Next Article in Journal
Effect of Compost and Titanium Dioxide Application on the Vegetative Yield and Essential Oil Composition of Coriander
Previous Article in Journal
Physical Education Teachers’ Perceived Digital Competences: Are They Prepared for the Challenges of the New Digital Age?
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

Improvement of the EC Performance in LCP-MOF Electrode Materials by Succinic Anhydrate Addition to the Electrolyte

by
Mohamed Gaber Moustafa
1,2,*,
Abdelaziz Mohamed Aboraia
3,4,*,
Vera Butova
3,
Alexander Guda
3,
Fatma Elmasry
5,6 and
Alexander Soldatov
3
1
Physics Department, College of Science and Arts, Jouf University, Qurayat 75911, Saudi Arabia
2
Physics Department, Faculty of Science, Al-Azhar University, Cairo 11884, Egypt
3
The Smart Materials Research Institute, Southern Federal University, Sladkova 178/24, 344090 Rostov-on-Don, Russia
4
Physics Department, Faculty of Science, Al-Azhar University, Assiut 71542, Egypt
5
Physics Department, College of Science and Arts, Jouf University, Tabrjal 74713, Saudi Arabia
6
Department of Physics, Faculty of Science, Suez Canal University, Ismailia 41522, Egypt
*
Authors to whom correspondence should be addressed.
Sustainability 2022, 14(1), 323; https://doi.org/10.3390/su14010323
Submission received: 26 September 2021 / Revised: 19 December 2021 / Accepted: 22 December 2021 / Published: 29 December 2021

Abstract

:
The optimization of the electrolyte composition for a canonical cathode such as LiCoPO4 olivine. The implemented succinic anhydride within a liquid electrolyte LiPF6 and dissolved in carbonate/diethyl considerably improves the discharge capacity of the electrode are shown. The introduction of succinic anhydride into the solid/electrolyte interphase (SEI) layer is responsible for the improved electrochemical performance of the electrode. We used LiCoPO4@C-ZrO2 as a cathode to prove the concept. The observed results could be applied for a wide range of cathodes. Moreover, the proposed additive to the electrolyte could help evaluate the performance of the materials without the side effects of the electrolyte.

1. Introduction

One of the most promising olivine structures is LiCoPO4 (LCP) as a cathode material due to its high redox potential of around 4.8 V, its high energy density, and its theoretical capacity of ~167 mAhg−1 [1,2,3]. Nevertheless, it undergoes a low electrochemical performance for many reasons, such as its low lithium-ion and electronic conductivity and its high voltage effect on the lifetime of the electrolyte (stability) [4,5]. Several works have used LiPF6 as a standard electrolyte. However, it suffers from a low thermostability and a fast capacity fading because of the oxidation of the organic carbonate solvents at high voltages, and the decomposition of LiPF6 [6,7]. Regrettably, this degradation affects the electrochemical performance. In particular, once the working potential exceeds 4.4 V, it initiates a continuous reduction of the electrolyte due to an oxidative carbonate decomposition. Furthermore, the LiPF6 converts to PF5 and LiF under high voltage; thus, the cobalt is dissolved from and causes the structural collapse of the LCP, which is the result of undergoing from HF attack. Here, we report the protective effect of various amounts of succinic anhydride additive on LiPF6 electrolyte properties.

2. Experimental Work

UiO-66 Preparation

To synthesize UiO-66, we used the same technique from Ref. [4]. The ZrCl4 was dispersed in a DMF, then deionized water and benzoic acid (BA) were added and totally dissolved. The terephthalic acid (H2BDC) linker was poured into a solution with a molar ratio Zr:BDC:BA:H2O:DMF that was 1:1:10:3:300. The net solution was placed into a capped vessel in the oven for 24 h at 120 °C. When the temperature was cooled to room temperature, the white precipitate was washed with DMF once as well as methanol, and washed overnight at 100 °C. The size of the particle was ~100 nm and the area of the surface was 1500 m2 g1. The XRD confirmed that UiO-66 has a single phase, as shown in Figure S1.

3. LiCoPO4/C Coated by UiO-66 MOF Composite Preparation

The active material was prepared by a one-time facile method in three hours, as published elsewhere [4]. We used two solutions, A and B; since solution A consists of LiOH.H2O (0.0735 g), it was dispersed in 333 μL of deionized (DI) water plus ethylene glycol (6.67 mL). In solution B, we mixed LiOH.H2O (0.0420 g) with 1 mL DI water, H3PO4 (68.3 μL), 132 mL DI water, 0.2910 g of Co(NO3)2·6H2O, 1026 × 10−4 g of C6H12O6, and 145 × 10−3 g of the UiO-66, then it was mixed by a magnetic stirrer. In the end, we mixed solutions A and B into a Teflon vessel at 220 °C in a microwave (MARS) for three hours under 800 W. The final precipitate (blue color) was separated via centrifuging and washed once with water and three times with ethanol. The final product was activated under air for seven hours at 650 °C.

3.1. X-ray Characterization

The as-prepared sample was examined by the X-ray diffractometer D2 Phaser (Bruker, Germany) using Cu Kα1 radiation (λ = 1.540598 Å). The element analysis of the as-prepared samples was carried out by utilizing the Bruker M4-Tornado X-ray fluorescence spectrometer.

3.2. TEM Photos

The microstructures of the as-prepared samples were examined by the FEI Tecnai G2 Spirit TWIN transmission electron microscope, operated at an accelerating voltage of 80 kV.

3.3. Electrochemical Characterization

The electrochemical performance of LiCoPO4@UiO-66 was examined by galvanostatic lithiation/delithiation utilizing a P-20X potentiostat/galvanostat device (Elins, Russia). The active material (7.5 mg cm−2 load of active material) was mixed with carbon black 80% and 20%, respectively. The mixture was located in the cell as a half-cell of the cathode materials and the anode was lithium foil. The used separator was a glass microfiber filter and 1 M LiPF6 in EC/DMC = 50/50 (v/v) (Sigma-Aldrich) as an electrolyte, with different ratios of succinic anhydride as an additive (0 wt.%, 2 wt.%, 3 wt.%). The cell was collected under Ar in a glove bag purchased from Sigma-Aldrich, and the cycling was performed in 3–5.1 V with current C/10.

3.4. Result and Discussion

The sample was identified by X-ray diffraction. Figure 1 demonstrates the PXRD of LiCoPO4/c@UiO-66 nanoparticles, which were synthesized by the microwave-assisted solvothermal route. It exhibits that all peaks of (2 0 0), (1 0 0), (2 1 0), (2 0 1), (0 2 0), (3 0 1), (1 2 1), (4 0 1), and (2 3 1) planes were matched with Cod: 2300246. This result proved that the LCP/C@UiO-66 has a single orthorhombic phase with a Pnma space group without any additional peaks corresponding to other phases, and lattice parameters as follows: a = 10.2 Å, b = 5.9 Å, and c = 4.7 Å, as shown in Figure 1. A small amount of UiO-66 coated the LiCoPO4, thus the UiO-66 formed on the surface and did not appear in the XRD. The TEM photos confirmed the presence of some tiny crystals of ZrO2 on the surface of LiCoPO4, since the average size of LiCoPO4 is 100 nm, but the ZrO2 is around 9 nm, as exhibited in Figure 2a,b. To identify the type of the small particles, we used X-ray fluorescence spectroscopy, which confirmed a small concentration of Zr at around 3.7% and 67% of cobalt.
The cell was assembled under Ar by using the conventional liquid electrolyte LiPF6. The charge/discharge process of the LCP was carried out at C/10 in the voltage range 2.75–5.1 V. The result displayed that the initial discharge capacity of LCP without additives is around ~105 mAh.g−1. An increase in the concentration of additives enhances the electrochemical performance, as shown in Figure 3a. Since the discharge capacity with 2% of succinic anhydrate is around 120 mAh/g, a synergistic 3% of succinic anhydrate improved the first discharge capacity up to 147 mAh/g. Furthermore, from the first to the fourth cycles, a good enhancement in the electrochemical performance appears, as demonstrated in Figure 3b. Meanwhile, inserting a concentration of succinic anhydride of more than 3% stopped the electrochemical performance of the cell; therefore, we preferred the 3%, as seen in Figure S2.
Figure 4a–c show the comparisons of the electrochemical performance of LiCoPO4/C@UiO-66 with different concentrations of additives (succinic, 0%, 2%, and 3%). The enhancement in the electrochemical performance is apparent, and the discharge capacity of the sample without any additives was 105 mAh/g for the first cycle, as shown in Figure 4a. However, inserting 2% of the succinic led to an enhancement of the discharge capacity to 121 mAh/g, and 3% improved the discharge capacity to 147 mAh/g. Meanwhile, the concentration was limited to 3% because inserting more than 3% (such as 4% and 7%) stopped the discharge and the cycle was not completed; thus, the best concentration of succinic is 3%. The second cycle of LiCoPO4/C@UiO-66 with different concentrations of additives (succinic, 0%, 2%, and 3%) was improved from 60 to 119 mAh/g, as demonstrated in Figure 4a–c. We note that the fade in the discharge capacity of all the samples was improved, according to Figure 4a–c. An introduction of a small amount (3 wt.%) of succinic anhydrate into the liquid electrolyte could improve the electrochemical performance of the LiCoPO4@UiO-66 electrode during cycling without sacrificing the charge–discharge potential. This enhancement in the electrochemical performance of a LiCoPO4@UiO-66 electrode is found to be due to the modification of the SEI layer on the LCP surface with the introduction of the succinic anhydrate additive. The presence of succinic anhydrate can prevent the decomposition of the LiPF6 salt on the LCP surface.
To better understand what occurred for the active materials during the charge and discharge process, we measured the ex situ XAS for the LiCoPO4 coated by the UiO-66. The Co(II) is almost transformed to Co(III), thus nearly all of the lithium ions were extracted completely, as shown in Figure 5. We observed a two-step system in the first charge process, which implies the development of the intermediate Li0.7CoPO4 phase, as observed by Bramnik et al. [8].

4. Conclusions

The LiCoPO4 coated by UiO-66 was prepared by a microwave-assisted solvothermal route. The XRD proved that the LiCoPO4 coated by UiO-66 is a single-phase without any crystal impurities. The TEM images ensure that there are some nanoparticles of ZrO2 on the surface of LiCoPO4. The electrochemical performance of LiCoPO4 is low due to the performance of the LiPF6; thus, the incorporated succinic as an additive in the LiPF6 electrolyte led to the enhancement of the electrochemical performance of LiCoPO4/C coated by UiO-66 and a discharge capacity from 105 to 147 mAh/g. The best concentration of the succinic anhydrate additive was 3% in the LiPF6 electrolyte. Meanwhile, concentrations of more than 3% had side effects on the electrochemical performance. We observed a two-step system in the first charge process, which implies the development of the intermediate Li0.7CoPO4 phase.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/su14010323/s1, Figure S1: 1(a) Experimental (red) and calculated (black) profiles of the synthesized sample UiO-66. Vertical lines indicate calculated pick positions. A difference plot (blue) isprovided at the bottom. Figure S2: the electrochemical performance of LiCoPO4@UiO-66 with 4% addative.

Author Contributions

Conceptualization, A.M.A. and V.B.; methodology, A.M.A.; software, M.G.M.; validation, A.M.A., V.B. and A.G.; formal analysis, M.G.M.; investigation, F.E.; resources, M.G.M.; data curation, A.M.A.; writing—original draft preparation, A.M.A. and V.B.; writing—review and editing, M.G.M. and A.G.; visualization, A.M.A. and F.E.; su-pervision, A.S.; project administration, M.G.M.; funding acquisition, M.G.M. All authors have read and agreed to the published version of the manuscript.

Funding

Deputyship for Research and Innovation, Ministry of Education, Saudi Arabia, for funding this work through the project number “1470020316”.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors extend their appreciation to the Deputyship for Research and Innovation, Ministry of Education, Saudi Arabia, for funding this work through the project number “1470020316”. The authors would like to extend their sincere appreciation to the central laboratory at Jouf University for their support in this study.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Wu, X.; Meledina, M.; Tempel, H.; Kungl, H.; Mayer, J.; Eichel, R.-A. Morphology-controllable synthesis of LiCoPO4 and its influence on electrochemical performance for high-voltage lithium ion batteries. J. Power Sources 2020, 450, 227726. [Google Scholar] [CrossRef]
  2. Wu, X.; Lin, Y.; Ji, Y.; Zhou, D.; Liu, Z.; Sun, X. Insights into the Enhanced Catalytic Activity of Fe-Doped LiCoPO4 for the Oxygen Evolution Reaction. ACS Appl. Energy Mater. 2020, 3, 2959–2965. [Google Scholar] [CrossRef]
  3. Gnewuch, S.; Rodriguez, E.E. Distinguishing the Intrinsic Antiferromagnetism in Polycrystalline LiCoPO4 and LiMnPO4 Olivines. Inorg. Chem. 2020, 59, 5883–5895. [Google Scholar] [CrossRef] [PubMed]
  4. Aboraia, A.M.; Shapovalov, V.V.; Guda, A.A.; Butova, V.V.; Soldatov, A. One-pot coating of LiCoPO4/C by a UiO-66 metal–organic framework. RSC Adv. 2020, 10, 35206–35213. [Google Scholar] [CrossRef]
  5. Aboraia, A.M.; Shapovalov, V.V.; Guda, A.A.; Butova, V.V.; Zahran, H.Y.; Yahia, I.S.; Soldatov, A.V. Activation of LiCoPO4 in Air. J. Electron. Mater. 2021, 50, 3105–3110. [Google Scholar] [CrossRef]
  6. Han, J.-G.; Jeong, M.-Y.; Kim, K.; Park, C.; Sung, C.H.; Bak, D.W.; Kim, K.H.; Jeong, K.-M.; Choi, N.-S. An electrolyte additive capable of scavenging HF and PF5 enables fast charging of lithium-ion batteries in LiPF6-based electrolytes. J. Power Sources 2020, 446, 227366. [Google Scholar] [CrossRef]
  7. Tarnopolskiy, V.; Kalhoff, J.; Nádherná, M.; Bresser, D.; Picard, L.; Fabre, F.; Rey, M.; Passerini, S. Beneficial influence of succinic anhydride as electrolyte additive on the self-discharge of 5 V LiNi0.4Mn1.6O4 cathodes. J. Power Sources 2013, 236, 39–46. [Google Scholar] [CrossRef]
  8. Bramnik, N.N.; Nikolowski, K.; Baehtz, C.; Bramnik, K.G.; Ehrenberg, H. Phase Transitions Occurring upon Lithium Insertion−Extraction of LiCoPO4. Chem. Mater. 2007, 19, 908–915. [Google Scholar] [CrossRef] [Green Version]
Figure 1. PXRD of pure LiCoPO4 and LiCoPO4 coated by UiO-66.
Figure 1. PXRD of pure LiCoPO4 and LiCoPO4 coated by UiO-66.
Sustainability 14 00323 g001
Figure 2. (a) TEM photo of LiCoPO4@UiO-66. (b) The histogram of the small nano ZrO2 particle distribution.
Figure 2. (a) TEM photo of LiCoPO4@UiO-66. (b) The histogram of the small nano ZrO2 particle distribution.
Sustainability 14 00323 g002
Figure 3. (a) Comparison of the initial cycles of LiCoPO4/C@UiO-66 with different concentrations of additives (succinic). (b) Comparison of the ten cycles of LiCoPO4/C@UiO-66 with varying concentrations of additives.
Figure 3. (a) Comparison of the initial cycles of LiCoPO4/C@UiO-66 with different concentrations of additives (succinic). (b) Comparison of the ten cycles of LiCoPO4/C@UiO-66 with varying concentrations of additives.
Sustainability 14 00323 g003
Figure 4. First five cycles of (a) LiCoPO4 without additives, (b) LiCoPO4 with 2% additives, and (c) LiCoPO4 with 2% additives.
Figure 4. First five cycles of (a) LiCoPO4 without additives, (b) LiCoPO4 with 2% additives, and (c) LiCoPO4 with 2% additives.
Sustainability 14 00323 g004
Figure 5. The XAS for first cycle and last spectra of first discharge.
Figure 5. The XAS for first cycle and last spectra of first discharge.
Sustainability 14 00323 g005
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Moustafa, M.G.; Aboraia, A.M.; Butova, V.; Guda, A.; Elmasry, F.; Soldatov, A. Improvement of the EC Performance in LCP-MOF Electrode Materials by Succinic Anhydrate Addition to the Electrolyte. Sustainability 2022, 14, 323. https://doi.org/10.3390/su14010323

AMA Style

Moustafa MG, Aboraia AM, Butova V, Guda A, Elmasry F, Soldatov A. Improvement of the EC Performance in LCP-MOF Electrode Materials by Succinic Anhydrate Addition to the Electrolyte. Sustainability. 2022; 14(1):323. https://doi.org/10.3390/su14010323

Chicago/Turabian Style

Moustafa, Mohamed Gaber, Abdelaziz Mohamed Aboraia, Vera Butova, Alexander Guda, Fatma Elmasry, and Alexander Soldatov. 2022. "Improvement of the EC Performance in LCP-MOF Electrode Materials by Succinic Anhydrate Addition to the Electrolyte" Sustainability 14, no. 1: 323. https://doi.org/10.3390/su14010323

APA Style

Moustafa, M. G., Aboraia, A. M., Butova, V., Guda, A., Elmasry, F., & Soldatov, A. (2022). Improvement of the EC Performance in LCP-MOF Electrode Materials by Succinic Anhydrate Addition to the Electrolyte. Sustainability, 14(1), 323. https://doi.org/10.3390/su14010323

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop