Next Article in Journal
A Miniaturized Amperometric Hydrogen Sulfide Sensor Applicable for Bad Breath Monitoring
Next Article in Special Issue
Static and Fatigue Tests on Cementitious Cantilever Beams Using Nanoindenter
Previous Article in Journal
Step-Double-Zone-JTE for SiC Devices with Increased Tolerance to JTE Dose and Surface Charges
Previous Article in Special Issue
Calibration of a Constitutive Model from Tension and Nanoindentation for Lead-Free Solder
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Localized Deformation and Fracture Behaviors in InP Single Crystals by Indentation

1
School of Mechanical and Automotive Engineering, Xiamen University of Technology, No.600 Ligong Road, Jimei District, Xiamen 361024, China
2
Department of Materials Science and Engineering, I-Shou University, Kaohsiung 840, Taiwan
3
Department of Physics and Biophysics, Faculty of Basic Sciences, Can Tho University of Medicine and Pharmacy, 179 Nguyen Van Cu Street, Can Tho 94000, Vietnam
4
Department of Electrophysics, National Chiao Tung University, Hsinchu 300, Taiwan
*
Authors to whom correspondence should be addressed.
Micromachines 2018, 9(12), 611; https://doi.org/10.3390/mi9120611
Submission received: 11 October 2018 / Revised: 14 November 2018 / Accepted: 18 November 2018 / Published: 22 November 2018
(This article belongs to the Special Issue Small Scale Deformation using Advanced Nanoindentation Techniques)

Abstract

:
The indentation-induced deformation mechanisms in InP(100) single crystals were investigated by using nanoindentation and cross-sectional transmission electron microscopy (XTEM) techniques. The results indicated that there were multiple “pop-in” events randomly distributed in the loading curves, which were conceived to arise primarily from the dislocation nucleation and propagation activities. An energetic estimation on the number of nanoindentation-induced dislocations associated with pop-in effects is discussed. Furthermore, the fracture patterns were performed by Vickers indentation. The fracture toughness and the fracture energy of InP(100) single crystals were calculated to be around 1.2 MPa·m1/2 and 14.1 J/m2, respectively.

1. Introduction

Nowadays, nanoindentation is extensively used to characterize the mechanical properties (such as hardness and elastic modulus) and elastic or plastic deformation behaviors of various nanoscale materials [1,2,3,4,5,6] and thin films [7,8,9,10,11,12]. In general, from the nanoindentation responses manifested in the load-displacement (P-h) curves, one can obtain the primary mechanical characteristics of the materials being measured. For instance, the onset of plastic deformation behaviors in crystalline materials is often characterized by sudden bursts of displacements at a nearly constant indentation load in the P-h curves. These phenomena, known as “pop-in,” have been ubiquitously observed and often considered to be a result of dislocation activity during the nanoindentation process [13,14]. Lorenz et al. [15] proposed that the pop-in event is originated from homogeneous dislocation nucleation beneath the indenter tip. This scenario is reasonably in line with the low probability of encountering the pre-existing dislocations. Furthermore, previous cross-sectional transmission electron microscopy (XTEM) observations [14,16,17] evidenced the intimate correlations between pop-in events and dislocation activities in many nanoindentation studies [14,15,16,17].
Owing to its high electron velocity and the direct bandgap (~1.35 eV), zincblende-structured indium phosphide (InP) has been regarded as one of the most important III–V semiconductors. Currently, applications based on InP have been realized in a wide variety of electronic and photonic devices and systems, such as high-power and high-frequency electronics, solar cells, photodiodes, photodetectors, light-emitting diodes (LEDs), field effect transistors (FETs), and micro-electro-mechanical systems (MEMS) [18,19,20]. From an application point of view, in addition to its optoelectronic properties, a full understanding of the mechanical properties of InP is equally essential in order to widen its applications and manipulate the performance of devices.
For InP(100) single crystals, however, two different types of P-h curves obtained from nanoindentation studies were reported, namely single-discontinuity [21] and multi-discontinuities [22]. Such behavior remains intangible because the onset of nanoscale plasticity can be strongly influenced by various factors, such as indenter tip radius, temperature, and crystal plane [23,24]. Therefore, in order to understand nanoindentation-induced pop-in mechanisms and clarify the outstanding issues of nanoscale plasticity in InP(100) single crystals, a combination of XTEM and selected area diffraction (SAD) analyses were carried out in this work. The number of nanoindentation-induced dislocation loops in InP(100) single crystals was estimated within the context of the classical dislocation theory [25]. Moreover, the Vickers-indentation induced fracture toughness and fracture energy of InP (100) single crystals were calculated and discussed in details.

2. Materials and Methods

The (100)-oriented single-crystal InP used in this work was purchased from Semiconductor Wafer Inc. (Hsinchu, Taiwan) The nanoindentation tests were performed using a Nanoindenter MTS NanoXP® system (MTS Cooperation, Nano Instruments Innovation Center, Oak Ridge, TN, USA) with a diamond pyramid-shaped Berkovich indenter tip having a radius of curvature of ~50 nm. The mechanical properties of single-crystal InP(100) were obtained using the continuous stiffness measurements (CSM) technique, commonly practiced in the nanoindentation community [26]. Hardness and Young’s modulus of single-crystal InP(100) were obtained using Oliver and Pharr method [27], as shown in Figure 1.
The hardness of the measured material is defined as the applied indentation loading divided by the projected contact area, H = Pm/Ap, where Ap is the projected contact area and Pm is the maximum indentation load. For a perfect Berkovich indenter, the projected area is given by A p = 24.56 h c 2 with hc being the contact depth. In addition, the elastic modulus of the material can be calculated based on the relationship proposed by Sneddon [28]: S = 2 β E r A p / π . Here, S is the contact stiffness of the material and β is a geometric constant, with β = 1.00 for the Berkovich indenter. The reduced elastic modulus, Er, can be calculated from the following equation:
1 E r = ( 1 v 2 E ) d + ( 1 v 2 E ) I n P
with v and E being Poisson’s ratio and Young’s modulus, respectively. The subscripts “d” and “InP” indicate the properties of the indenter and material, respectively. For the diamond indenter tip, E d = 1141 GPa, v d = 0.07 [27], and v I n P = 0.25 were assumed for single-crystal InP(100).
After being deformed by an indentation load of 150 mN, XTEM samples of InP(100) single crystals were prepared using a dual-beam focused ion beam (FIB) station (FEI Nova 220) with the lift-out technique. Pictorial illustrations of the FIB milling procedures are displayed in Figure 2. The sample was then picked up by a carbon membrane and placed on the TEM grid using a sharp glass tip under an optical microscopy (OM) outside the FIB station. The XTEM lamella was examined in a FEI TECNAI G2 TEM operating at 200 kV.
Vickers indentation testing was carried out in single-crystal InP(100) to characterize the cracking behavior with five indents at a loading of 1.96 N by using a hardness tester (Akashi MVK-H11, Kanagawa, Japan). All indentations were made in ambient air at room temperature with a relative humidity of about 55%. The cracking patterns were examined and analyzed with an optical microscope (OM).

3. Results

3.1. Nanoindentation Responses

A typical CSM P-h curve of single-crystal InP(100) reflecting the elastic behavior and plastic deformation during nanoindentation is shown in Figure 1a. The results clearly show that there are several pop-ins occurring at different loading stages, as indicated by the arrows located at different indentation loadings, which is consistent with a previous report [22]. Hardness and Young’s modulus versus penetration depth curves obtained from the CSM analyses for single-crystal InP(100) are displayed in Figure 1b,c, respectively. Both curves exhibit very similar depth-dependent trends, namely an initial quasi-linear increase to a maximum value within the first 10–15 nm, followed by a subsequent steep decrease in the 20–30-nm range, and finally reaching a constant value. It is interesting to note that the steep decrease after the first stage essentially coincides with where the first pop-in event is observed, indicating that a bursting activity of dislocation might have occurred.
For a uniform material, hardness and Young’s modulus do not change significantly with increasing penetration depth. The initial increase seen in Figure 1b,c is owing to the fact that the practical indenter tip is of a finite radius of shape point. This effectively sets the limit on the indentation depth that is necessary to obtain reliable hardness and Young’s modulus records of the measured material. As shown in Figure 1b,c, hardness and Young’s modulus reach a constant value at a similar moderate indentation depth. Thus, the values of hardness and Young’s modulus obtained at this stage can be regarded as intrinsic properties of single-crystal InP(100). In this report, both mechanical parameters were determined by taking the average values within a penetration depth ranging from 60 nm to100 nm.
Hardness and Young’s modulus of single-crystal InP(100) thus obtained are about 7.5 GPa and 101.8 GPa, respectively. These values are both substantially larger than those reported by Bradby et al. [21], where hardness and Young’s modulus for InP(100) were ~5.1 GPa and ~82 GPa, respectively. We note that in their experiments, a spherical indenter with a radius of ~4.2 μm and a load up to 50 mN were used, whereas in the present study a pyramid shape Berkovich indenter with a tip radius of ~40 nm (facing 65.3° from the vertical axis) and a typical load of less than 2 mN were used. It is reasonable to speculate that in the present study the probed deformation region could be more localized, which might also give rise to the apparent discrepancies between the mechanical parameters obtained from different experimental set-ups and operation modes.
Within the dominant deformation mechanism in the context of dislocation, the multiple “pop-ins” (indicated by the arrows in Figure 1a) can be regarded as the trigger of sudden collective activities of dislocation [29,30,31] (such as dislocation generation or movement bursts), giving rise to the seemingly discontinuous plastic deformation during nanoindentation. Such massive dislocation activities are also consistent with the conjectures of the resultant “noisy” features seen in the depth-dependent curves of hardness and Young’s modulus (Figure 1b,c), as well as those reported by Almeida et al. [32] and Jian et al. [22]. The multiple “pop-in” behaviors had also been observed in Reference [32]. From Figure 1a, the first “pop-in” is observed on the loading curve at a load of about 0.08 mN in the present work, which is substantially smaller than that (~0.2 mN) reported previously by Almeida et al. [32]. It is noted that the indenter used in Reference [32] was a cono-spherical-type tip with a radius of ~260 nm equipped in a Hysitron Triboscope nanoindenter system. It is possible that different operating modes, indenter geometrical shapes, and size of radius may lead to the vastly dissimilar nanoindentation results.
However, as mentioned above, when a spherical indenter with a larger tip radius was used, only a single “pop-in” event was observed [21]. This discrepancy, as we discussed above, might originate primarily from the differences in operating modes and the geometric shape of the indenter being used to probe the nanoindentation properties of the same material. The other feature to be noted is that no evidence of reverse discontinuities in the unloading segment (the so-called “pop-out”) can be identified in the present case. This indicates that the pressure-induced phase transformation commonly observed in single-crystal silicon [33] is probably not happening in InP, although the zincblende crystalline structure of InP is in fact not that different from the diamond structure of Si. In any case, in order to gain a more comprehensive understanding of the underlying indentation-induced deformation mechanism, direct microstructural investigations such as SEM and XTEM analyses are certainly indispensable.

3.2. XTEM and SAD Analyses

Figure 3a shows a SEM image of the InP(100) single-crystal surface after being indented with a load of 150 mN, featuring the characteristics of Berkovich nanoindentation-induced cracks. Although it appears that the paths of cracking propagation are not straight and the propagation directions are somewhat random, the directions, nevertheless, can be roughly divided into <100> and <110> directions [22]. A bright-field XTEM image of the area immediately beneath the tip of the Berkovich indenter is shown in Figure 3b. It is clearly evident that the slip bands are oriented at ~54.7° to the (100) surface, indicating that the dislocations have been gliding along the <110>{111} slip systems expected for the zincblende-structured InP. The rosette arm patterns ubiquitously observed in materials with similar crystal structure [32,34] are also evident, as indicated in Figure 3b. A closer examination by select area diffraction (SAD) further reveals that the deformation zone immediately beneath the indent consists of a mixture of slip-bands and micro-twins. This is clearly illustrated by the double spots and streaks seen in the [011] zone-axis SAD pattern displayed in Figure 3c. The SAD pattern also indicates that the dislocations and twins are lying parallel on the {111} planes. The direct microstructural observations by XTEM, thus, clearly confirm that indentation-induced deformation in single-crystal InP(100) is exclusively dominated by dislocation activities, and mechanisms such as phase transformation and amorphization are not involved in the nanoindentation process. In the present study, the Berkovich nanoindentation-induced multiple “pop-in” behaviors exhibited on the loading curve are attributed to the formation of slip-bands and micro-twins in single-crystal InP(100). Whereas, based on their observations, Almeida et al. [32] proposed that the multiple “pop-in” behaviors resulted from the Lomer-Cottrell locks, work-hardened region, and a high density of dislocation loops formed beneath the cono-spherical tip. From this viewpoint, the geometrical shape of the indenter tip may have played an important role on the activation of the slip system or/and the formation of dislocations. This may also explain the different number of pop-in events often observed in materials with the same crystal structure during nanoindentation, such as zincblende-structured InP [21,22,32] and hexagonal-structured GaN thin films [14,16].
Moreover, from Figure 3b, the number of dislocations (N) generated by the indenter can be roughly estimated using the following expression: N = hr/bz, where hr is the residual depth of the indenter and bz is the component of the dislocations along the loading axis [35]. Taking hr ~1200 nm, it is estimated that there were about 3000 dislocations formed underneath the indenter tip in this work. This number is about an order of magnitude smaller than the dislocation loops with critical size generated during first pop-ins obtained using thermodynamics energetic estimation (see below). However, considering that the above estimation was made based on the TEM image taken after the entire indentation was completed and the applied stress was removed, this, in fact, is quite consistent. This is because with further increasing load, the dislocation loops formed during the first pop-in may slide and merge to form twins and slip-bands, resulting in multiple pop-ins in the later stage of indentation and reducing the number of dislocations in the residual indentation depth, as revealed in the TEM image. Further, the average dislocation densities (ρ) were estimated using the relationship ρ = 2N/Lt [36], where L is the total length of random lines projected on a given area of XTEM image and t is the foil thickness. In this experimental result, ρ is thus estimated in the order of about 1014 m−2.

3.3. Homogeneous Dislocation Nucleation

In the scenario described above, the first pop-in event appearing in the loading segment naturally reflects the onset of plasticity in single-crystal InP(100) manifested by sudden dislocation nucleation and propagation. In other words, the corresponding loading is likely intimately associated with the critical shear stress (τmax), and the energy associated with the pop-in depth may directly account for the number of indentation-induced newly nucleated dislocation loops. Following the analytical model by Johnson [37], τmax can be related to an indentation load (Pc) at which a discontinuity in the load-displacement curve takes place, through the following equation:
τ max = 0.31 ( 6 P c E r 2 π 3 R 2 ) 1 / 3
where R is the radius of the indenter tip. Thus, the obtained τmax for single-crystal InP(100) is about 2.3 GPa. We assume that the τmax is responsible for the homogeneous dislocation nucleation underneath the indenter tip. Therefore, the shear stress that initiates plastic deformation and the energy required for generating a dislocation loop to prevail the deformation can be estimated from the present data. The free energy (U) of a circular dislocation loop of radius (r) is given as:
U = γ d i s 2 π r τ b π r 2
where γ d i s is the line energy of the dislocation loop, b is the magnitude of Burgers vector (~0.4 nm) [38], and τ is the external shear stress acting on the dislocation loop. The energy required to create a dislocation loop in a defect-free lattice is described in the first term on the right-hand side of Equation (3) and is also equal to the increased lattice energy due to the formation of a dislocation loop. The second term of Equation (3) is nothing but the strain energy released via work done by the applied stress (τ) to expand the dislocation loop over a displacement of one Burgers vector. The lattice strain in the vicinity of the dislocation for r > rcore, thus γ d i s , is given by Reference [25]:
γ d i s = G b 2 8 π 2 v I n P 1 v I n P [ ln ( 4 r r c o r e ) 2 ]
where G is the shear modulus, and for single-crystal InP(100) G ≈ 31 GPa [39]. The value of the radius of dislocation core rcore is usually assumed to be about one lattice constant. By using Equations (1), (3) and (4) can be rewritten as:
U = G b 2 4 ( 2 v I n P 1 v I n P ) ( ln 4 r r c o r e 2 ) r π b r 2 τ c
This relates the material properties and observed pop-in load to the free energy responsible for dislocation nucleation. The resolved shear stress (τc) is usually taken as the half of τmax [39]. The U has a maximum at a critical radius (rc) above which the system gains energy by increasing r. According to Equation (5), this maximum energy decreases with increasing load and a pop-in, i.e., the homogeneous formation of a circular dislocation loop becomes possible without thermal energy at U = 0 [40]. With this condition and setting dU/dr = 0 for a maximum, this yields τ c = 2 γ d i s / b r and r c = ( e 3 r c o r e ) / 4 . Consequently, rcore ≈ 0.43 nm and rc = 2.15 nm are obtained. The value rcore ≈ 0.43 nm is slightly smaller than a ≈ 0.587 nm for InP, however, it is consistent with the atomic distance along the <110> orientation (≈0.42 nm), indicating that the above analysis is reasonable. The fact that the critical radius of the dislocation loop rc (=2.15 nm) needs to extend over a distance of about 5 times the dislocation core to become stable is also interesting. This suggests that the system is more prone to accommodate strain energy with larger dislocations loops.
The number of dislocation loops formed in the first pop-in can be estimated from the associated work (Wp) done during nanoindentation. As depicted in Figure 4, Wp is estimated to be about 0.2 × 10−12 Nm, implying that ~3 × 104 dislocation loops with a radius larger than rc have been generated during the pop-in event. This number is relatively low and consistent with the scenario of homogeneous dislocation nucleation-induced pop-in, instead of activated collective motion of pre-existing dislocations [15]. Moreover, as discussed above, this number is also in line with the number of dislocations estimated from the TEM image taken from the region of residual indentation depth. Alternatively, one can take the total dissipation energy as the energy to estimate the number of dislocations with critical radius being generated during entire nanoindentation practice. In that case, as many as ~106 dislocation loops may have been formed during nanoindentation. However, this number can only be regarded as an upper limit because it is quite unlikely that all the dissipated indentation energy is completely transferred to form dislocation loops within the deformation region in single-crystal InP(100).

3.4. Vickers Indentation Induced Fracture Behavior

Fracture toughness (KC) can be readily measured by the induced cracks at the corners of indentations made on the substrate materials. This method is known as the indentation microfracture [41,42,43]. Figure 5 shows the Vickers-indentation-induced cracking pattern on single-crystal InP(100) at a loading of 1.96 N. It can be found that the ratio of average cracking length (l = (c1 + c2)/4, where c1 and c2 are defined in Figure 5) to the half-diagonal of the indentation (a) meets the criteria of Palmqvist cracks with 0.25 ≤ l/a ≤ 2.5. Therefore, the formula proposed by Niihara et al. [41,42] was adopted to calculate the KC of single-crystal InP(100) here, as follows:
K C = 0.009 ( E I n P H ) 2 / 5   P a a l
where Pa is the applied load. The KC of single-crystal InP(100) obtained is about 1.2 MPa·m1/2. Comparing to the KIC values of 0.42~0.53 MPa·m1/2 for InP reported by Ericson et al. [44], the present result seems slightly too large. However, considering that KC is strongly dependent on specimen geometry and usually decreases with increasing thickness to reach a minimum value known as KIC, we believe that a factor of 2–2.5 difference is quite reasonable. Finally, the fracture energy (GC) can also be calculated using the equation G C = K C 2 [ ( 1 v I n P 2 ) / E I n P ] [45], yielding approximately 14.1 J·m−2 for single-crystal InP(100). This number indicates that InP is, in fact, quite ductile, which is also consistent with the dislocation-dominated deformation discussed above.

4. Conclusions

To sum up, the nano- and micro-scale deformation mechanisms and behaviors of single-crystal InP(100) were studied by combining indentation, SEM, and XTEM techniques. From the XTEM results and SAD analysis, the nanoindentation responses of single-crystal InP(100) involve the the formation of slip-bands and micro-twins. Preliminary energetic estimations indicate that the number of dislocation loops induced by nanoindentation to trigger the plastic deformation accounting for the first pop-in event was in the order of 104 with a critical radius rc ≈ 2.15 nm. Furthermore, from Vickers indentation tests, the obtained values of KC and GC of single-crystal InP(100) were about 1.2 MPa·m1/2 and 14.1 Jm−2, respectively.

Author Contributions

Y.-J.C. and T.-J.L. contributed to the nanoindentation experiments and analyses. S.-R.J., J.-Y.J., and P.H.L. contributed to the discussion on materials characterizations. S.-R.J. designed the experiments and drafted the manuscript. All authors read and approved the final manuscript.

Funding

Financial support from the Ministry of Science and Technology, Taiwan under Contract Nos.: MOST 106-2112-M009-013-MY3, MOST 103-2112-M-009-015-MY3, MOST 107-2112-M-214-001, MOST 106-2112-M-214-001, and MOST 105-2112-M-214-001. This work was supported by the Fujian Nature foundation, No. 2016J01039; Xiamen City Project No. 3502Z20173037.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Li, X.D.; Gao, H.; Murphy, C.J.; Gou, L. Nanoindentation of Cu2O Nanocubes. Nano Lett. 2004, 4, 1903–1907. [Google Scholar] [CrossRef]
  2. Li, X.D.; Wang, X.; Xiong, Q.; Eklund, P.C. Mechanical Properties of ZnS Nanobelts. Nano Lett. 2005, 5, 1982–1986. [Google Scholar] [CrossRef] [PubMed]
  3. Raichman, Y.; Kazakevich, M.; Rabkin, E.; Tsur, Y. Inter-Nanoparticle Bonds in Agglomerates Studied by Nanoindentation. Adv. Mater. 2006, 18, 2028–2030. [Google Scholar] [CrossRef]
  4. Tao, X.; Li, X.D. Catalyst-Free Synthesis, Structural, and Mechanical Characterization of Twinned Mg2B2O5 Nanowires. Nano Lett. 2008, 8, 505–510. [Google Scholar] [CrossRef] [PubMed]
  5. Bao, L.; Xu, Z.H.; Li, R.; Li, X.D. Catalyst-Free Synthesis and Structural and Mechanical Characterization of Single Crystalline Ca2B2O5·H2O Nanobelts and Stacking Faulted Ca2B2O5 Nanogrooves. Nano Lett. 2010, 10, 255–262. [Google Scholar] [CrossRef] [PubMed]
  6. Jian, S.R.; Sung, T.H.; Huang, J.C.; Juang, J.Y. Deformation behaviors of InP pillars under uniaxial compression. Appl. Phys. Lett. 2012, 101, 151905. [Google Scholar] [CrossRef]
  7. Jian, S.R.; Chen, G.J.; Lee, J.W. Effects of annealing temperature on nanomechanical and microstructural properties of Cu-doped In2O3 thin films. Appl. Phys. A 2017, 123, 726. [Google Scholar] [CrossRef]
  8. Jian, S.R.; Le, P.H.; Luo, C.W.; Juang, J.Y. Nanomechanical and wettability properties of Bi2Te3 thin films: Effects of post-annealing. J. Appl. Phys. 2017, 121, 175302. [Google Scholar] [CrossRef]
  9. Lai, H.D.; Jian, S.R.; Tuyen, L.T.C.; Le, P.H.; Luo, C.W.; Juang, J.Y. Nanoindentation of Bi2Se3 Thin Films. Micromachines 2018, 9, 518. [Google Scholar] [CrossRef] [PubMed]
  10. Chen, G.J.; Jian, S.R. Effects of Cu doping on the structural and nanomechanical properties of ZnO thin films. Appl. Phys. A 2018, 124, 575. [Google Scholar] [CrossRef]
  11. Chiu, Y.J.; Shen, C.Y.; Chang, H.W.; Jian, S.R. Characteristics of Iron-Palladium alloy thin films deposited by magnetron sputtering. Results Phys. 2018, 9, 17–22. [Google Scholar] [CrossRef]
  12. Chen, G.J.; Jian, S.R.; Juang, J.Y. Surface Analysis and Optical Properties of Cu-Doped ZnO Thin Films Deposited by Radio Frequency Magnetron Sputtering. Coatings 2018, 8, 266. [Google Scholar] [CrossRef]
  13. Morris, J.R.; Bei, H.; Pharr, G.M.; George, E.P. Size Effects and Stochastic Behavior of Nanoindentation Pop In. Phys. Rev. Lett. 2011, 106, 165502. [Google Scholar] [CrossRef] [PubMed]
  14. Chien, C.H.; Jian, S.R.; Wang, C.T.; Juang, J.Y.; Huang, J.C.; Lai, Y.S. Cross-sectional transmission electron microscopy observations on the Berkovich indentation-induced deformation microstructures in GaN thin films. J. Phys. D Appl. Phys. 2007, 40, 3985–3990. [Google Scholar] [CrossRef]
  15. Lorenz, D.; Zeckzer, A.; Hilpert, U.; Grau, P.; Johnson, H.; Leipner, H.S. Pop-in effect as homogeneous nucleation of dislocations during nanoindentation. Phys. Rev. B 2003, 67, 172101. [Google Scholar] [CrossRef]
  16. Bradby, J.E.; Kucheyev, S.O.; Williams, J.S.; Leung, J.W.; Swain, M.V.; Munroe, P.; Li, G.; Phillips, M.R. Indentation-induced damage in GaN epilayers. Appl. Phys. Lett. 2002, 80, 383. [Google Scholar] [CrossRef]
  17. Bradby, J.E.; Williams, J.S.; Leung, J.W.; Swain, M.V.; Munroe, P. Nanoindentation-induced deformation of Ge. Appl. Phys. Lett. 2002, 80, 2651. [Google Scholar] [CrossRef]
  18. Robidas, D.; Arunseshan, C.; Deepthi, K.R.; Arivuoli, D. Nanomechanical characterization of indium phosphide epilayer using nanoindentation technique. Int. J. Mech. Ind. Eng. 2013, 3, 22–26. [Google Scholar]
  19. Zafar, F.; Iqbal, A. Indium phosphide nanowires and their applications in optoelectronic devices. Proc. R. Soc. A 2016, 472, 20150804. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  20. Tay, C.J.; Quan, C.; Gopal, M.; Shen, L.; Akkipeddi, R. Nanoindentation techniques in the measurement of mechanical properties of InP-based free-standing MEMS structures. J. Micromech. Microeng. 2008, 18, 025015. [Google Scholar] [CrossRef]
  21. Bradby, J.E.; Williams, J.S.; Leung, J.W.; Swain, M.V.; Munroe, P. Mechanical deformation of InP and GaAs by spherical indentation. Appl. Phys. Lett. 2001, 78, 3235. [Google Scholar] [CrossRef]
  22. Jian, S.R.; Jang, J.S.C. Berkovich nanoindentation on InP. J. Alloys Compd. 2009, 482, 498–501. [Google Scholar] [CrossRef]
  23. Lu, J.Y.; Ren, H.; Deng, D.M.; Wang, Y.; Chen, K.J.; Lau, K.M.; Zhang, T.Y. Thermally activated pop-in and indentation size effects in GaN films. J. Phys. D Appl. Phys. 2012, 45, 085301. [Google Scholar] [CrossRef]
  24. Huang, J.; Xu, K.; Fan, Y.M.; Niu, M.T.; Zeng, X.H.; Wang, J.F.; Yang, H. Nanoscale anisotropic plastic deformation in single crystal GaN. Nanoscale Res. Lett. 2012, 7, 150. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  25. Hirth, J.P.; Lothe, J. Theory of Dislocations, 2nd ed.; John Wiley and Sons: Hoboken, NJ, USA, 1982. [Google Scholar]
  26. Li, X.D.; Bhushan, B. A review of nanoindentation continuous stiffness measurement technique and its applications. Mater. Charact. 2002, 48, 11–36. [Google Scholar] [CrossRef]
  27. Oliver, W.C.; Pharr, G.M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. J. Mater. Res. 1992, 7, 1564–1583. [Google Scholar] [CrossRef]
  28. Sneddon, I.N. The relation between load and penetration in the axisymmetric Boussinesq problem for a punch of arbitrary profile. Int. J. Eng. Sci. 1965, 3, 47–57. [Google Scholar] [CrossRef]
  29. Jian, S.R.; Ku, S.A.; Luo, C.W.; Juang, J.Y. Nanoindentation of GaSe thin films. Nanoscale Res. Lett. 2012, 7, 403. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  30. Jian, S.R.; Tasi, C.H.; Huang, S.Y.; Luo, C.W. Nanoindentation pop-in effects of Bi2Te3 thermoelectric thin films. J. Alloys Compd. 2015, 622, 601–605. [Google Scholar] [CrossRef]
  31. Mosca, D.H.; Mattoso, N.; Lepienski, C.M.; Veiga, W.; Mazzaro, I.; Etgens, V.H.; Eddrief, M. Mechanical properties of layered InSe and GaSe single crystals. J. Appl. Phys. 2002, 91, 140. [Google Scholar] [CrossRef]
  32. Almeida, C.M.; Prioli, R.; Wei, Q.Y.; Ponce, F.A. Early stages of mechanical deformation in indium phosphide with the zinc blende structure. J. Appl. Phys. 2012, 112, 063514. [Google Scholar] [CrossRef]
  33. Jian, S.R.; Chen, G.J.; Juang, J.Y. Nanoindentation-induced phase transformation in (1 1 0)-oriented Si single-crystals. Curr. Opin. Solid State Mater. Sci. 2010, 14, 69–74. [Google Scholar] [CrossRef]
  34. Patriarche, G.; Le Bourhis, E. Low-load deformation of InP under contact loading; comparison with GaAs. Phil. Mag. A 2002, 82, 1953–1961. [Google Scholar] [CrossRef]
  35. Le Bourhis, E.; Patriarche, G. TEM-nanoindentation studies of semiconducting structures. Micron 2007, 38, 377–389. [Google Scholar] [CrossRef] [PubMed]
  36. Ham, R.K. The determination of dislocation densities in thin films. Phil. Mag. 1961, 6, 1183–1184. [Google Scholar] [CrossRef]
  37. Johnson, K.L. Contact Mechanics; Cambridge University Press: Cambridge, UK, 1985. [Google Scholar]
  38. Yonenaga, I.; Suzuki, T. Indentation hardnesses of semiconductors and a scaling rule. Phil. Mag. Lett. 2002, 82, 535–542. [Google Scholar] [CrossRef]
  39. Chiu, Y.L.; Ngan, A.H.W. Time-dependent characteristics of incipient plasticity in nanoindentation of a Ni3Al single crystal. Acta Mater. 2002, 50, 1599–1611. [Google Scholar] [CrossRef]
  40. Leipner, H.S.; Lorenz, D.; Zeckzer, A.; Lei, H.; Grau, P. Nanoindentation pop-in effect in semiconductors. Phys. B 2001, 308–310, 446–449. [Google Scholar] [CrossRef]
  41. Niihara, K.; Morena, R.; Hasselman, D.P.H. Evaluation of KIc of brittle solids by the indentation method with low crack-to-indent ratios. J. Mater. Sci. Lett. 1982, 1, 13–16. [Google Scholar] [CrossRef]
  42. Niihara, K.; Morena, R.; Hasselman, D.P.H. A fracture mechanics analysis of indentation-induced Palmqvist crack in ceramics. J. Mater. Sci. Lett. 1983, 2, 221–223. [Google Scholar] [CrossRef]
  43. Schiffmann, K.I. Determination of fracture toughness of bulk materials and thin films by nanoindentation: Comparison of different models. Philos. Mag. 2011, 91, 1163–1178. [Google Scholar] [CrossRef]
  44. Ericson, F.; Johansson, S.; Schweitz, J.-A. Hardness and fracture toughness of semiconducting materials studied by indentation and erosion techniques. Mater. Sci. Eng. A 1988, 105–106, 131–141. [Google Scholar] [CrossRef]
  45. Rafiee, M.A.; Rafiee, J.; Srivastava, I.; Wang, Z.; Song, H.; Yu, Z.Z.; Koratkar, N. Fracture and Fatigue in Graphene Nanocomposites. Small 2010, 6, 179–183. [Google Scholar] [CrossRef] [PubMed]
Figure 1. Nanoindentation results of single-crystal InP(100): (a) load-displacement curve showing the multiple “pop-ins” (arrows) during loading, (b) hardness-displacement curve and, (c) Young’s modulus-displacement curve.
Figure 1. Nanoindentation results of single-crystal InP(100): (a) load-displacement curve showing the multiple “pop-ins” (arrows) during loading, (b) hardness-displacement curve and, (c) Young’s modulus-displacement curve.
Micromachines 09 00611 g001aMicromachines 09 00611 g001b
Figure 2. A typical procedure of focused ion beam (FIB) milling for single-crystal InP(100) is shown. Sample preparation starts with a line of nanoindentations. After depositing a protection layer of Pt (a), two big trenches are etched on either side of the indentation line by a high current ion beam (7~20 nA) (b) Further, the middle strip is thinned (c). An ion dose of 50 pA is used for final clearing steps and, finally thinned to a thickness of ~100 nm (d).
Figure 2. A typical procedure of focused ion beam (FIB) milling for single-crystal InP(100) is shown. Sample preparation starts with a line of nanoindentations. After depositing a protection layer of Pt (a), two big trenches are etched on either side of the indentation line by a high current ion beam (7~20 nA) (b) Further, the middle strip is thinned (c). An ion dose of 50 pA is used for final clearing steps and, finally thinned to a thickness of ~100 nm (d).
Micromachines 09 00611 g002
Figure 3. An indented InP(100) single crystal under an indentation load of 150 mN. (a) SEM micrograph showing the cracking behaviors. (b) Bright-field XTEM image: micro-twins are indicated by solid white lines; dash lines are used to guide the eyes for lattice fringes. (c) SAD pattern of sample underneath the Berkovich indenter.
Figure 3. An indented InP(100) single crystal under an indentation load of 150 mN. (a) SEM micrograph showing the cracking behaviors. (b) Bright-field XTEM image: micro-twins are indicated by solid white lines; dash lines are used to guide the eyes for lattice fringes. (c) SAD pattern of sample underneath the Berkovich indenter.
Micromachines 09 00611 g003
Figure 4. The corresponding pop-in event (red arrow) from Figure 2a is zoomed in. The plastic strain work is Wp: critical loading × sudden incremental displacement.
Figure 4. The corresponding pop-in event (red arrow) from Figure 2a is zoomed in. The plastic strain work is Wp: critical loading × sudden incremental displacement.
Micromachines 09 00611 g004
Figure 5. Vickers indentation at 1.96 N in single-crystal InP(100): Palmqvist cracks emitting from Vickers indentation, where a is the half-diagonal of the indentation and l = (c1 + c2)/4 is the average length of the radial cracks for each indentation.
Figure 5. Vickers indentation at 1.96 N in single-crystal InP(100): Palmqvist cracks emitting from Vickers indentation, where a is the half-diagonal of the indentation and l = (c1 + c2)/4 is the average length of the radial cracks for each indentation.
Micromachines 09 00611 g005

Share and Cite

MDPI and ACS Style

Chiu, Y.-J.; Jian, S.-R.; Liu, T.-J.; Le, P.H.; Juang, J.-Y. Localized Deformation and Fracture Behaviors in InP Single Crystals by Indentation. Micromachines 2018, 9, 611. https://doi.org/10.3390/mi9120611

AMA Style

Chiu Y-J, Jian S-R, Liu T-J, Le PH, Juang J-Y. Localized Deformation and Fracture Behaviors in InP Single Crystals by Indentation. Micromachines. 2018; 9(12):611. https://doi.org/10.3390/mi9120611

Chicago/Turabian Style

Chiu, Yi-Jui, Sheng-Rui Jian, Ti-Ju Liu, Phuoc Huu Le, and Jenh-Yih Juang. 2018. "Localized Deformation and Fracture Behaviors in InP Single Crystals by Indentation" Micromachines 9, no. 12: 611. https://doi.org/10.3390/mi9120611

APA Style

Chiu, Y. -J., Jian, S. -R., Liu, T. -J., Le, P. H., & Juang, J. -Y. (2018). Localized Deformation and Fracture Behaviors in InP Single Crystals by Indentation. Micromachines, 9(12), 611. https://doi.org/10.3390/mi9120611

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop