Next Article in Journal
The Armor of the Chinese Sturgeon: A Study of the Microstructure and Mechanical Properties of the Ventral Bony Plates
Previous Article in Journal
Three-Dimensional Performance Evaluation of Hemispherical Coriolis Vibratory Gyroscopes
Previous Article in Special Issue
Synergistic Electric and Thermal Effects of Electrochromic Devices
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis of Er3+:YAG Nanocrystals and Comparative Spectroscopic Analysis with Bulk Counterparts

1
Department of Physics and Astronomy, The University of Texas at San Antonio, San Antonio, TX 78249, USA
2
Department of Science and Mathematics, Texas A&M University San Antonio, San Antonio, TX 78224, USA
*
Author to whom correspondence should be addressed.
Micromachines 2023, 14(2), 255; https://doi.org/10.3390/mi14020255
Submission received: 15 November 2022 / Revised: 24 December 2022 / Accepted: 17 January 2023 / Published: 19 January 2023
(This article belongs to the Special Issue Light Emitting Devices: From Fundamental Research to Applications)

Abstract

:
Single-crystal Er3+:YAG has long been used as a laser material, and recent work has shown polycrystalline ceramic Er3+:YAG to be a suitable laser material, with benefits of lower cost and easier production. However, relatively little work has been done with the synthesis and spectroscopic characterization of Er3+:YAG nanocrystals. In this work, we present the synthesis of nanocrystalline Er3+:YAG and the results of comparative spectroscopic characterization with single-crystal and polycrystalline ceramic counterparts. The results show good agreement between the optical properties of the three hosts, with the nanocrystals demonstrating relatively higher intensity in the 1.53 μ m emission. These results demonstrate the viability of Er3+:YAG nanocrystals as a potential laser material.

1. Introduction

In recent years, trivalent erbium (Er3+) has been extensively studied for use in a wide variety of applications, including sensing, range finding, medical procedures, and communications [1,2,3], where it is used in near infrared (NIR) lasers. Of particular interest for these applications are eye-safe lasers with a wavelength of 1.53–1.66 μ m [1,4,5]. While single-crystal Y3Al5O12 yttrium aluminum garnet (YAG) has long been used as a laser host material doped with Nd3+ and other trivalent rare-earth (RE3+) ions [6], developments in nanotechnology have drawn a significant amount of attention to transparent ceramic materials [7,8]. In particular, polycrystalline ceramic YAG doped with RE3+ ions such as Nd3+ and Er3+ have been shown to be suitable laser materials, which can be easier and less expensive to grow than their single-crystal counterparts [4,9,10,11,12,13,14].
While the spectroscopic properties of Er3+ in single-crystal YAG have been thoroughly studied [15,16], relatively little research has been done with Er3+ in polycrystalline ceramic and nanocrystal YAG hosts [17,18,19,20]. Nanocrystals can have the advantage of being faster, less expensive, and easier to grow when compared to both polycrystalline ceramics and single crystals.
In this article, we present the comparative spectroscopic properties of Er3+ doped in single-crystal, polycrystalline ceramic, and nanocrystal YAG hosts. Room-temperature fluorescence spectra are taken in the near-infrared region, and the room-temperature fluorescence decay times are measured for the 1650 nm emission and compared between the three samples. Finally, the spectroscopic properties of these materials are analyzed and compared.

2. Materials and Methods

A polycrystalline ceramic YAG half-disk of 15.5 mm diameter and 1.56 mm thickness with 50 at.% Er3+ content was acquired from Quarles at VLOC [21]. A single-crystal YAG disk of 4 mm diameter and 1.2 mm thickness with 50 at.% Er3+ content was obtained from Kokta at Bicron Crystal Products [22]. Details of the production of both samples can be found in prior publications by our group [11,17].
The Er3+-doped YAG nanocrystals were prepared through a modified co-precipitation method similar to that outlined by Dai et al. [23]. Samples were prepared according to the stoichiometry of Er0.06Y2.94Al5O12 to obtain a dopant concentration of 2.0 at.%. The dopant concentration was selected based on prior work by our group, where similar materials singly-doped with lanthanides exhibited strong emission quenching from non-radiative losses and reabsorption above this concentration [24,25,26,27]. A precursor solution was prepared with stoichiometric amounts of Er, Y, and Al nitrates in 50 mL of deionized water at a total cation concentration of 0.16 M. A 50 mL precipitant solution of 80 mM ammonium bicarbonate (NH4HCO3) was separately prepared and adjusted to a pH of 10.5 through the addition of ammonium hydroxide (NH4OH). Lastly, 0.2 g of ammonium sulfate ((NH4)2SO4) was added to the precipitant solution to aid in dispersion.
The precipitant solution was heated to 40 °C under vigorous stirring, and the precursor solution was added dropwise at 2 mL/min. A white colloidal precipitate of metal hydroxide intermediates was formed, which was then collected through centrifugation and washed through sonication several times with deionized water to remove excess unreacted precursors before being freeze-dried overnight to yield a fine white powder. The dried powder was subsequently calcined at 1100 °C in a tube furnace in a mixed 95% N2, 5% H2 atmosphere to complete the formation of Er3+:YAG nanoparticles, remove absorbed water, and repair defects in the crystal structure to reduce non-radiative energy losses.

3. Results

3.1. Morphology

The X-ray diffraction (XRD) pattern (Cu K α , λ = 1.54 Å) in Figure 1 shows that the Er3+:YAG powder matches the YAG reference without any additional phases. The lattice parameter was calculated to be 12.03 ± 0.02 Å, compared to the reference value [28] of 12.01 ± 0.02 Å. The increase in the lattice parameter is attributed to the partial substitution of Y3+ by Er3+.
Finally, from the Scherrer equation,
t = 1.2 λ B cos θ
where t represents the crystallite size, B is the full width at half maximum (FWHM), λ is the X-ray wavelength, and 1.2 is a shape factor used to account for the rectangular shape observed from TEM measurements (JEOL, Tokyo, Japan), the crystallite size for the particles was calculated as 29 nm for the (220) plane, 25 nm for the (420) plane, and 36 nm for the (444) plane. As XRD measurements (Panalytical, Westborough, MA, USA) are taken from powder and thus represent many nanocrystals rather than individual particles, the Scherrer analysis provides an approximation of the lower range of particle sizes rather than being representative of the average particle size.

3.2. Microscopy

Elemental analysis was performed using energy-dispersive X-ray spectroscopy (EDS) with a Hitachi S5500 scanning transmission electron microscope (STEM, Hitachi, Tokyo, Japan) equipped with a solid-state Bruker detector (Bruker, Billerica, MA, USA). The results shown in Figure 2 confirm the YAG composition of the nanocrystals. High-resolution transmission electron microscopy (HRTEM, JEOL, Tokyo, Japan) was performed with a JEOL 2010F (JEOL, Tokyo, Japan). TEM images (Figure 3a–e) were used to calculate the size distribution of the synthesized nanocrystals by averaging the horizontal, vertical, and diagonal dimensions, which showed particles ranging from 18 nm to 60 nm with an average particle size of 35 nm, represented by the histogram in Figure 3g. The size distribution observed here provides agreement with the Scherrer calculations of crystallite sizes, which tends to underestimate particle sizes for non-spherical particles.

3.3. Spectroscopy

Figure 4 shows emission spectra in the NIR region, collected at room temperature by exciting the samples with a 980 nm diode laser and collecting the signal with a QuantaMaster 51 spectrofluorometer (PTI, Birmingham, NJ, USA) from Photon Technology International (PTI) equipped with an InGaAs detector. The single-crystal and ceramic samples were excited by directing the laser into the narrow side of the sample and collecting the emission signal from the broad side, to minimize quenching. The nanocrystal powder was placed in a thin quartz cuvette for the measurements. We have previously published a detailed analysis of the energy level transitions of the Er3+:YAG single-crystal and polycrystalline ceramic samples used here, where we provide the results of Judd–Ofelt analysis along with measured and calculated fluorescence line strengths and emission cross-sections [11,17].
Fluorescence decay times shown in Figure 5 for the 1650 nm emission were collected with the PTI system and a nanosecond-pulsed nitrogen pumped dye laser from PTI operated at 525 nm. The 1650 nm emission was chosen for lifetime measurements due to being the most intense emission observed consistently between all three samples. The decay time for each emission was calculated by fitting a single exponential function,
I ( t ) = A 1 e t / τ 1
where A1 represents the fitting parameter and τ 1 is the fluorescence decay time. The lifetime of the 1650 nm emission was calculated to be 1.14 ms for the single-crystal, 7.04 ms for the ceramic, and 2.15 ms for the nanocrystals. Due to a tendency for dopants to favor selection sites near the surface of nanoparticles and at grain boundaries [29], the nanocrystals were expected to have a fluorescence lifetime in between that of single-crystals where the dopants are dispersed throughout the crystal lattice and that of polycrystalline ceramics where the dopants tend to aggregate toward the grain boundaries, and this is observed in the measured lifetimes.

3.4. Crystal Structure

To perform a study of the crystal grain boundaries, the commercially fabricated 50 at.% Er3+:YAG polycrystalline ceramic sample was prepared using a focused ion beam (FIB, Zeiss, Jena, Germany) Zeiss Crossbeam 340 using 30, 5, and 2 kV gallium ions. Selected area electron diffraction patterns (SAED) under precession electron diffraction (PED) mode [30] were collected using a JEOL 2010F TEM operated at 200 kV and equipped with a NANOMEGAS precession unit. PED patterns were obtained under nanobeam diffraction mode with a precession angle of 0.48°, which has been performed to reduce the dynamical effects produced by the multiple interactions within the specimen (Figure 6b,c). In addition, to reduce the thermal diffusion scattering, a Gatan 626 double tilt liquid nitrogen cryo sample holder was used to collect the PED patterns at approximately 96 K. PED patterns were captured using a TVIPS 16 megapixel F416 CMOS camera (TVIPS, Gauting, Germany). Scanning transmission electron microscopy (STEM, JEOL, Tokyo, Japan) was employed to obtain high angle annular dark field (HAADF) images.
HAADF-STEM shows an incoherent image nature that depends on the atomic number (Z) and thickness of the sample (t), where the intensity is approximately [31] I ∝ tZ2. In Z-contrast imaging, the diffraction contrast is significantly reduced, resulting in a quantitative chemical-sensitive contrast. With this method, a Z-contrast image was collected at the grain boundary between grains 1 and 2 shown in Figure 6. The spherical aberration corrected (Cs) HAADF-STEM image shows an increase in contrast at the grain boundary due to the migration of erbium atoms (with heavier atomic number Z), see inset of Figure 6b. Chemical profiling was performed using EDS and STEM at the grain boundary, in which an increase in the signal of erbium was measured, as well as a crystallographic phase mapping [30]. The atomic segregation of erbium atoms at the grain boundary is consistent with the migration of atoms at the surface in the nanocrystal counterparts, which results in the optical response reported here.

4. Conclusions

The comparison of the NIR emissions is in good agreement between the three hosts, while the nanocrystals demonstrate significantly higher relative emission intensity in the 1.5–1.6 μ m emission bands commonly used for medical lasers. As emission quenching occurs through cross-relaxation processes that depend on the distance between dopant ions, the dopant distribution of the nanocrystals presented in this work yields the advantage of a much lower dopant concentration than that required for the bulk materials where dopant ions are distributed throughout the crystal matrix. The fluorescence lifetime of the nanocrystals is within range of the lifetimes measured for the single-crystal and ceramic hosts, indicating comparable internal quantum efficiency between all hosts [32,33]. Electron diffraction and Cs-STEM Z-contrast imaging show clear evidence of erbium segregation at the grain boundaries. This migration of erbium atoms at the interface reduces the optical quantum efficiency compared with the more uniformly-dispersed dopants of the single-crystal. In this regard, the use of Er3+:YAG nanocrystals improves the optical response of the polycrystalline nature and ensures they are good candidates for technological applications. Nanocrystal size distribution yielded an average of 35 nm, making the particles suitable for a variety of applications where particle size may be critical. The results of these spectroscopic and morphological studies indicate the viability of Er3+:YAG nanocrystals as a synthesis route for the production of transparent ceramics with applications in laser materials.

Author Contributions

Conceptualization, C.R. and D.S. (Dhiraj Sardar); methodology, C.R., G.A. and A.P.; data curation, J.E.; validation, E.O. and D.S. (David Sanchez); writing—original draft preparation, C.R. and A.P.; writing—review and editing, C.R.; supervision, D.S. (Dhiraj Sardar) and A.P.; and funding acquisition, D.S. (Dhiraj Sardar). All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by National Science Foundation Partnerships for Research and Education in Materials (NSF-PREM) under Grant No. DMR-0934218.

Data Availability Statement

Not applicable.

Acknowledgments

C.R. would like to thank the Department of Physics and Astronomy at UTSA for support during this work. The authors would like to thank the University of Texas at San Antonio Kleberg Advanced Microscopy Center for providing access to microscopy facilities.

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
YAGYttrium aluminum garnet
NIRNear-infrared
RERare-earth
XRDX-Ray diffraction
FWHMFull width at half maximum
EDSEnergy-dispersive X-ray spectroscopy
STEMScanning transmission electron microscope
TEMTransmission electron microscopy
HRTEMHigh-resolution transmission electron microscopy
PTIPhoton technology international
FIBFocused ion beam
SAEDSelected area electron diffraction
PEDPrecession electron diffraction
HAADFHigh-angle annular dark field
CsSpherical aberration correction

References

  1. Koechner, W. Solid-State Laser Engineering; Springer Series in Optical Sciences; Springer: New York, NY, USA, 2006; Volume 1. [Google Scholar] [CrossRef]
  2. Taccheo, S.; Laporta, P.; Longhi, S.; Svelto, O.; Svelto, C. Diode-pumped bulk erbium-ytterbium lasers. Appl. Phys. B 1996, 63, 425–436. [Google Scholar] [CrossRef]
  3. Schweizer, T.; Jensen, T.; Heumann, E.; Huber, G. Spectroscopic properties and diode pumped 1.6 μm laser performance in Yb-codoped Er:Y3Al5O12 and Er:Y2SiO5. Opt. Commun. 1995, 118, 557–561. [Google Scholar] [CrossRef]
  4. Qin, X.; Yang, H.; Shen, D.; Chen, H.; Zhou, G.; Luo, D.; Zhang, J.; Wang, S.; Ma, J.; Tang, D. Fabrication and Optical Properties of Highly Transparent Er:YAG Polycrystalline Ceramics for Eye-Safe Solid-State Lasers. Int. J. Appl. Ceram. Technol. 2013, 10, 123–128. [Google Scholar] [CrossRef]
  5. Wang, P.; Dawes, J.M.; Burns, P.; Piper, J.A.; Zhang, H.; Zhu, L.; Meng, X. Diode-pumped cw tunable Er3+:Yb3+:YCOB laser at 1.5–1.6 μm. Opt. Mater. 2002, 19, 383–387. [Google Scholar] [CrossRef]
  6. Dieke, G.H. Spectra and Energy Levels of Rare Earth Ions in Crystals. Am. J. Phys. 1970, 38, 399–400. [Google Scholar] [CrossRef]
  7. Greskovich, C.; Chernoch, J.P. Polycrystalline ceramic lasers. J. Appl. Phys. 1973, 44, 4599–4606. [Google Scholar] [CrossRef]
  8. Sekita, M.; Haneda, H.; Shirasaki, S.; Yanagitani, T. Optical spectra of undoped and rare-earth-(=Pr, Nd, Eu, and Er) doped transparent ceramic Y3Al5O12. J. Appl. Phys. 1991, 69, 3709–3718. [Google Scholar] [CrossRef]
  9. Kumar, G.A.; Jianren, L.; Kaminskii, A.A.; Ueda, K.I.; Yagi, H.; Yanagitani, T.; Unnikrishnan, N.V. Spectroscopic and stimulated emission Characteristics of Nd3+ in transparent YAG ceramics. IEEE J. Quantum Electron. 2004, 40, 747–758. [Google Scholar] [CrossRef]
  10. Lupei, V.; Lupei, A.; Ikesue, A. Transparent polycrystalline ceramic laser materials. Opt. Mater. 2008, 30, 1781–1786. [Google Scholar] [CrossRef]
  11. Gruber, J.B.; Nijjar, A.S.; Sardar, D.K.; Yow, R.M.; Russell, C.C.; Allik, T.H.; Zandi, B. Spectral analysis and energy-level structure of Er3+(4f11) in polycrystalline ceramic garnet Y3Al5O12. J. Appl. Phys. 2005, 97, 063519. [Google Scholar] [CrossRef]
  12. Ikesue, A.; Kinoshita, T.; Kamata, K.; Yoshida, K. Fabrication and optical properties of high-performance polycrystalline Nd:YAG ceramics for solid-state lasers. J. Am. Ceram. Soc. 1995, 78, 1033–1040. [Google Scholar] [CrossRef]
  13. Lu, J.; Prabhu, M.; Xu, J.; Ueda, K.i.; Yagi, H.; Yanagitani, T.; Kaminskii, A.A. Highly efficient 2% Nd: Yttrium aluminum garnet ceramic laser. Appl. Phys. Lett. 2000, 77, 3707–3709. [Google Scholar] [CrossRef]
  14. Lu, J.; Ueda, K.i.; Yagi, H.; Yanagitani, T.; Akiyama, Y.; Kaminskii, A.A. Neodymium doped yttrium aluminum garnet (Y3Al5O12) nanocrystalline ceramics—A new generation of solid state laser and optical materials. J. Alloys Compd. 2002, 341, 220–225. [Google Scholar] [CrossRef]
  15. Shi, W.Q.; Bass, M.; Birnbaum, M. Effects of energy transfer among Er3+ ions on the fluorescence decay and lasing properties of heavily doped Er:Y3Al5O12. J. Opt. Soc. Am. B 1990, 7, 1456–1462. [Google Scholar] [CrossRef]
  16. Zhekov, V.I. Cooperative process in Y3Al5O12:Er3+ crystals. Sov. J. Quantum Electron. 1986, 16, 274–276. [Google Scholar] [CrossRef]
  17. Sardar, D.K.; Russell, C.C.; Gruber, J.B.; Allik, T.H. Absorption intensities and emission cross sections of principal intermanifold and inter-Stark transitions of Er3+ (4f11) in polycrystalline ceramic garnet Y3Al5O12. J. Appl. Phys. 2005, 97, 123501. [Google Scholar] [CrossRef] [Green Version]
  18. Saladino, M.L.; Caponetti, E.; Martino, D.C.; Enzo, S.; Ibba, G. Effect of the dopant selection (Er, Eu, Nd or Ce) and its quantity on the formation of yttrium aluminum garnet nanopowders. Opt. Mater. 2008, 31, 261–267. [Google Scholar] [CrossRef]
  19. Nishi, M.; Tanabe, S.; Inoue, M.; Takahashi, M.; Fujita, K.; Hirao, K. Optical-telecommunication-band fluorescence properties of Er3+-doped YAG nanocrystals synthesized by glycothermal method. Opt. Mater. 2005, 27, 655–662. [Google Scholar] [CrossRef]
  20. Rodríguez, R.A.; Tobar, E.H.; la Rosa, E.D.; Díaz-Torres, L.A.; Salas, P.; Torres, A.; Felix, M.V.; Castañeda-Contreras, J.; Yacaman, M.J. Structural and photoluminescence characterization of nanocrystalline YAG: Er3+ prepared with the addition of PVA and UREA. Proc. SPIE 2007, 6639, 66390K. [Google Scholar] [CrossRef]
  21. Quarles, G.J.; VLOC, 7826 Photonics Drive, New Port Richey, FL 34655, USA. Personal Communication, 2020.
  22. Kokta, M.R.; Bicron Crystal Products, 750 South 32nd Street, Washougal, WA 98671, USA. Personal Communication, 2020.
  23. Dai, P.; Ji, C.; Shen, L.; Qian, Q.; Guo, G.; Zhang, X.; Bao, N. Photoluminescence properties of YAG:Ce3+,Pr3+ nano-sized phosphors synthesized by a modified co-precipitation method. J. Rare Earths 2017, 35, 341–346. [Google Scholar] [CrossRef]
  24. Pokhrel, M.; Kumar, G.A.; Ma, C.G.; Brik, M.G.; Langloss, B.W.; Stanton, I.N.; Therien, M.J.; Sardar, D.K.; Mao, Y. Electronic and optical properties of Er-doped Y2O2S phosphors. J. Mater. Chem. C 2015, 3, 11486–11496. [Google Scholar] [CrossRef]
  25. Saltmarsh, N.; Kumar, G.; Kailasnath, M.; Shenoy, V.; Santhosh, C.; Sardar, D. Spectroscopic characterizations of Er doped LaPO4 submicron phosphors prepared by homogeneous precipitation method. Opt. Mater. 2016, 53, 24–29. [Google Scholar] [CrossRef] [Green Version]
  26. Mimun, L.C.; Ajithkumar, G.; Rightsell, C.; Langloss, B.W.; Therien, M.J.; Sardar, D.K. Synthesis and characterization of Na(Gd0.5Lu0.5)F4: Nd3+, a core-shell free multifunctional contrast agent. J. Alloys Compd. 2017, 695, 280–285. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  27. Gayathri, K.; Kumar, G.A.; Manrique, S.I.R.; Santhosh, C.; Sardar, D.K. Optical characterization of infrared emitting Nd3+ doped hydroxyapatite nanoparticles prepared by hydrothermal method. J. Lumin. 2017, 185, 180–186. [Google Scholar] [CrossRef] [Green Version]
  28. Yoder, H.; Keith, M. Complete substitution of aluminum for silicon: The system 3MnO·Al2O3·3SiO2–3Y2O3·5Al2O3. Am. Mineral. J. Earth Planet. Mater. 1951, 36, 519–533. [Google Scholar]
  29. Jüstel, T.; Nikol, H.; Ronda, C. New Developments in the Field of Luminescent Materials for Lighting and Displays. Angew. Chem. Int. Ed. 1998, 37, 3084–3103. [Google Scholar] [CrossRef]
  30. Ortega, E.; Sanchez, D.; Sardar, D.; Arellano, J.; Ponce, A. Microstructural Analysis of Polycrystalline Er:YAG using Automated Crystal Orientation Mapping. Proc. Microsc. Microanal. 2018, 24, 218–219. [Google Scholar] [CrossRef] [Green Version]
  31. Pennycook, S. Z-contrast stem for materials science. Ultramicroscopy 1989, 30, 58–69. [Google Scholar] [CrossRef]
  32. Pokhrel, M.; Kumar, G.A.; Samuel, P.; Ueda, K.I.; Yanagitani, T.; Yagi, H.; Sardar, D.K. Infrared and upconversion spectroscopic studies of high Er3+ content transparent YAG ceramic. Opt. Mater. Express 2011, 1, 1272–1285. [Google Scholar] [CrossRef] [Green Version]
  33. Pokhrel, M.; Ray, N.; Kumar, G.A.; Sardar, D.K. Comparative studies of the spectroscopic properties of Nd3+: YAG nanocrystals, transparent ceramic and single-crystal. Opt. Mater. Express 2012, 2, 235–249. [Google Scholar] [CrossRef]
Figure 1. XRD pattern of Er3+:YAG nanocrystals with comparison to the reference standard of pure YAG (COD ID: 1529037).
Figure 1. XRD pattern of Er3+:YAG nanocrystals with comparison to the reference standard of pure YAG (COD ID: 1529037).
Micromachines 14 00255 g001
Figure 2. EDS profile of a selected nanoparticle confirming YAG composition. The erbium concentration of 2 at.% is below the sensitivity of the EDS detector.
Figure 2. EDS profile of a selected nanoparticle confirming YAG composition. The erbium concentration of 2 at.% is below the sensitivity of the EDS detector.
Micromachines 14 00255 g002
Figure 3. (af) A set of TEM images of Er3+:YAG nanoparticles, scale bar in all images is 20 nm. (g) Histogram showing particle size distribution profile and average size of the particles.
Figure 3. (af) A set of TEM images of Er3+:YAG nanoparticles, scale bar in all images is 20 nm. (g) Histogram showing particle size distribution profile and average size of the particles.
Micromachines 14 00255 g003
Figure 4. Normalized NIR fluorescence spectra of Er3+:YAG single-crystal, nanocrystal, and polycrystalline ceramic at room temperature under 980 nm excitation. Denotes transition used for lifetime calculations.
Figure 4. Normalized NIR fluorescence spectra of Er3+:YAG single-crystal, nanocrystal, and polycrystalline ceramic at room temperature under 980 nm excitation. Denotes transition used for lifetime calculations.
Micromachines 14 00255 g004
Figure 5. Fluorescence decay times for the 1650 nm emissions of all three samples excited at 525 nm.
Figure 5. Fluorescence decay times for the 1650 nm emissions of all three samples excited at 525 nm.
Micromachines 14 00255 g005
Figure 6. (a) Low magnification TEM image of the polycrystalline sample prepared by FIB. (b) HAADF-STEM image showing the atomic segregation of erbium atoms at the grain boundary. (c,d) SAED patterns collected under precession electron diffraction mode with liquid nitrogen cooling.
Figure 6. (a) Low magnification TEM image of the polycrystalline sample prepared by FIB. (b) HAADF-STEM image showing the atomic segregation of erbium atoms at the grain boundary. (c,d) SAED patterns collected under precession electron diffraction mode with liquid nitrogen cooling.
Micromachines 14 00255 g006
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Rightsell, C.; Sanchez, D.; Escudero, J.; Ortega, E.; Ajithkumar, G.; Sardar, D.; Ponce, A. Synthesis of Er3+:YAG Nanocrystals and Comparative Spectroscopic Analysis with Bulk Counterparts. Micromachines 2023, 14, 255. https://doi.org/10.3390/mi14020255

AMA Style

Rightsell C, Sanchez D, Escudero J, Ortega E, Ajithkumar G, Sardar D, Ponce A. Synthesis of Er3+:YAG Nanocrystals and Comparative Spectroscopic Analysis with Bulk Counterparts. Micromachines. 2023; 14(2):255. https://doi.org/10.3390/mi14020255

Chicago/Turabian Style

Rightsell, Chris, David Sanchez, José Escudero, Eduardo Ortega, Gangadharan Ajithkumar, Dhiraj Sardar, and Arturo Ponce. 2023. "Synthesis of Er3+:YAG Nanocrystals and Comparative Spectroscopic Analysis with Bulk Counterparts" Micromachines 14, no. 2: 255. https://doi.org/10.3390/mi14020255

APA Style

Rightsell, C., Sanchez, D., Escudero, J., Ortega, E., Ajithkumar, G., Sardar, D., & Ponce, A. (2023). Synthesis of Er3+:YAG Nanocrystals and Comparative Spectroscopic Analysis with Bulk Counterparts. Micromachines, 14(2), 255. https://doi.org/10.3390/mi14020255

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop