Silicon Nitride Whisker-Reinforced Aluminum Matrix Composites: Twinning and Precipitation Behavior

1
School of Materials Science and Engineering, Tongji University, Shanghai 200092, China
2
School of Materials Science and Engineering, Harbin Institute of Technology, Harbin 150001, China
3
College of Mechatronics and Control Engineering, Shenzhen University, Shenzhen 518060, China
4
Department of Mechanical and Industrial Engineering, Ryerson University, Toronto, ON M5B 2K3, Canada
*
Authors to whom correspondence should be addressed.
Metals 2020, 10(3), 420; https://doi.org/10.3390/met10030420
Submission received: 18 February 2020 / Revised: 16 March 2020 / Accepted: 22 March 2020 / Published: 24 March 2020

Abstract

:
Aluminum composites reinforced with ceramic whiskers exhibited a unique combination of high specific strength and superior specific modulus. A 20 vol.% Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni (wt.%) composite was fabricated via squeeze casting in the present study. It was observed that the addition of silicon nitride (Si3N4) whiskers in the Al-Si cast alloy promoted extensive twinning in the eutectic silicon particles due to a coupled role of thermal stresses between the matrix and silicon and residual stresses present in the composite. Double aging peaks were present in the age-hardening curves. The precipitation mechanism involved the formation of Mg2Si and Al2CuMg phases. The presence of Si3N4 whiskers in the composite retarded the nucleation process of Mg2Si precipitate while enhancing its growth rate.

1. Introduction

Aluminum matrix composites (AMCs) have been widely used for the lightweight structural applications in the aerospace, automotive, and other sectors because of their superior mechanical properties arising from the judicious combination and interaction between the matrix and reinforcement [1,2,3,4,5]. The matrix acts not only as a medium to transfer the load to reinforcements, but also as a load bearer [4,6]. There are different types of reinforcement, such as, SiCw, Si3N4w, carbon nanotubes (CNTs) [7,8], graphene nanoplatelets (GNPs) [9], and various ceramic particles in micro- or nano-sizes, etc. Thus, AMCs especially with precipitation-hardenable matrices possess superior strengths due to the added impediment to the motion of dislocations by precipitates [10]. Generally, the precipitation behavior of AMCs depends on the matrix material, type of reinforcements, processing route and aging temperature [11,12,13,14]. Previous studies indicated that the precipitation sequence in AMCs remained the same as the matrix alloys, but the aging kinetics was observed to be changed [5,15].
An accelerated aging response was reported in a number of composite systems, e.g., B4C/Al-Zn-Mg alloy [15], SiCp/2014Al [16], and SiCw/Al-Li alloys [17,18]. A mechanism proposed to explain the accelerated aging in AMCs was related to the enhanced nucleation and/or growth of precipitates in the heavily dislocated matrix regions adjacent to the reinforcement [19,20]. The dislocation density in the composite (~1013–1014) was significantly (about 1~2 orders of magnitude) higher than that in the matrix alloys due to the coefficient of thermal expansion mismatch between the matrix and reinforcement [21,22,23]. Dislocations facilitated some precipitation due to the significantly decreasing activation energy for nucleation [24]. Thus, the high density of dislocations served as heterogeneous nucleation sites, leading to the accelerated aging kinetics in the composites [25,26].
However, significant retardation in the aging kinetics of the composites has also been reported due to a reduction in the retained vacancies and the formation of interfacial phases [13,27,28,29,30]. The interfaces and dislocations could act as sinks for the vacancies, leading to a delayed formation of Guinier-Preston (GP) zones [31,32]. In addition, some studies indicated that there was a critical reinforcement size and volume fraction below which the aging behavior was unaltered [33,34].
Al-Si cast alloys exhibited superior wear resistance, strength, thermal conductivity, and low thermal expansion coefficient, and good casting characteristics [35,36,37,38]. The main alloying element silicon imparted high fluidity and low shrinkage, resulting in good castability and weldability [39,40,41]. Typical microstructures in the hypoeutectic Al-Si alloys consisted of primary aluminum solid solution (α-Al) and Al-Si eutectic structure [42,43]. In the eutectic system where one phase solidifies in a faceted manner and the other nonfaceted, it was well known that the eutectic microstructure may change markedly with solidification conditions (cooling/growth rates) and also with minor additions of some modifying agents [44,45]. Semi-coherent interface between Al and Si phases with crystal orientation relationships, [110]Al//[110]Si and (111)Al//(220)Si, indicated that the Si phase tended to grow along (111)Al plane [46]. Generally, Sr- and Na-based treatment was common practice for the modification of eutectic Si phase [47]. Mg and Cu were also important alloying elements in the Al-Si alloy, which greatly influenced aging kinetics. Cu/Mg and Mg/Si ratios affected the nature of various precipitates that form [48]. It was well accepted that two precipitation sequences were mainly responsible for the precipitation hardening of Al-Si-Cu/Al-Si-Mg alloys as follows [49]:
α S S S G P   z o n e β β β   p h a s e   ( M g 2 S i ) α S S S G P   z o n e θ θ θ   p h a s e   ( A l 2 S i )
where SSS stands for the supersaturated solid solution, Al2Cu and Mg2Si are two main strengtheners in the peak-aged condition [48]. Some other phases (e.g., S (Al2CuMg) [50], and Q-Al5Cu2Mg8Si6 [40] or Q-Al3Cu2Mg9Si7 [51]) also existed in the aged Al-Si-Cu-Mg alloys. Double aging peaks in the Al-Si-Cu-Mg alloy were also reported by Li et al. [50].
In the AMCs the size, morphology and volume fraction of the reinforcement were important factors controlling the plasticity and residual stresses in the matrix. The sink effect due to the presence of interfaces between the matrix and reinforcement may also play a part in the precipitation kinetics. Our previous studies [42,52] indicated that the addition of Si3N4 whiskers accelerated the melting of the composite. The presence of Si3N4 whiskers led to a refinement of Al-Si eutectic structure and primary α-Al dendrites. It also changed the morphology of primary α-Al from dendrite-like to equiaxed, and the Al-Si eutectic structure from network-like to particulate [42]. However, it is unclear how the presence of Si3N4 whiskers affects the aging kinetics of matrix. Furthermore, while a number of researchers have reported twinning, i.e., the so-called impurity induced twinning (IIT) in the eutectic silicon phase of Al-Si cast alloys [44,53], no information on the twinning of Si3N4w/Al-Si composite is available in the literature so far. The present study was aimed to identify the effect of Si3N4 whiskers on the aging behavior of the composite, focusing on the Al-Si eutectic structure and twinning of eutectic silicon phase.

2. Materials and Methods

A 20 vol.% Si3N4w/4032Al composite was fabricated via squeeze casting at a pouring temperature of 800 °C. The composition of 4032Al matrix alloy was Al-11.5Si-1.0Mg-0.5Cu-0.5Ni with Fe ≤ 0.33 and Mn ≤ 0.15 (wt.%). The α-Si3N4 whiskers had an average length of 20 μm and 0.1–1 μm in diameter. A preform with a size of Φ90 × 22 mm contained 103 g α-Si3N4 whiskers. X-ray diffraction (XRD, Philips Xpert Panalytical ) and the subsequent JAD 6.5 software were used to identify the phases in the composite and the corresponding matrix alloy. Microstructure of the composite was examined via scanning electron microscope (SEM, HITACHI S-4700, Tokyo, Japan) equipped with energy-dispersive sectroscopy (EDS). The samples for SEM observations were polished and some of them were etched by hydrofluoric acid. Differential scanning calorimeter (DSC, Netzsch STA449C, Germany) measurements were performed at a heating rate of 10 °C min1. The aging behavior was investigated by using Vickers hardness measurements, DSC and transmission electron microscopy (TEM, Philips-CM12). The TEM specimens were mechanically thinned to 50~60 μm, followed by ion-milling at 6 kV, 0.2 mA and an incident angle of 7~15°. Typically, a sample of 20 mg in the form of Φ4 mm disk was heated at 10 °C/min from 30 to 500 °C in a flowing argon atmosphere at a flow rate of 25 mL/min. DSC samples were solution heat-treated at 515 °C for 2 h in a salt bath, followed by quenching into water at room temperature. The Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy and the composite were solution treated (typically at 515 °C for 40 min) and subsequently quenched in water. Aging was conducted at 175 °C for various dwelling times (1–28 h). The age-hardening response was determined by Vickers hardness measurements using HV-5 Vickers hardness tester at a load of 5 kg for 30 s at an aging time interval of 1 h. Each reported value was an average of at least five measurements.

3. Results and Discussion

Based on the Al-Si phase diagram, the basic microstructure was primary α-Al and Al-Si eutectic structure in the matrix Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy. The Al-Si eutectic structure was observed to distribute along the primary α-Al grain boundaries [42]. The addition of Si3N4 whiskers led to a refined Al-Si eutectic structure and primary α-Al dendrites [52], since the morphology of Al-Si eutectic structure was changed from network-like to particulate [42]. It has also been shown that the silicon in the Al-Si cast alloys formed a continuous network, and twinning is an important branching mechanism [44,54,55,56].
Figure 1a is a secondary electron (SE) image showing typical microstructures of the Al-11.5Si-1.0Mg-0.5Cu-0.5Ni, and Figure 1b is a SE image showing typical microstructures of the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite. It is seen that the base alloy consisted of (i) larger α-Al primary phase and (ii) characteristic two-phase eutectic structure (eutectic α-Al and eutectic Si) surrounding the primary α-Al grains, i.e., network-like eutectic structure (Figure 1a). The addition of Si3N4 whiskers played a beneficial part in refining the primary α-Al grains and eutectic structure, with a microstructure where both whiskers and Si particles were fairly uniformly distributed in the Al matrix (Figure 1b,c). Figure 1d shows a backscattered electron (BSE) image of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite, with the results of EDS analyses listed in Table 1. It is seen that the grey phase in Figure 1d was eutectic Si particles, while the white phase was a FeMnNi-containing intermetallic compound. Such intermetallic compounds were also reported in other Al-Si cast alloys by Manasijević et al. [57] and Abdelaziz et al. [58].
As shown in Figure 2a, in comparison with the matrix (or base) alloy, a large number of α-Si3N4 peaks were present, indicating that the current squeeze casting at a fairly high pouring temperature of 800 °C did not change the crystal structure of the α-Si3N4 whiskers added. The heat flow of the Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy and Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite, measured as a function of temperature, is shown in Figure 2b. Two endothermic peaks were observed in each curve, corresponding to the eutectic α-Al + Si peak (at a lower temperature) and primary α-Al solid solution peak (at a higher temperature), respectively. Obviously, the addition of Si3N4 whiskers moved ahead and accelerated the melting of the composite.
Figure 3a shows that eutectic Si particles in the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite contained multiple twins, which could be better seen in a magnified image in Figure 3b. Figure 3c shows the corresponding selected area diffraction pattern (SADP) from both parent and twinned silicon parts, showing the formation of (111) twinning in the eutectic Si. The presence of a large number of twins suggests that Si3N4 whiskers could effectively promote twinning in eutectic silicon particles. This is in agreement with the observations in [59], where the number of twins formed in a compressed Mg-5Zn alloy increased when precipitate particles were present, due to the additional Orowan stresses driving twin nucleation but inhibiting twin growth. Similar results were also reported in a ZEK110 (Mg-1Zn-1Gd-0.6Zr) alloy where the number density of twins nucleated was significantly high, although twin growth was retarded due to the presence of secondary phases [60]. Indeed, twinning in silicon has been observed, mainly (111) twins [61,62,63,64]. This is consistent with the present observations via SADP analysis in Figure 3c. In addition to the so-called impurity induced twinning (IIT), e.g., by strontium and cerium [44,53,65], the residual stresses or Orowan stresses caused by the difference in the coefficients of thermal expansion (ΔCTE) between the matrix and particles would play a major part in the composites. First, the huge ΔCTE difference between aluminum (~24 × 10−6 (°C)−1) and silicon (~2.6 × 10−6 (°C)−1) would lead to a potential residual strain (or mismatch strain) of as high as ~1.66%, estimated on the basis of thermal stress equation [Δε = Δαl⋅ΔT = (αmatrixαparticle)(TprocessTRT)] assuming that the matrix and particles are well bonded, where Tprocess is the processing temperature (i.e., 800 °C in this study) and TRT is room (or test) temperature (~25 °C). Even if the eutectic temperature of 577 °C in the Al-Si alloy system is used, instead of the processing/pouring temperature of 800 °C, the estimated mismatch strain is still ~1.18%. This was equivalent to exert a strong restraint pressure on the silicon particles, causing the occurrence of twinning. The presence of Si3N4 whiskers would further enhance the twinning of silicon particles, since the residual stresses or Orowan stresses present in the matrix of a composite stemming from the existence of ceramic particles can play an added role in pressing the silicon particles, thus promoting the formation of multiple twins in the silicon phase, as shown in Figure 3.
Figure 4a shows the change of Vickers hardness of the composite and the corresponding matrix alloy with time on a semi-logarithmic scale during artificial aging. The enhanced hardness generated by the addition of Si3N4 whiskers was significant. The double aging peaks were observed to be present in both the composite and matrix alloy. For the composite, the first and second peak appeared after aging for 5 and 12 h, respectively. The peak hardness was due to co-precipitation of Mg2Si and Al2CuMg phases, which could be revealed via DSC as suggested by Charai et al. [66]. Typical DSC curves are shown in Figure 4b, where two distinct exothermic peaks A and B were visible in the composite and matrix alloy, respectively. One was due to the formation of two kinds of GP II zones, and the other due to two kinds of metastable precipitates (Figure 4b). The first exothermic peak appeared when the temperature exceeded 240 °C, and the second peak occurred at ~285 °C in the matrix alloy. The two precipitation exothermic peaks of the composite were partially overlapped at 286 °C and 306 °C. It can also be seen that the heat flow for peak A was higher than that for peak B in both composite and matrix alloy. Two exothermic peaks in the matrix alloy were significantly sharper than those in the composite. The transition from GP II to metastable phases in DSC curve, i.e., the dissolution of GP zones and the nucleation of metastable phases on dislocations, may be the main reason for the formation of double aging peaks [50]. It is clear that the DSC results in Figure 4b corresponded well to the hardness changes in Figure 4a.
The high density of dislocations generated at the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni interfaces can be seen from Figure 5a, indicating the presence of residual stresses in the composite and corroborating the higher hardness in Figure 4a, while Figure 5b,c show the precipitates of the matrix in the composite after aging for 5 and 6 h, respectively. The TEM images uncovered two types of precipitates: needle-shaped precipitates and lamellar phase, which were homogenously distributed in the matrix (Figure 5c), and revealed via SADP (Figure 5d) to be β-Mg2Si and S-Al2CuMg phase, respectively. The needles were seen to have coarsened into rods. These coarse rod-like precipitates were the metastable β phase. A lot of fine needle-shaped precipitates, determined to be β phase by the SADP, could also be seen in the matrix alloy (Figure 6). The quantity of precipitates was larger in the matrix alloy, in comparison with the composite.
The addition of Si3N4 whiskers directly influenced the aging kinetics by the segregation of the solute atoms at the matrix/reinforcement interface. Furthermore, the addition of Si3N4 whiskers modified the precipitate nucleation condition associated with dislocation density and vacancy concentration, resulting in accelerating or delaying precipitation kinetics. A high dislocation density and the interfacial stresses affected not only the heterogeneous nucleation of precipitates, but also served as short-circuit paths for pipe diffusion which could accelerate the aging process. Dislocations are known to be sites for heterogeneous nucleation and paths for increased atomic transport during growth [19]. However, the Mg2Si phase basically nucleated on vacancy [19]. First, the high dislocation density in the composite retarded the nucleation process of Mg2Si precipitates by the reduction of the excess vacancy concentration in the matrix due to the absorption of vacancies into the interfaces between the whisker and matrix, or at dislocations. The screw dislocations absorbed the vacancies to form the coil dislocations, and the edge dislocations absorbed the vacancies to form dislocation jogs. Second, the high dislocation density may also enhance Mg2Si precipitate growth rate by serving as short-circuit paths for solute diffusion [11]. The enhanced diffusivity of Mg and Cu atoms would therefore increase the growth rate of Mg2Si phase, resulting in a larger size of Mg2Si precipitates with a lower number density in the composite (Figure 5c) than that in the matrix alloy (Figure 6a).

4. Conclusions

(1)
The addition of Si3N4 whiskers in the Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy played an important role in refining primary α-Al grains and eutectic structure, where both whiskers and Si particles were fairly uniformly distributed in the Al matrix.
(2)
The presence of Si3N4 whiskers promoted multiple twinning in the eutectic silicon of the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite.
(3)
Double aging peaks were present in the aging hardening curves of the composite and the corresponding matrix alloy. The precipitation mechanism involved the formation of β-Mg2Si and S-Al2CuMg phases in both composite and matrix alloy.
(4)
The added Si3N4 whiskers retarded the nucleation process of Mg2Si precipitates, while accelerating the growth of Mg2Si precipitates.

Author Contributions

Conceptualization, S.Q., L.G., and D.C.; methodology, A.F. and J.S.; investigation, S.Q. and A.F.; writing—original draft preparation, S.Q.; validation, S.Q. and J.S.; writing—review and editing, A.F. and D.C.; project administration, L.G. and D.C. All authors have read and agreed to the published version of the manuscript.

Funding

The authors are grateful for the finance support from the National Nature Science Foundation of China (Grant No.50071018) and Natural Sciences and Engineering Research Council of Canada (NSERC) in the form of international collaboration.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Mohammed, S.M.A.K.; Chen, D.L. Carbon nanotube-reinforced aluminum matrix composites. Adv. Eng. Mater. 2019, 54, 8655–8664. [Google Scholar] [CrossRef]
  2. Shao, C.W.; Zhao, S.; Wang, X.G.; Zhu, Y.K.; Zhang, Z.F.; Ritchie, R.O. Architecture of high-strength aluminum-matrix composites processed by a novel microcasting technique. NPG Asia Mater. 2019, 11, 69. [Google Scholar] [CrossRef]
  3. Schmidt, A.; Siebeck, S.; Goetze, U.; Wagner, G.; Nestler, D. Particle-Reinforced Aluminum Matrix Composites (AMCs)-selected results of an integrated technology, user, and market analysis and forecast. Metals 2018, 8, 143. [Google Scholar] [CrossRef] [Green Version]
  4. Surappa, M.K. Aluminium matrix composites: Challenges and opportunities. Sadhana 2003, 28, 319–334. [Google Scholar] [CrossRef]
  5. Chen, S.P.; Mussert, K.M.; Zwaag, S.V.D. Precipitation kinetics in Al6061 and in an Al6061-alumina particle composite. J. Mater. Sci. 1998, 33, 4477–4483. [Google Scholar] [CrossRef]
  6. Shakeri, H.R.; Wang, Z. Effect of alternative aging process on the fracture and interfacial properties of particulate Al2O3-reinforced Al (6061) metal matrix composite. Metall. Mater. Trans. A 2002, 33A, 1699–1713. [Google Scholar] [CrossRef]
  7. Liu, Z.Y.; Xiao, B.L.; Wang, W.G.; Ma, Z.Y. Developing high-performance aluminum matrix composites with directionally aligned carbon nanotubes by combining friction stir processing and subsequent rolling. Carbon 2013, 62, 35–42. [Google Scholar] [CrossRef]
  8. Chen, B.; Shen, J.; Ye, X.; Imai, H.; Umeda, J.; Takahashi, M.; Kondoh, K. Solid-state interfacial reaction and load transfer efficiency in carbon nanotubes (CNTs)-reinforced aluminum matrix composites. Carbon 2017, 114, 198–208. [Google Scholar] [CrossRef]
  9. Zhang, Z.W.; Liu, Z.Y.; Xiao, B.L.; Ni, D.R.; Ma, Z.Y. High efficiency dispersal and strengthening of graphene reinforced aluminum alloy composites fabricated by powder metallurgy combined with friction stir processing. Carbon 2018, 135, 215–223. [Google Scholar] [CrossRef]
  10. Wolverton, C. Crystal structure and stability of complex precipitate phases in Al-Cu-Mg-(Si) and Al-Zn-Mg alloys. Acta Mater. 2001, 49, 3129–3142. [Google Scholar] [CrossRef]
  11. Dutta, I.; Allen, S.M.; Hafley, J.L. Effect of reinforcement on the aging response of cast 6061 Al-Al2O3 particulate composites. Metall. Trans. 1991, 22A, 2553–2563. [Google Scholar] [CrossRef]
  12. Dutta, B.; Surappa, M.K. Age-hardening behaviour of Al-Cu-SiCp composites synthesized by casting route. Scr. Metall. Mater. 1995, 32, 731–736. [Google Scholar] [CrossRef]
  13. Daoud, A.; Reif, W. Influence of Al2O3 particulate on the aging response of A356 Al-based composites. J. Mater. Process. Technol. 2002, 123, 313–318. [Google Scholar] [CrossRef]
  14. Feng, A.H.; Xiao, B.L.; Ma, Z.Y. Effect of microstructural evolution on mechanical properties of friction stir welded AA2009/SiCp composite. Compos. Sci. Technol. 2008, 68, 2141–2148. [Google Scholar] [CrossRef]
  15. Wu, C.D.; Ma, K.; Zhang, D.L.; Wu, J.L.; Xiong, S.Y.; Luo, G.Q.; Zhang, J.; Chen, F.; Shen, Q.; Zhang, L.M.; et al. Precipitation phenomena in Al-Zn-Mg alloy matrix composites reinforced with B4C particles. Sci. Rep. 2017, 7, 9589. [Google Scholar] [CrossRef] [Green Version]
  16. Wang, Z.G.; Li, C.P.; Wang, H.Y.; Zhu, X.; Wu, M.; Li, J.H.; Jiang, Q.C. Aging behavior of nano-SiC/2014Al composite fabricated by powder metallurgy and hot extrusion techniques. J. Mater. Sci. Technol. 2016, 32, 1008–1012. [Google Scholar] [CrossRef]
  17. Sun, D.L.; Chen, S.Q.; Mao, J.F.; Yang, D.Z. Microstructure and deformation behavior of a SiC whisker reinforced aluminum-lithium alloy. Mater. Chem. Phys. 1994, 36, 217–221. [Google Scholar] [CrossRef]
  18. Dong, S.L.; Mao, J.F.; Yang, D.Z.; Cui, Y.X.; Jiang, L.T. Age-hardening behavior of a SiCw/Al-Li-Cu-Mg-Zr composite. Mater. Sci. Eng. A 2002, A327, 213–223. [Google Scholar] [CrossRef]
  19. Dutta, I.; Bourell, D.L. Influence of dislocation density and distribution on the aging behavior of 6061 Al-SiCw composites. Acta Metall. Mater. 1990, 38, 2041–2049. [Google Scholar] [CrossRef]
  20. Borrego, A.; Ibanez, J.; Lopez, V.; Lieblich, M.; Doncel, G.G. Influence of Extrusion Temperature on the Aging Behavior of 6061Al-15vol%SiCw Composites. Scr. Mater. 1996, 34, 471–479. [Google Scholar] [CrossRef] [Green Version]
  21. Vogelsang, M.; Arsenault, R.J.; Fisher, R.M. An in situ HVEM study of dislocation generation at Al/SiC interfaces in metal matrix composites. Metall. Trans. 1986, 17A, 379–389. [Google Scholar] [CrossRef] [Green Version]
  22. Zhang, Z.; Chen, D.L. Consideration of Orowan strengthening effect in particulate-reinforced metal matrix nanocomposites: A model for predicting their yield strength. Scr. Mater. 2006, 54, 1321–1326. [Google Scholar] [CrossRef]
  23. Zhang, Z.; Chen, D.L. Contribution of Orowan strengthening effect in particulate-reinforced metal matrix nanocomposites. Mater. Sci. Eng. A 2008, 483–484, 148–152. [Google Scholar] [CrossRef]
  24. Verwerft, M. On the precipitation of magnesium silicide in irradiated aluminium-magnesium alloys. Acta Mater. 2000, 48, 1097–1104. [Google Scholar] [CrossRef]
  25. Kiourtsidis, G.E.; Skolianos, S.M.; Litsardakis, G.A. Aging response of aluminium alloy 2024 silicon carbide particles (SiCp) composites. Mater. Sci. Eng. A 2004, A382, 351–361. [Google Scholar] [CrossRef]
  26. Mitlin, D.; Radmilovic, V.; Dahmen, U.; Morris, J.W. Precipitation and aging in Al-Si-Ge-Cu. Metall. Mater. Trans. A 2001, 32, 197–199. [Google Scholar] [CrossRef]
  27. Fu, H.; Ge, B.C.; Xin, Y.C.; Wu, R.Z.; Fernandez, C.; Huang, J.Y. Achieving high strength and ductility in magnesium alloys via densely hierarchical double contraction nanotwins. Nano Lett. 2017, 17, 6117–6124. [Google Scholar] [CrossRef]
  28. Ourang, S.M.R.; Ekrami, A.; Reihani, S.M.S.; Abarghouie, S.M.R.M. Aging Behaviors of Al 6061 and Al 6061/SiCp Composite. Adv. Mater. Res. 2011, 410, 240–244. [Google Scholar] [CrossRef]
  29. Wozniak, J.; Kostecki, M.; Broniszewski, K.; Bochniak, W.; Olszyna, A. Aging behaviour of AA6061/SiCp composites produced by direct extrusion with areversibly rotating die method. Arch. Metall. Mater. 2015, 60, 1755–1761. [Google Scholar] [CrossRef] [Green Version]
  30. Pal, S.; Mitra, R.; Bhanuprasad, V.V. Aging behaviour of Al-Cu-Mg alloy-SiC composites. Mater. Sci. Eng. A 2008, 480, 496–505. [Google Scholar] [CrossRef]
  31. Saheb, N.; Khalil, A.; Hakeem, A.S.; Laoui, T.; Aqeeli, N.A.; Qutub, A.M.A. Age hardening behavior of carbon nanotube reinforced aluminum nanocomposites. J. Nano Res. 2013, 21, 29–35. [Google Scholar] [CrossRef]
  32. Massardier, V.; Pelletier, L.; Merle, P. Influence of the introduction of ceramic particles in Al-Cu alloys on GP zone formation. Mater. Sci. Eng. A 1998, A249, 121–133. [Google Scholar] [CrossRef]
  33. Bekheet, N.E.; Gadelrab, R.M.; Salah, M.F.; EI-Azim, A.N.A. The effects of aging on the hardness and fatigue behavior of 2024 Al alloy/SiC composites. Mater. Des. 2002, 23, 153–159. [Google Scholar] [CrossRef]
  34. Hu, J.; Fei, W.D.; Yao, C.K. Aging behaviors of alumina borate whisker reinforced AC8A-Al composite. J. Mater. Sci. 2001, 36, 4817–4821. [Google Scholar] [CrossRef]
  35. Tjong, S.C.; Wu, S.Q.; Liao, H.C. Wear behaviour of an Al-12% Si alloy reinforced with a low volume fraction of SiC particles. Compos. Sci. Technol. 1997, 57, 1551–1558. [Google Scholar] [CrossRef]
  36. Javidani, M.; Larouche, D. Application of cast Al-Si alloys in internal combustion engine components. Int. Mater. Rev. 2014, 59, 132–158. [Google Scholar] [CrossRef]
  37. Cai, Q.; Mendis, C.L.; Chang, I.T.H.; Fan, Z.Y. Microstructure evolution and mechanical properties of new die-cast Al-Si-Mg-Mn alloys. Mater. Des. 2020, 187, 108394. [Google Scholar] [CrossRef]
  38. Li, Y.; Hu, B.; Liu, B.; Nie, A.; Gu, Q.F.; Wang, J.F.; Li, Q. Insight into Si poisoning on grain refinement of Al-Si/Al-5Ti-B system. Acta Mater. 2020, 187, 51–65. [Google Scholar] [CrossRef]
  39. Mondolfo, L.F. Aluminum Alloys Structure and Properties; William Clowes & Sons Limited: Beccles, UK, 1976. [Google Scholar]
  40. Dong, X.X.; Amirkhanlou, S.; Ji, S.X. Formation of strength platform in cast Al-Si-Mg-Cu alloys. Sci. Rep. 2019, 9, 9582. [Google Scholar] [CrossRef] [Green Version]
  41. Barrirero, J.; Pauly, C.; Engstler, M.; Ghanbaja, J.; Ghafoor, N.; Li, J.; Schumacher, P.; Oden, M.; Muecklich, F. Eutectic modification by ternary compound cluster formation in Al-Si alloys. Sci. Rep. 2019, 9, 5506. [Google Scholar] [CrossRef]
  42. Feng, A.H.; Geng, L.; Zhang, J.; Yao, C.K. Hot compressive deformation behavior of a eutectic Al-Si alloy based composite reinforced with a-Si3N4 whisker. Mater. Chem. Phys. 2003, 82, 618–621. [Google Scholar] [CrossRef]
  43. Zhang, Y.H.; Ye, C.Y.; Shen, Y.P.; Chang, W.; StJohn, D.H.; Wang, G.; Zhai, Q.J. Grain refinement of hypoeutectic Al-7wt.%Si alloy induced by an Al–V–B master alloy. J. Alloys Compd. 2020, 812, 152022. [Google Scholar] [CrossRef]
  44. Lu, S.Z.; Hellawell, A. The mechanism of silicon modification in Aluminum-Silicon alloys: Impurity induced twinning. Metall. Trans. 1987, 18A, 1721–1733. [Google Scholar] [CrossRef]
  45. Chen, Z.N.; Kang, H.J.; Fan, G.H.; Li, J.H.; Lu, Y.P.; Jie, J.C.; Zhang, Y.B.; Li, T.J.; Jian, X.G.; Wang, T.M. Grain refinement of hypoeutectic Al-Si alloys with B. Acta Mater. 2016, 120, 168–178. [Google Scholar] [CrossRef]
  46. Miao, Q.Y.; Wu, D.J.; Chai, D.S.; Zhan, Y.; Bi, G.J.; Niu, F.Y.; Ma, G.Y. Comparative study of microstructure evaluation and mechanical properties of 4043 aluminum alloy fabricated by wire-based additive manufacturing. Mater. Des. 2020, 186, 108205. [Google Scholar] [CrossRef]
  47. Lehmhus, D.; Huenert, D.; Mosler, U.; Martin, U.; Weise, J. Effects of eutectic modification and grain refinement on microstructure and properties of PM AlSi7 metallic foams. Metals 2019, 9, 1241. [Google Scholar] [CrossRef] [Green Version]
  48. Lopez, I.A.; Zepeda, C.M.; Reyes, J.G.G.; Flores, A.M.; Rodriguez, J.S.; Gomez, L.B. TEM microstructural characterization of melt-spun aged Al-6Si-3Cu-xMg alloys. Mater. Charact. 2007, 58, 509–518. [Google Scholar] [CrossRef]
  49. Heugue, P.; Larouche, D.; Breton, F.; Massinon, D.; Martinez, R.; Chen, X.G. Precipitation kinetics and evaluation of the interfacial mobility of precipitates in an AlSi7Cu3.5Mg0.15 cast alloy with Zr and V additions. Metals 2019, 9, 777. [Google Scholar] [CrossRef] [Green Version]
  50. Li, R.X.; Li, R.D.; Zhao, Y.H.; He, L.Z.; Li, C.X.; Guan, H.R.; Hu, Z.Q. Age-hardening behavior of cast Al-Si base alloy. Mater. Lett. 2004, 58, 2096–2101. [Google Scholar] [CrossRef]
  51. Maeda, T.; Kaneko, K.; Namba, T.; Koshino, Y.; Sato, Y.; Teranishi, R.; Aruga, Y. Structural and compositional study of precipitates in under-aged Cu-added Al-Mg-Si alloy. Sci. Rep. 2018, 8, 16629. [Google Scholar] [CrossRef]
  52. Qu, S.J.; Feng, A.H.; Geng, L.; Ma, Z.Y.; Han, J.C. DSC analysis of liquid volume fraction and compressive behavior of the semi-solid Si3N4w/Al-Si composite. Scr. Mater. 2007, 56, 951–954. [Google Scholar] [CrossRef]
  53. Mao, F.; Wei, S.Z.; Chen, C.; Zhang, C.; Wang, X.D.; Cao, Z.Q. Modification of the silicon phase and mechanical properties in Al-40Zn-6Si alloy with Eu addition. Mater. Des. 2020, 186, 108268. [Google Scholar] [CrossRef]
  54. Heiberg, G.; Arnberg, L. Investigation of the microstructure of the Al-Si eutectic in binary aluminium-7 wt% silicon alloys by electron backscatter diffraction (EBSD). J. Light Met. 2001, 1, 43–49. [Google Scholar] [CrossRef]
  55. Sha, X.C.; Chen, X.F.; Ning, H.Y.; Xiao, L.R.; Yin, D.D.; Mao, L.; Zheng, J.; Zhou, H. Modification of Eutectic Si in Al-Si-(Ba) Alloy by Inducing a Novel 9R Structure in Twins. Materials 2018, 11, 1151. [Google Scholar] [CrossRef] [Green Version]
  56. Liu, X.R.; Zhang, Y.D.; Beausir, B.; Liu, F.; Esling, C.; Yu, F.X.; Zhao, X.; Zuo, L. Twin-controlled growth of eutectic Si in unmodified and Sr-modified Al–12.7%Si alloys investigated by SEM/EBSD. Acta Mater. 2015, 97, 338–347. [Google Scholar] [CrossRef]
  57. Manasijevic, S.; Dolic, N.; Raic, K.; Radisa, R. Identification of phases formed by Cu and Ni in Al-Si Piston Alloys. Metall. Ital. 2014, 3, 11–17. [Google Scholar]
  58. Abdelaziz, M.H.; Samuel, A.M.; Doty, H.W.; Valtierra, S.; Samuel, F.H. Effect of additives on the microstructure and tensile properties of Al-Si alloys. J. Mater. Res. Technol. 2019, 8, 2255–2268. [Google Scholar] [CrossRef]
  59. Robson, J.D.; Stanford, N.; Barnett, M.R. Effect of particles in promoting twin nucleation in a Mg-5 wt.% Zn alloy. Scr. Mater. 2010, 63, 823–826. [Google Scholar] [CrossRef]
  60. Basu, I.; Samman, T.A. Hierarchical twinning induced texture weakening in lean magnesium alloys. Front. Mater. 2019, 6, 187. [Google Scholar] [CrossRef] [Green Version]
  61. Salkovitz, E.I.; Batchelder, F.W.V. Twinning in silicon. J. Met. 1952, 165. [Google Scholar] [CrossRef] [Green Version]
  62. Stokkan, G. Twinning in multicrystalline silicon for solar cells. J. Cryst. Growth 2013, 384, 107–113. [Google Scholar] [CrossRef]
  63. Jhang, J.W.; Jain, T.; Lin, H.K.; Lan, C.W. Possible twinning operations during directional solidification of multicrystalline silicon. Cryst. Growth Des. 2018, 18, 2518–2524. [Google Scholar] [CrossRef]
  64. Zhai, S.M.; Zhang, C.; Zhou, N.; Huang, L.; Lin, M.H.; Zhou, L. The twin formations on different growth planes of silicon crystal growth from melt by a molecular dynamics study. Phys. B Condens. Matter 2019, 572, 184–189. [Google Scholar] [CrossRef]
  65. Niu, G.D.; Mao, J.; Wang, J. Effect of Ce addition on fluidity of casting aluminum alloy A356. Metall. Mater. Trans. A 2019, 50A, 5935–5944. [Google Scholar] [CrossRef]
  66. Charai, A.; Walther, T.; Alfonso, C.; Zahra, A.M.; Zahra, C.Y. Coexistence of clusters, GPB zones, S’’-, S’- and S-phases in an Al-0.9% Cu-1.4% Mg alloy. Acta Mater. 2000, 48, 2751–2764. [Google Scholar] [CrossRef]
Figure 1. Typical SEM images showing the microstructures of Al-11.5Si-1.0Mg-0.5Cu-0.5Ni base alloy and Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) SE image of the base alloy; (b) SE image of the composite; (c) secondary electron (SE) image and (d) backscattered electron (BSE) image of the composite at a lower magnification for an overall view.
Figure 1. Typical SEM images showing the microstructures of Al-11.5Si-1.0Mg-0.5Cu-0.5Ni base alloy and Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) SE image of the base alloy; (b) SE image of the composite; (c) secondary electron (SE) image and (d) backscattered electron (BSE) image of the composite at a lower magnification for an overall view.
Metals 10 00420 g001aMetals 10 00420 g001b
Figure 2. (a) X-ray diffraction (XRD) patterns and (b) DSC curves of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite and matrix, where DSC curves were obtained at a heating rate of 10 K/min.
Figure 2. (a) X-ray diffraction (XRD) patterns and (b) DSC curves of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite and matrix, where DSC curves were obtained at a heating rate of 10 K/min.
Metals 10 00420 g002
Figure 3. TEM images showing eutectic Si in the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) Eutectic Si particles; (b) Twinning in the eutectic Si; and (c) The corresponding selected area diffraction pattern (SADP) in Figure 1b.
Figure 3. TEM images showing eutectic Si in the Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) Eutectic Si particles; (b) Twinning in the eutectic Si; and (c) The corresponding selected area diffraction pattern (SADP) in Figure 1b.
Metals 10 00420 g003
Figure 4. (a) Hardness-time curves during age-hardening; and (b) Differential scanning calorimeter (DSC) curves for the Al-11.5Si-1.0Mg-0.5Cu-0.5Ni matrix alloy and Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite.
Figure 4. (a) Hardness-time curves during age-hardening; and (b) Differential scanning calorimeter (DSC) curves for the Al-11.5Si-1.0Mg-0.5Cu-0.5Ni matrix alloy and Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite.
Metals 10 00420 g004
Figure 5. Transmission electron microscopy (TEM) micrographs of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) As-cast composite; (b) Composite after aging for 5 h; (c) Composite after aging for 6 h; and (d) The corresponding SADP of matrix, S-Al2CuMg and β-Mg2Si phases in (c).
Figure 5. Transmission electron microscopy (TEM) micrographs of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite: (a) As-cast composite; (b) Composite after aging for 5 h; (c) Composite after aging for 6 h; and (d) The corresponding SADP of matrix, S-Al2CuMg and β-Mg2Si phases in (c).
Metals 10 00420 g005
Figure 6. TEM images of Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy after aging for 6 h: (a) A bright field image; and (b) Precipitates near Si phase.
Figure 6. TEM images of Al-11.5Si-1.0Mg-0.5Cu-0.5Ni alloy after aging for 6 h: (a) A bright field image; and (b) Precipitates near Si phase.
Metals 10 00420 g006
Table 1. Results of EDS analyses of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite in Figure 1d.
Table 1. Results of EDS analyses of Si3N4w/Al-11.5Si-1.0Mg-0.5Cu-0.5Ni composite in Figure 1d.
Composition (wt.%)AlSiMnFeNi
Point 1: White phase57.915.111.88.46.8
Point 2: Grey phase3.396.7

Share and Cite

MDPI and ACS Style

Qu, S.; Feng, A.; Geng, L.; Shen, J.; Chen, D. Silicon Nitride Whisker-Reinforced Aluminum Matrix Composites: Twinning and Precipitation Behavior. Metals 2020, 10, 420. https://doi.org/10.3390/met10030420

AMA Style

Qu S, Feng A, Geng L, Shen J, Chen D. Silicon Nitride Whisker-Reinforced Aluminum Matrix Composites: Twinning and Precipitation Behavior. Metals. 2020; 10(3):420. https://doi.org/10.3390/met10030420

Chicago/Turabian Style

Qu, Shoujiang, Aihan Feng, Lin Geng, Jun Shen, and Daolun Chen. 2020. "Silicon Nitride Whisker-Reinforced Aluminum Matrix Composites: Twinning and Precipitation Behavior" Metals 10, no. 3: 420. https://doi.org/10.3390/met10030420

APA Style

Qu, S., Feng, A., Geng, L., Shen, J., & Chen, D. (2020). Silicon Nitride Whisker-Reinforced Aluminum Matrix Composites: Twinning and Precipitation Behavior. Metals, 10(3), 420. https://doi.org/10.3390/met10030420

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop