Next Article in Journal
Understanding the Long-Term Vegetation Dynamics of North Korea and Their Impact on the Thermal Environment
Next Article in Special Issue
Compression of Acetylated Beech (Fagus sylvatica L.) Laminated Veneer Lumber (LVL)
Previous Article in Journal
Predicting Climate Change Impacts on the Rare and Endangered Horsfieldia tetratepala in China
Previous Article in Special Issue
Potential of Using Natural and Synthetic Binder in Wood Composites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Physical Properties of Hydrothermally Treated Rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] in Different Buffered Media

by
Md. Rowson Ali
1,2,
Ummi Hani Abdullah
1,3,*,
Zaidon Ashaari
1,
Lee Seng Hua
3,
Norul Hisham Hamid
1,3 and
Siti Hasnah Kamarudin
4
1
Department of Wood and Fiber Industries, Faculty of Forestry and Environment, Universiti Putra Malaysia, Serdang 43400, Selangor, Malaysia
2
Seasoning and Timber Physics Division, Bangladesh Forest Research Institute, Chattogram 4217, Bangladesh
3
Institute of Tropical Forestry and Forest Products (INTROP), Universiti Putra Malaysia, Serdang 43400, Selangor, Malaysia
4
Department of Ecotechnology, School of Industrial Technology, Faculty of Applied Science, UiTM Shah Alam, Shah Alam 40450, Selangor, Malaysia
*
Author to whom correspondence should be addressed.
Forests 2022, 13(7), 1052; https://doi.org/10.3390/f13071052
Submission received: 23 May 2022 / Revised: 20 June 2022 / Accepted: 22 June 2022 / Published: 4 July 2022
(This article belongs to the Special Issue Frontiers in Modification of Wood and Wood-Based Composites)

Abstract

:
The dimensional instability of rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] is one of the major drawbacks that limits its utilization. Therefore, treatment is needed to improve these properties. Hydrothermal treatment in different buffered media is one of the techniques that improve its dimensional stability. The physical properties of hydrothermally treated rubberwood in different buffered media (pH 4, 6, 8, 10) and tap water (pH 7.43) with different temperatures (160 °C, 180 °C and 200 °C) were studied. In this study, physical properties such as equilibrium moisture content (EMC), density (ρ), mass loss (ML), water absorption (WA), volumetric swelling coefficient (VSC), thickness swelling (TS) and anti-swelling efficiency (ASE) were investigated for both treated and untreated specimens. Both the buffered media and temperature significantly affected the physical properties. The results indicated that the EMC (%), ρ (kg/m3), ML (%), VSC (%), TS (%) of treated rubberwood samples reduced as the treatment temperature increased. With the exception of WA (%), as WA increased when the treatment temperature increased from 160 °C to 180 °C but started to decrease when the temperature was further increased to 200 °C. The research study also exhibited that hydrothermal treatment using buffered media at different temperatures enhanced the dimensional stability of the treated samples. Alkaline media gave the best results on the physical properties compared to other treatment medias.

1. Introduction

Rubber trees [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] were introduced into Peninsular Malaysia more than a hundred years ago. Rubber trees are the main source of natural latex, a distinctive biopolymer of significant economic importance and an important commodity in Southeast Asian countries [1]. The rubber tree is commonly cut down after 30 years when its latex production capability starts to slow down and it stops being economical. Owing to its light color, rubberwood is a favorable wood for the production of furniture. However, rubberwood is a lignocellulosic material that is considered as non-homogeneous in nature and its density is not uniform [2]. One of the major drawbacks of rubberwood is its dimensional instability when in use [3]. To improve this disadvantage, thermal treatment can be employed and has been recognized as an effective technique to enhance the stability of this wood [4]. Unfortunately, a reduction in strength properties following thermal treatment is one of the major limitations.
Thermal treatment of wood can be carried out under different treating media such as air, nitrogen, water and oil [5,6]. Wood treated in different media results in varying property alterations. Dissimilarly to thermally treated wood under air conditions, the latter (nitrogen and oil) aims to block off the oxygen that would lead to an oxidative process, which reduces the strength of the treated wood. Thermal treatment using water as a treating medium is also of interest and is one of the most prominent thermal treatment techniques for wood [7,8]. Hydrothermal treatment is the most commercially advanced technique for treating wood [9]. It is an alternative way of treating wood without using chemicals and the wood’s properties can be enhanced considerably by converting hydrophilic (-OH) groups into more hydrophobic groups; it also reduces the wood’s equilibrium moisture content. In addition, it is different from other methods because of the existence of a hydrolysis step. Nowadays, hydrothermal treatment of wood has been implemented by several researchers [7,8,10,11]. The efficacy of hydrothermal treatment is mainly dependent on treatment temperature, duration and also the heating media [12]. When wood is treated using a hydrothermal treatment, some alterations are found such as the removal of extractives, the reduction of hydroxyl groups, the degradation of hemicellulose and a change in cellulose and lignin materials [13,14]. The presence of free water affects the chemical structure of thermally modified wood and heat is easily transferred into the wood. The wood’s properties can be improved considerably by converting hydrophilic (-OH) groups into more hydrophobic groups.
Hydrothermal treatment using buffered media is also known as an effective technique to control and neutralize the destructive effects of the acids that form through the destruction of carbohydrates during the treatment. A buffered solution is a non-chemical solution that does not pollute the environment [15,16]. Formic and acetic acid are generated during the thermal treatment of wood under moist conditions. Therefore, buffered solution is used in order to nullify the effect of the acid generated during thermal treatment [17]. The acidity or pH level of a hydrothermal medium may become more acidic due to hydrothermal treatment. The buffered medium can be used to ensure a lower change in pH level due to the hydrothermal process in order to control the destructive effects caused by the released acid [18,19]. Acidic conditions and high temperatures can degrade wood by hydrolysis. Under acidic conditions, the degradation rate of carbohydrates is high, which is promoted by the high availability and low crystallinity of hemicelluloses [19]. On the other side, an alkaline medium can control the degradation of hydroxyl (OH-) groups. Furthermore, buffered media, especially those of pH 7 and 8, neutralize the released acids and fix the pH to a neutral level. They also buffer the medium in hydrothermal treatment to a neutral level, which prevents strength loss and extends the usage of heat-treated beech (Fagus orientalis Lipsky) wood in load-bearing applications [20]. However, until now, information regarding the influence of more acidic and alkaline buffer solutions on the properties of wood is scarce. Several techniques have already been implemented to enhance the physical properties of rubberwood, such as thermal treatment, oil-heat treatment and chemical modification. However, there has been no scientific information available so far on the hydrothermal treatment of rubberwood using different buffered media, especially on physical properties. Therefore, the aim of this research work was to determine the effects of hydrothermal treatment using buffered media of varying pH levels and temperatures on the selected physical properties of rubberwood.

2. Materials and Methods

2.1. Buffer Preparation

An acidic buffer (pH 4, 6), an alkaline buffer (pH 8, 10) and tap water (pH 7.43) were selected as the hydrothermal treatment media. The buffer solutions were prepared by using disodium hydrogen phosphate (Na2HPO4·2H2O) and monosodium dihydrogen phosphate (NaH2PO4·2H2O). Hydrochloric acid and sodium hydroxide were used to adjust the pH of the buffered media. All the chemicals were purchased from R&M Chemicals, Malaysia.

2.2. Sample Preparation

Matured rubberwood logs, aged more than 25 years, were purchased from a rubberwood processing company in Pahang, Malaysia. Each girth of each log was 100–125 cm and divided into butt, middle and top positions. All the logs were fair and free from natural defects. The rubber logs were then processed and cut into sample sticks with dimensions of 300 mm × 20 mm × 20 mm (length × width × thickness) in longitudinal, tangential and radial measurements (Figure 1).
The sample sticks were predried to 10–11% moisture content (kiln dry basis) before hydrothermal treatments. In addition, the samples (having a density of around 650 kg/m3) were then randomly divided into 16 groups (15 hydrothermal treatment groups and 1 untreated group as a control). Each of the treatment groups had an equal number of replicates [21].

2.3. Heat Treatment

Hydrothermal treatment was carried out in the laboratory digester (model no: GDT-15L; origin country: Korea). The cylinders were filled with wood specimens and the aqueous media (tap water and buffer solutions) separately. The temperatures used were 160 °C, 180 °C and 200 °C and the treatment duration was 2 h. For each treatment, 10 samples were used. Other conditions were kept unchanged for all treatments. Untreated samples (controls) were used for comparison purposes. After heat treatment, the cylinders were gradually cooled to avoid any defects in the wood. The treated specimens were then placed in a conditioning room to attain equilibrium moisture content. The room temperature was about 28 °C and had a relative humidity (RH) of 75%. A total of 15–20 days were required for the samples to attain constant weights.

2.4. Color Changes

The color measurement was performed on the treated and untreated rubberwood samples. The surface colors of the specimens were measured using the Color Reader (CR-10, Minolta Co., Ltd.; made in Japan; 9229-1865-11) with an illuminated area of 8 mm before and after treatment. All color measurements were performed using conditions of the standard illuminant D65 with specular component included (SCI). Three measurements were taken at the middle position on each treated and untreated sample. Herein, measurements were performed on 3 samples. The color was defined using the CIE L*, a*, b* system, which was established by the International Commission on Illumination in 1976. This system comprises three perpendicular axes, where the color coordinate L* is the lightness from 0 (dark) to 100 (white) or the black–white relation, a* is the red–green factor and b* is the yellow–blue factor. The total color change ∆E* caused by the various treatments were calculated as follows:
Δ E = Δ L 2 + Δ a 2 + Δ b 2
where ΔL* is the change in value of the black–white coordinate, Δa* is the change in the value of the red–green coordinate and Δb* is the change in the yellow–blue coordinate.

2.5. Wet Chemical Analysis

For the evaluation of wet chemicals, 6 cm long conditioned splints were taken from each of the treated and untreated samples. Herein, the splints were ground into powder form. Afterwards, the particles were screened using a 40- to 60-mesh (0.4 to 0.6 mm) sieve in order to obtain homogeneous particle sizes. The powdered samples were then analysed for holocellulose, cellulose, hemicelluloses, lignin and extractive content.

2.6. Physical Properties

Physical properties were evaluated to assess the efficiency of the hydrothermal treatment in different buffered media. For the evaluation of physical properties, 10 samples were cut into dimensions of 20 mm × 20 mm × 20 mm after the treatments were performed. When all the samples reached a constant weight, equilibrium moisture content (EMC%), wood density ρ (kg/m3) and mass loss (ML%) were calculated by using the procedure given in the British-adopted European standard test method [22]. These properties were calculated as follows:
EMC   % = M u M O M O × 100
where EMC (%) is the equilibrium moisture content, MO  M O is the mass (g) of the oven-dried sample and M u is the mass (g) for the equilibrium moisture content state;
ML   % = W 1 OD W 2 OD W 2 OD × 100
where ML (%) is the mass loss (%),   W 1 OD   is the oven-dried weight (g) of the samples before treatment and W 2 OD   is the weight (g) of the oven-dried samples after treatment.
Water absorption (WA %), volumetric swelling coefficient ( VSC % ) , thickness swelling (TS%) and anti-swelling efficiency (ASE%) were calculated by using the equations below [23]:
WA   % = Wt Wo   Wo × 100
where, WA (%) is the water absorption (%), W t is the weight (g) of the wet samples after reconditioning and Wo is the weight (g) of the oven-dried samples;
VSC   % = Vw Vo   Vo × 100
where, VSC   % is the volumetric swelling coefficient, Vw is the green-state volume of the sample and Vo is the oven-dried volume of the sample. V is the volume calculated from the longitudinal (L), tangential (T) and radial (R) directions;
TS   % = T 2 T 1 T 1 × 100
where, TS   % is the thickness swelling, T 2 is the thickness of the saturated samples and T 1 is the oven-dried thickness of the samples (T is the thickness calculated from the tangential direction);
ASE   % = S u S t S u × 100
where, ASE   % is the anti- swelling coefficient, S u is the thickness swelling coefficient of the untreated samples and S t is the thickness swelling coefficient of the treated samples.

2.7. Statistical Analysis

The test results were analyzed by two-way analysis of variance (ANOVA) (CRD factorial) using SAS (Version 9.4) to evaluate the effect of the buffered media and temperature of the hydrothermal treatment on the physical properties of the rubberwood. The significant differences between the mean values of the testing groups were investigated using Tukey’s test (95% significant level).

3. Results and Discussion

3.1. Acidity Variation in Rubberwood

A pH meter was used to measure the acidity variation in the rubberwood samples before and after each hydrothermal treatment in different buffered media. Figure 2 depicts the pH change after hydrothermolysis in various buffered media and tap water at temperatures of 160 °C, 180 °C and 200 °C. The acidity of the wood samples varied according to pH and temperature. After treatment, the wood became more acidic. Regardless of buffered media, samples treated at 160 °C showed a pH range of 3.97 to 7.18 while samples treated at 200 °C had a pH range of 3.15 to 4.66. The trends indicated that the acidity of the wood increased along with an increasing treatment temperature. These findings supported a previous study in which the authors discovered a change in acidity from pH 6.7 (water) to 3.49 and pH 8.0 to 6.85 as samples were treated at 140 °C for 2 h [24].
The removal of carbonic acids and acetic acid caused by the breaking of acetyl groups in hemicellulose increases the acidity of the wood during hydrothermal treatment [7,25]. According to Tjeerdsma et al. [26], the formation of formic and acetic acid during moist thermal treatment increases the acidity of the wood. The findings also demonstrated that hydrothermal treatment in buffered media could control the destructive effects and resist the formation of removed acid, which was consistent with previous research [18,27,28]. Furthermore, buffered media can neutralize and regulate the acidity of the media [29,30].

3.2. Color Changes of Rubberwood

Figure 3 displays the visual observation of the color changes of the rubberwood after being treated in different buffered media and temperatures.
The most visible effect of treatment was a darkening of the color of the wood. Figure 3 depicts photographs of wood samples treated with hydrothermal treatment at various temperatures in different buffered media (acidic, water and alkaline). As can be seen in Figure 3, increased treatment temperatures increased the intensity of discoloration. Different media exhibited color differences at low temperatures, but there were no discernible changes in color at high temperatures. Lower temperatures (160 and 180 °C) caused less color changes in pH 6, 8 and 10 compared to acidic and water media, while high temperatures (200 °C) caused the most color changes. The hydrothermal treatment changed the color of the sample significantly as the treatment temperature increased [31,32,33]. This finding was consistent with the research findings in [34]. Color changes (wood darkening) are frequently attributed to the formation of oxidation and degradation elements from wood components [35,36]. The decrease in lightness caused by thermal treatment primarily indicates the formation of several components that absorb visible light [37]. According to Chen et al. [36], the condensation reactions of lignin and some extractives, as well as the formation of biproducts, contribute to an increase in the intensity of red tone in wood samples. Table 1 shows the chromatic value changes of treated and control rubberwood samples.
The chromatic values L*, a* and b* were measured for evaluating the overall color changes (ΔE*). Table 1 shows that the lightness (L*) values of all treated wood samples decreased when compared to untreated wood, indicating that the wood darkened after treatment. The L* value of the untreated wood was 76.91. The L* value on the wood treated by hydrothermal treatment with different media decreased as the temperature increased. In general, treatment temperature had a greater impact on the darkening of wood than the buffered media. Rubberwood treated with pH 6 at 160 °C had the smallest reduction in L* value (52.43). Meanwhile, the most severe reduction in lightness was observed in rubberwood treated in tap water at 200 °C. The decrease in lightness with increasing temperature during the hydrothermal treatment in different buffered media in this work could be attributed to extractive migration on the wood surface [38].
Green–red coordinate (a*) values of the treated rubberwood increased after treatment at 160 °C and 180 °C in all buffered media (acidic, water and alkaline), indicating that the samples turned redder. However, when the samples were treated at 200 °C, the a* value decreased, indicating that the samples were beginning to turn green. The findings agreed with those of Cai et al. [39] and Lee et al. [40]. The samples treated at 160 °C in pH 6 had the highest a* value, while the samples treated at 200 °C in pH 4.0 had the lowest a* value. The treatment, on the other hand, reduced the yellow–blue coordinate (b*) values. A decrease in b* indicated that the samples became bluer after treatment. Similarly, the highest b* value was recorded in pH 6 media at 160 °C, while the lowest b* value was recorded in tap water media at 200 °C.
Previous studies found that treating the wood surface in different buffered media resulted in color changes due to the removal of extractives, hydrolysis of hemicellulose and oxidation of these components [38,41,42]. To validate the color changes of the wood, the total color differences ΔE* were calculated, which involved changing all color coordinates (ΔL*, Δa*, Δb*). The E* value gradually increased with increasing treatment temperature, as shown in Table 1. Different media displayed different values of ΔE*. The greater color changes caused by hydrothermal treatments in the water media compared to other media (acidic, alkaline) were due to a greater contribution from the chromaticity coordinates, namely ΔL*, Δa* and Δb*. Overall, E* increased as the treatment temperature increased and the effect of the buffered media was less noticeable.

3.3. Physical Properties of Rubberwood

Equilibrium moisture content (EMC %), wood density ρ (kg/m3), mass loss (ML%), water absorption (WA%) and volumetric swelling coefficient (VSC%) were evaluated in this study. The equilibrium moisture content of treated and untreated rubberwood samples are presented in Table 2.
Table 2 shows that the highest and lowest EMC values of the treated rubberwood samples were 9.05% in pH 8 at 160 °C and 7.03% in pH 4.0 at 200 °C, respectively, while the untreated sample (control) had a value of 10%. There was a significant difference between the samples treated in buffered media with different pH values. As the reduction in EMC of the wood was directly proportional to the intensification of temperature [43], treatment temperatures were found to be a more influential factor in reducing the EMC of the treated samples. On the other hand, alkaline media (pH 8, 10) reduced EMC the least. The main reason for the decrease in EMC was the loss of hydroxyl groups after heat treatment. Due to the lack of these hydroxyl groups, the cell walls were able to absorb less water [44]. Furthermore, the decrease in EMC could be caused by increased cellulose crystallinity, which reduces the availability of hydroxyl (OH-) groups to water molecules [30,31]. The hydrothermal treatment might have an effect on the chemical constituents of the rubberwood samples. When compared to cellulose and lignin, the degradation of OH- groups in hemicellulose occurred even at low temperatures [44]. As a result of the degradation of OH- groups from hemicelluloses, the treated samples had lower EMCs than the untreated samples. As hemicelluloses contain a greater number of OH- groups than cellulose and lignin components, they are more hygroscopic. Table 3 shows the effects of the hydrothermal treatment in various media (acidic, water, alkaline) on the content of holocellulose, cellulose, hemicellulose, lignin and extractives in the rubberwood. A reduction in hemicellulose content after treatment was observed, ranging from 18.78% to 39.50% compared to that of 39.97% in the control samples.
Table 4 shows the density of the rubberwood before and after treatment in different buffered media. Before treatment, the average density of the rubberwood was 644.94 kg/m3. After treatment, the density of the rubberwood decreased to a different extent. Generally, the reduction in density increased along with increasing temperature. It was observed that the rubberwood treated with the acidic medium (pH 4) had the highest density reduction, particularly those treated at 200 °C, which experienced a 16.3% reduction in density compared to that of untreated samples. Samples treated with an alkaline medium (pH 8 and pH 10) experienced a lower reduction in density. The lowest density reduction of 0.5% was recorded in the samples treated in pH 8 at 160 °C. These findings were in line with previous work where the authors reported density losses that ranged from 1.89%–5.67% in different media (water, acidic, neutral, alkaline) at 160 °C and 2.96%–7.84% at 180 °C, respectively [20].
Mass loss (ML%) of hydrothermally treated rubberwood samples is presented in Figure 4. Mass loss increased along with the increasing treatment temperature.
Temperatures of 200 °C in pH 4 (25.39%) and 160 °C in pH 8 (2.58%) resulted in the highest and lowest percentage of mass loss, respectively. According to Tjeerdsma et al. [26], acidic hydrolysis at various hydrothermal treatments can significantly increase the degradation rate of wood polymers. According to Theander and Nelson [19], the degradation rate of carbohydrates is high in acidic conditions, which is facilitated by the high availability and low crystallinity of hemicelluloses. In general, the exclusion of hydrogen (H+) and hydroxide (-OH) ions in hydrothermal treatment has no effect on the pH of the hydrothermally treated medium. Furthermore, in hydrothermal treatments using buffered media, the pH can be kept constant at a certain level and the destructive effects of the released acid can be controlled [29].
Untreated samples had a water absorption (WA) of 20.5%. The samples treated in pH 8 at 180 °C had the highest WA value of 25.02%, while the samples treated in pH 4 at 200 °C had the lowest WA value of 22.42% (Table 5). It is worth noting that WA increased as the treatment temperature increased from 160 °C to 180 °C, but began to decrease as the temperature was raised to 200 °C. This phenomenon might be explained by heat-induced damage within the wood structure. This study’s findings were consistent with previous studies [5,42,43]. Figure 5 shows the cracks that occurred on the samples after being treated at a higher temperature of 200 °C.
Table 6 shows the effects of pH and treatment temperature on the VSC of untreated and treated rubberwood. The VSC of the hydrothermally treated rubberwood was lower than that of the untreated samples (8.09%). When the samples were treated in pH 8 at 200 °C, the lowest VSC value of 6.97% was observed. Similarly, as the treatment temperature increased, the VSC values decreased. Lower VSC values indicated that the samples are more dimensionally stable. In general, alkaline-treated samples had lower VSC values and, thus, better dimensional stability.
TS and ASE of the treated and untreated rubberwood samples are presented in Table 7.
TS and ASE values varied according to pH and temperature. The hydrothermally treated rubberwood samples had lower TS values than the control samples. The highest TS value for the treated samples was 3.47% at 160 °C in pH 4, while the lowest TS (2.95%) was recorded in the samples treated at 200 °C in pH 8. According to Table 7, the ASE values of the samples ranged from 7.23 to 13.91% (pH 4.0, 160–200 °C), 12.85–18.17% (pH 6.0, 160–200 °C), 8.33 to 16.82% (tap water, 160–200 °C), 16.05 to 21.18% (pH 8.0, 160–200 °C) and 15.13 to 20.06% (pH 10.0, 160–200 °C). Furthermore, both the treatment temperature and the buffered media had a significant effect on ASE values. The samples treated in alkaline media had a lower TS than the samples treated in acidic and water media. These observations were in agreement with the finding that was revealed by Ebadi et al. [18].

4. Conclusions

The changes in selected physical properties of rubberwood caused by hydrothermal treatment in different pH-buffered media at different temperatures were investigated in this study. The study’s findings revealed that the acidity of the treated medium increased after hydrothermal treatment in various buffered media. It was found that the buffer solution could reduce and control the destructive effect of acid on the wood components. After hydrothermal modification, there were clear variations in wood acidity. Furthermore, the equilibrium moisture content decreased, which might have had an impact on the decrements in wood quality. According to the findings of the study, hydrothermal treatment could improve the dimensional stability of rubberwood. Wood density was reduced after hydrothermal treatment and was found to be minimal in alkaline media. Mass loss was caused by the degradation of hemicellulose and extractives content, and mass loss was directly proportional to the decline of density and strength properties. It also affected the wood color, and the color changes of rubberwood become darker after treatment. As alkaline media could control the destructive effects of released acid, minimal mass loss was observed when compared to other treatment media. Furthermore, the neutralization effect of buffered media could control the rate of carbohydrate degradation and medium acidity, which could help to improve some of the wood’s properties. Among the treatment media, alkaline media at a lower temperature was selected as the best treatment condition to improve the performance of some of the rubberwood’s physical properties.

Author Contributions

Conceptualization, M.R.A., U.H.A. and Z.A.; methodology, M.R.A., U.H.A. and L.S.H.; formal analysis, M.R.A.; investigation, M.R.A., U.H.A., L.S.H., N.H.H. and S.H.K. writing—original draft preparation, M.R.A.; writing—review and editing, U.H.A.; supervision, U.H.A., L.S.H. and Z.A. All authors have read and agreed to the published version of the manuscript.

Funding

This study was funded by the National Agricultural Technology Program-Phase II (NATP-2), Bangladesh Agricultural Research Council (BARC), Bangladesh (Research Vote No. 6282522).

Acknowledgments

The authors are thankful to the authority of the Ministry of Environment, Forest and Climate Change, Bangladesh, the Bangladesh Forest Research Institute, Chattogram for allowing M.R.A. to attend the PhD program and Phase II of National Agricultural Technology Program (NATP-2), Bangladesh Agricultural Research Council (BARC) for the financial support to accomplish this research work. In addition, the authors would like to gratefully thank the technicians and scientific associates from the Faculty of Forestry and Environment and Institute of Tropical Forestry and Forest Products, Universiti Putra Malaysia for providing their assistance.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Hakimi, N.M.F.; Lee, S.H.; Lum, W.C.; Mohamad, S.F.; Osman Al Edrus, S.S.; Park, B.-D.; Azmi, A. Surface Modified Nanocellulose and Its Reinforcement in Natural Rubber Matrix Nanocomposites: A Review. Polymers 2021, 13, 3241. [Google Scholar] [CrossRef]
  2. Teoh, Y.P.; Don, M.M.; Ujang, S. Assessment of the properties, utilization, and preservation of rubberwood Assessment of the properties, utilization, and preservation of rubberwood (Hevea brasiliensis): A case study in Malaysia. J. Wood Sci. 2011, 57, 255–266. [Google Scholar] [CrossRef]
  3. Umar, I.; Zaidon, A.; Lee, S.H.; Halis, R. Oil-heat treatment of rubberwood for optimum changes in chemical constituents and decay resistance. J. Trop. For. Sci. 2016, 28, 88–96. [Google Scholar]
  4. H’ng, P.S.; Lee, S.H.; Lum, W.C. Effect of post heat treatment on dimensional stability of UF bonded particleboard. Asian J. Appl. Sci. 2012, 5, 299–306. [Google Scholar] [CrossRef] [Green Version]
  5. Dahali, R.; Lee, S.H.; Ashaari, Z.; Bakar, E.S.; Ariffin, H.; Khoo, P.S.; Bawon, P.; Salleh, Q.N. Durability of Superheated Steam-Treated Light Red Meranti (Shorea spp.) and Kedondong (Canarium spp.) Wood against White Rot Fungus and Sub-terranean Termite. Sustainability 2020, 12, 4431. [Google Scholar] [CrossRef]
  6. Lee, S.H.; Ashaari, Z.; Lum, W.C.; Halip, J.A.; Ang, A.F.; Tan, L.P.; Chin, K.L.; Tahir, P.M. Thermal treatment of wood using vegetable oils: A review. Constr. Build. Mater. 2018, 181, 408–419. [Google Scholar] [CrossRef]
  7. Tjeerdsma, B.F.; Militz, H. Chemical Changes in Hydrothermal Treated Wood: FTIR Analysis of Combined Hydrothermal and Dry Heat- Treated Wood Wood. Holz Als Roh-Und Werkst. 2005, 63, 102–111. [Google Scholar] [CrossRef]
  8. Endo, K.; Obataya, E.; Zeniya, N.; Matsuo, M. Effects of Heating Humidity on the Physical Properties of Hydrothermally Treated Spruce Wood. Wood Sci. Technol. 2016, 50, 1161–1179. [Google Scholar] [CrossRef] [Green Version]
  9. Hill, C.A.S. Wood Modification: Chemical, Thermal and Other Processes; John Wiley & Sons: Hoboken, NJ, USA, 2006. [Google Scholar] [CrossRef]
  10. Ali, M.R.; Abdullah, U.H.; Ashaari, Z.; Hamid, N.H.; Hua, L.S. Hydrothermal Modification of Wood: A Review. Polymers 2021, 13, 2612. [Google Scholar] [CrossRef]
  11. Rahimi, S.; Singh, K.; DeVallance, D. Effect of different hydrothermal treatments (steam and hot compressed water) on physical properties and drying behavior of yellow-poplar (Liriodendron tulipifera). For. Prod. J. 2019, 69, 42–52. [Google Scholar] [CrossRef]
  12. Saliman, M.A.R.; Ashaari, Z.; Bakar, E.S.; Hua, L.S.; Tahir, P.M.; Halip, J.A.; Leemon, N.F. Hydrothermal treatment of oil palm wood: Effect of treatment variables on dimensional stability using response surface methodology. J. Oil Palm Res. 2017, 29, 130–135. [Google Scholar] [CrossRef] [Green Version]
  13. Garrote, G.; Domínguez, H.; Parajó, J.C. Hydrothermal processing of lignocellulosic materials. Holz Als Roh-Und Werkst. 1999, 57, 191–202. [Google Scholar] [CrossRef]
  14. Sandberg, D.; Navi, P. Introduction to Thermo-Hydro-Mechanical (THM) Wood Processing; Växjö Universitet Skog & Trä: Kalmar, Sweden, 2007; ISBN 9789176365618. [Google Scholar]
  15. Fukuta, S.; Asada, F.; Sasaki, Y. Manufacture of compressed wood fixed by phenolic resin impregnation through drilled holes. J. Wood Sci. 2008, 54, 100–106. [Google Scholar] [CrossRef]
  16. Bakar, B.F.A.; Tahir, P.M.; Karimi, A.; Bakar, E.S.; Uyup, M.K.A.; Yong Choo, A.C. Evaluations of some physical properties for oil palm as alternative biomass resources. Wood Mater. Sci. Eng. 2013, 8, 119–128. [Google Scholar] [CrossRef] [Green Version]
  17. Ebadi, S.E.; Karimi, A.; Choo, A.C.Y.; Ashari, Z.; Naji, H.R.; Soltani, M.; Ridzuan, S.M.A. Physical Behavior of Hydro-thermally Treated Oil Palm Wood in Different Buffered pH Media. BioResources 2015, 10, 5317–5329. [Google Scholar] [CrossRef] [Green Version]
  18. Theander, O.; Nelson, D.A. Aqueous, high-temperature transformation of carbohydrates relative to utilization of biomass. Adv. Carbohydr. Chem. Biochem. 1988, 46, 273–326. [Google Scholar] [CrossRef]
  19. Talaei, A.; Karimi, A. Compression Strength, Hardness and Shear Strength of Heat Treated Beech (Fagus Orientalis) Wood in Buffered Mediums. Int. J. Mech. Prod. Eng. 2015, 3, 6–9. [Google Scholar]
  20. Yang, T.H.; Chang, F.R.; Lin, C.J.; Chang, F.C. Effects of temperature and duration of heat treatment on the physical, surface, and mechanical properties of japanese cedar wood. BioResources 2016, 11, 3947–3963. [Google Scholar] [CrossRef]
  21. BS 373; Methods of Testing Small Clear Specimens of Timber. British Standards Institution: London, UK, 1957; ISBN 1260995011.
  22. Rasdianah, D.; Zaidon, A.; Hidayah, A.; Lee, S.H. Effects of superheated steam treatment on the physical and mechanical properties of light red meranti and kedondong wood. J. Trop. For. Sci. 2018, 30, 384–392. [Google Scholar] [CrossRef]
  23. Ebadi, S.E.; Ashaari, Z.; Naji, H.R.; Jawaid, M.; Soltani, M.; San, H.P. Mechanical behavior of hydrothermally treated oil palm wood in different buffered ph media. Wood Fiber Sci. 2016, 48, 1–9. [Google Scholar]
  24. Sundqvist, B.; Karlsson, O.; Westermark, U. Determination of formic-acid and acetic acid concentrations formed during hydrothermal treatment of birch wood and its relation to colour, strength and hardness and hardness. Wood Sci. Technol. 2006, 40, 549–561. [Google Scholar] [CrossRef]
  25. Tjeerdsma, B.F.; Boonstra, M.; Pizzi, A.; Tekely, P.; Militz, H. Characterisation of thermally modified wood: Molecular reasons for wood performance improvement. Holz Als Roh-Und Werkst. 1998, 56, 149–153. [Google Scholar] [CrossRef]
  26. Talaei, A.; Karimi, A. Chemical analysis of hydrothermally treated beech wood in buffered mediums. In Proceedings of the IRG43 Conference, Kuala Lumpur, Malaysia, 6–10 May 2012. [Google Scholar]
  27. Taghiyari, H.R.; Rangavar, H.; Bibalan, O.F. Effect of nano-silver on reduction of hot-pressing time and improvement in physical and mechanical properties of particleboard. BioResources 2011, 6, 4067–4075. [Google Scholar] [CrossRef]
  28. Talaei, A. Effects of Hydrothermal Treatment in Buffered Medium on Natural Durability and Mechanical Properties of Beech Wood; University of Tehran: Tehran, Iran, 2010. [Google Scholar]
  29. Talaei, A.; Karimi, A.; Thevenon, M.F. Influence of heat treatment medium on fungal resistance of beech wood. In Proceedings of the International Research Group on Wood Preservation, IRG/WP 13-40643, Stockholm, Sweden, 16–20 June 2013. [Google Scholar]
  30. Cai, S.; Zhang, N.; Li, K.; Li, Y.; Wang, X.; Cai, S. Effect of pressurized hot water treatment on the mechanical properties, surface color, chemical composition and Crystallinity of pine wood. Wood Res. 2019, 64, 389–400. [Google Scholar]
  31. Geffer, A.; Geffertová, J.; Výbohová, E.; Dudiak, M. Impact of steaming mode on chemical characteristics and colour of birch wood. Forests 2020, 11, 478. [Google Scholar] [CrossRef] [Green Version]
  32. Wu, Z.; Deng, X.; Li, L.; Xi, X.; Tian, M.; Yu, L.; Zhang, B. Effects of Heat Treatment on Interfacial Properties of Pinus Massoniana Wood. Coatings 2021, 11, 543. [Google Scholar] [CrossRef]
  33. Shi, J.; Lu, Y.; Zhang, Y.; Cai, L.; Shi, S.Q. Effect of thermal treatment with water, H2SO4 and NaOH aqueous solution on color, cell wall and chemical structure of poplar wood. Sci. Rep. 2018, 8, 17735. [Google Scholar] [CrossRef]
  34. Bekhta, P.; Niemz, P. Effect of high temperature on the change in color, dimensional stability and mechanical properties of spruce wood. Holzforschung 2003, 57, 539–546. [Google Scholar] [CrossRef]
  35. Chen, Y.; Gao, J.; Fan, Y.; Tshabalala, M.A.; Stark, N.M. To Heat-induced chemical and color changes of extractive-freeblacklocust (Rosinia pseudoacacia) Wood. BioResources 2012, 7, 2236–2248. [Google Scholar]
  36. Srinivas, K.; Pandey, K.K. Effect of heat treatment on color changes, dimensional stability, and mechanical properties of wood. J. Wood Chem. Technol. 2012, 32, 304–316. [Google Scholar] [CrossRef]
  37. Sundqvist, B.; Morén, T. The influence of wood polymers and extractives on wood colour induced by hydrothermal treatment. Holz Als Roh-Und Werkst. 2002, 60, 375–376. [Google Scholar] [CrossRef]
  38. Fan, Y.; Gao, J.; Chen, Y. Colour responses of black locust (Robinia pseudoacacia L.) to solvent extraction and heat treatment. Wood Sci. Technol. 2010, 44, 667–678. [Google Scholar] [CrossRef]
  39. Lee, S.H.; Zaidon, A.; Rasdianah, D.; Lum, W.C.; Aisyah, H.A. Alteration in colour and fungal resistance of thermally treated oil palm trunk and rubberwood particleboard using palm oil. J. Oil Palm Res. 2020, 32, 83–89. [Google Scholar]
  40. Dzurenda, L. Modification of wood colour of fagus sylvatica l. to a brown-pink shade caused by thermal treatment. Wood Res. 2013, 58, 475–482. [Google Scholar]
  41. Kamperidou, V.; Barboutis, I.; Vasileiou, V. Response of colour and hygroscopic properties of Scots pine wood to thermal treatment. J. For. Res. 2013, 24, 571–575. [Google Scholar] [CrossRef]
  42. Lee, S.H.; Zaidon, A.; Lum, W.C.; San, H.P.; Peng, T.L.; Jinn, C.M.; Chai, E.W.; Ling, C.K. Properties of particleboard with oil palm trunk as core layer in comparison to three-layer rubberwood particleboard. J. Oil Palm Res. 2015, 27, 67–74. [Google Scholar]
  43. Jamsa, S.; Viitaniemi, P. Heat treatment of wood better durability without chemicals. In Proceedings of the Special Seminar: Review on Heat Treatments of Wood; Rapp, A.O., Ed.; The European Commission: Brussels, Belgium, 2001; pp. 17–22. [Google Scholar]
  44. Wikberg, H.; Maunu, S.L. Characterisation of thermally modified hard—And softwoods by13C CPMAS NMR. Carbohydr. Polym. 2004, 58, 461–466. [Google Scholar] [CrossRef]
Figure 1. Photograph of prepared rubberwood samples with dimensions of 300 mm × 20 mm × 20 mm (length × width × thickness) for hydrothermal treatment.
Figure 1. Photograph of prepared rubberwood samples with dimensions of 300 mm × 20 mm × 20 mm (length × width × thickness) for hydrothermal treatment.
Forests 13 01052 g001
Figure 2. The acidity variation of samples in buffered media and tap water after the hydrothermal treatment.
Figure 2. The acidity variation of samples in buffered media and tap water after the hydrothermal treatment.
Forests 13 01052 g002
Figure 3. Visual observation of the color changes of untreated and hydrothermally treated rubberwood samples.
Figure 3. Visual observation of the color changes of untreated and hydrothermally treated rubberwood samples.
Forests 13 01052 g003
Figure 4. Mass loss (ML%) variations of treated and untreated (control) rubberwood samples in buffered media after the hydrothermal treatment.
Figure 4. Mass loss (ML%) variations of treated and untreated (control) rubberwood samples in buffered media after the hydrothermal treatment.
Forests 13 01052 g004
Figure 5. Visual appearance of untreated and treated rubberwood at different temperatures.
Figure 5. Visual appearance of untreated and treated rubberwood at different temperatures.
Forests 13 01052 g005
Table 1. Changes in chromatic value of treated and untreated samples of rubberwood.
Table 1. Changes in chromatic value of treated and untreated samples of rubberwood.
GroupTemp. in °CLightness (L*)Red–Green Factor (a*)Yellow–Blue Factor (b*)ΔE*
Control-76.91 a (0.95)4.97 e (0.84)21.69 a (1.57)-
pH 416046.85 c (1.76)9.52 a (0.10)13.60 cd (0.72)31.46
18041.94 e (0.58)6.79 d (0.50)8.28 fg (0.99)37.50
20033.82 f (0.18)0.58 f (0.31)0.04 hi (0.20)48.42
pH 616052.43 b (1.01)9.46 a (0.40)16.94 b (0.52)25.34
18041.66 e (0.66)7.37 cd (0.26)9.72 fg (0.90)37.31
20034.84 f (0.31)1.20 f (0.13)0.89 hi (0.07)47.08
* Tap water16043.78 de (0.79)8.21 abcd (0.30)11.08 def (0.16)34.93
18041.30 e (1.07)6.90 d (0.45)7.69 g (0.97)38.32
20033.62 f (0.45)2.20 f (0.44)−1.23 i (0.20)49.06
pH 816050.84 b (0.80)9.27 ab (0.09)15.42 bc (0.22)27.15
18045.13 cd (0.79)8.38 abcd (0.62)12.86 cde (0.81)33.17
20034.51 f (0.85)2.14 f (0.24)1.97 h (0.15)46.85
pH 1016045.88 cd (0.89)8.77 abc (0.24)13.61 cd (0.79)32.30
18041.09 e (1.12)7.78 bcd (0.69)10.21 efg (1.68)37.74
20034.82 f (0.17)2.21 f (0.46)1.91 h (0.29)46.59
[Note: * denotes pH 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Table 2. EMC of treated and untreated samples of rubberwood at 28 °C and 65% RH.
Table 2. EMC of treated and untreated samples of rubberwood at 28 °C and 65% RH.
GroupTemp. in °CEquilibrium Moisture Content (EMC%)
Control-10.00 a (0.30)
pH 41608.52 d (0.18)
1807.20 efg (0.17)
2007.03 g (0.10)
pH 61608.79 bc (0.45)
1807.39 efg (0.16)
2007.13 fg (0.10)
* Tap water1608.64 cd (0.24)
1807.32 efg (0.17)
2007.10 g (0.12)
pH 81609.05 b (0.16)
1807.57 e (0.18)
2007.39 efg (0.14)
pH 101608.96 bc (0.19)
1807.49 ef (0.20)
2007.23 efg (0.14)
[Note: * denotes pH 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Table 3. Chemical analysis of treated and untreated rubberwood.
Table 3. Chemical analysis of treated and untreated rubberwood.
GroupTemp. in °CHolocellulose (%)Cellulose (%)Hemicellulose (%)Lignin (%)Extractives (%)
Control-77.3837.4139.9728.132.59
pH 4160 °C74.4945.8928.5930.964.78
180 °C72.1451.4220.7230.187.30
200 °C70.5147.0623.4532.169.80
pH 6160 °C75.2337.6337.6029.134.52
180 °C73.0346.2326.8028.566.91
200 °C71.4142.0329.3829.008.13
Tap water (pH 7.43)160 °C74.8245.3329.4929.207.07
180 °C72.6153.8318.7827.129.93
200 °C70.9649.0621.9031.0912.01
pH 8160 °C76.8337.3339.5029.004.93
180 °C74.4143.2331.1829.006.18
200 °C71.7639.0832.6827.128.9
pH 10160 °C76.2337.838.4327.005.56
180 °C73.6344.5629.0725.007.86
200 °C71.1638.7832.3827.009.18
Table 4. Density of rubberwood before and after hydrothermal treatment at different temperatures and using buffered media.
Table 4. Density of rubberwood before and after hydrothermal treatment at different temperatures and using buffered media.
GroupTemp. in °CDensity, ρ (kg/m3)
Control-644.94 (15.11)
BeforeAfterReduction (%)
pH 4160644.48 (18.86)617.36 (14.4)4.2
180645.63(16.56)560.49 (11.0)13.2
200643.21 (16.11)538.13 (13.8)16.3
pH 6160645.14 (16.45)633.85 (14.8)1.8
180643.88 (20.82)579.33 (15.7)10.0
200644.34 (18.71)549.69 (15.8)14.7
* Tap water160644.41 (18.56)622.78 (18.0)3.4
180645.30 (15.6)575.75 (12.0)10.8
200645.56 (16.76)544.18 (13.6)15.7
pH 8160645.1 (20.32)641.72 (18.3)0.5
180644.6 (16.67)598.89 (12.8)7.1
200645.0 (19. 37)554.68 (13.1)14.0
pH 10160645.77 (19.98)638.9 (15.2)1.1
180643.94 (13.90)594.54 (14.9)7.7
200644.27 (17.49)551.0 (15.0)14.5
[Note: * denotes pH 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Table 5. WA of treated and untreated samples of rubberwood.
Table 5. WA of treated and untreated samples of rubberwood.
GroupTemp. in °CWater Absorption (WA%)
Control-20.56 g (0.46)
pH 416023.01 cdef (0.59)
18023.56 bcde (0.17)
20022.42 f (0.10)
pH 616023.99 abc (0.51)
18024.44 ab (1.06)
20022.72 def (0.73)
* Tap water16023.05 cdef (0.50)
18023.64 bcde (0.63)
20022.63 ef (0.74)
pH 816024.43 ab (1.03)
18025.02 a (1.01)
20023.78 bcd (0.78)
pH 1016024.36 ab (0.63)
18024.68 ab (0.72)
20023.03 cdef (0.86)
[Note: * denotes 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Table 6. Volumetric swelling coefficient of treated and untreated samples of rubberwood.
Table 6. Volumetric swelling coefficient of treated and untreated samples of rubberwood.
GroupTemp. in °CVolumetric Swelling Coefficient (VSC%)
Control-8.09 a (0.15)
pH 41607.68 b (0.19)
1807.47 bcd (0.23)
2007.44 bcdef (0.16)
pH 61607.54 bcdef (0.30)
1807.41 bcdef (0.19)
2007.28 defg (0.18)
* Tap water1607.66 bc (0.17)
1807.45 bcde (0.24)
2007.35 cdef (0.27)
pH 81607.41 bcdef (0.23)
1807.13 fg (0.22)
2006.97 g (0.12)
pH 101607.45 bcde (0.21)
1807.15 efg (0.16)
2007.0 g (0.12)
[Note: * denotes 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Table 7. Thickness swelling (TS) and anti-swelling efficiency (ASE) of treated and untreated samples of rubberwood.
Table 7. Thickness swelling (TS) and anti-swelling efficiency (ASE) of treated and untreated samples of rubberwood.
GroupTemp. in °CTS (%)ASE (%)
Control-3.74 a (0.25)-
pH 41603.47 b (0.04)7.23 j (0.90)
1803.33 bcd (0.05)11.07 hi (1.36)
2003.22 cde (0.08)13.91 efgh (1.67)
pH 61603.26 bcde (0.12)12.85 gh (2.28)
1803.13 def (0.10)16.38 cde (1.38)
2003.06 ef (0.11)18.17 bc (2.01)
* Tap water1603.43 bc (0.06)8.33 ij (1.38)
1803.25 bcde (0.10)13.19 fgh (2.80)
2003.11 def (0.06)16.82 cde (1.54)
pH 81603.14 def (0.08)16.05 cdef (2.31)
1803.07 ef (0.09)17.80 bcd (2.33)
2002.95 f (0.09)21.18 a (2.42)
pH 101603.17 def (0.06)15.13 defg (1.67)
1803.10 def (0.04)17.00 cd (1.16)
2002.99 f (0.08)20.06 ab (2.24)
[Note: * denotes 7.43 and means with different letters represent significant differences within groups at the 0.05 probability level by Tukey’s test. The values in parentheses represent the calculated standard deviation (SD)].
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Ali, M.R.; Abdullah, U.H.; Ashaari, Z.; Hua, L.S.; Hamid, N.H.; Kamarudin, S.H. Physical Properties of Hydrothermally Treated Rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] in Different Buffered Media. Forests 2022, 13, 1052. https://doi.org/10.3390/f13071052

AMA Style

Ali MR, Abdullah UH, Ashaari Z, Hua LS, Hamid NH, Kamarudin SH. Physical Properties of Hydrothermally Treated Rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] in Different Buffered Media. Forests. 2022; 13(7):1052. https://doi.org/10.3390/f13071052

Chicago/Turabian Style

Ali, Md. Rowson, Ummi Hani Abdullah, Zaidon Ashaari, Lee Seng Hua, Norul Hisham Hamid, and Siti Hasnah Kamarudin. 2022. "Physical Properties of Hydrothermally Treated Rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] in Different Buffered Media" Forests 13, no. 7: 1052. https://doi.org/10.3390/f13071052

APA Style

Ali, M. R., Abdullah, U. H., Ashaari, Z., Hua, L. S., Hamid, N. H., & Kamarudin, S. H. (2022). Physical Properties of Hydrothermally Treated Rubberwood [Hevea brasiliensis (Willd. ex A. Juss.) Müll. Arg.] in Different Buffered Media. Forests, 13(7), 1052. https://doi.org/10.3390/f13071052

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.