Next Article in Journal
Cold Sintering Isomagnetic Dielectric NaCl-Nickel Zinc Ferrite Composite Ceramics
Next Article in Special Issue
Particle Swarm Method for Optimization of ATIG Welding Process to Joint Mild Steel to 316L Stainless Steel
Previous Article in Journal
Anomalous Ferromagnetic Phase in the Gd1−xErxB4 Series: Crystal Growth, Thermal, and Magnetic Properties
Previous Article in Special Issue
Structure–Property Correlation between Friction-Welded Work Hardenable Al-4.9Mg Alloy Joints
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of Microchemistry Elements in Relation of Laser Welding Parameters on the Morphology 304 Stainless Steel Welds Using Response Surface Methodology

by
Kamel Touileb
1,*,
Elawady Attia
2,
Rachid Djoudjou
1,
Abdejlil Chihaoui Hedhibi
3,
Abdallah Benselama
4,
Albaijan Ibrahim
1 and
Mohamed M. Z. Ahmed
1,5
1
Department of Mechanical Engineering, College of Engineering in Al-Kharj, Prince Sattam bin Abdulaziz University, P.O. Box 655, Al-Kharj 16273, Saudi Arabia
2
Department of Industrial Engineering, College of Engineering in Al-Kharj, Prince Sattam bin Abdulaziz University, P.O. Box 655, Al-Kharj 16273, Saudi Arabia
3
Laboratory of mechanics of Sousse (LMS), National Engineering School of Sousse, University of Sousse, BP 264, Erriaydh city, Sousse 4023, Tunisia
4
Department of Electrical Engineering, College of Engineering in Al-Kharj, Prince Sattam Bin Abdulaziz University, P.O. Box 655, Al-Kharj 16273, Saudi Arabia
5
Department of Metallurgical and Materials Engineering, Faculty of Petroleum and Mining Engineering, Suez University, Suez 43512, Egypt
*
Author to whom correspondence should be addressed.
Crystals 2023, 13(7), 1138; https://doi.org/10.3390/cryst13071138
Submission received: 28 June 2023 / Revised: 13 July 2023 / Accepted: 18 July 2023 / Published: 21 July 2023

Abstract

:
Small differences in the contents of surface active elements can change flow direction and thus heat transfer, even for different batches of a given alloy. This study aims to determine the effects of sulfur on weld bead morphology in the laser process. The paper presents the results related to the weld bead shape of two thin AISI 304 industrial stainless steel casts. One cast contains 80 ppm (0.008%) of sulfur, considered as a high sulfur content, and the other one contains 30 ppm (0.003%) sulfur, which can be considered low sulfur. The welds were executed using a CO2 laser. The effects of laser power (3.75, 3.67, 6 kW), welding speed (1.25, 2.40, 2.45, 3.6 m/min), focus point position (2, 7, 12 mm), and shield gas (Helium, mixed 40% helium + 60% argon and mixed 70% helium + 30% argon) with a flow rate of 10 L/min on the depth of the weld (D) and the aspect ratio (R = D/W) were investigated using RSM (response surface methodology). The experimental results show that the transfer of energy from the laser beam to the workpiece can be total in cases where the selected welding parameters prevent plasma formation. For the 304 HS cast, the focus point is the major factor in determining the depth of penetration, and its contribution is up to 52.35%. However, for 304 LS, the interaction between shield gas and focus point seems to play an important role, and the contribution of their interaction raises to 28% in relation to the laser depth of the weld. Moreover, the study shows that sulfur plays a surface-active role only in the case of partial penetration beads, so that a 56% partially penetrated weld supports the hypothesis of its surface-active role in the formation of the weld pool. However, a penetration of only 36% confirms the effects of a sulfur surface-active when the bead is fully penetrated.

1. Introduction

Nowadays, laser welding is widely used in many industries, such as in automobiles, aircraft, marines, shipbuilding and aviation. Laser welding is used in modern industry, and has many advantages such as less distortion, greater deep weld bead, and narrow welds compared to traditional welding technologies. As the beam can be concentrated in a small area, it provides a concentrated heat source, leading to narrow and highly penetrated welds [1,2]. Laser welding can be performed without filler materials and single-pass laser procedures have been employed in materials of up to 32 mm thick. This technique is strongly recommended for use on welding zones requiring high precision and high quality. The laser can be readily mechanized for automated, high-speed welding. Laser welding is a technique that meets the requirements of modern manufacturing in terms of the repeatability of the process and its easy automation. The lasers predominantly used in industrial material processing and welding tasks are the 1.0 µm YAG laser and the 10.6 µm CO2 laser, with the most common active elements employed in these two types of lasers being neodymium (Nd) ion and CO2 molecule, respectively [3]. Laser welding processes are classified as focused heat source or high-intensity and high-energy beams. Laser beam welding is one of the most promising welding techniques owing to the higher welding speeds it offers, and the lower dimensions and distortions in the welds. Moreover, its high strength-to-weld geometries and minimal heat-affected zones make it advantageous for various industrial applications. Lasers are characterized by requiring less time, which implies a lower labor cost.
The most commonly used casts of stainless alloys are austenitic steels, known as 8–18 types, which contain 16 to 18% Cr, 6–8% N and 0.03–0.1% C. Austenitic stainless steels are widely used for different applications in the chemical, petrochemical, food processing and nuclear industries, given their good mechanical and plastic properties. Austenitic stainless steels are widely used in a variety of applications owing of their corrosion resistance, good ductility, toughness, and ease of manufacture. The 300 series alloys designated by the American Iron and Steel Institute (AISI) are the most widely used of the austenitic casts. Stainless steels can generally be welded with all methods of fusion welding and solid-state welding [4,5].
The soundness of the weld is intimately related to multiple input parameters. The mastering of these inputs leads to welds with fewer defects. Finding out the optimal combinations is the main target in any research study, and finding the effective combinations is essential [6]. The optimization of welding conditions is useful in order to achieve good properties in the joints. Many researchers have applied various optimization methods to define the desired output variables, by developing mathematical models to specify the relationship between depth and welding parameters. Sampreeta et al. [7] examined bead-on-plate welding on Hastelloy C-276 plates of 1.6 mm thickness using the CO2 laser welding process. The welding was performed based on the Taguchi L9 design, considering laser power, welding speed and the flow rate of the shielding gas as input parameters. They found that a laser power of 1600 W, welding speed of 2 m/min and shielding gas flow rate of 10 L/min gave the best results. Using analysis of variance (ANOVA), it was found that laser power is the most influential parameter on the quality of the welds.
Another study conducted by Sathiya et al. [8] was dedicated to the optimization of laser bead-on-plate welding parameters with a 3.5 kW laser using Taguchi technique. The experiments were conducted on two different shielding gases: 100% nitrogen and a gas mixture of 50% nitrogen and 50% argon. The most suitable input process parameters, such as beam power, travel speed and focus position, were selected in order to obtain the desired output, i.e., bead width and depth of penetration. They concluded that beam power (42.35%) has a greater influence on welding, followed by focus position (27.48%) and travel speed (19.07%), when 100% nitrogen shielding gas is used. However, when a mixed gas (50% N, 50% Ar) was tested, they found that the travel speed (35.06%) has more influence on the welding, followed by focus position (29.71%) and beam power (28.81%). Anawa et al. [9] successfully applied a CO2 laser welding process and optimized the process parameters for joining dissimilar AISI 316 stainless steel and AISI 1009 low carbon steel plates. RSM was used to develop the mathematical models employed to predict the heat input and to describe the laser weld bead profile for a continuous wave 1.5 kW CO2 laser. In their study, the laser input parameters, such as laser power, welding speed and focused position, were taken into consideration. Benyounis et al. [10] conducted a study to optimize autogenous laser welded joints to get the maximum penetration, and the minimum fusion zone width and heat-affected zone width. In order to achieve these objectives, the authors developed a mathematical model and optimized the weld bead profiles. Several studies have confirmed the preponderant role played by surface active elements such as Se, Te, O, and S in the determination of the weld bead [11,12]. These studies, most of which were carried out in TIG (tungsten inert gas), show that a sulfur-rich cast presents a narrow and deep weld appearance. Contrarily, a cast free of sulfur presents a wide and more shallow bead [13]. In spite of the large amount of literature available on the effects of surfactant elements on TIG welding, very little work has been reported so far on the effects of the above-mentioned element during laser welding. Zhao et al. [14] were interested in the effects of adding oxygen as a surfactant on convection molten metal. Stainless steel samples were subjected to laser spot welding in an environmentally controlled chamber in order to observe fluid flow behavior and examine the influence of oxygen concentration on the flow. Transitions in fluid flow direction were observed during laser spot welding, whereby an initial outward flow changed to an inward flow in the presence of an oxidizing atmosphere. This behavior can be explained in terms of changes in surface tension gradients driven by oxygen dissolution in the liquid metal. Flow reversal only occurs in the presence of sufficient environmental oxygen. CO2 lasers are still the predominant type of laser used in the manufacturing industry, and in the higher power ranges in particular. Conduction mode welding occurs when heat is transferred from the surface into the material via thermal conduction. Conduction welding is made possible when the absorbed energy is sufficient to melt the weld zone, but insufficient for vaporization and plasma formation [15,16]. On the other hand, keyhole welding represents a type of welding wherein the laser beam energy is transferred deep into the material through a cavity filled with ionized metal vapor.
In simulations of heat conduction laser welding, the effect of the temperature-dependent surface tension coefficient (Marangoni effect) was identified as the primary driving force of the liquid melt. This coefficient is the most important driving force of the melt in conventional welding. In this study, the simulations show large differences in flow behavior caused merely by inverting the temperature dependency of γ(T). Therefore, the Marangoni effect is very important in deep laser welding. The simulations confirm and clarify the observed variations in weld bead geometry that arise due to very different flow patterns. These differences result from the marginal fluctuations in the chemical composition within the tolerance of the standard defining the material composition of a special alloy [17]. C. R. Heiple et al. [18] confirmed that the addition of small concentrations of a surface active element (Se) to stainless steel dramatically increased the D/W ratio of a severely defocused and decoupled laser weld. A defocused laser weld strongly supports the surface tension-driven fluid flow model.
Kaul et al. [19] studied the effects of the active flux laser beam welding of austenitic stainless steel sheets on plasma plume. Laser welding using SiO2 flux significantly modified the shape of the fusion zone (FZ), which produced narrower and deeper welds. The development of such a weld bead is caused by a reversal in the direction of the Marangoni flow caused by the oxygen-induced inversion of surface tension gradient. Ding et al. [20] reported that both the surface-activating flux and surface active element S produce significant effects on the YAG laser weld shape in terms of increased weld penetration and depth/width ratio. Su et al. [21] reported that the CO2 LBW (laser beam welding) of AISI 304 stainless steel sheets with active flux resulted in an increased weld depth through a decrease in the electron density of the plasma plume. In contrast, active flux had little effect on the depth of Nd:YAG laser welds [22]. The direction of the convective (or Marangoni) flow in the weld pool is governed by the sign of the surface tension gradient dγ/dT.
The research focuses on weldability problems related to the cast-to-cast variation in the weld pool geometry and penetration between materials with almost the same chemical compositions. The aim of our study is to analyze the influence of the basic parameters of laser welding (i.e., laser beam power, welding speed, shield gas types and focal point position) on the weld shape. This study is conducted on two industrial casts comprising AISI 304 austenitic stainless steel sheets of 3.0 mm thickness. The RSM optimization method is used to develop a mathematical model of depth and aspect ratio in terms of welding parameters. The optimal surface design in terms of response is used to design the experiment. The model required 15 points, and another 15 points were added randomly to increase the model efficiency using Design Expert Software. After performing the multi-regression analysis using Design Expert software, equations were obtained.
The laser welding parameter plays an important role in the quality of the weld, and hence the quality of the joint produced in industry. These results reveal the welding conditions that allow the surface active elements to play their fullest role. Furthermore, the results obtained in this study offer interesting data for researchers to relate the heat applied (welding parameters) with heat the weld profile, and the ensuing changes in microstructure. The microstructural properties are strongly affected by heat transfer and metal flow in the weld pool.

2. Materials and Methods

2.1. Materials

Two casts of austenitic stainless steel, AISI 304 LS and AISI 304 HS, with thicknesses of 3 mm were investigated in this study. The chemical compositions are presented in Table 1.
The sulfur content, thermal gradient and surface tension at melting temperature of the casts used are given in Table 2. Figure 1 shows the evolution of surface tension versus the temperature for both casts.
The surface tension of the liquid metal is dependent upon its temperature, and therefore dependent upon the distance from the center of the weld pool, since a molten weld pool has a radial temperature gradient such that the highest temperature is directly beneath the source of heat, and the lowest is at the solid–liquid interface. The combination of the dependence of the surface tension (γ) on the temperature (T) and the presence of a temperature gradient causes a surface tension gradient (dγ/dT) even in a small region.
Figure 1 represents the variation in surface tension against temperature in the center of the weld pool. In molten metal, in the case of a 304 LS cast, a decrease in the surface tension as the temperature increases is ascribed to the absence or quasi-absence of surfactants (30 ppm of Sulfur). In the case of 304 LS, the slope is negative (the temperature coefficient of the surface tension is negative).
However, in 304 HS (with 80 ppm), by contrast, the surface tension is highest at the center. As the melting point is reached, the molten metal flows from the center to the edge. Sulfur is a strongly surface-active element that segregates in the surface layer and reduces surface tension. However, as the temperature increases, sulfur desorbs into the bulk of the liquid metal, causing an increase in surface tension. This applies to alloys with a sulfur content greater than 50 ppm [24,25]. The surface tension will be highest at the center and thus the surface flow will be radially inward, and this will induce a downward flow in the center, called inverse Marangoni convection. In the case of 304 HS, the slope is positive (positive temperature coefficient of surface tension). A shallow, wide weld bead can be obtained in low-sulfur (S) stainless steel (30 ppm); however, a deep, narrow penetration weld is obtained in the case of a sulfur (S) content of 80 ppm.

2.2. Welding Procedure

The welding tests were carried out using the laser installation of the central school of Nantes (France), with a carbon dioxide (CO2) laser capable of producing a maximum output of 6 kW and emitting radiation in the infrared band of l0.6 μm and a pressure of 100 Pa. The laser gas was composed of He + N2 + CO2. Figure 2a depicts the CO2 laser welding modes, and Figure 2b shows laser beam welding in progress, with a shiny dazzling light.
Table 3 depicts the physical properties of the shield gas used. A preliminary study of the welding parameters is necessary to adjust the specific energy supplied to the sheets. The experiments involved welding a 120 mm line on a rectangular plate of 3 mm thickness, 150 mm length and 80 mm width. Before welding, the plates were cleaned with acetone.
In this study, 30 tests were carried out on each cast. Four factors were considered at different levels, as presented in Table 4. Three focus lengths were tested (+2, +7, +12 mm). Four welding speeds were investigated (1.25, 2.40, 2.45, 3.6 m/min). Three levels of power were applied (3.75, 3.67, 6 kW). In addition, three levels of the shield gas were considered according to the proportion of helium (40% helium mixed with 60% of argon, 70% helium mixed with 30% argon, and 100% helium). Figure 3 depicts the focus point positions used during the CO2 laser beam welding experiments.
The surface design yielding the optimal response has been used to design this experiment. The model required 15 points, and another 15 points were added randomly to increase the model efficiency using Design Expert software. First, a series of trials were conducted to master the welding parameters that were to be selected for our tests. In each test, three coupons were cut from the welding line to ensure the reproducibility and reliability of the results obtained. The samples were prepared by grinding, and subsequently polished, with a diamond suspension of 6 µm and 1 µm, respectively, then etched by immersion in Carpenters solution (8.5 gm FeCl3, 2.4 gm CuCl2, 122 mL alcohol, 122 mL HCl, 6 mL HNO3) for macrographic analysis. The samples were observed and checked using Motic software integrated with an optical microscope. The results of the weld aspect (depth of penetration, weld width) represent an average of the three readings.

2.3. Mathematical Modeling

Using regression analysis, a mathematical model can be obtained that relates the output responses to the function of the input parameters. After the preliminary investigation, a mathematical formulation can be formed using the cubic polynomial relation. The cubic or third order polynomial function can be expressed as represented in Equation (1).
Y = b o + i = 1 n b i X i + j > i n b i j X i X j + i = 1 n b i i X i 2 + k > j > i n b i j k X i X j X k + j > i n b i j X i X j 2 + i = 1 n b i i i X i 3 + ε
where Xi represents the four input factors, such that i ∈{f, s, p, g}; b represents the coefficient corresponding to the specified terms; bo is the constant term, bi is the coefficient of the linear terms; bij is the coefficient of the linear interaction terms and bijk is the coefficient of the interaction terms among the linear and quadratic order; biii is the coefficient of the cubic terms. We used Design Expert software, with the cubic model and auto selection of terms relying on the adjusted R2.

3. Results and Discussion

3.1. 304 HS Stainless Steel Cast

Figure 4 represents the micrographs of the laser welding of high-sulfur content casts, carried out with a power of 6 kW, a welding speed of 2.4 m·min−1, and a shield gas comprising 70% He + 30% Ar. It shows a keyhole weld bead with a focus distance of 2 mm and 7 mm. However, we see that the weld is partially penetrated when the focus point is 12 mm away from the workpiece.
The effects of the laser welding parameters on the welds’ morphology are gathered in Table 5, where the input (investigated) factors and responses are presented.
Based on the results depicted in Table 5, the first 14 experiments gave full penetrated welds. All the cited runs were executed with different welding speeds and powers, but with a constant focus point of 2 mm. In this case, keyhole mode heat transfer occurred. A high-energy density laser beam vaporizes the workpiece during the welding process to form a hole, which allows the laser beam to penetrate into the metal to produce a deep, narrow melt pool, thus leading to a high aspect ratio. The range of values of the weld aspect ratio is between 1.14 and 2.17. The combination of a high ionization energy and the high thermal conductivity of helium favors higher weld aspects in comparison to mixing gas (He, Ar). Once the laser beam is defocussed at focus point 7 mm or 12 mm from the workpiece, the weld becomes partially penetrated, despite the high content of sulfur in the cast 304 HS. The effect of sulfur as a surfactant element is hidden and not obvious.
At a high energy level, helium as well as mixed gas (70% He + 30% Ar) produces larger weld beads than those produced under the shield gas mixture (40% He + 60% Ar). This is attributed to the fact that helium is characterized by a high ionization potential, which provides better protection of the weld pool by expelling the plasma and ensuring less heat loss transfer. On the other hand, at high linear energy and under a gas mixture with 60% argon, there is a risk of argon ionization, which causes the formation of plasma.

3.1.1. Regression Model for Weld Depth (Yd)

After performing the multi-regression analysis using Design Expert software, excluding two outliers, the mathematical model shown in Equation (2) can be obtained for the responses variable Yd.
Yd = 7.03481 + 0.10019 Xf + 0.85970 Xs − 1.18023 Xp − 13.46056 Xg − 0.49642 Xf Xs + 0.19418 Xf Xp + 0.52264 Xf Xg + 2.55656 Xp Xg − 0.04246 Xf2 + 9.12357 Xg2 + 0.03329 Xf2 Xs − 0.01132 Xf2 Xp − 0.35694 Xf Xg2 − 1.73172 Xp Xg2
The statistical indicators specify the significance of the proposed mathematical model. Figure 5 shows (a) the normal plot of residuals and (b) the predicted transformed data as compared to the actual transformed data. The normal plot of residuals depicts that the residuals (errors) are approximately normally distributed. This means the errors are independent and random. Also, this distribution indicates the quality of the regression model. The ANOVA results confirm the statistical significance of the proposed mathematical model, as listed in Table 6. The proposed mathematical model is significant when F-value = 73.46 is sufficiently high. The values of R2 are as follows: obtained R2 = 0.9875, adjusted R2 = 0.9741, and predicted R2 = 0.9438. The difference between R2 and the adjusted R2 is small (less than 0.2), which indicates the statistical significance of the equation. Moreover, the signal-to-noise ratio is sufficiently high, S/N = 21.417, which shows the adequacy of the model in representing data that can be used to design high-quality systems.
As regards the ANOVA results, the major contributor is the factor focus point (Xf), which contributes about 52.35% of the data variance with a linear effect. The second parameter is welding speed (Xs); its linear effect contributes about 9.04% of the data variance. The third factor is Xp, which shows a percentage of 5.66%. The interaction effect between the quadratic form (Xf) and Xs gives a contribution of about 5.54%. This interaction effect can be seen in Figure 6a, where the contour lines are not linear. The interaction effect between Xf and Xp is significant, with a contribution of 3.39%, as shown in Figure 6b, where the contour lines seem to be linear. Many other terms are significant; however, their contributions are small. For example, the quadratic from of Xf2 shows 2.84%, and the interaction form (Xf Xs) shows 1.29%. Some terms give a contribution of about 1%, for example, (XpXg2), (Xf2 Xp), (Xf Xg2), and (Xg2). In this model, there are five terms with p-value > 0.05, which indicates the statistical insignificance of these terms, which are (XpXg), (Xf Xg), (Xg2), (Xf Xg2) and (Xg). However, these terms were kept in the equation to conserve the hierarchical relation of the model, with very small coefficients.

3.1.2. Regression Model for Aspect Ratio (Yr)

With the same methodology, the mathematical formulation of Yr can be formulated as in Equation (3) after excluding two outlier points.
Yr = 0.08185 − 0.01150 Xf + 1.32215 Xs − 0.06562 Xp + 0.26042 Xg − 0.35371 Xf Xs + 0.14512 Xf Xp − 0.08525 Xs Xp − 0.00748 Xf2 + 0.02270 Xf2 Xs − 0.00942 Xf2 Xp
The statistical indicators show the significance of the proposed formulation. As shown in Figure 7a, the residuals are normally distributed. The residuals sit approximately around the line, which indicates that the errors are normally distributed. Moreover, Figure 7b shows a good distribution of the actual data against the predicted data. The ANOVA results for Yr are listed in Table 7. As shown, the F-value of the model is high—F-value = 43.59—with a p-value < 0.0001, which indicates the good fit of the proposed equation for modeling the measured data. The obtained R2 = 0.9625, the adjusted R2 = 0.9404, and the predicted R2 = 0.9145; these good values confirm the statistical significance of the mathematical model. The signal to noise ratio S/N = 17.725 > 4, i.e., an adequate signal. The statistics in Figure 8a,b support the statistical significance of the proposed relation for predicting the effects of Yr on the functions of the four parameters Xf, Xs, Xp, and Xg.
Concerning the different terms of the equation, only ten terms are kept in the equation. The ANOVA results show the statistical significance of the linear terms. The factor Xf is responsible for the main effect, which contributes about 80% of the variance. The effects of the other variables are small compared to Xf. The second contributor is the third-order term (Xf2 Xs), which contributes with only 2.81%. The interaction relationships between Xf and Xs are shown in Figure 8a. This figure shows that the contour lines are not linear. The other statistically significant terms represent Xs, Xf Xs, Xp, and Xf2 Xp, which contribute, respectively, to 2.1%, 1.97%, 1.53%, and 0.92%. As shown in Figure 8b, the interaction relationships between Xf and Xp are weak and nonlinear. There are four insignificant terms that are kept to conserve the hierarchy of the equation, which include Xg, Xs Xp, Xf Xp, and Xf2.

3.2. 304 LS Stainless Steel Cast

Figure 9 shows micrographs of the laser welding of a high-sulfur content cast, carried out with a power of 3.674 kw, a welding speed of 2.450 m·min−1, and a shield gas comprising 70% He + 30% Ar. It produces a keyhole weld bead with focus distance of 2 mm. However, the weld is partially penetrated when the focus point is 7 mm or 12 mm from the workpiece.
The effects of the laser welding parameters on the welds’ morphology are gathered in Table 8, which represents the investigated factors and the responses. We can specifically see that all the welds are partially penetrated. The weld is determined by the thermal conduction mode and surface tension-driven fluid flow in the weld pool. Marangoni convection forces the molten fluid to move from the center to the edges. The welds executed with a 2 mm focus point show greater penetration. Among the 30 experiments, only 7 gave aspect ratio values greater than 1, and the remaining results were all less than 1. These results confirm that the 304 LS welds were wider.

3.2.1. Regression Model for Weld Depth (Yd)

The weld depth (Yd) can be modeled as a function of the four parameters using the following equation, after excluding one outlier point:
ln(Yd) = +1.93616 − 0.598436 Xf − 1.59819 Xs + 0.123277 Xp − 2.16420 Xg + 0.465780 Xf Xs − 0.146866 Xf Xp + 1.93070 Xf Xg + 0.145050 Xs Xp − 0.020255 Xf2 + 1.74479 Xg2 − 0.019693 Xf Xs Xp − 0.027802 Xf2 xs + 0.015243 Xf2 Xp − 1.40293 Xf Xg2
The obtained F-value = 21.51 and p-value < 0.0001, which indicates the statistical significant of the mathematical model. There is only a 0.01% chance that an F-value could occur due to noise. Moreover, the obtained value R2 = 0.9556, the adjusted value R2 = 0.9112, and the S/N = 17.388 indicate a satisfactory fitting of the proposed equation to the data. The accuracy of the mathematical model can be represented by plotting the predicted against the experimental data, as shown in Figure 10b, and by interpreting the normal plot of the residuals shown in Figure 10a. There is a small difference in some points between the experimental and predicted data.
The ANOVA results are shown in Table 9. They indicate the statistical significance of most of the equation terms. Any term with p-value < 0.05 is considered as statistically significant. One can notice that the interactions between the variables and the higher orders are significant. In this case, xf, xf xp, xf2, xg2, xf2xs, xf2xp and xf xg2 are significant model terms. Values greater than 0.1 indicate that the model terms are not significant. Also, the lack of fit is insignificant, as it confirms the statistical significance of the proposed model as regards its ability to express the effect of the four parameters on the depth.
The major contributor is factor Xg2, which contributes about 36% of the data variance with a linear effect. The second parameter is Xf Xg2; its linear effect contributes about 27% of the data variance. The third factor is Xf, which contributes a percentage of 6.78%. The interaction effect between the quadratic form Xg and Xf gives a contribution of about 2.5%. This interaction effect can be inferred from Figure 11a, where the contour lines are not linear. The interaction effect between Xf and Xp is significant, with a contribution of 3.2%, as shown by Figure 11b. The interaction effect between Xs and Xf is significant, with a contribution of 3.5%, as shown in Figure 11c.

3.2.2. Regression Model for Aspect Ratio (Yr)

The ratio can be modeled as a function of the four parameters, as is written in Equation (5) after excluding one outlier point:
Yr = −0.611 + 0.1327 Xf + 0.0677 Xs + 0.0052 Xp + 2.8902 Xg − 0.012 Xf2 xp − 2.004Xg2
The statistical indicators show the weak significance of the effects of the model’s parameters on Yr. The proposed mathematical model can be used to represent Yr, where F-value = 6.98 and p-value = 0.0003. However, the obtained value R2 = 0.6556, the adjusted value R2 = 0.5617, and the signal to noise ratio S/N = 8.094 indicate a satisfactory fitting of the proposed equation to the data. The accuracy of the mathematical model can be represented by plotting the predicted against the experimental data, as shown in Figure 12b, and in the form of a normal plot of the residuals, as shown in Figure 12a. There is a difference in some points between the experimental and the predicted data. The ANOVA results are shown in Table 10, and these indicate the statistical significant of the equation terms. The main effect on Yr is related to the variation in the focus point Xf. There is no interaction between the factors. The variation in Yr is mainly related to the linear variation of Xf and the quadratic variation of Xf and Xg.
As shown in Table 10, the major contributor is the factor Xf, which contributes to almost 50% of the data variance, with a linear effect. The interaction effect between Xf and Xg can be seen in Figure 13a. It shows a contribution of 0.8%, as the contour lines are not linear. The interaction effect between Xf and Xp is not significant, with a contribution of 1%, as shown in Figure 13b.

3.3. Contributions of Surface Active Elements to AISI 304 CO2 Laser Weld Morphology

In total, 30 tests were carried out on both casts 304 HS and 304 LS. All the tests carried out on the 304 LS led to partial-penetration welds. However, only 14 welds carried out on 304 HS were fully penetrated welds, as depicted in Table 11.
In total, 16 partial penetration welds were obtained for both casts under the same welding conditions (from trial 15 to 30, see Table 11). With the welding conditions chosen for experiments 1 to 14, we achieved full-penetration welds with 304 HS and partial weld penetration with 304 LS. Among the 16 cases in which both casts gave rise to partial weld penetration, the role of sulfur as a surfactant element was only obvious in 9. As such, 56% of the partial penetration welds verify the mechanism proposed by C.R Heiple et al. [18], as depicted in Table 12. We must remember that the mechanism proposed by C.R Heiple et al. [18] stipulates that casts with a high sulfur content exhibit greater weld depth than those with low sulfur content, owing to the reverse Marangoni convection leading to deeper weld beads. On the other hand, the width of the weld bead of a low-sulfur content cast is larger than that of a high-sulfur cast, due to the occurrence of Marangoni convection.
In the remaining 14 cases, in which the welds were fully penetrated for 304 HS and partially penetrated for 304 LS, only in 5 tests were the mechanisms proposed by C.R Heiple et al. [18] confirmed. The role of sulfur as a surfactant is disturbed or completely reduced when keyhole-mode welding occurs. In laser welding, many complicated factors are involved, especially those associated with weld pool dynamics, melt evaporation, plasma formation, keyhole instability, the aerodynamic currents of the shield gas and the interaction between the laser beam and the plasma plume. The accumulation of hot fumes at the beam focus point, under certain conditions, can turn into a plasma cloud that strongly affects the beam, and absorbs and disperses it. All the above mentioned phenomena contribute to hiding surface active role of sulfur in determining the laser weld shape. As depicted in Table 12, the rate of achievement of reverse Marangoni convection was 56% for partially penetrated welds, compared to 36% when the welds were fully penetrated (keyhole mode). When weld penetration is governed by a keyhole mechanism, the role of surface tension gradients is diminished or completely hidden.

4. Conclusions

In this work, the effects of variations in microchemistry on the laser welding of industrial austenitic stainless steel casts 304 HS and 304 LS have been studied. The effect of laser power, welding speed, focus point position, and shield gas on depth of weld (Yd) and aspect ratio (Yr) were investigated using RSM. An optimal response surface design was employed to design the experiment. The model required 15 points, and another 15 points were added randomly to increase the model efficiency using Design Expert software. The following conclusions can be drawn:
  • For 304 HS, the focus point (Xf) is the major factor in determining the depth of penetration of the laser weld, within a range of chosen welding parameters. The last input parameter is the main input factor, such that its contribution reaches 52.35% in determining the depth of the laser weld. The second parameter is welding speed (Xs); its linear effect contributes about 9.04% of the data variance. The third factor is the Xp, which represents a percentage of 5.66%;
  • For 304 LS, the depth of the laser weld is primarily determined by the focus point, with a contribution of up to 6.78% (far greater than the other input factors if we consider only the effects of singular input factors individually). However, the interaction between shield gas and focus point distance from workpiece seems to play an important role, with a contribution of up to 28%;
  • The role of the shield gas in protecting the weld pool is also linked to the level of energy supplied. Thus, at a high energy level, helium as well as mixed gas (70% He + 30% Ar) produces weld beads larger than those produced with the shield gas mixture (40% He + 60% Ar). This is attributed to the fact that helium is characterized by a high ionization potential, protecting the weld pool more effectively by expelling the plasma and ensuring less heat loss transfer. On the other hand, under a gas mixture with 60% argon, at a high linear energy, there is a risk of argon ionization causing the formation of plasma;
  • A statistical study shows that a partially penetrated weld rate of 56% supports the hypothesis of the role of surface active elements in the formation of the weld pool. In contrast, in the case of full penetration welds, a rate of only 36% confirms the surface active effects of sulfur. Based on all these results, we can conclude that the laser weld morphology depends on the surface active effects of sulfur only if the chosen weld parameters result in partially penetrated welds. The surface active role of sulfur is reduced, if not eliminated, owing to melt evaporation, plasma formation, keyhole instability, the aerodynamic currents of the shield gas, and the interaction between the laser beam and the plasma. The above phenomena are more pronounced when the chosen welding parameters lead to fully penetrated welds;
  • The results obtained from this work constitute an interesting database for research dedicated to the numerical simulation of thermal profiles in order to validate mathematical models. The thermal profile and solidification mode can be used to predict the microstructural and mechanical properties. On the other hand, these results may be of great use in industrial applications relating to the laser welding of thin austenitic stainless steel sheets.

Author Contributions

Conceptualization, K.T.; methodology, K.T., A.I. and R.D.; software, K.T., E.A. and A.B.; validation, K.T., E.A. and A.I.; formal analysis, K.T. and A.C.H.; investigation, K.T., R.D. and E.A.; resources, A.I.; data curation, K.T. and M.M.Z.A.; writing—original draft preparation, K.T. and E.A.; writing—review and editing, K.T., R.D. and E.A.; visualization, K.T., A.B. and A.C.H.; supervision, K.T., A.I. and M.M.Z.A. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The data used to support the findings of this study are included within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Biswas, A.R.; Banerjee, N.; Sen, A.; Maity, S.R. Applications of laser beam welding in automotive sector—A Review. In Advances in Additive Manufacturing and Metal Joining; Springer: Berlin/Heidelberg, Germany, 2023; pp. 43–57. [Google Scholar]
  2. Narayana, R.B.; Hema, P.; Padmanabhan, G. Experimental investigation on similar and dissimilar alloys of stainless steel joints by laser beam welding. Adv. Mater. Process. Technol. 2022, 8, 13–28. [Google Scholar]
  3. Hollatz, S.; Hummel, M.; Jaklen, L.; Lipnicki, W.; Olowinsky, A.; Gillner, A. Processing of keyhole depth measurement data during laser beam micro welding. J. Mater. Des. Appl. 2020, 234, 722–731. [Google Scholar] [CrossRef]
  4. Olson, D.L.; Siewert, T.A.; Liu, S.; Edwards, G.R. (Eds.) ASM Handbook, Volume 6: Welding, Brazing, Soldering; ASM International: Materials Park, OH, USA, 2014. [Google Scholar]
  5. Kurc-Lisiecka, A.; Kciuk, M. The influence of chemical composition on structure and mechanical properties of austenitic Cr-Ni steels. J. Achiev. Mater. Manuf. Eng. 2013, 61, 210–215. [Google Scholar]
  6. Dong, X.; Wang, G.; Ghaderi, M. Experimental investigation of the effect of laser parameters on the weld bead shape and temperature distribution during dissimilar laser welding of stainless steel 308 and carbon steel St 37. Infrared Phys. Technol. 2021, 116, 103774. [Google Scholar] [CrossRef]
  7. Sampreeta, K.R.; Vasareddy, M.; Deepan, B.K.T. Optimization of process parameters in CO2 laser welding of Hastelloy C-276. Mater. Today Proc. 2020, 22, 1572–1581. [Google Scholar] [CrossRef]
  8. Sathiya, P.; Abdul Jaleel, M.Y.; Katherasan, D. Optimization of welding parameters for laser bead-on-plate welding using Taguchi method. Prod. Eng. 2010, 4, 465–476. [Google Scholar] [CrossRef]
  9. Anawa, E.; Olabi, A.; Hashmi, M. Optimization of ferritic/austenitic laser welded components. In Proceedings of the AMPT2006 International Conference, Las Vegas, NV, USA, 30 July–3 August 2006. [Google Scholar]
  10. Benyounis, K.Y.; Olabi, A.G.; Hashmi, M.S.J. Optimization the laser-welded butt joints of medium carbon steel using RSM. J. Mater. Process. Technol. 2005, 164-165, 986–989. [Google Scholar] [CrossRef] [Green Version]
  11. Indacochea, J.E.; Olson, D.L. Relationship of Weld Metal Microstructure and Penetration to Weld Metal Oxygen Content. J. Mater. Energy Syst. 1983, 5, 139–148. [Google Scholar] [CrossRef]
  12. Klapczynski, V.; Le Maux, D.; Courtois, M.; Bertrand, E.; Paillard, P. Surface tension measurements of liquid pure iron and 304L stainless steel under different gas mixtures. J. Mol. Liq. 2022, 350, 118558. [Google Scholar] [CrossRef]
  13. Heiple, C.R.; Burgardt, P. Effect of SO2 Shielding Gas Additions on GTA Weld Shape Welding. Weld. J. 1985, 64, 159–162. [Google Scholar]
  14. Zhao, C.X.; Kwakernaak, C.; Pan, Y.; Richardson, I.M.; Saldi, Z.; Kenjeres, S.; Kleijn, R. The effect of oxygen on transitional Marangoni flow in laser spot welding. Acta Mater. 2010, 5, 6345–6357. [Google Scholar] [CrossRef]
  15. Wenchao, K.; Zhi, Z.; Oliveira, J.P.; Bei, P.; Jiajia, S.; Caiwang, T.; Xiaoguo, S.; Wentao, Y. Heat transfer and melt flow of keyhole, transition and conduction modes in laser beam oscillating welding. Int. J. Heat Mass Transf. 2023, 203, 123821. [Google Scholar]
  16. Coviello, D.; D’Angola, A.; Sorgente, D. Numerical Study on the Influence of the Plasma Properties on the Keyhole Geometry in Laser Beam Welding. Front. Phys. 2022, 9, 754672. [Google Scholar] [CrossRef]
  17. Hou, Y.C.; Lu, W.; Wentao, Y. Influence of oxygen content on melt pool dynamics in metal additive manufacturing: High-fidelity modeling with experimental validation. Acta Mater. 2023, 249, 118824. [Google Scholar]
  18. Heiple, C.R.; Roper, J.R.; Stagner, R.T.; Aden, R.J. Surface Active Element Effects on the Shape of GTA, Laser, and Electron Beam Welds. Weld. J. 1983, 62, 72–77. [Google Scholar]
  19. Kaul, R.; Ganesh, P.; Singh, N.; Jagadeesh, R.; Bhagat, M.S.; Kumar, H.; Tiwari, P.; Vora, H.S.; Nath, A.K. Effect of active flux addition on laser welding of austenitic stainless steel. Sci. Technol. Weld. Join. 2007, 12, 127–137. [Google Scholar] [CrossRef]
  20. Ding, F.; Ruihua, Z.; Nakata, K.; Tanaka, M.; Ushio, M. YAG laser welding with surface activating flux. China Weld. 2003, 12, 83–86. [Google Scholar]
  21. Su, Y.; Aarts, R.G.K.M.; Meijer, J.; Guan, Q. Study on effect of active-fluxes in laser welding. In Proceedings of the International Congress of Applications of Lasers & Electro-Optics, Dearborn, MI, USA, 2–5 October 2000; Laser Institute of America: Orlando, FL, USA, 2000; pp. 35–41. [Google Scholar]
  22. Kou, S. Welding Metallurgy; John Wiley & Sons: Toronto, ON, Canada, 1987; Volume 431, pp. 223–225. [Google Scholar]
  23. Shahab, A. Contribution a L’etude de la Metallurgie du Soudage de L’inconel 625 et Des Aciers Inoxydables 304 et 316. Ph.D. Thesis, University of Nantes, Nantes, France, 1990. [Google Scholar]
  24. Novák, V.; Řeháčková, L.; Váňová, P.; Sniego, M.; Matýsek, D.; Konecná, K.; Smetana, B.; Rosypalová, S.; Tkadlecková, M.; Drozdová, L.; et al. The Effect of Trace Oxygen Addition on the Interface Behavior of Low-Alloy Steel. Materials 2022, 15, 1592. [Google Scholar] [CrossRef] [PubMed]
  25. Kamel, T.; Abdelil, C.H.; Rachid, D.; Abousoufiane, O.; Abdallah, B.; Albaijan, I.; Hany, S.A.; Mohamed, M.Z.A. Mechanical, Microstructure, and Corrosion Characterization of Dissimilar Austenitic 316L and Duplex 2205 Stainless-Steel, ATIG Welded Joints. Materials 2022, 15, 2470. [Google Scholar]
  26. Besnea, D.; Dontu, O.; Gheorghe, G.I.; Ciobanu, R.; Cuta, A. Laser micro welding of mechatronics components, Romanian Review Precision Mechanics. Opt. Mechatron. 2014, 46, 7–10. [Google Scholar]
  27. Narayana Reddy, B.; Hema, P.; Padmanabhan, G. Influence of CO2 Laser Beam Welding Process Parameters on Mechanical Properties of Alloy AISI 4130 Steel Welded Joints. In Recent Advances in Material Sciences; Lecture Notes on Multidisciplinary Industrial Engineering; Springer: Singapore, 2019; pp. 65–76. [Google Scholar]
Figure 1. Surface tension against temperature of 304 SS casts [23].
Figure 1. Surface tension against temperature of 304 SS casts [23].
Crystals 13 01138 g001
Figure 2. (a) Laser welding modes [26], (b) laser beam welding in progress [27].
Figure 2. (a) Laser welding modes [26], (b) laser beam welding in progress [27].
Crystals 13 01138 g002
Figure 3. Scheme of the CO2 laser beam focus positions used: (a) focus point = 2 mm, (b) focus point = 7 mm, (c) focus point = 12 mm.
Figure 3. Scheme of the CO2 laser beam focus positions used: (a) focus point = 2 mm, (b) focus point = 7 mm, (c) focus point = 12 mm.
Crystals 13 01138 g003
Figure 4. Effect of focus point on 304 HS laser weld carried out with a power 6 kw, welding speed 2.4 m·min−1, and shield gas comprising 70% He + 30% Ar.
Figure 4. Effect of focus point on 304 HS laser weld carried out with a power 6 kw, welding speed 2.4 m·min−1, and shield gas comprising 70% He + 30% Ar.
Crystals 13 01138 g004
Figure 5. Statistical indicators model. (a) Normal plot of residuals; (b) predicted vs. actual observations for Yd.
Figure 5. Statistical indicators model. (a) Normal plot of residuals; (b) predicted vs. actual observations for Yd.
Crystals 13 01138 g005
Figure 6. The interaction relationships between (a) Xf and Xs and (b) Xf and Xp for Yd.
Figure 6. The interaction relationships between (a) Xf and Xs and (b) Xf and Xp for Yd.
Crystals 13 01138 g006
Figure 7. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted vs. actual observations.
Figure 7. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted vs. actual observations.
Crystals 13 01138 g007
Figure 8. The interaction relationships between (a) Xf and Xs and (b) Xf and Xp for Yr.
Figure 8. The interaction relationships between (a) Xf and Xs and (b) Xf and Xp for Yr.
Crystals 13 01138 g008
Figure 9. Effect of focus point on 304 LS laser weld carried out with a power of 3.674 kw, a welding of speed 2.450 m·min−1, and a shield gas comprising 70% He + 30% Ar.
Figure 9. Effect of focus point on 304 LS laser weld carried out with a power of 3.674 kw, a welding of speed 2.450 m·min−1, and a shield gas comprising 70% He + 30% Ar.
Crystals 13 01138 g009
Figure 10. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted observations vs. actual observations.
Figure 10. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted observations vs. actual observations.
Crystals 13 01138 g010
Figure 11. The interaction relationships between (a) Xf and Xg, (b) Xf and Xp and (c) Xf and Xs.
Figure 11. The interaction relationships between (a) Xf and Xg, (b) Xf and Xp and (c) Xf and Xs.
Crystals 13 01138 g011
Figure 12. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted observations vs. actual observations.
Figure 12. Model statistical indicators. (a) Normal plot of residuals. (b) The predicted observations vs. actual observations.
Crystals 13 01138 g012
Figure 13. The interaction relationships between (a) Xf and Xg and (b) Xf and Xp.
Figure 13. The interaction relationships between (a) Xf and Xg and (b) Xf and Xp.
Crystals 13 01138 g013
Table 1. Chemical composition (wt. %) of 304 stainless steel casts.
Table 1. Chemical composition (wt. %) of 304 stainless steel casts.
ElementsCMnSiPSCrNiFe
304HS SS0.060.860.410.0240.00818.298.40Balance
304LS SS0.061.060.570.0320.00318.298.45Balance
Table 2. Surface tension at melting temperature, thermal gradient and sulfur content of used casts [23].
Table 2. Surface tension at melting temperature, thermal gradient and sulfur content of used casts [23].
Elementsγ (N/m) at Melting Temperaturedγ/dT (N/m °K)Sulfur Content (%)
304HS SS1.62+8 × 10−50.008
304LS SS1.74−10−50.003
Table 3. Physical properties of shield gas used.
Table 3. Physical properties of shield gas used.
Laser Welding GasMolecular Weight (g/mol)Thermal Conductivity at 1 bar, 15 °C (W/m·K)Ionization Energy (ev)Dissociation Energy (ev)Density Relative to Air
Helium40.1536324.600.14
Argon400.0173215.801.38
Table 4. Laser welding parameters.
Table 4. Laser welding parameters.
RunsFocus Point Position (mm)Welding Speed (m/min)Power (kW)Linear Energy (J/cm)Shield Gas
12.001.253.751801 (70% He + 30% Ar)
22.002.453.67901 (70% He + 30% Ar)
32.002.406.001501 (70% He + 30% Ar)
42.003.606.001001 (70% He + 30% Ar)
57.001.253.751801 (70% He + 30% Ar)
67.002.406.001501 (70% He + 30% Ar)
72.001.253.751802 (100% He)
82.002.453.67902 (100% He)
92.002.406.001502 (100% He)
102.003.606.001002 (100% He)
112.001.253.751803 (40% He + 60% Ar)
122.002.453.67903 (40% He + 60% Ar)
132.003.606.001003 (40% He + 60% Ar)
142.002.406.001503 (40% He + 60% Ar)
1512.001.253.751802 (100% He)
1612.002.453.67902 (100% He)
1712.002.406.001502 (100% He)
1812.003.606.001002 (100% He)
197.002.406.001503 (40% He + 60% Ar)
207.002.406.001502 (100% He)
2112.001.253.751803 (40% He + 60% Ar)
2212.002.453.67903 (40% He + 60% Ar)
2312.002.406.001503 (40% He + 60% Ar)
2412.003.606.001003 (40% He + 60% Ar)
257.002.453.67901 (70% He + 30% Ar)
267.002.406.001501 (70% He + 30% Ar)
2712.001.253.751801 (70% He + 30% Ar)
2812.002.453.67901 (70% He + 30% Ar)
2912.002.406.001501 (70% He + 30% Ar)
3012.003.606.001001 (70% He + 30% Ar)
Table 5. Investigated factors and the responses for 304 HS.
Table 5. Investigated factors and the responses for 304 HS.
RunsInvestigated FactorsResponse Variables
Xf
(Focus Point) (mm)
Xs
(Weld Speed) (m/min)
Xp
(Power) (kW)
Xg
(Shield Gas Type)
Yd
Depth (mm)
Yr R (D/W)
121.253.751 (70% He + 30% Ar)31.6
222.453.6741 (70% He + 30% Ar)31.8
322.461 (70% He + 30% Ar)31.42
423.66.0011 (70% He + 30% Ar)31.75
571.253.751 (70% He + 30% Ar)31.17
672.461 (70% He + 30% Ar)31.36
721.253.752 (100% He)31.41
822.453.6742 (100% He)32.1
922.462 (100% He)32.1
1023.66.0012 (100% He)32.14
1121.253.753 (40% He + 60% Ar)31.14
1222.453.6743 (40% He + 60% Ar)31.71
1322.46.003 (40% He + 60% Ar)31.76
1423.66.0013 (40% He + 60% Ar)32.17
15121.253.752 (100% He)0.60.29
16122.453.6742 (100% He)0.410.26
17122.46.002 (100% He)1.400.77
18123.66.0012 (100% He)0.550.31
1972.46.003 (40% He + 60% Ar)2.010.82
2072.46.002 (100% He)1.920.71
21121.253.753 (40% He + 60% Ar)0.70.39
22122.453.6743 (40% He + 60% Ar)0.40.28
23122.46.003 (40% He + 60% Ar)0.790.47
24123.66.0013 (40% He + 60% Ar)0.410.23
2572.453.6741 (70% He + 30% Ar)1.640.77
2673.66.0011 (70% He + 30% Ar)1.960.73
27121.253.751 (70% He + 30% Ar)0.50.25
28122.453.6741 (70% He + 30% Ar)0.480.31
29122.46.001 (70% He + 30% Ar)1.770.61
30123.66.0011 (70% He + 30% Ar)1.911.08
Table 6. ANOVA results of the Yd in function of Xf, Xs, Xp and Xg.
Table 6. ANOVA results of the Yd in function of Xf, Xs, Xp and Xg.
SourceSum of SquaresDFMean SquareF-Valuep-ValueContribution (%)
Model34.37142.4673.46<0.0001
Xf8.3418.34249.44<0.000152.35
Xs1.4411.4443.06<0.00019.04
Xp0.90110.90126.960.00025.66
Xg0.018110.01810.54140.47490.11
Xf Xs0.205810.20586.160.02751.29
Xf Xp0.539310.539316.140.00153.39
Xf Xg0.018910.01890.56580.46540.12
Xp Xg0.032910.03290.98570.33890.21
Xf20.452910.452913.550.00282.84
Xg20.132610.13263.970.06780.83
Xf2 Xs0.881910.881926.390.00025.54
Xf2 Xp0.167610.16765.020.04321.05
Xf Xg20.137610.13764.120.06340.86
Xp Xg20.169710.16975.080.04211.07
Residual0.4344130.0334
Cor Total34.82715.9317
Table 7. ANOVA results of the effects of Yr on the function of Xf, Xs, Xp and Xg.
Table 7. ANOVA results of the effects of Yr on the function of Xf, Xs, Xp and Xg.
SourceSum of SquaresDFMean SquareF-Valuep-ValueContribution (%)
Model12.86101.2943.59<0.0001
Xf11.64111.64394.76<0.000179.76
Xs0.306110.306110.380.0052.10
Xp0.223810.22387.590.01351.53
Xg0.097710.09773.310.08650.67
Xf Xs0.287510.28759.750.00621.97
Xf Xp0.073810.07382.50.1320.51
Xs Xp0.092910.09293.150.09390.64
Xf20.008510.00850.28860.59810.06
Xf2 Xs0.4110.4113.90.00172.81
Xf2 Xp0.13410.1344.540.04790.92
Residual0.5014170.0295
Cor Total13.362714.5938
Table 8. Investigated factors and the responses for 304 LS.
Table 8. Investigated factors and the responses for 304 LS.
RunsInvestigated FactorsResponse Variables
Xf
(Focus Point) (mm)
Xs
(Weld Speed) (m/min)
Xp
(Power kW)
Xg
(Shield Gas Type)
Yd
Depth (mm)
Yr R(D/W)
121.253.751 (70% He + 30% Ar)1.800.84
222.453.6741 (70% He + 30% Ar)2.751.06
322.461 (70% He + 30% Ar)1.270.66
423.66.0011 (70% He + 30% Ar)1.261.01
571.253.751 (70% He + 30% Ar)1.750.64
672.461 (70% He + 30% Ar)1.590.70
721.253.752(100% He)1.600.88
822.453.6742(100% He)0.800.51
922.462(100% He)1.320.75
1023.66.0012(100% He)1.261.01
1121.253.753(40% He + 60% Ar)1.070.61
1222.453.6743(40% He + 60% Ar)1.120.59
1322.46.003(40% He + 60% Ar)0.820.65
1423.66.0013(40% He + 60% Ar)1.241.02
15121.253.752(100% He)0.520.24
16122.453.6742(100% He)0.370.22
17122.462(100% He)0.770.38
18123.66.0012(100% He)0.390.21
1972.46.003(40% He + 60% Ar)1.240.65
2072.46.002(100% He)0.690.34
21121.253.753(40% He + 60% Ar)0.320.16
22122.453.6743(40% He + 60% Ar)0.900.37
23122.463(40% He + 60% Ar)0.390.18
24123.66.0013(40% He + 60% Ar)2.621.48
2572.453.6741 (70% He + 30% Ar)2.651.20
2673.66.0011 (70% He + 30% Ar)1.860.66
27121.253.751 (70% He + 30% Ar)1.530.58
28122.453.6741 (70% He + 30% Ar)1.51.07
29122.461 (70% He + 30% Ar)1.760.66
30123.66.0011 (70% He + 30% Ar)1.800.70
Table 9. ANOVA results for Yd.
Table 9. ANOVA results for Yd.
SourceSum of SquaresDFMean SquareF-Valuep-ValueContribution (%)
Model9.30140.664021.51<0.0001
Xf 0.527310.527317.080.00106.78
Xs0.077210.07722.500.13600.99
Xp 0.075210.07522.440.14090.97
Xg 0.003010.00300.09710.75990.04
Xf Xs 0.079810.07982.580.13021.03
Xf Xp 0.158310.15835.130.03992.04
Xf Xg 0.041910.04191.360.26330.54
Xs Xp 0.000610.00060.01890.89250.01
Xf20.225910.22597.320.01712.90
Xg22.8612.8692.57<0.000136.77
Xf Xs Xp 0.109410.10943.540.08071.41
Xf2 Xs 0.307610.30769.970.00703.95
Xf2 Xp 0.456610.456614.790.00185.87
Xf Xg22.1612.1669.84<0.000127.77
Residual0.4321140.0309
Lack of Fit0.3837120.03201.320.5094not significant
Pure Error0.048420.0242
Cor Total9.7328
Table 10. ANOVA results for Yr.
Table 10. ANOVA results for Yr.
SourceSum of SquaresdfMean SquareF-Valuep-ValueContribution (%)
Model1.5860.26376.980.0003significant
Xf 0.780510.780520.660.000249.83
Xs0.046910.04691.240.2772.99
Xp 0.000610.00060.01570.90150.04
Xg 0.010810.01080.2870.59750.69
Xf20.23510.2356.220.020615.00
Xg20.176510.17654.670.041811.27
Residual0.831220.0378
Lack of Fit0.8022200.04012.790.2972not significant
Pure Error0.028820.0144
Cor Total2.4128
Table 11. Depth penetration and width weld bead measurements for 304 HS and LS casts.
Table 11. Depth penetration and width weld bead measurements for 304 HS and LS casts.
Exp. #Cast 304 HSCast 304 LSOccurrences of the Mechanism Proposed by C.R Heiple et al. [18]
Inverse Marangoni Convection
Crystals 13 01138 i001
Marangoni Convection
Crystals 13 01138 i002
Weld
Depth
(D) (mm)
Weld
Width
(W) (mm)
Full Weld
Penetration
(F.P)/Partial Penetration
Weld (P.P)
Weld
Depth
(D) (mm)
Weld
Width
(W) (mm)
Full Weld
Penetration
(F.P)/Partial Penetration Weld (P.P)
131.88F.P1.802.14P.PYes
231.67F.P2.752.6P.PYes
332.1F.P1.270.66P.PNo
431.71F.P1.261.25P.PNo
532.56F.P1.752.73P.PYes
632.2F.P1.592.07P.PNo
732.13F.P1.601.82P.PNo
831.42F.P0.801.57P.PYes
931.42F.P1.321.76P.PYes
1032.63F.P1.261.01P.PNo
1132.63F.P1.070.61P.PNo
1231.75F.P1.121.25P.PNo
1331.70F.P0.821.26P.PNo
1431.38F.P1.241.21P.PNo
150.62.06P.P0.522.17P.PYes
160.411.58P.P1.551.22P.PNo
171.401.80P.P0.772.02P.PYes
180.551.77P.P0.391.86P.PYes
192.011.91P.P1.242.45P.PYes
201.922.03P.P0.692.70P.PYes
210.71.78P.P0.321.94P.PYes
220.41.43P.P0.902.43P.PNo
230.791.69P.P0.392.14P.PYes
240.411.78P.P2.621.77P.PNo
252.102.13P.P2.652.23P.PNo
261.962.68P.P1.862.8P.PYes
270.52P.P1.532.64P.PNo
280.481.55P.P1.51.4P.PNo
291.772.90P.P1.762.67P.PNo
301.911.76P.P1.802.57P.PYes
Table 12. Percentages of occurrence of the mechanism proposed by C.R Heiple et al. [18] in the laser welding process.
Table 12. Percentages of occurrence of the mechanism proposed by C.R Heiple et al. [18] in the laser welding process.
Types of Weld BeadTimes Getting Partial Penetration
Weld (PP) for Both Casts or Full Penetration
Weld (FP) for 304 HS Cast Weld Bead out of 30 Tests
Occurrences of the Mechanism Proposed by C.R Heiple et al.
[18] %
Non-Occurrences of
the Mechanism
Proposed by
C.R Heiple et al.
[18] %
Percentages of Occurrences of the Mechanism
Proposed by
C.R Heiple et al.
[18] %
Partial penetration weld (PP) for both casts.169756
Full penetration weld (FP) for 304 HS and partial penetration weld (PP) for 304 LS cast weld. 145936
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Touileb, K.; Attia, E.; Djoudjou, R.; Hedhibi, A.C.; Benselama, A.; Ibrahim, A.; Ahmed, M.M.Z. Effect of Microchemistry Elements in Relation of Laser Welding Parameters on the Morphology 304 Stainless Steel Welds Using Response Surface Methodology. Crystals 2023, 13, 1138. https://doi.org/10.3390/cryst13071138

AMA Style

Touileb K, Attia E, Djoudjou R, Hedhibi AC, Benselama A, Ibrahim A, Ahmed MMZ. Effect of Microchemistry Elements in Relation of Laser Welding Parameters on the Morphology 304 Stainless Steel Welds Using Response Surface Methodology. Crystals. 2023; 13(7):1138. https://doi.org/10.3390/cryst13071138

Chicago/Turabian Style

Touileb, Kamel, Elawady Attia, Rachid Djoudjou, Abdejlil Chihaoui Hedhibi, Abdallah Benselama, Albaijan Ibrahim, and Mohamed M. Z. Ahmed. 2023. "Effect of Microchemistry Elements in Relation of Laser Welding Parameters on the Morphology 304 Stainless Steel Welds Using Response Surface Methodology" Crystals 13, no. 7: 1138. https://doi.org/10.3390/cryst13071138

APA Style

Touileb, K., Attia, E., Djoudjou, R., Hedhibi, A. C., Benselama, A., Ibrahim, A., & Ahmed, M. M. Z. (2023). Effect of Microchemistry Elements in Relation of Laser Welding Parameters on the Morphology 304 Stainless Steel Welds Using Response Surface Methodology. Crystals, 13(7), 1138. https://doi.org/10.3390/cryst13071138

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop