Next Article in Journal
Experimental Evaluation of Low Velocity Impact Properties and Damage Progression on Bamboo/Glass Hybrid Composites Subjected to Different Impact Energy Levels
Next Article in Special Issue
Polymeric Coatings with Antimicrobial Activity: A Short Review
Previous Article in Journal
Formulation and Characterization of Gelatin-Based Hydrogels for the Encapsulation of Kluyveromyces lactis—Applications in Packed-Bed Reactors and Probiotics Delivery in Humans
Previous Article in Special Issue
The Synergistic Microbiological Effects of Industrial Produced Packaging Polyethylene Films Incorporated with Zinc Nanoparticles
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Antimicrobial Properties of Polyaniline and Polypyrrole Decorated with Zinc-Doped Copper Oxide Microparticles

by
Moorthy Maruthapandi
1,
Arumugam Saravanan
1,
John H. T. Luong
2 and
Aharon Gedanken
1,*
1
Bar-Ilan Institute for Nanotechnology and Advanced Materials, Department of Chemistry, Bar-Ilan University, Ramat-Gan 52900, Israel
2
School of Chemistry, University College Cork, Cork T12 YN60, Ireland
*
Author to whom correspondence should be addressed.
Polymers 2020, 12(6), 1286; https://doi.org/10.3390/polym12061286
Submission received: 11 May 2020 / Revised: 29 May 2020 / Accepted: 2 June 2020 / Published: 4 June 2020
(This article belongs to the Special Issue Current Trends in Antimicrobial Polymeric Materials)

Abstract

:
Polyaniline (PANI) and polypyrrole (PPY) were synthesized by carbon dots (CDs) under UV irradiation and then sonicated together with zinc acetate and copper acetate to form the PANI-Zn@CuO and PPY-Zn@Cu composites. The former consisted of agglomerated spherical particles with diameters of 1–5 µm, whereas the latter displayed irregular stick shapes with similar diameters. The bacterial potency of the composites against Escherichia coli and Staphylococcus aureus was enhanced remarkably with Zn doping in the CuO matrix, designated as Zn0.11Cu0.89O, at 0.144 mg/mL. The cell death was mainly attributed to the release of reactive oxygen species (ROS) that would severely damage DNA, proteins, and lipids. Bacteria could adhere to neutral surfaces of the composites by van der Waals attractive forces. The binding event disrupted the native surface charge of bacterial cells to induce cell lysis and result in eventual cell death.

1. Introduction

Metal oxide nanoparticles (NPs), particularly ZnO and CuO, have emerged as potential antimicrobial agents to overcome the rising global issue of antimicrobial resistance against conventional antibiotics. Their appealing features include durability and high stability with low mammalian cell toxicity, compared with organic counterparts. ZnO reduces oxygen to water, and this reaction involves the release of three intermediate reactive oxygen species (ROS): superoxide, hydrogen peroxide, and hydroxyl radical [1,2]. Such species play an essential role in eradicating both Gram-negative and Gram-positive pathogens. Copper is a well-known antimicrobial agent, and its action against bacteria is related to Fenton type reactions [3,4,5]. Cupric oxide (Cu=O) is the most widely studied because Cu2O and Cu2O3 are not stable materials. Copper NPs kill bacteria most likely via the release of Cu2+ ions [6]. Albeit, the mechanism of copper in cell death is not fully understood, and bacterial resistance to copper particles has been noted [7]. The combined antimicrobial properties of ZnO and CuO can be realized by doping copper in a ZnO matrix [8] or doping zinc in a CuO matrix [9]. It becomes a formidable task for bacteria to develop strong resistance pathways against such hybridized metal particles [10]. However, NPs suffer from particle instability and degradation, resulting in reduced NP efficacy or longevity. In aqueous media, the use of NPs is complicated by their propensity toward agglomeration to reduce the active surface area, the key parameter of their interaction with bacteria. Thus, polymer composites prepared from conducting polymers and metal NPs might be a solution to circumvent these shortcomings.
Among several conducting polymers, polyaniline (PANI) and polypyrrole (PPY), have received considerable interest because of their unique properties and ease of preparation by chemical or electrochemical methods. PANI and PPY can also be easily prepared using carbon dots (CDs) or nitrogen-doped CDs (N@CDs) as an effective initiator [11,12]. Of importance is the pioneering synthesis and applications of Cu0.89Zn0.11O (marked here as Zn@CuO, MW = 79.75) as an antibacterial agent [13,14]. Hybridized metal oxide nanomaterials, e.g., Zn-doped CuO (Zn@CuO), are of specific interest, owing to their size-dependent biological, optical, and electrical properties. To date, PPY, PANI, and other polymers are synthesized and decorated with metals or metal oxide nanoparticles and used as antibacterial agents (Table 1). However, these polymer composites have several drawbacks such as complex synthesis, toxicity, and the high cost of noble metals (Au, Pt, Ag, and Pd).
This study aims to synthesize and evaluate the antibacterial activities of two polymers decorated with Zn@CuO microparticles. PANI and PPY are polymerized from their corresponding monomers using CDs as an initiator. The prepared Zn-doped CuO is decorated on such polymers via a one-step sonochemical method. The antibacterial effects of the polymer composites are evaluated against Escherichia coli (Gram-negative) and Staphylococcus aureus (Gram-positive). A mechanism of bacterial death is postulated in corroboration with the experimental data.

2. Experimental Section

2.1. Preparation of CDs

Polyethylene glycol (40 mL, PEG-400) was transferred into a 50 mL beaker and placed in a water bath at 70 °C. The tip of an ultrasonic transducer was dipped in the PEG-400 and sonicated for 3 h with a 40% amplitude [11,12,25,26].

2.2. Preparation of PANI

The reaction mixture consisting of 1.0 g aniline (1.1 mmol), 25 mL of HNO3 (2 M), and 3 mL of the CD solution (5 mg CDs) was illuminated with UV light for 48 h. The resulting blackish-brown slurry was filtered, washed with deionized water, and dried at room temperature [11].

2.3. Preparation of PPY

Pyrrole (11 mmol, 0.74 g) was mixed with 25 mL of 0.3 M nitric acid and 2.5 mL (8 mg) of CDs. After activation under UV light for two days, the blackish-brown solid obtained by filtration was washed with deionized water and ethanol to remove unreacted CDs and dried at room temperature [11,25,26].

2.4. Synthesis of PANI-Zn@CuO and PPY-Zn@CuO

An amount of 0.1 g of PANI (0.11 mmol) or PPY (0.16 mmol) was dissolved in 90 mL of ethanol. The copper acetate and zinc acetate (3:1 molar ratio) salt solution (10 mL) was then added, resulting in a final concentration (0.01 M of 3:1 molar ratio). The reaction mixture was sonicated until the temperature reached 70 °C, and the solution was maintained at pH 8–9 by adding an ammonia solution. The blue-tinted solution turned blackish-brown and was placed in an ice bath and sonicated for another 30 min [26].

2.5. Antibacterial Tests

E. coli or S. aureus were incubated overnight under aerobic conditions at 37 °C in Luria–Bertani (LB) broth. This broth contains 10 mg/mL tryptone (a mixture of peptides prepared from casein), 5 mg/mL yeast extract, 5–10 or 10 mg/mL NaCl, and 1 mg/mL glucose. The bacterial concentrations were related to the absorbance at 595 nm (OD595) until the final concentration of 107 cells was attained. For the antibacterial tests, 500 µL of the polymer composite was added to the 500 µL of the bacterial suspension. The mixture was incubated at 37 °C with shaking at 200 rpm. A 100 µL aliquot was taken after 0, 3, and 12 h, and diluted to 10-fold in the 20% LB medium and plated on the nutrient gar plates. After the plates were incubated for 16 h at 37 °C, bacterial colonies at appropriate dilutions were counted to estimate the number of viable bacteria by the colony-forming unit (CFU) method. A colony-forming unit is a unit used in microbiology to estimate the number of viable bacteria in a sample. The visible bacteria were counted by visualization.

2.6. Analytical Techniques

FTIR spectra of the polymer composites were measured using a Transon 27 spectrometer (Bruker, Karlsruhe, Germany), whereas their crystalline nature was analyzed using X-ray diffraction (Bruker, AXS D8 Advance diffractometer, Germany). SEM (FEI Magellan 400 L microscope, Hillsboro, OR, USA) was performed to probe the size and morphology of the composites. For SEM analysis, the samples were prepared by placing a small amount of the dried powder on a carbon tape attached to a copper strip, and the material was coated with gold to improve conductivity. 13C solid-state nuclear magnetic resonance (NMR) spectra of the composites were acquired using a Bruker 5000 Ultra Shield spectrometer (Bruker, Billerica, MA, USA). The zeta potential was measured using a Malvern Zetasizer Nano-ZS (Malvern, UK).

3. Result and Discussion

3.1. FTIR Spectra and X-ray Diffraction Pattern

The doping of Zn in the CuO matrix deserves a brief comment, albeit this nanocomposite has been well reported elsewhere [13,14]. Among all transition metals, Zn causes more effective doping, as it has a comparable ionic radius with Cu2+ (0.074 vs. 0.072 nm) and possesses the same oxidation states [27,28,29]. Thus, the CuO host lattice might not undergo any significant local structural changes. However, the presence of the Zn2+ dopant can effectively produce defects in CuO nanostructures, an appealing feature for biological applications [30]. During the composite formation, Zn@CuO particles interact with the polymers through the chemical bond or polymer chains. Thus, FTIR, XRD, and solid-state NMR were conducted to characterize these two composites [31].
The FTIR spectra of PPY and PANI (Figure 1a–c) exhibit some typical broad bands at 3100–3390 cm−1 (N–H stretching) and ~1585–1520 cm−1 (C=C stretching). The peaks at 3095 and 2981 cm−1 are attributed to the C–H aromatic stretching, whereas the peak at 1330 cm−1 is assigned to the C–N stretching. The presence of =C–H in-plane vibrations is confirmed by two peaks at 1120 and 1260 cm−1. These similar peaks also appear in the polymer composites as shown in Figure 1a. However, the stretching vibrations of N–H, C=C, C–N, and =C–H of the composites display noticeable peak shifting and reduced peak intensities and form as broader bands. The XRD patterns of the polymers and their composites are shown in Figure 1b,d. The two polymers are amorphous as reflected by a broad peak around 2θ = 10°–40°, a common feature of amorphous compounds. The polymer composites exhibited a broad XRD peak around 2θ = 12°–36.6°, due to periodicity parallel to the polymer chain (Figure 1b). A shift of 14.3° confirmed the incorporation of Zn@CuO particles in the polymer chains. The composites also had minor sharp peaks around 2θ = 32.1°, 35.1°, and 41.6°, as a typical signature of the Zn@CuO powder. Other small and broad peaks were also noted, in agreement with the literature [13,14]. These peaks were slightly shifted for the PPY composite but disappeared in the PANI composite. These results illustrated the presence of Zn@CuO in the composites and that at least the PPY composites with Zn@CuO are partially crystalline.

3.2. Morphology and Elemental Analysis

SEM micrographs of PANI-Zn@CuO and PPY-Zn@CuO macro-nanocomposites are shown in Figure 2. The PPY-Zn@CuO composites exhibit agglomerated particles with spherical shapes and diameters ranging from 1 to 5 µm. The PANI-Zn@CuO composite displays irregular stick shapes with a broad range diameter from 1 to 5 µm, compared with 20–200 nm of the Zn@CuO NPs’ diameter [13,14]. The EDX spectra and SEM-EDX elemental mapping spectra of the polymer composites show the elementary components (C, N, O, and Au) with uniform distribution. Figure 2d,e also confirmed the formation of the metal oxide of CuO. The SEM-EDX elemental mapping spectra of PPY-Zn@CuO and PANI-Zn@CuO further confirmed the presence of CuO. Zn was not detected by the SEM-EDX, possibly due to its very low percentage in the composites.

3.3. Solid-State 13C NMR Analysis

The solid-state NMR spectra of PPY-Zn@CuO and PANI-Zn@CuO exhibit a broad and a sharp peak (Figure 3). The peak at 125 ppm is attributed to the protonated carbon in the polymer chain. The shoulder peaks at 110 and 114 ppm corresponds to the protonated carbons in the aromatic rings and a peak at 124 ppm is related to the non-protonated carbons. The sharp peaks at 61 and 77 ppm are originated from the protonated C-9 and non-protonated C-16 carbon of the quinoid part of the polymer structure. The solid-state 13C-NMR spectra of PPY-Zn@CuO and PANI-Zn@CuO are almost similar compared with those of PANI and PPY. The spectra of composites are slightly shifted towards the upfield with lower shoulder peak intensities (a, b, and c), at 63, 108, and 115 ppm, lower than those of the bare polymers. These variations attest to the formation of a metal oxide composite with the polymer. The 13C-NMR spectra of PANI and PPY are available from the literature [11,25,26].

3.4. Zeta Potential Measurements

The zeta potential of PANI has been known to be pH-dependent and very close to 0 mV but still positive at pH 7 [32], as its isoelectric point (IEP) is reached at pH 8.2 (Figure 4, upper, left). In the cell culture medium, PANI exhibited a negative peak of around −85 mV, compared with ~0 mV for PANI-Zn@CuO (Figure 4, upper). Of notice was the presence of an additional positive peak (Figure 4, upper-left) for the zeta potential of PANI. The nonspecific adsorption of ions or polyelectrolytes onto the PANI or PANI-Zn@CuO surface, however, altered the value and polarity of the measured zeta potential significantly. However, such zeta potentials were still useful to compare the surface charges of PANI and PANI-Zn@CuO. A small positive peak ~ 70 mV could be attributed to the free ions or polyelectrolytes of the LB medium. Similarly, PPY-Zn@CuO displayed an asymmetrical broad peak around 0 mV, compared with −30 mV for PPY (Figure 4, lower). Polypyrrole undergoes protonation or deprotonation reactions in an alkaline or acid solution, resulting in the change of its surface charges (the surface changed between a charged and a neutral state) [33]. Again, a negative charge of PPY could be due to the adsorption of excess negatively charged molecules in the LB cell culture broth.

3.5. Antibacterial Activity

E. coli and S. aureus were eradicated after 8 h of their exposure to the PANI-Zn@CuO and PPY-Zn@CuO polymer composites at different concentrations to establish the minimum inhibition concentration for each composite. The results revealed a synergetic effect perceived for these composites compared with PANI and PPY and Zn@CuO (Figure 5). The Zn@CuO level in the composites was determined by ICP. The bacterial activity was performed at the minimum composite concentration of 1 mg/mL, comprising 0.144 mg/mL of Zn@CuO. This MIC was a significantly lower amount of Zn@CuO as compared with the literature value of 1 mg/mL of Zn@CuO after 24 h of exposure [9].
The minimal amount of Zn@CuO was of importance considering the plausible cytotoxic effect of metal oxide particles for their applications as antibacterial agents. E. coli was eradicated by PANI-Zn@CuO after 24 h of exposure (Figure 5a,b), whereas S. aureus was eradicated by the PANI-Zn@CuO and PPY-Zn@CuO composites after 12 and 8 h of exposure, respectively (Figure 5c,d). A noticeably shorter time of 8 h was observed when E. coli or S. aureus were exposed to the PPY-Zn@CuO composite (Figure 5e,f).
The cell surface of most bacteria has a moderately negative net charge at neutral pH [33]. Gram-positive bacteria possess a negative charge due to the presence of teichoic acids linked to the peptidoglycan or the underlying plasma membrane. The lipopolysaccharides impart a strong negative charge to the surface of Gram-negative bacterial cells. The zeta potentials of 22 E. coli strains were negatively charged in the 150 mM PBS (pH 7.4), ranging from −5 to −34 mV [34]. Both PANI and PPY with negative charges exhibited no antibacterial effect against E. coli and S. aureus, plausibly due to the much stronger net negative charge of PANI and PPY. A pronounced repulsive force between the bacteria and the polymers circumvented any adherence of the bacteria to the polymers.

3.6. A Postulated Mechanism of Cell Death

CuO [35] and ZnO [36] are known to generate reactive oxygen species (ROS) to eradicate both Gram-negative and Gram-positive bacteria. The release of reactive oxygen species (ROS) is expected to impair bacterial membranes, DNA, and proteins. Zn@CuO can generate ROS on its surface and this phenomenon is enhanced by excitation with UV light [37,38]. CuO NPs are also known to generate ROS to modify bacterial molecules and block the antioxidant defense system [39]. More defective sites are anticipated on the Zn@CuO surface compared with that of CuO due to the doping of Zn [28]. Thus, more oxygen is adsorbed on such defective sites of Zn@CuO, leading to more ROS on its surface as this hybridized metal oxide is capable of reducing oxygen to form water as follows (Scheme 1):
The effect of oxygen stress was confirmed by using the electron paramagnetic resonance (EPR) technique to measure the ROS generation with DMPO (5,5-dimethyl-1-pyrroline-N-oxide) as a spin trap [6]. DMPO captures hydroxyl (OH·) radicals and superoxide anions (O2−) to create DMPO–OH as a final adduct with a distinct quartet signal and a typical 1:3:3:1 signal intensity ratio. The PPY polymer produced more ROS compared with its counterpart, PANI (Figure 6), but was lower than the ROS level of Zn@CuO. Consequently, the ROS level of PPY-Zn@CuO was higher than that of PANI-Zn@CuO. The synergistic effect between PANI and PPY with Zn@CuO was attributed to the free electrons in the polymers, which could be combined with the O2 in the suspension to enhance the production of ROS [7]. The ROS include oxygen radicals such as peroxides, superoxide, hydroxyl radical, singlet oxygen, and α-oxygen. They are unstable molecules that readily react with cellular molecules, causing damage to DNA, RNA, and proteins that support cell growth and proliferation. Oxidative DNA damage is known as the primary cause of cell death [40,41]. Notice that the superoxide radical with a negative charge cannot penetrate the cell membrane, i.e., it only acts on the outer surface of bacteria. In contrast, hydrogen peroxide should be able to penetrate the bacterial cell wall to trigger cell plasmolysis. Of note is the presence of bacterial superoxide dismutase and catalases that degrade superoxide and hydrogen peroxide, respectively. However, no cellular detoxification mechanism is known for hydroxyl radicals. With such combined attacks and the release of hydroxyl radicals, the microbes cannot develop new resistant strains. Lipid peroxidation is a signature of ROS damage, as polyunsaturated fatty acids of lipids are susceptible to free radical-initiated oxidation and participate in chain reactions to damage biomolecules required to support cell growth and replication [42]. It was reasoned that Zn doping into the CuO matrix resulted in the formation of structural defects such as oxygen vacancies and Cu interstitial defects, serving as trapping centers for electrons [13,27].
Another plausible mechanism was attributed to the adhesion of bacteria to the composites. The direct interaction of bacteria and surfaces is governed by van der Waals attractive forces, whereas interionic forces are attractive or repulsive [43], even if bacteria and surfaces are charged alike, i.e., negative van der Waals forces can overcome repulsion and lead to adhesion [44]. Therefore, bacteria can adhere to hydrophobic or slightly negatively charged surfaces, e.g., glass and polystyrene. The zeta potentials of the two composites were close to 0 mV, i.e., the ionic interaction is negligible compared with van der Waals attractive forces. The two composites acted to disrupt the native surface charge of the bacterial cells, which induced cell lysis, resulting in cell death.
The cytotoxicity of Zn@CuO deserves a brief mention here because it induces only mild acute toxicity in Xenopus laevis embryos, African clawed frog, compared with ZnO [45]. Zn-CuO NPs exert noticeable anti-proliferation effects on cancer cells but these effects are relatively weak on normal cells [46]. The low cytotoxicity of Zn-CuO opens a new route for the development of effective antimicrobial composites with various biocompatible polymers. Of importance is the study of the shape-dependent cytotoxicity of polyaniline nanomaterials in human fibroblast cells [47]. The toxicity increases with the decreasing aspect ratio of the PANI nanomaterials (length/diameter ratio: 2.09, 2.94, 3.92, and 5.35). At the highest aspect ratio, the PANI nanomaterials showed similar results to the bulk PANI materials.
PPY at low concentrations (<9.7 µg/mL) is biocompatible to primary mouse embryonic fibroblasts, the mouse hepatoma cell line, and the human T lymphocyte Jurkat cell line (48), and the cytotoxic effect is dose-dependent [48]. Above 0.291 mg/mL, PPY is significantly toxic for all tested cells. Such information is useful to formulate novel antimicrobial agents for PANI-Zn@CuO and PPY-Zn@CuO pertaining to minimal cytotoxicity, an important topic of future endeavors.
The feasibility of using PANI as an antimicrobial agent has been well reported in the literature. As a cited example, PANI at 0.5% (w/v) or 5 mg/mL is required to suppress the growth of E. coli and S. aureus [49]. PANI induces the production of hydrogen peroxide, which promotes the formation of hydroxyl radicals, causing biomolecule damage and potentially cell death. Catalase, an enzyme of E. coli [50] is capable of scavenging hydrogen peroxide to water and oxygen. Thus, high PANI concentrations are required to ensure the H2O2 level is over the threshold that can be scavenged, resulting in cellular damage. In the context of cytotoxicity, the PANI amount of 5 mg/mL might cause significant cytotoxicity of fibroblastic cells as discussed earlier. In contrast, the PANI concentration of the PANI-Zn@CuO composite was 0.8 mg/mL, a distinct advantage of its potential use as an antimicrobial agent when the cytotoxicity aspect is taken into consideration. The MIC of the two composites (0.144 mg/mL) was comparable to those of PPY-NT (nanotube)/Ag-NP nanocomposites. In brief, the MIC of PPY-NT (nanotube)/Ag-NP nanocomposites is dependent upon the level of AgNPs. The lowest MIC values are 0.078 and 0.156 mg/mL for the nanocomposites having 15 wt % of Ag-NPs against E. coli and S. aureus, respectively [51]. Ag-NPs exhibit a spherical shape with an average diameter of 23.12 ± 3.23 nm, and are significantly smaller than the size of the Zn@CuO particles (1–5 µm) in this work.

4. Conclusions and Future Possibilities

Two conducting polymer composite materials PANI-Zn@CuO and PPY-Zn@CuO were synthesized using CDs as the only initiator. Zn-doped CuO particles were then decorated on the conducting polymers by simple ultrasonication. The polymer composites exhibited remarkable antimicrobial effects against E. coli and S. aureus. The mechanism of cell death was mainly attributed to the release of reactive oxygen species (ROS) to impair the bacterial membranes, DNA, and proteins. The adhesion of bacteria to the composites would disrupt the native surface charge of bacterial cells, which induced cell lysis, resulting in eventual cell death. The synthesis of the polymer composites is easy and relatively inexpensive with a broad range of antimicrobial effects against multidrug-resistant bacteria.
The two newly synthesized composites can be extended to other antibiotic-resistant bacteria, depending upon the intended applications and cytotoxicity aspects. Apparently, some potential applications include the fabrication of personal protective equipment (mask, glove, and clothing), bandages, and hygienic products with antimicrobial properties. Other advanced applications encompass the coating of prostheses and medical devices to prevent bacterial infection. In this context, the two polymers must be tested against some priority bacteria and yeast with high antibiotic resistance. Of importance is the incorporation of the two polymer composites in topical cream with antifungal properties against Candida albicans, Candida auris, and toenail fungus. Candida causes candidiasis in humans, which is acquired in hospitals by patients with weakened immune systems. Toenail fungus, also known as onychomycosis, is a common fungal infection of human toenail by Trichophyton rubrum and other fungi. Our polymer composites could be utilized as a “standalone” or an “adjunct” therapy with current antifungal drugs. The two polymer composites are expected to have high efficacy against T. rubrum as well as other bacteria and fungi that cause toenail infection. They will also be formulated with some chemicals to soften the infected area and speed up the course of treatment and effectiveness.
Therefore, the cytotoxicity aspect of the polymer composites must also be investigated to assess their safety uses. For external treatment, e.g., topical cream, hand sanitizer, and lacquer, the biocompatibility of the PANI and PPY composites can be conducted using different cell lines, but fibroblasts are the most frequently used line for the determination of cytotoxicity. Cytotoxicity testing is very involved according to the ISO protocol 10,993-5 and several biomarkers are analyzed to decipher the cell death. Of notice is the use of cell-based impedance spectroscopy (ECIS) for the assessment of toxic materials and nanomaterials [52,53]. Cytotoxicity effects on cells are difficult to measure and time-consuming, however, ECIS label-free technology offers quantitative results for cell toxicology and viability in real-time and continuously.
In brief, our paper unravels the synthesis of two new polymer composites, and they are well characterized by different modern equipment. We have also demonstrated a synergic effect by the combination of PPY or PANI with Zn@CuO for inhibiting the growth of S. aureus and E. coli, two common bacteria, which have been used extensively in the literature. The cytotoxicity aspect of our newly synthesized polymer composites needs to be investigated, depending upon their intended uses.

Author Contributions

Formal analysis, A.S.; investigation, J.H.T.L.; supervision, A.G.; writing—original draft, M.M. All authors have read and agreed to the published version of the manuscript.

Funding

This work receives no funding.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhao, X.; Ren, X.; Zhu, R.; Luo, Z.; Ren, B. Zinc oxide nanoparticles induce oxidative DNA damage and ROS-triggered mitochondria-mediated apoptosis in zebrafish embryos. Aqua. Toxicol. 2016, 180, 56–70. [Google Scholar] [CrossRef]
  2. Jones, N.; Ray, B.; Ranjit, K.T.; Manna, A.C. Antibacterial activity of ZnO nanoparticle suspensions on a broad spectrum of microorganisms. FEMS Microbiol. Lett. 2008, 279, 71–76. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  3. Hassan, I.A.; Parkin, I.P.; Nair, S.P.; Carmalt, C.J. Antimicrobial activity of copper and copper (I) oxide thin films deposited via aerosol-assisted CVD. J. Mater. Chem. B 2014, 2, 2855–2860. [Google Scholar] [CrossRef] [PubMed]
  4. Santo, C.E.; Morais, P.V.; Grass, G. Isolation and characterization of bacteria resistant to metallic copper surfaces. Appl. Environ. Microbiol. 2010, 76, 1341–1348. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  5. Bhachu, D.S.; Sathasivam, S.; Sankar, G.; Scanlon, D.O.; Cibin, G.; Carmalt, C.J.; Parkin, I.P.; Watson, G.W.; Bawaked, S.M.; Obaid, A.Y.; et al. Solution processing route to multifunctional titania thin films: Highly conductive and photocatalytically active Nb: TiO2. Adv. Funct. Mater. 2014, 24, 5075–5085. [Google Scholar] [CrossRef]
  6. Hans, M.; Erbe, A.; Mathews, S.; Chen, Y.; Solioz, M.; Mücklich, F. Role of copper oxides in contact killing of bacteria. Langmuir 2013, 29, 16160–16166. [Google Scholar] [CrossRef]
  7. Kadiyala, U.; Kotov, N.A.; VanEpps, J.S. Antibacterial metal oxide nanoparticles: Challenges in interpreting the literature. Curr. Pharm. Des. 2018, 24, 896–903. [Google Scholar] [CrossRef]
  8. Hassan, I.A.; Sathasivam, S.; Nair, S.P.; Carmalt, C.J. Antimicrobial properties of copper-doped ZnO coatings under darkness and white light illumination. ACS Omega 2017, 2, 4556–4562. [Google Scholar] [CrossRef] [Green Version]
  9. Eshed, M.; Lellouche, J.; Gedanken, A.; Banin, E. A Zn-doped CuO nanocomposite shows enhanced antibiofilm and antibacterial activities against Streptococcus mutans compared to nanosized CuO. Adv. Funct. Mater. 2014, 24, 1382–1390. [Google Scholar] [CrossRef]
  10. Liong, M.; Lu, J.; Kovochich, M.; Xia, T.; Ruehm, S.G.; Nel, A.E.; Tamanoi, F.; Zink, J.I. Multifunctional inorganic nanoparticles for imaging, targeting, and drug delivery. ACS Nano 2008, 2, 889–896. [Google Scholar] [CrossRef] [Green Version]
  11. Moorthy, M.; Kumar, V.B.; Porat, Z.; Gedanken, A. Novel polymerization of aniline and pyrrole by carbon dots. N. J. Chem. 2018, 42, 535–540. [Google Scholar] [CrossRef]
  12. Maruthapandi, M.; Kumar, V.B.; Gedanken, A. Carbon dot initiated synthesis of poly (4,4′-diaminodiphenylmethane) and its methylene blue adsorption. ACS Omega 2018, 3, 7061–7068. [Google Scholar] [CrossRef] [PubMed]
  13. Malka, E.; Perelshtein, I.; Lipovsky, A.; Shalom, Y.; Naparstek, L.; Perkas, N.; Patick, T.; Lubart, R.; Nitzan, Y.; Banin, E.; et al. Eradication of multi-drug resistant bacteria by a novel Zn-doped CuO nanocomposite. Small 2013, 9, 4069–4076. [Google Scholar] [CrossRef] [PubMed]
  14. Nagvenkar, A.P.; Gedanken, A. Cu0.89Zn0.11O, A new peroxidase-mimicking nanozyme with high sensitivity for glucose and antioxidant detection. ACS Appl. Mater. Interfaces 2016, 8, 22301–22308. [Google Scholar] [CrossRef]
  15. Ebrahimiasl, S.; Zakaria, A.; Kassim, A.; Basri, S.N. Novel conductive polypyrrole/zinc oxide/chitosan bionanocomposite: Synthesis, characterization, antioxidant, and antibacterial activities. Int. J. Nanomed. 2014, 10, 217–227. [Google Scholar] [CrossRef] [Green Version]
  16. Liu, F.; Yuan, Y.; Li, L.; Shang, S.; Yu, X.; Zhang, Q.; Jiang, S.; Wu, Y. Synthesis of polypyrrole nanocomposites decorated with silver nanoparticles with electrocatalysis and antibacterial property. Compos. Part B Eng. 2015, 69, 232–236. [Google Scholar] [CrossRef]
  17. Maráková, N.; Humpolíček, P.; Kašpárková, V.; Capáková, Z.; Martinková, L.; Bober, P.; Trchová, M.; Stejskal, J. Antimicrobial activity and cytotoxicity of cotton fabric coated with conducting polymers, polyaniline or polypyrrole, and with deposited silver nanoparticles. Appl. Surf. Sci. 2017, 396, 169–176. [Google Scholar] [CrossRef]
  18. Nazarzadeh Zare, E.; Mansour Lakouraj, M.; Mohseni, M. biodegradable polypyrrole/dextrin conductive nanocomposite: Synthesis, characterization, antioxidant and antibacterial activity. Synth. Met. 2014, 187, 9–16. [Google Scholar] [CrossRef]
  19. Ghaffari-Moghaddam, M.; Eslahi, H. Synthesis, characterization and antibacterial properties of a novel nanocomposite based on polyaniline/polyvinyl alcohol/Ag. Arab. J. Chem. 2014, 7, 846–855. [Google Scholar] [CrossRef] [Green Version]
  20. Bideau, B.; Bras, J.; Saini, S.; Daneault, C.; Loranger, E. Mechanical and antibacterial properties of a nanocellulose-polypyrrole multilayer composite. Mater. Sci. Eng. C 2016, 69, 977–984. [Google Scholar] [CrossRef]
  21. Patil, S.L.; Pawar, S.G.; Chougule, M.A.; Raut, B.T.; Godse, P.R.; Sen, S.; Patil, V.B. Structural, morphological, optical, and electrical properties of PANI-ZnO nanocomposites. Int. J. Polym. Mater. 2012, 61, 809–820. [Google Scholar] [CrossRef]
  22. Boomi, P.; Prabu, H.G.; Mathiyarasu, J. Synthesis, characterization and antibacterial activity of polyaniline/Pt–Pd nanocomposite. Eur. J. Med. Chem. 2014, 72, 18–25. [Google Scholar] [CrossRef] [PubMed]
  23. Boomi, P.; Prabu, H.G.; Mathiyarasu, J. Synthesis and characterization of polyaniline/Ag–Pt nanocomposite for improved antibacterial activity. Colloids Surf. B 2013, 103, 9–14. [Google Scholar] [CrossRef] [PubMed]
  24. Boomi, P.; Prabu, H.G.; Manisankar, P.; Ravikumar, S. Study on antibacterial activity of chemically synthesized PANI-Ag-Au nanocomposite. Appl. Surf. Sci. 2014, 300, 66–72. [Google Scholar] [CrossRef]
  25. Maruthapandi, M.; Gedanken, A. A short report on the polymerization of pyrrole and its copolymers by sonochemical synthesis of fluorescent carbon dots. Polymers 2019, 11, 1240. [Google Scholar] [CrossRef] [Green Version]
  26. Maruthapandi, M.; Nagvenkar, A.P.; Perelshtein, I.; Gedanken, A. Carbon-dot initiated synthesis of polypyrrole and polypyrrole@ CuO micro/nanoparticles with enhanced antibacterial activity. ACS Appl. Polym. Mater. 2019, 1, 1181–1186. [Google Scholar] [CrossRef]
  27. Sonia, S.; Jose Annsi, I.; Suresh Kumar, P.; Mangalaraj, D.; Viswanathan, C.; Ponpandian, N. Hydrothermal synthesis of novel Zn-doped CuO nanoflowers as an efficient photodegradation material for textile dyes. Mater. Lett. 2015, 144, 127–130. [Google Scholar] [CrossRef]
  28. Yathisha, R.O.; Arthoba Nayaka, Y. Structural, optical and electrical properties of zinc incorporated copper oxide nanoparticles: Doping effect of Zn. J. Mater. Sci. 2018, 53, 678–691. [Google Scholar] [CrossRef]
  29. Iqbal, J.; Jan, T.; Ul-Hassan, S.; Ahmed, I.; Mansoor, Q.; Umair Ali, M.; Abbas, F.; Ismail, M. Facile synthesis of Zn-doped CuO hierarchical nanostructures: Structural, optical and antibacterial properties. AIP Adv. 2015, 5, 127112. [Google Scholar] [CrossRef] [Green Version]
  30. Jan, T.; Iqbal, J.; Mansoor, Q.; Ismail, M.; Naqvi, M.S.H.; Gul, A.; Naqvi, S.F.U.H.; Abbas, F. Synthesis, physical properties and antibacterial activity of Ce doped CuO: A novel nanomaterial. J. Phys. D Appl. Phys. 2014, 47, 355301. [Google Scholar] [CrossRef]
  31. Cabuka, M.; Yavuzb, M.; Unal, H.I. Electrokinetic properties of biodegradable conducting polyaniline-graft-chitosan copolymer in aqueous and non-aqueous media. Colloids Surfaces A Physicochem. Eng. Asp. 2014, 460, 494–501. [Google Scholar] [CrossRef]
  32. Zhang, X.; Bai, R. Surface Electric Properties of Polypyrrole in Aqueous Solutions. Langmuir 2003, 19, 10703–10709. [Google Scholar] [CrossRef]
  33. Sonohara, R.; Muramatsu, N.; Ohshima, H.; Kondo, T. Difference in surface properties between Escherichia coli and Staphylococcus aureus as revealed by electrophoretic mobility measurements. Biophys. Chem. 1995, 55, 273–277. [Google Scholar] [CrossRef]
  34. Li, J.; McLandsborough, L.A. The effects of the surface charge and hydrophobicity of Escherichia coli on its adhesion to beef muscle. Int. J. Food Microbiol. 1999, 53, 185–193. [Google Scholar] [CrossRef]
  35. Meghana, S.; Kabra, P.; Chakraborty, S.; Padmavathy, N. Understanding the pathway of antibacterial activity of copper oxide nanoparticles. RSC Adv. 2015, 5, 12293. [Google Scholar] [CrossRef]
  36. Xie, Y.; He, Y.; Irwin, P.L.; Jin, T.; Shi, X. Antibacterial activity and mechanism of action of zinc oxide nanoparticles against Campylobacter jejuni. Appl. Environ. Microbiol. 2011, 77, 2325–2331. [Google Scholar] [CrossRef] [Green Version]
  37. Raghupathi, K.R.; Koodali, R.T.; Manna, A.C. Size-dependent bacterial growth inhibition and mechanism of antibacterial activity of zinc oxide nanoparticles. Langmuir 2011, 27, 4020–4028. [Google Scholar] [CrossRef]
  38. He, W.; Kim, H.K.; Wamer, W.G.; Melka, D.; Callahan, J.H.; Yin, J.J. Photogenerated charge carriers and reactive oxygen species in ZnO/Au hybrid nanostructures with enhanced photocatalytic and antibacterial activity. J. Am. Chem. Soc. 2014, 136, 750–757. [Google Scholar] [CrossRef]
  39. Chang, Y.-N.; Mingyi Zhang, M.; Xia, L.; Zhang, J.; Gengmei Xing, G. The toxic effects and mechanisms of CuO and ZnO nanoparticles. Materials 2012, 5, 2850–2871. [Google Scholar] [CrossRef] [Green Version]
  40. Burgess, R.C.; Misteli, T.; Oberdoerffer, P. DNA damage, chromatin, and transcription: The trinity of aging. Curr. Opin. Cell Biol. 2012, 24, 724–730. [Google Scholar] [CrossRef] [Green Version]
  41. Luijsterburg, M.S.; Van Attikum, H. Chromatin and the DNA damage response: The cancer connection. Mol. Oncol. 2011, 5, 349–367. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  42. Dutta, R.K.; Nenavathu, B.P.; Gangishetty, M.K.; Reddy, A.V.R. Studies on antibacterial activity of ZnO nanoparticles by ROS induced lipid peroxidation. Colloids Surf. B 2012, 94, 143–150. [Google Scholar] [CrossRef] [PubMed]
  43. Rijnaarts, H.H.M.; Norde, W.; Bouwer, E.J.; Lyklema, J.; Zehnder, A.J.B. Reversibility and mechanism of bacterial adhesion. Colloids Surf. B Biointerfaces 1995, 4, 5–22. [Google Scholar] [CrossRef]
  44. Loosdrecht, C.M.M.; Lyklema, J.; Norde, W.; Schraa, G.; Zehnder, A.J.B. The role of bacterial cell wall hydrophobicity in adhesion. Appl. Environ. Microbiol. 1987, 53, 1893–1897. [Google Scholar] [CrossRef] [Green Version]
  45. Mantecca, P.; Moschini, E.; Bonfanti, P.; Fascio, U.; Perelshtein, I.; Lipovsky, A.; Chirico, G.; Bacchetta, R.; Del Giacco, L.; Colombo, A.; et al. Toxicity evaluation of a new Zn-doped CuO nanocomposite with highly effective antibacterial properties. Toxicol. Sci. 2015, 146, 16–30. [Google Scholar] [CrossRef] [Green Version]
  46. Yuan, R.; Xu, H.; Liu, X.; Tian, Y.; Li, C.; Chen, X.; Su, S.; Perelshtein, I.; Gedanken, A.; Lin, X. Zinc-doped copper oxide nanocomposites inhibit the growth of human cancer cells through reactive oxygen species-mediated NF-κB activations. ACS Appl. Mater. Interfaces 2016, 8, 31806–31812. [Google Scholar] [CrossRef]
  47. Oh, W.-K.; Kim, S.; Kwon, O.; Jang, J. Shape-dependent cytotoxicity of polyaniline nanomaterials in human fibroblast cells. J. Nanosci. Nanotechnol. 2011, 11, 4254–4260. [Google Scholar] [CrossRef]
  48. Vaitkuviene, A.; Kaseta, V.; Voronovic, J.; Ramanauskaite, G.; Biziuleviciene, G.; Ramanaviciene, A.; Ramanavicius, A. Evaluation of cytotoxicity of polypyrrole nanoparticles synthesized by oxidative polymerization. J. Hazard. Mater. 2013, 250, 167–174. [Google Scholar] [CrossRef]
  49. Robertson, J.; Gizdavic-Nikolaidis, M.R.; Swift, S. Investigation of polyaniline and a functionalised derivative as antimicrobial additives to create contamination resistant surfaces. Materials 2018, 11, 436. [Google Scholar] [CrossRef] [Green Version]
  50. Imlay, J.A. The molecular mechanisms and physiological consequences of oxidative stress: Lessons from a model bacterium. Nat. Rev. Microbiol. 2013, 11, 443–454. [Google Scholar] [CrossRef] [Green Version]
  51. Upadhyay, J.; Kumar, B.; Gogoi, A.; Buragohain, A.K. Antibacterial and hemolysis activity of polypyrrole nanotubes decorate with silver nanoparticles by an in-situ reduction process. Mater. Sci. Eng. C 2015, 54, 8–13. [Google Scholar] [CrossRef] [PubMed]
  52. Xiao, C.; Luong, J.H.T. On-line monitoring of cell growth and cytotoxicity using electric cell-substrate impedance sensing (ECIS). Biotechnol. Prog. 2003, 19, 1000–1005. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  53. Mahmoud, K.A.; Mena, J.A.; Male, K.B.; Hrapovic, S.; Kamen, A.; Luong, J.H.T. Effect of surface charge on the cellular uptake and cytotoxicity of fluorescent labeled cellulose nanocrystals. ACS Appl. Mater. Interfaces 2010, 2, 2924–2932. [Google Scholar] [CrossRef] [PubMed] [Green Version]
Figure 1. (a,c) FTIR spectrum and (b,d) XRD diffraction patterns of polymers and polymers’ macro-nanocomposites. In Figure 1b, the two highest peaks of Zn@CuO are known as (−1, 1, 1) and (1, 1, 1), followed by (2, 0, 2). The identities of other peaks can be found in Reference [28]. A very small peak (1, 1, 0) before the (−1, 1, 1) peak has been reported in the literature, e.g., Reference [27] but only appears as a broad peak in our experimental conditions.
Figure 1. (a,c) FTIR spectrum and (b,d) XRD diffraction patterns of polymers and polymers’ macro-nanocomposites. In Figure 1b, the two highest peaks of Zn@CuO are known as (−1, 1, 1) and (1, 1, 1), followed by (2, 0, 2). The identities of other peaks can be found in Reference [28]. A very small peak (1, 1, 0) before the (−1, 1, 1) peak has been reported in the literature, e.g., Reference [27] but only appears as a broad peak in our experimental conditions.
Polymers 12 01286 g001
Figure 2. SEM and EDX images of the polymer composites. Notes: (a,b) SEM of polypyrrole (PPY)-Zn@CuO, polyaniline (PANI)-Zn@CuO; (c,d) EDX of PPY-Zn@CuO, PANI-Zn@CuO.
Figure 2. SEM and EDX images of the polymer composites. Notes: (a,b) SEM of polypyrrole (PPY)-Zn@CuO, polyaniline (PANI)-Zn@CuO; (c,d) EDX of PPY-Zn@CuO, PANI-Zn@CuO.
Polymers 12 01286 g002
Figure 3. Solid-state 13C NMR spectra of PPY-Zn@CuO and PANI-Zn@CuO macro-nanocomposites.
Figure 3. Solid-state 13C NMR spectra of PPY-Zn@CuO and PANI-Zn@CuO macro-nanocomposites.
Polymers 12 01286 g003
Figure 4. Zeta potentials of PANI, PANI-Zn@Cu-O, PPY, and PPY-Zn@CuO.
Figure 4. Zeta potentials of PANI, PANI-Zn@Cu-O, PPY, and PPY-Zn@CuO.
Polymers 12 01286 g004
Figure 5. (a,b) Antimicrobial effects of PANI-Zn@CuO and PPY-Zn@CuO on E. coli and (c,d) antimicrobial effects of PANI-Zn@CuO and PPY-Zn@CuO on S. aureus. The concentration of pure PANI or PPY is 1 mg/mL, the concentration of Zn@CuO is 0.144 mg/mL, and the polymer composite consists of 0.8 mg/mL of PANI or PPY together with 0.144 mg/mL of Zn@CuO.
Figure 5. (a,b) Antimicrobial effects of PANI-Zn@CuO and PPY-Zn@CuO on E. coli and (c,d) antimicrobial effects of PANI-Zn@CuO and PPY-Zn@CuO on S. aureus. The concentration of pure PANI or PPY is 1 mg/mL, the concentration of Zn@CuO is 0.144 mg/mL, and the polymer composite consists of 0.8 mg/mL of PANI or PPY together with 0.144 mg/mL of Zn@CuO.
Polymers 12 01286 g005
Scheme 1. The reduction of oxygen to form water by Zn@CuO, which is involved in the release of superoxide anions, hydrogen peroxide, and hydroxyl radicals.
Scheme 1. The reduction of oxygen to form water by Zn@CuO, which is involved in the release of superoxide anions, hydrogen peroxide, and hydroxyl radicals.
Polymers 12 01286 sch001
Figure 6. Electron paramagnetic resonance (EPR) measurement for (a) PANI-Zn@CuO and (b) PPY-Zn@CuO.
Figure 6. Electron paramagnetic resonance (EPR) measurement for (a) PANI-Zn@CuO and (b) PPY-Zn@CuO.
Polymers 12 01286 g006
Table 1. The literature on different polymer composites.
Table 1. The literature on different polymer composites.
Polymer CompositeReferences
PPY/ZnO/chitosan[15]
PPY-Ag[16]
PPY-Ag-NPs[17]
PPY/dextrin[18]
PANI/PVA (polyvinyl alcohol)/Ag[19]
TOCN (TEMPO *-oxidized cellulose nanofibers)/PVA-PPYfilm[20]
PANI@ZnO[21]
PANI/Pt-Pd[22]
PANI/Ag–Pt[23]
PANI-Ag-Au[24]
* TEMPO: (2,2,6,6-Tetramethylpiperidin-1-yl) oxyl or (2,2,6,6-tetramethylpiperidin-1-yl) oxidanyl.

Share and Cite

MDPI and ACS Style

Maruthapandi, M.; Saravanan, A.; Luong, J.H.T.; Gedanken, A. Antimicrobial Properties of Polyaniline and Polypyrrole Decorated with Zinc-Doped Copper Oxide Microparticles. Polymers 2020, 12, 1286. https://doi.org/10.3390/polym12061286

AMA Style

Maruthapandi M, Saravanan A, Luong JHT, Gedanken A. Antimicrobial Properties of Polyaniline and Polypyrrole Decorated with Zinc-Doped Copper Oxide Microparticles. Polymers. 2020; 12(6):1286. https://doi.org/10.3390/polym12061286

Chicago/Turabian Style

Maruthapandi, Moorthy, Arumugam Saravanan, John H. T. Luong, and Aharon Gedanken. 2020. "Antimicrobial Properties of Polyaniline and Polypyrrole Decorated with Zinc-Doped Copper Oxide Microparticles" Polymers 12, no. 6: 1286. https://doi.org/10.3390/polym12061286

APA Style

Maruthapandi, M., Saravanan, A., Luong, J. H. T., & Gedanken, A. (2020). Antimicrobial Properties of Polyaniline and Polypyrrole Decorated with Zinc-Doped Copper Oxide Microparticles. Polymers, 12(6), 1286. https://doi.org/10.3390/polym12061286

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop