Next Article in Journal
Significantly Improved Electrical Properties of Photo-Initiated Auxiliary Crosslinking EPDM Used for Cable Termination
Next Article in Special Issue
Damage Evolution and Fracture Events Sequence Analysis of Core-Shell Nanoparticle Modified Bone Cements by Acoustic Emission Technique
Previous Article in Journal
Effects of Molecular Chain Length on the Contact Line Movement in Water/n-Alkane/Solid Systems
Previous Article in Special Issue
In-Situ Dynamic Response Measurement for Damage Quantification of 3D Printed ABS Cantilever Beam under Thermomechanical Load
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

A Modified Aging Kinetics Model for Aging Condition Prediction of Transformer Polymer Insulation by Employing the Frequency Domain Spectroscopy

College of Electrical Engineering, Guangxi University, Nanning 530004, Guangxi, China
*
Author to whom correspondence should be addressed.
Polymers 2019, 11(12), 2082; https://doi.org/10.3390/polym11122082
Submission received: 12 November 2019 / Revised: 4 December 2019 / Accepted: 10 December 2019 / Published: 12 December 2019

Abstract

:
The aging kinetics model is of great interest to scholars since it is capable of describing the variation law between the degree of polymerization (DP) and the aging duration of transformer polymer (cellulose) insulation. However, it is difficult to determine the moisture content inside the transformer polymer insulation without destroying it, so that the model parameters cannot be confirmed. Such limitation greatly restricts its application. It is interesting to note that as long as the moisture content of the transformer polymer insulation could be characterized (replaced) by a certain feature parameter, the above issue will be solved naturally. The existing researches indicate that the Frequency Domain Spectroscopy (FDS) is sensitive to moisture. Consequently, the feature parameter that could characterize the moisture inside transformer polymer insulation (extracted from the FDS curve) can be used to report a modified aging kinetics model, which could perform the aging condition prediction of transformer polymer insulation under various test conditions, including aging duration, aging temperature, and initial moisture. In that respect, the average relative error of prediction results of prepared samples is equal to 7.41%, which reveals that the reported model might be serviced as a potential tool for the aging condition prediction of transformer polymer insulation.

Graphical Abstract

1. Introduction

The aging condition of transformer polymer insulation determines the overall service life of the transformer. Existing researches show that the degree of polymerization (DP) can be serviced as the most direct and effective indicator for reflecting the aging condition (mechanical strength) of polymer insulation [1,2,3]. Reviewing the published researches, we found out that the method for predicting (or measuring) the DP value of transformer polymer insulation consists of several prevailing approaches, such as the direct method (viscosity testing) [4] and indirect methods (including the Frequency Dielectric Spectroscopy (FDS) [5,6,7,8,9] technique, aging kinetics model [10,11,12], etc.). Although the viscosity test method is accurate enough, it is not appropriate for analyzing the field equipment due to its destructiveness. Consequently, the indirect method is of great interest to scholars in contrast with the direct method.
It is widely accepted that the aging by-products, such as moisture, acids, alcohols, aldehydes, etc., produced in the degradation process of transformer polymer insulation could regularly affect its FDS [13]. Therefore, the qualitative or quantitative analysis of the DP value of polymer materials can be realized by the relevant feature parameter extracted from the FDS data. In literature [14,15], the integral value of the FDS curve is computed and applied as the feature parameter for achieving the above goal. In addition, the equivalent circuit model that is capable of analyzing the corresponding aging condition is also reported, such as the Cole–Cole model [16], the Havriliak–Negami model [17], the Davidson–Cole model [18], and the Dissado–Hill model [19]. However, it is a fact that the contribution of the aging condition on measured FDS data could be easily covered by the moisture effect [13,14,15]. Therefore, it is rather difficult to accurately analyze the aging condition of the transformer polymer insulation and merely rely on the FDS technique in case the inside moisture is too high.
The published researches pointed out that the aging kinetics model can be employed to describe the degradation process of transformer polymer insulation under different conditions, including temperature, aging duration, and especially the initial moisture content mc% [20,21,22,23,24,25]. Thus, the discussion of the aging kinetics model can make up for the limitation of the FDS technique. At present, the research on the aging kinetics model of polymer insulation is mainly based on the Ekamstam equation [24]. Furthermore, Emsley et al. found that the degradation rate of polymer (cellulose) materials will not always have a constant attributed to the leveling-off degree of the polymerization (LODP) phenomenon [21,22,23]. A second-order kinetics model is thus proposed [23,25]. The findings reveal that the second-order kinetics model can accurately describe the variation law of the DP value of polymer materials under different reaction conditions. Therefore, as long as the model parameters are determined, the above model can be applied to accurately predict the DP value of the polymer insulation materials. However, it is difficult to determine the moisture content inside the unknown sample without destroying it for sampling, which makes the model parameters also uncertain. Such limitation greatly restricts its application on aging condition prediction.
In view of these issues, this research attempts to report a modified aging kinetics model for aging condition prediction by employing the FDS technique, which aims to overcome the mentioned limitations. In the present research, depending on the combination of the advantages of both FDS (sensitive to moisture content) and the aging kinetics model (capable of describing the variation law of DP), an available modified model is proposed. Findings indicated that the proposed model could be utilized to predict the aging condition of transformer polymer insulation under various test conditions, including diverse aging temperature, aging duration, and initial moisture content. Moreover, the average relative error of prediction results of oil-immersed polymer (cellulose) pressboards is less than 10%, which further verify the accuracy and feasibility of the reported model. In that respect, the present contribution reveals that the reported modified aging kinetics model might be serviced as a potential and effective tool for aging condition prediction.

2. Sample Construction

The transformer polymer (cellulose) insulation material (pressboard) and mineral oil are utilized in this paper so as to investigate its frequency response characteristic under different insulation conditions. Therefore, a series of experiments were carried out under controlled laboratory conditions, and the oil-immersed polymer (cellulose) pressboards with various insulation conditions were later prepared. The details of both polymer pressboard and oil are described in Table 1.
The pressboards with various initial moisture contents were completed by moisture absorption. Then, the moisture balance distribution process was later performed at 45 °C and lasted for 48 h so as to perform the FDS test. Subsequently, the DP value and moisture content obtained by DP tester (by means of viscosity tester, Sierda scientific instrument co., LTD, Shanghai, China) and moister tester (by means of Karl Fischer Titration, Wantong co., LTD, Switzerland) can be found in Figure 1.

3. The Establishment of the Traditional Aging Kinetics Model of Transformer Polymer Insulation.

3.1. The Derivation of the Traditional Aging Kinetics Model

Cellulose material is a kind of natural organic polymer homopolymer. Its basic structural unit is glucose monomer (C6H10O5), and its repeating unit is cellobiose, its general formula is (C6H10O5)n in which n is known as the degree of polymerization (DP) [11,12]. The adjacent glucose monomers are linked by 1-4-β glycoside bond, the degradation process of cellulose materials is actually completed by the break of the glycoside bond. In the course of the operation, the glycoside bond of the cellulose materials gradually breaks due to the suffered stresses, including thermal, oxidation, and hydrolysis stress. In this case, the average number of glucose monomers in each cellulose fiber decreased. Consequently, the corresponding DP value decreased with the increase of aging duration.
The kinetics model is widely used to describe the change law of DP of polymer materials under the thermal stress [20,21,22,23,24,25]. If N is the total number of glucose monomers in the polymer insulation, and Mt is the total number of polymer molecules when the aging duration reaches time t, then the corresponding average value of DP of polymer insulation can be regarded as DPt.
D P t = N M t
Chain scission number (CSN) is defined as the times of broken chains per polymer chain during the aging of polymer insulation, the formula for calculating the CSN is as follows:
C S N = D P 0 D P t 1
where DP0 is defined as the initial DP value, which is assumed to be 1100 in this paper. The scission fraction of the polymer unit (SFCU) is defined as the ratio of glucose monomer broken in a polymer chain to the total number of glucose monomers.
S F C U = C S N D P 0 = 1 D P t 1 D P 0
The existing research on the kinetics model of polymer degradation is mainly based on the aging kinetics model of linear high molecular polymers. These researches suggest that the degradation of polymer belongs to a random chain scission reaction (the probability of breaking each bond between polymer fibers is equal) [20,24]. Further, the degradation rate k is considered to be a constant over a certain temperature range. Thus, a kinetics equation for describing the variation law between the DP value and the aging duration of polymer insulation materials is proposed [24].
1 D P t 1 D P 0 = k · t
However, Heywood [26] pointed out that as long as the DP value of polymer (cellulose) insulation materials drops to a certain value, its trajectory will gradually deviate from the first-order kinetics model. In this case, the chemical reaction rate is no longer a constant, which is also known as the leveling-off degree of polymerization [23]. In other words, the parameter k shown in Equation (4) is a variable that changes with the alteration of aging time, which can be represented by Equation (5).
k ( t ) = l i m Δ t 0 m t N · Δ t = k 1 · e k 2 · t
From Equation (5), parameters k1 and k2 are equal to a constant, which are both related to the initial moisture content inside the polymer insulation materials. If there exists a total of m glycosidic bond breaks in the polymer molecule per unit time, the average degree of polymerization DPt+Δt at tt can be written as the following form:
D P t + Δ t = N M t + m
Moreover, the change amount in the DP value (△DPt+t) is shown in Equation (7).
Δ D P t + Δ t = N M t + m N M t = N · m · Δ t ( M t + m ) · M t · Δ t
The simultaneity of Equations (1) and (7) provide an expression characterizing the rate of decrease in the DP value of polymer insulation materials.
D P t = l i m Δ t 0 Δ D P t + Δ t Δ t = l i m Δ t 0 N 2 m ( M t + m ) · M t · N · Δ t l i m Δ t 0 N 2 m M t 2 · N · Δ t = D P t 2 · l i m Δ t 0 m N · Δ t = d D P t d t
Substituting Equation (5) into Equation (8), the Equation (8) can be expressed by another form, shown in Equation (9).
1 D P t 2 d D P t = k ( t ) d t = k 1 · e k 2 · t d t
From Equation (9), the formula for expressing the relationship among the DP, reaction rate, and reaction duration is obtained by employing the integral operation.
D P 0 D P t 1 D P 2 d D P = k 1 · e k 2 · t d t 1 D P t 1 D P 0 = k 1 k 2 ( 1 e k 2 · t )
The above formula is known as the second-order aging kinetics model, which is utilized for describing the quantitative relationship between the DP value and the reaction time of polymer materials. The second-order kinetics model can accurately reflect the change of the polymerization degree of polymer insulation overall aging processes, and thus has been widely reported [21,23]. However, since the aging rate k(t) is an attenuation function used to describe the slowing down of the degradation rate of polymer materials when involving the leveling-off degree of polymerization (LODP) phenomenon, it inevitably lacks a clear physical meaning [25]. Afterwards, depending on the analysis of polymer degradation at the molecular level, a kinetics model based on the “percentage DP loss” of polymer materials [25].
ω ( t ) = 1 D P t D P 0 = ω D P · ( 1 e k D P · t )
From Equation (11), ωDP is assumed as the amplitude of the attenuation function, parameter kDP is named as the degradation rate of polymer, ω(t) represents the capacity of the “DP loss”. Thus, different aging conditions can be represented by the diverse values of ω(t). If the polymer material has not been degraded so far, the corresponding ω(t) is equal to 0, and the value is equal to 1 in the case that polymer materials are completely degraded.

3.2. The Aging Kinetics Model for Aging Condition Analysis

In this part, several oil-immersed polymer pressboards (shown in Table 1) with different initial moisture content (including 0.78%, 1.32%, 2.07%, 2.74%, and 3.82%) are firstly prepared. Then, the above pressboards are utilized to perform the alternate thermal aging experiment at 150 °C. The DP values of the same pressboard with the different aging duration are recorded in the course of the aging experiment. If the horizontal axis and vertical axis are represented by aging duration (hours) and DP values, respectively, the resulting picture that adopted to describing the variation law between aging duration and DP values can be easily plotted.
Moreover, it is clear that Equation (11) can be utilized to describe the degradation process of polymer insulation. Provided that Equation (11) is adopted to fitting the presented variation law of DP vs. aging duration, the parameters (ωDP and kDP) in the formula can be naturally computed, and results are shown in Figure 2.
It is obvious that the higher the initial moisture content inside the polymer insulation, the faster the DP value decreases, and the less time it takes for the curve to become flat. Meanwhile, the impact generated by the initial moisture content can be also observed in the values of computed parameters. These values and error bursts (EB) are shown in Table 2, and the significant figures in the experiment are reserved for 2 digits.
The values of parameters shown in Table 2 are subjected to present an increasing trend with the rising initial moisture content. Such the phenomenon has also pointed out that the quantitative relationship of mc% vs. ωDP and mc% vs. kDP can be studied by fitting analysis. The fitting curves and fitting equation can be found in Figure 3 and Table 3, respectively, where the RSS and R2 represent the residual sum of squares and determination coefficient. The closer the value of RSS is to 0 and the closer the value of R2 is to 1, the better the fitting results.
It is obvious that equations shown in Table 3 could describe the functional relationship between relevant parameters (ωDP and kDP) and initial moisture content. It means that the higher the moisture content, the larger the value of the ωDP and kDP, and thus the faster the degradation rate of polymer insulation materials. By employing a combination of the formulas shown in Equation (11) and Table 3, a universal model for estimating the remaining life L(t) [27,28] of transformer polymer insulation under any initial moisture content is readily obtained, which can be expressed in the form of Equation (12).
L ( t ) = L n ( 1 1 D P t / D P ω D P ( m c % ) ) k D P ( m c % )
However, it is rather difficult to obtain accurate DPt values during the operation. In other words, it is impractical to predict the remaining life of a real transformer by using Equation (12). Therefore, an improved equation to predict the aging degree of polymer insulation of the transformer is required. An improved equation that can predict the DP value of transformer polymer insulation is proposed, which is shown in Equation (13).
D P t ( t ) = D P 0 · [ 1 ω D P ( m c % ) · ( 1 e k D P ( m c % ) · t ) ]

4. The Improved Aging Kinetics Model by Employing Frequency Dielectric Spectrum

On the condition that Equation (13) is desired to perform the analysis activities of the aging condition, a crucial basis is that the moisture content inside the polymer insulation materials is accurately determined. However, the determination of the moisture content inside an unknown cellulose sample is also difficult.
In view of the above issues, the existing researches reveal that dielectric frequency response might be used as an available approach to achieve the moisture analysis of polymer insulation materials [2,6,7,10,11]. Provided that the relevant parameter extracted from the analysis of FDS can be adopted to reflect the moisture content inside the cellulose insulation, the quantitative relationship between the extracted frequency dielectric response parameter and either ωDP (mc%) or kDP (mc%) can be established. Consequently, Equation (13) could be readily employed to carry out the aging condition prediction without the determination of the moisture content.
The purpose of this chapter is to find out the relevant frequency response feature parameter, which could characterize the moisture content but slightly affected by its aging condition. In the previous researches [14,15], the authors demonstrated that with the aggravating of the aging degree of transformer polymer insulation, the FDS curve changes remarkably in low-frequency regions, while remaining unchanged in high-frequency regions. Therefore, the frequency response information extracted from the high-frequency regions can be used to characterize the moisture content inside the transformer polymer insulation without being affected by its aging condition.
In order to obtain the desired relevant parameters, the frequency dielectric response test is performed. It is launched in the three-electrode test cell under 45 °C. The test platform is shown in Figure 4. The FDS curves of non-aged cellulose pressboards with various mc% (including 0.78%, 1.29%, 2.32%, 3.15%, 3.43%, and 4.03%) are measured and plotted in Figure 5. Whereas dielectric loss (tanδ) is the ratio of imaginary part to the real part of ε*(ω), which is not affected by insulation geometry. Thus, the parameter extracted from the tanδ curve is more appropriate for various cellulose insulation materials.
As mentioned above, the tanδ curve in the high-frequency regions could merely reflect the information related to moisture content, and thus the selected high-frequency regions are defined as feature frequency regions, and a range of 100–1000 Hz is selected for this paper. In order to reduce errors in FDS data due to experimental operations, the integral operation (in 100–1000 Hz) is therefore utilized to extract the expected frequency response parameter. Equation (14) shows the calculation formula of these integral values (IV). The computed IV values are shown in Table 4.
I V = f a f b tan δ ( f ) · f = 100 1000 tan δ ( f ) d f
An obvious exponential relationship of IV vs. mc% can be observed, and this viewpoint is proved by the fitting analysis. Its results are shown in Figure 6 and Table 5, respectively.
Form Table 5, the functional relationship between mc% and IV can be expressed by the means of IV = f(mc%), thus, the inverse function formula of IV could be expressed as mc% = f −1(IV). Furthermore, from Table 3, provided that ωDP = g(mc%), and kDP = p(mc%), it means that the moisture content utilized in the formula of ωDP and kDP can be replaced by the inverse function of IV. Furthermore, if the mc% in the formula is offset and the quantitative relationship between IV and ωDP/kDP is established directly, the processed formula is written as ωDP = g[f −1(IV)], and kDP = p[f −1(IV)]. Then, the model for aging condition prediction based on IV can be derived, which is shown in Equation (15).
D P t ( t ) = D P 0 · [ 1 ω D P · [ f 1 ( I V ) ] · ( 1 e k D P · [ f 1 ( I V ) ] · t ) ]
The functional relationship between IV and ωDP/kDP is derived by simultaneous analysis of the equations shown in Table 3 and Table 5. Then, Figure 7 and Table 6 present the corresponding fitting curves and fitting equations, respectively. From Table 6, ωDP and kDP can be calculated by the integral value (IV) of the tanδ curve. The modified model introduced in Equation (15) will promote the practice of aging condition prediction of the unknown polymer samples on the condition that its moisture content is not determined.

5. A Modified Aging Kinetics Model for Aging Condition Prediction Including the Temperature Effect

In the previous chapter, the integral value IV was applied to calculate the value of ωDP and kDP corresponding to the same moisture content. Thus, the modified model considering the parameter IV can be applied to predict the aging condition of samples with various moisture contents. However, the values of ωDP and kDP are obtained by analyzing the variation law of DP vs. aging duration at 150 °C. Theoretically speaking, the proposed model is only suitable for transformer polymer insulation operating at 150 °C. This defect will greatly limit its versatility.
Fortunately, the time-temperature superposition theory [29,30] indicates that the effect generated by increasing temperature and prolonging the reaction duration on the molecular motion is equivalent. In other words, a similar degradation degree of the transformer polymer insulation under high temperature can be also observed in other conditions (both a lower temperature and longer duration). Such property can be expressed as follows, tref·Tref = t·T, Tref (T) is regarded as the reference temperature (different operating or thermal aging temperature), tref (t) is the time (hours) required for the chemical reaction to reach a certain aging degree at the temperature of Tref (T). Review the Arrhenius theory, which is utilized to interpret the variation law between chemical reaction rate and reaction temperature [17,18] as is shown in Equation (16).
k i = A · e E a R · T i
where the A is the pre-exponential factor, which is related to the moisture content inside the polymer insulation material, R is a gas constant, R = 8.314 J/mol·K, ki represents the chemical reaction rate of the same reaction under i-th types of temperature, and Ea is activation energy and assumed to be 103 kJ/mol [27]. In this paper, 423.15 K (150 °C) is regarded as the Tref. Therefore, the ratio of the reaction rates at the Tref and T can be expressed by Equation (17), which is defined as shift factor αT.
α T = T T r e f = k k r e f = e E a R ( 1 T r e f 1 T )
Thus, the formula for calculating the time t required to reach a given degree of reaction at temperature T can be represented by Equation (18) [25].
t r e f = t · α T = t · e E a R ( 1 T r e f 1 T )
Obviously, relying on the simultaneous analysis of Equation (15) and Equation (18), the resulting modified model will be suitable for predicting the aging condition of transformer polymer insulation operating (or prepared) at different temperatures, which is presented in Equation (19).
{ D P t ( t , I V , T ) = D P 0 · [ 1 ω D P ( I V ) · ( 1 e k D P ( I V ) · t r e f ) ] ω D P ( I V ) = 0.27 · e I V / 11.8 + 0.81 k D P ( I V ) = 0.047 · e I V / 12.7 + 0.020 I V = 100 1000 tan δ ( f ) · f = 100 1000 tan δ ( f ) d f t r e f = t · α T ( T ) α T ( T ) = e E a R ( 1 T r e f 1 T )
It is obvious that the aging condition of the transformer polymer insulation in this model relies on three crucial factors (parameters), including aging duration t in the hour (at temperature T), initial moisture content (represented by integral value IV), and operating (thermal aging) temperature T. Moreover, the crucial basis of Equation (19) is that its FDS data (tanδ) is already known, and then, the prediction results of aging conditions at the reference temperature (150 °C) can be extended to different operating (thermal aging) temperatures by considering the shift factor shown in Equation (18). Thus, Equation (19) can be applied to predict the DP value of the transformer polymer insulation with different initial moisture content after t hours of operation (or thermal aging) at temperature T. The aging condition (DP value) of transformer polymer insulation at a different initial moisture (integral value) content and operating (thermal aging) temperature can be predicted by using Equation (19), respectively, and the resulting picture is presented in Figure 8. Figure 8a plots the DP vs. t and T, in the case of mc% = 2.0%. Figure 8b plots the DP vs. t and mc%, and T equal to 423.15 K.

6. Feasibility Investigation of the Proposed Modified Aging Kinetics Model

A novel modified aging kinetics model for predicting the aging condition (i.e., DP value) of transformer polymer insulation materials has been put forward. It is observed that once the FDS data, aging duration, and the aging temperature is determined, Equation (19) could be employed to predict the DP value immediately. In order to demonstrate the feasibility of the proposed model, the investigation experiments of DP prediction of transformer polymer insulation prepared in lab condition is performed. The prediction schedule is plotted in Figure 9.
In this chapter, several transformer polymer insulation pressboards with different insulation conditions are selected to verify the feasibility of the proposed model. The preparation schedule of these pressboards is referred to in Figure 1, and its details are described in Table 7. Pressboards 1–4 show low initial mc%, while pressboards 5–8 contain high initial mc%.
Moreover, the FDS test is performed at 45 °C, the resulting tanδ curves corresponding to the above eight samples are presented in Figure 10. Afterwards, the integral values in a range of 100–1000 Hz are calculated based on these tanδ curves, and the calculated values are shown in Table 3 as well.
Substituting the parameter (T, t, and IV, shown in Table 7) into Equation (19), the relevant model parameters (including the ωDP, kDP, and αT) and predicted DP values of these pressboards with different initial moisture content, aging duration, and thermal aging temperature are obtained immediately and shown in Table 8.
The formula of relative error is shown in Equation (20). It is found from Table 8 that the relative error between the predicted results and the measured results keep in 1%–12%, and the average value of these relative errors is equal to 7.41%. Furthermore, the estimation error in Table 8 is plotted in Figure 11, which is represented by the distance between the measured value and the predicted value. The comparison of the actual aging state and the predicted state of the prepared samples are also shown in Figure 11 according to the aging state division involving the operating experience.
Relative   error = | Predicted   value Measured   value | Measured   value × 100 %
It is worth noting that the reported fitting equations, models, and selected parameters significantly depend on the individual materials and material conditions used during the experiments (both for the oil and the pressboard). Fortunately, the parameters for describing the microstructure or physicochemical property of transformer polymer (cellulose) insulation materials follow similar variation rules (or laws) in the course of the degradation process. Therefore, if the proposed model is supported to perform the aging condition prediction of polymer insulation under other test conditions (such as the various thickness, density, etc., of experiment materials), the contained parameters should be revised in advance.

7. Conclusions

Since the moisture content inside the unknown sample is difficult to determine, the traditional aging kinetics model is thus not appropriate to perform the aging condition prediction of transformer polymer insulation materials. Fortunately, provided that the moisture content of the polymer materials could be characterized (replaced) by a certain feature parameter, the above issue will be solved naturally. According to this attempt, a modified aging kinetics model improved by employing the FDS technique is reported. The present analysis and contributions have led to the following conclusions.
1. The integral value of the tanδ curve (IV) can be utilized to characterize the moisture content inside the transformer polymer insulation materials accurately. Therefore, relying on the analysis of the relationship between the model parameters (ωDP and kDP) and IV, its functional relationship can be established;
2. Depending on the simultaneous analysis, this paper reported a modified aging kinetics model, which could be applied to perform the aging condition prediction of transformer polymer insulation materials under various test conditions, including aging duration, aging temperature, and initial moisture content. Moreover, the average relative error of prediction results of oil-immersed polymer (cellulose) pressboards is equal to 7.41%, which verified its accuracy and feasibility;
3. The reported fitting equations, models, and selected parameters significantly depend on the individual materials and material conditions used during the experiments. Therefore, if the proposed model is supported to be applied to other test conditions (such as the various thickness, density, etc., of experiment materials), the contained parameters should be revised in advance.

Author Contributions

In this research activity, J.L. and X.F. designed the experiments and wrote the paper; Y.Z. helped writing the paper; all authors have analyzed the data and approved the submitted manuscript.

Funding

This research was supported by the National Natural Science Foundation of China (61473272; 51867003; 51907034), the Natural Science Foundation of Guangxi (2018JJB160056; 2018JJB160064; 2018JJA160176), the Guangxi thousand backbone teachers training program, the Boshike award scheme for young innovative talents, the Basic Ability Promotion Project for Yong Teachers in Universities of Guangxi (2019KY0046; 2019KY0022), and the Guangxi Bagui young scholars special funding in support of this research.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Feng, D.W.; Yang, L.J.; Zhou, L.W.; Liao, R.J.; Chen, X. Effect of Oil–Paper–Pressboard Mass Ratio on Furfural Content in Transformer Oil. IEEE Trans. Dielectr. Electr. Insul. 2019, 26, 1289–1296. [Google Scholar] [CrossRef]
  2. Feng, D.W.; Yang, L.J.; Liao, R.J.; Zhou, L.W. Effect of Moisture Content on the Production and Partitioning of Furfural in Oil–Paper Insulation. IEEE Trans. Dielectr. Electr. Insul. 2018, 25, 2389–2397. [Google Scholar] [CrossRef]
  3. Zhang, Y.Y.; Li, X.; Zheng, H.B.; Yao, H.L.; Liu, J.F.; Zhang, C.H.; Peng, H.B.; Jiao, J. A Fault Diagnosis Model of Power Transformers Based on Dissolved Gas Analysis Features Selection and Improved Krill Herd Algorithm Optimized Support Vector Machine. IEEE Access 2019, 7, 102803–102811. [Google Scholar] [CrossRef]
  4. International Electrotechnical Commission. Amendment 1-Measurement of the Average Viscometric Degree of Polymerization of New and Aged Cellulosic Electrically Insulating Materials; International Electrotechnical Commission: Geneva, Switzerland, 2007. [Google Scholar]
  5. Koch, M.; Prevost, T. Analysis of Dielectric Response Measurements for Condition Assessment of Oil-Paper Transformer Insulation. IEEE Trans. Dielectr. Electr. Insul. 2012, 19, 1908–1915. [Google Scholar] [CrossRef]
  6. Liu, J.F.; Fan, X.H.; Zhang, Y.Y.; Zheng, H.B.; Jiao, J. Temperature Correction to Frequency Dielectric Modulus and Activation Energy Prediction of Immersed Cellulose Insulation. IEEE Trans. Dielectr. Electr. Insul. 2019. [Google Scholar] [CrossRef]
  7. Zhang, Y.Y.; Liu, J.F.; Zheng, H.B.; Wang, K. Feasibility of a universal approach for temperature correction in frequency domain spectroscopy of transformer insulation. IEEE Trans. Dielectr. Electr. Insul. 2018, 25, 1766–1773. [Google Scholar] [CrossRef]
  8. Liu, J.F.; Fan, X.H.; Zhang, Y.Y.; Zheng, H.B.; Zhu, M.Z. Quantitative evaluation for moisture content of cellulose insulation material in paper/oil system based on frequency dielectric modulus technique. Cellulose 2019. [Google Scholar] [CrossRef]
  9. Liu, J.F.; Fan, X.H.; Zhang, Y.Y.; Zheng, H.B.; Yao, H.L.; Zhang, C.H.; Zhang, Y.B.; Li, D.J. A Novel Universal Approach for Temperature Correction on Frequency Domain Spectroscopy Curveof Transformer Polymer Insulation. Polymers 2019, 11, 1126. [Google Scholar] [CrossRef] [Green Version]
  10. Lelekakis, N.; Martin, D.; Wijaya, J. Ageing rate of paper insulation used in power transformers Part 1: Oil/paper system with low oxygen concentration. IEEE Trans. Dielectr. Electr. Insul. 2012, 19, 1999–2008. [Google Scholar] [CrossRef]
  11. Lelekakis, N.; Martin, D.; Wijaya, J. Ageing rate of paper insulation used in power transformers Part 2: Oil/paper system with medium and high oxygen concentration. IEEE Trans. Dielectr. Electr. Insul. 2012, 19, 2009–2018. [Google Scholar] [CrossRef]
  12. Emsley, A.M.; Xiao, X.; Heywood, R. Degradation of cellulosic insulation in power transformers. Part 2: Formation of furan products in insulating oil. IEE Proc. Sci. Meas. Technol. 2000, 147, 110–114. [Google Scholar] [CrossRef]
  13. Jadav, R.B.; Ekanayake, C.; Saha, T.K. Understanding the Impact of Moisture and Ageing of Transformer Insulation on Frequency Domain Spectroscopy. IEEE Trans. Dielectr. Electr. Insul. 2014, 21, 369–379. [Google Scholar] [CrossRef]
  14. Liao, R.J.; Liu, J.F.; Yang, L.J.; Wang, K.; Hao, J.; Ma, Z.Q.; Gao, J.; Lv, Y.D. Quantitative analysis of insulation condition of oil-paper insulation based on frequency domain spectroscopy. IEEE Trans. Dielectr. Elect. Insul. 2015, 22, 322–334. [Google Scholar] [CrossRef]
  15. Liu, J.F.; Fan, X.H.; Zhang, Y.Y.; Zhang, C.H. Condition Prediction for Oil-immersed Cellulose Insulation in Field Transformer Using Fitting Fingerprint Database. IEEE Trans. Dielectr. Electr. Insul. 2019. [Google Scholar] [CrossRef]
  16. Ojha, S.K.; Purkait, P.; Chatterjee, B.; Chakravorti, S. Application of Cole–Cole model to transformer oil-paper insulation considering distributed dielectric relaxation. High Volt. 2019, 4, 72–79. [Google Scholar] [CrossRef]
  17. Zheng, Y.M.; Wang, Z.J. Study on Broadband Loss Characteristics of Oil-immersed Papers for Fast Transient Modeling of Power Transformer. IEEE Trans. Dielectr. Electr. Insul. 2012, 20, 564–570. [Google Scholar] [CrossRef]
  18. Morsalin, S.; Phung, B.T. Modeling of dielectric dissipation factor measurement for XLPE cable based on Davidson-Cole model. IEEE Trans. Dielectr. Electr. Insul. 2019, 26, 1018–1026. [Google Scholar] [CrossRef]
  19. Dissado, L.A.; Hill, R.M. A cluster approach to the structure of imperfect materials and their relaxation spectroscopy Proceedings of the Royal Society A: Mathematical. Phys. Eng. Sci. 1983, 390, 131–180. [Google Scholar] [CrossRef]
  20. Emsley, A.M. Kinetics and mechanisms of the low-temperature degradation of cellulose. Cellulose 1994, 1, 26–56. [Google Scholar] [CrossRef]
  21. Emsley, A.M. On the kinetics of degradation of cellulose. Cellulose 1997, 4, 1–5. [Google Scholar] [CrossRef]
  22. Calvini, P.; Gorassini, A.; Merlani, A.L. On the kinetics of cellulose degradation: Looking beyond the pseudo zero order rate equation. Cellulose 2007, 15, 193–203. [Google Scholar] [CrossRef]
  23. Calvini, P. The influence of levelling-off degree of polymerization on the kinetics of cellulose degradation. Cellulose 2005, 12, 445–447. [Google Scholar] [CrossRef]
  24. Ekenstam, A. The behavior of cellulose in mineral acid solutions: Kinetics study of the decomposition of cellulose in acid solutions. BER 1936, 69, 540–553. [Google Scholar]
  25. Ding, H.Z.; Wang, Z.D. On the degradation evolution equations of cellulose. Cellulose 2008, 15, 205–224. [Google Scholar] [CrossRef]
  26. Heywood, R.J.; Stevens, G.C.; Ferguson, C.; Emsley, A.M. Life assessment of cable paper using slow thermal ramp methods. Thermochim. Acta 1999, 332, 189–195. [Google Scholar] [CrossRef]
  27. Verma, H.C.; Baral, A.; Pradhan, A.K.; Chakravorti, S. A Method to Estimate Activation Energy of Power Transformer Insulation Using Time Domain Spectroscopy Data. IEEE Trans. Dielectr. Electr. Insul. 2017, 24, 3245–3253. [Google Scholar] [CrossRef]
  28. Martin, D.; Cui, Y.; Ekanayake, C.; Ma, H. An Updated Model to Determine the Life Remaining of Transformer Insulation. IEEE Trans. Power Deliv. 2015, 30, 395–402. [Google Scholar] [CrossRef]
  29. Gillen, K.T.; Celina, M. The wear-out approach for predicting the remaining lifetime of materials. Polym. Degrad. Stab. 2000, 71, 15–30. [Google Scholar] [CrossRef] [Green Version]
  30. Urzhumtsev, Y.S. Time-temperature superposition. Rev. Mech. Compos. Mater. 1975, 11, 57–72. [Google Scholar]
Figure 1. The experimental schedule of oil-immersed polymer (cellulose) pressboard.
Figure 1. The experimental schedule of oil-immersed polymer (cellulose) pressboard.
Polymers 11 02082 g001
Figure 2. The variation law of the degree of polymerization (DP) value vs. aging duration.
Figure 2. The variation law of the degree of polymerization (DP) value vs. aging duration.
Polymers 11 02082 g002
Figure 3. The fitting curves of the parameters in the kinetics model. (a) ωDP, (b) kDP.
Figure 3. The fitting curves of the parameters in the kinetics model. (a) ωDP, (b) kDP.
Polymers 11 02082 g003
Figure 4. The frequency dielectric response test platform.
Figure 4. The frequency dielectric response test platform.
Polymers 11 02082 g004
Figure 5. The ε*(ω) of non-aged polymer pressboards with various moisture contents. (a) ε׳(ω), (b) ε׳׳(ω), (c) tanδ.
Figure 5. The ε*(ω) of non-aged polymer pressboards with various moisture contents. (a) ε׳(ω), (b) ε׳׳(ω), (c) tanδ.
Polymers 11 02082 g005
Figure 6. The fitting equation of IV vs. mc%.
Figure 6. The fitting equation of IV vs. mc%.
Polymers 11 02082 g006
Figure 7. The fitting curves. (a) ωDP vs. IV, (b) kDP vs. IV.
Figure 7. The fitting curves. (a) ωDP vs. IV, (b) kDP vs. IV.
Polymers 11 02082 g007
Figure 8. The DP prediction under different conditions. (a) DP vs. t and T, (b) DP vs. t and mc%.
Figure 8. The DP prediction under different conditions. (a) DP vs. t and T, (b) DP vs. t and mc%.
Polymers 11 02082 g008
Figure 9. The prediction schedule of the DP of the transformer polymer insulation.
Figure 9. The prediction schedule of the DP of the transformer polymer insulation.
Polymers 11 02082 g009
Figure 10. The Frequency Domain Spectroscopy (FDS) of polymer pressboards. (a) Dry pressboard, (b) wet pressboard.
Figure 10. The Frequency Domain Spectroscopy (FDS) of polymer pressboards. (a) Dry pressboard, (b) wet pressboard.
Polymers 11 02082 g010
Figure 11. Comparison of the measured value and predicted value.
Figure 11. Comparison of the measured value and predicted value.
Polymers 11 02082 g011
Table 1. Primary parameters of both cellulose pressboard and oil used in the experiment.
Table 1. Primary parameters of both cellulose pressboard and oil used in the experiment.
Transformer Polymer PressboardTransformer Insulating Oil
BrandT4 Weidmann
transformer pressboard
BrandKaramay No.25 naphthenic
mineral oil
Thickness0.5 mmDielectric loss4 × 10−4
Tensile strengthMD: 98 MPa,
CMD: 47 MPa
Pour point≤−45 °C
Density0.96 g/cm3Flash point135 °C
Table 2. The details of the used parameters in the aging kinetics model.
Table 2. The details of the used parameters in the aging kinetics model.
mc%0.78%1.32%2.07%2.74%3.82%
valueEB (±)valueEB (±)valueEB(±)valueEB (±)valueEB (±)
ωDP0.732.36
× 10−4
0.751.38
× 10−4
0.784.45
× 10−4
0.796.13
× 10−4
0.816.99
× 10−4
kDP0.00346.34
× 10−4
0.00742.76
× 10−4
0.0121.25
× 10−3
0.0162.36
× 10−4
0.0191.41
× 10−3
Table 3. The fitting equation of mc% vs. ωDP and mc% vs. kDP.
Table 3. The fitting equation of mc% vs. ωDP and mc% vs. kDP.
Fitting Equation
ω D P ( m c % ) = 0.16 · e m c % / 2.6 + 0.85
k D P ( m c % ) = 0.033 · e m c % / 3.3 + 0.030
Table 4. The parameters of integral value (IV) and mc%.
Table 4. The parameters of integral value (IV) and mc%.
ParametersMeasured Value
mc%0.78%1.29%2.32%3.15%3.43%4.03%
IV12.917.924.432.644.285.1
Table 5. The fitting equation of IV vs. mc%.
Table 5. The fitting equation of IV vs. mc%.
Fitting Equation of IV
  I V ( m c % ) = 21.5 + 0.045 e m c % / 0.56 32.3 e m c % / 0.60
Table 6. The fitting equation of ωDP vs. IV and kDP vs. IV.
Table 6. The fitting equation of ωDP vs. IV and kDP vs. IV.
Fitting Equation
ω D P ( I V ) = 0.27 · e I V / 11.8 + 0.81
k D P ( I V ) = 0.047 · e I V / 12.7 + 0.020
Table 7. The details of the prepared pressboards.
Table 7. The details of the prepared pressboards.
PressboardDry PressboardWet Pressboard
Parameters 12345678
Measured mc%0.98%1.02%1.12%1.15%2.31%2.93%3.87%4.12%
Measured DPm1093897751548832644472394
Aging temperature (T)/K423.15423.15423.15423.15403.15403.15403.15403.15
Aging duration (t)/h24 729616896168264336
Integral value (IV)14.715.016.116.222.842.160.182.0
Table 8. Predicted results of the DP value of the prepared polymer pressboards.
Table 8. Predicted results of the DP value of the prepared polymer pressboards.
PressboardDry PressboardWet Pressboard
Parameters 12345678
Parameters ωDP0.7380.7400.7470.7470.7760.8070.8130.815
Parameters kDP0.00490.00520.00640.00650.0120.0180.0190.020
Parameters αT1.01.01.01.00.200.200.200.20
Measured DPm1093897751548832644472394
Predicted DPp1010845720554924693523438
Relative error7.59%5.80%4.13%1.09%11.06%7.61%10.81%11.17%

Share and Cite

MDPI and ACS Style

Liu, J.; Fan, X.; Zhang, Y.; Zheng, H.; Wang, Z.; Zhao, X. A Modified Aging Kinetics Model for Aging Condition Prediction of Transformer Polymer Insulation by Employing the Frequency Domain Spectroscopy. Polymers 2019, 11, 2082. https://doi.org/10.3390/polym11122082

AMA Style

Liu J, Fan X, Zhang Y, Zheng H, Wang Z, Zhao X. A Modified Aging Kinetics Model for Aging Condition Prediction of Transformer Polymer Insulation by Employing the Frequency Domain Spectroscopy. Polymers. 2019; 11(12):2082. https://doi.org/10.3390/polym11122082

Chicago/Turabian Style

Liu, Jiefeng, Xianhao Fan, Yiyi Zhang, Hanbo Zheng, Zixiao Wang, and Xixi Zhao. 2019. "A Modified Aging Kinetics Model for Aging Condition Prediction of Transformer Polymer Insulation by Employing the Frequency Domain Spectroscopy" Polymers 11, no. 12: 2082. https://doi.org/10.3390/polym11122082

APA Style

Liu, J., Fan, X., Zhang, Y., Zheng, H., Wang, Z., & Zhao, X. (2019). A Modified Aging Kinetics Model for Aging Condition Prediction of Transformer Polymer Insulation by Employing the Frequency Domain Spectroscopy. Polymers, 11(12), 2082. https://doi.org/10.3390/polym11122082

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop