apparent and Physically-Based Approaches. J. Mater. Eng. Perform. 2015, 24, 1095–1099. [Google Scholar] [CrossRef]
  35. Chen, X.M.; Lin, Y.C.; Hu, H.W.; Luo, S.C.; Zhou, X.J.; Huang, Y. An Enhanced Johnson–Cook Model for Hot Compressed A356 Aluminum Alloy. Adv. Eng. Mater. 2021, 23, 2000704. [Google Scholar] [CrossRef]
  36. Detrois, M.; Antonov, S.; Tin, S.; Jablonski, P.D.; Hawk, J.A. Hot deformation behavior and flow stress modeling of a Ni-based superalloy. Mater. Charact. 2019, 157, 109915. [Google Scholar] [CrossRef]
  37. Quan, G.Z.; Pan, J.; Wang, X. Prediction of the Hot Compressive Deformation Behavior for Superalloy Nimonic 80A by BP-ANN Model. Appl. Sci. 2016, 6, 66. [Google Scholar] [CrossRef]
  38. Lu, Y.L.; Liu, J.X.; Li, X.K.; Liang, J.P.; Li, Z.J.; Wu, G.Y.; Zhou, X.T. Hot deformation behavior of Hastelly C276 superalloy. Trans. Nonferrous Met. Soc. China 2012, 22, s84–s88. [Google Scholar] [CrossRef]
  39. Chen, Z.J.; Lin, Y.C.; He, D.G.; Lou, Y.M.; Chen, M.S. A unified dislocation density-based model for an aged polycrystalline Ni-based superalloy considering the coupled effects of complicate deformation mechanisms and initial δ phase. Mater. Sci. Eng. A 2021, 827, 142062. [Google Scholar] [CrossRef]
  40. Wen, D.X.; Yue, T.Y.; Xiong, Y.B.; Wang, K.; Wang, J.K.; Zheng, Z.Z.; Li, J.J. High-temperature tensile characteristics and constitutive models of ultrahigh strength steel. Mater. Sci. Eng. A 2021, 803, 140491. [Google Scholar] [CrossRef]
  41. He, D.G.; Yan, X.T.; Lin, Y.C.; Zhang, S.; Chen, Z.J. Microstructure evolution and constitutive model for a Ni-Mo-Cr base alloy in double-stages hot compression with step-strain rates. Mater. Charact. 2022, 194, 112385. [Google Scholar] [CrossRef]
  42. Chen, F.; Wang, H.; Zhu, H.J.; Zhu, H.Y.; Ren, F.C.; Cui, Z.S. High-temperature deformation mechanisms and physical-based constitutive modeling of ultra-supercritical rotor steel. J. Manuf. Process. 2019, 38, 223–234. [Google Scholar] [CrossRef]
  43. Dini, H.; Svoboda, A.; Andersson, N.E.; Ghassemali, E.; Lindgren, L.E.; Jarfors, A.E.W. Optimization and validation of a dislocation density based constitutive model for as-cast Mg-9%Al-1%Zn. Mater. Sci. Eng. A 2018, 710, 17–26. [Google Scholar] [CrossRef]
  44. Opela, P.; Schindler, L.; Kawulok, P.; Kawulok, R.; Rusz, S.; Sauer, M. Shallow and deep learning of an artificial neural network model describing a hot flow stress Evolution: A comparative study. Mater. Des. 2022, 220, 110880. [Google Scholar] [CrossRef]
  45. Churyumov, A.; Kazakova, A.; Churyumova, T. Modelling of the Steel High-Temperature Deformation Behaviour Using Artificial Neural Network. Metals 2022, 12, 447. [Google Scholar] [CrossRef]
  46. He, D.G.; Lin, Y.C.; Chen, J.; Chen, D.D.; Huang, J.; Tang, Y.; Chen, M.S. Microstructural evolution and support vector regression model for an aged Ni-based superalloy during two-stage hot forming with stepped strain rates. Mater. Des. 2018, 154, 51–62. [Google Scholar] [CrossRef]
  47. He, D.G.; Chen, S.B.; Lin, Y.C.; Xie, H.; Li, C.B. Hot tensile behavior of a 7046-aluminum alloy: Fracture mechanisms and constitutive models. Mater. Today Commun. 2023, 34, 105209. [Google Scholar] [CrossRef]
  48. Wan, P.; Zou, H.; Wang, K.L.; Zhao, Z.Z. Research on hot deformation behavior of Zr-4 alloy based on PSO-BP artificial neural network. J. Alloys Compd. 2020, 826, 154047. [Google Scholar] [CrossRef]
  49. Huang, K.; Logé, R.E. A review of dynamic recrystallization phenomena in metallic materials. Mater. Des. 2016, 111, 548–574. [Google Scholar] [CrossRef]
  50. Jiang, Y.Q.; Lin, Y.C.; Pang, G.D.; He, D.G.; Kotkunde, N. Constitutive Model and Processing Maps for a Ti-55511 Alloy in beta Region. Adv. Eng. Mater. 2020, 22, 1900930. [Google Scholar] [CrossRef]
  51. Mecking, H.; Kocks, U.F. Kinetics of flow and strain-hardening. Acta Mater. 1981, 29, 1865–1875. [Google Scholar] [CrossRef]
  52. He, D.G.; Su, G.; Lin, Y.C.; Jiang, Y.Q.; Li, Z.; Chen, Z.J.; Yan, X.T.; Xia, Y.C.; Xie, Y.C. Microstructural Variation and a Physical Mechanism Model for a Ti-55511 Alloy during Double-Stage Hot Deformation with Stepped Strain Rates in the beta Region. Materials 2021, 14, 6371. [Google Scholar] [CrossRef] [PubMed]
  53. Xue, S.; Chen, H.L.; Zheng, X.L. Detection and quantification of anomalies in communication networks based on LSTM-ARIMA combined model. Int. J. Mach. Learn. Cybern. 2022, 13, 3159–3172. [Google Scholar] [CrossRef] [PubMed]
Figure 1. The initial microstructure of the Hastelloy C276 alloy: (a) inverse pole figure (IPF); (b) the kernel average misorientation (KAM).
Figure 1. The initial microstructure of the Hastelloy C276 alloy: (a) inverse pole figure (IPF); (b) the kernel average misorientation (KAM).
Materials 16 06192 g001
Figure 2. Flow stress curves of the researched alloy at (a) ε ˙   =   10   s 1 ; (b) T = 1150 °C.
Figure 2. Flow stress curves of the researched alloy at (a) ε ˙   =   10   s 1 ; (b) T = 1150 °C.
Materials 16 06192 g002
Figure 3. EBSD-KAM maps under different temperatures: (a) 1000 °C; (b) 1050 °C; (c) 1150 °C.
Figure 3. EBSD-KAM maps under different temperatures: (a) 1000 °C; (b) 1050 °C; (c) 1150 °C.
Materials 16 06192 g003
Figure 4. The TEM micrographs at (a) T = 1000 °C, ε ˙ = 0.01 s−1; (b) T = 1150 °C, and ε ˙ = 0.01 s−1.
Figure 4. The TEM micrographs at (a) T = 1000 °C, ε ˙ = 0.01 s−1; (b) T = 1150 °C, and ε ˙ = 0.01 s−1.
Materials 16 06192 g004
Figure 5. Typical EBSD-IPF maps at: (a,b) 1000 °C; (c,d) 1050 °C; (e,f) 1150 °C.
Figure 5. Typical EBSD-IPF maps at: (a,b) 1000 °C; (c,d) 1050 °C; (e,f) 1150 °C.
Materials 16 06192 g005aMaterials 16 06192 g005b
Figure 6. EBSD-KAM maps at the ε ˙ of (a) 0.1 s−1; (b) 1 s−1; (c) 10 s−1.
Figure 6. EBSD-KAM maps at the ε ˙ of (a) 0.1 s−1; (b) 1 s−1; (c) 10 s−1.
Materials 16 06192 g006
Figure 7. The TEM micrographs at (a) T = 1150 °C, ε ˙ = 1 s−1; (b) T = 1150 °C, ε ˙ = 10 s−1.
Figure 7. The TEM micrographs at (a) T = 1150 °C, ε ˙ = 1 s−1; (b) T = 1150 °C, ε ˙ = 10 s−1.
Materials 16 06192 g007
Figure 8. EBSD-IPF maps at: (a,b) 1150 °C/0.1 s−1; (c,d) 1150 °C/1 s−1; (e,f) 1150 °C/10 s−1.
Figure 8. EBSD-IPF maps at: (a,b) 1150 °C/0.1 s−1; (c,d) 1150 °C/1 s−1; (e,f) 1150 °C/10 s−1.
Materials 16 06192 g008
Figure 9. Comparison of the experimental and predicted flow stress at (a) ε ˙ = 10 s−1; (b) ε ˙ = 1 s−1; (c) ε ˙ = 0.1   s 1 ; (d) ε ˙ = 0.01 s−1.
Figure 9. Comparison of the experimental and predicted flow stress at (a) ε ˙ = 10 s−1; (b) ε ˙ = 1 s−1; (c) ε ˙ = 0.1   s 1 ; (d) ε ˙ = 0.01 s−1.
Materials 16 06192 g009
Figure 10. Typical structural network of an LSTM model.
Figure 10. Typical structural network of an LSTM model.
Materials 16 06192 g010
Figure 11. The data transmission process of the LSTM unit.
Figure 11. The data transmission process of the LSTM unit.
Materials 16 06192 g011
Figure 12. The flow chart of the PSO-optimized LSTM neural network.
Figure 12. The flow chart of the PSO-optimized LSTM neural network.
Materials 16 06192 g012
Figure 13. The training process of the PSO-LSTM algorithm.
Figure 13. The training process of the PSO-LSTM algorithm.
Materials 16 06192 g013
Figure 14. Comparison of the experimental true stress and predicted results of the PSO-LSTM model at (a) ε ˙ = 10 s−1; (b) ε ˙ = 1 s−1; (c) ε ˙ = 0.1   s 1 ; (d) ε ˙ = 0.01 s−1.
Figure 14. Comparison of the experimental true stress and predicted results of the PSO-LSTM model at (a) ε ˙ = 10 s−1; (b) ε ˙ = 1 s−1; (c) ε ˙ = 0.1   s 1 ; (d) ε ˙ = 0.01 s−1.
Materials 16 06192 g014aMaterials 16 06192 g014b
Figure 15. The relationship between the experimental stresses and predicted value by: (a) the PB constitutive model; (b) the PSO-LSTM model. (The black dots represent the forecasted data and the straight lines represent the standard lines).
Figure 15. The relationship between the experimental stresses and predicted value by: (a) the PB constitutive model; (b) the PSO-LSTM model. (The black dots represent the forecasted data and the straight lines represent the standard lines).
Materials 16 06192 g015
Table 1. Composition of the experimental Hastelloy C276 alloy (wt. %).
Table 1. Composition of the experimental Hastelloy C276 alloy (wt. %).
ElementsCSiCrMoFeCoWVPSNi
Contents0.0070.0615.816.26.51.94.20.300.0350.025Bal.
Table 2. The calibrated material parameters.
Table 2. The calibrated material parameters.
Material ParameterValueMaterial ParameterValue
Aw1.696Av206,710.508
Qw (kJ/mol)294.993Qv (kJ/mol)247.962
nw0.118nv−0.431
Ag0.002AX0.004
Qg (kJ/mol)336.114QX (kJ/mol)249.845
ng0.306nX0.366
Ay128.233ny7.643
Qy (kJ/mol)573,636.89ny3.907 × 10−22
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

He, D.; Chen, S.; Lin, Y.; Yan, X.; Liu, G. Hot Deformation Behavior of Hastelloy C276 Alloy: Microstructural Variation and Constitutive Models. Materials 2023, 16, 6192. https://doi.org/10.3390/ma16186192

AMA Style

He D, Chen S, Lin Y, Yan X, Liu G. Hot Deformation Behavior of Hastelloy C276 Alloy: Microstructural Variation and Constitutive Models. Materials. 2023; 16(18):6192. https://doi.org/10.3390/ma16186192

Chicago/Turabian Style

He, Daoguang, Shibing Chen, Yongcheng Lin, Xintao Yan, and Guan Liu. 2023. "Hot Deformation Behavior of Hastelloy C276 Alloy: Microstructural Variation and Constitutive Models" Materials 16, no. 18: 6192. https://doi.org/10.3390/ma16186192

APA Style

He, D., Chen, S., Lin, Y., Yan, X., & Liu, G. (2023). Hot Deformation Behavior of Hastelloy C276 Alloy: Microstructural Variation and Constitutive Models. Materials, 16(18), 6192. https://doi.org/10.3390/ma16186192

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop