Next Article in Journal
Growth Morphologies and Primary Solidification Modes in a Dissimilar Weld between a Low-Alloy Steel and an Austenitic Stainless Steel
Next Article in Special Issue
Metallic Glass Structures for Mechanical-Energy-Dissipation Purpose: A Review
Previous Article in Journal
Skeletonization, Geometrical Analysis, and Finite Element Modeling of Nanoporous Gold Based on 3D Tomography Data
Previous Article in Special Issue
Martensitic Transformation and Plastic Deformation of TiCuNiZr-Based Bulk Metallic Glass Composites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

The Effects of Metalloid Elements on the Nanocrystallization Behavior and Soft Magnetic Properties of FeCBSiPCu Amorphous Alloys

1
State Key Laboratory for Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083, China
2
School of Mechanical Engineering, Dongguan University of Technology, Dongguan 523808, China
3
Institute for Advanced Materials and Technology, University of Science and Technology Beijing, Beijing 100083, China
*
Author to whom correspondence should be addressed.
Metals 2018, 8(4), 283; https://doi.org/10.3390/met8040283
Submission received: 23 March 2018 / Revised: 13 April 2018 / Accepted: 17 April 2018 / Published: 19 April 2018
(This article belongs to the Special Issue Metallic Glasses: Pathways to Viable Applications)

Abstract

:
Soft magnetic properties of Fe-based metallic glasses (MGs) are dependent on their nanocrystallization behavior, particularly the precipitation of α-Fe embedded in the amorphous matrix. In this study, the effects of metalloid elements of C, B, Si, and P on thermal stability, nanocrystallization behavior, and soft magnetic properties of typical Fe-based amorphous alloys, i.e., the Fe-Cu-(CBSiP) glassy alloys, were investigated systematically. It is found that the addition of the metalloid elements can effectively retard the precipitation process of α-Fe during reheating of the Fe-based MGs due to the long-range diffusion of the metalloids; however, their individual effects on the compositional portioning and formation of other crystalline phases are varied. To achieve desirable soft magnetic properties, a species of metalloids and their concentrations have to be carefully controlled so that the formation of α-Fe does not interfere with that of other crystalline phases, especially those hard-magnetic phases.

1. Introduction

Fe-based metallic glasses (MGs) have attracted extensive attention due to their unique combination of good mechanical and soft magnetic properties [1,2,3,4,5]. Currently, a variety of soft magnetic Fe-based amorphous alloys and their composites have been developed, such as METGLAS, FINEMET, NANOPERM, HITPERM, and NANOMET [6,7,8,9,10]. Some of them have been widely using in transformer, motor, sensor, and other electric and electronic parts [11,12,13,14,15]. By proper annealing of these Fe-based metallic glasses, nanocrystallization of α-Fe would occur, resulting in a composite structure consisting of ultrafine grains homogenously distributed in amorphous matrix. The coupling effect between α-Fe particles and the amorphous matrix, and the release of residual stress generated during preparation, tend to lead to better magnetic properties, including higher saturation magnetization MS and lower coercivity HC. It was reported that to achieve desirable soft magnetic properties, the following aspects should be taken into account:
  • Primary nanocrystallization of α-Fe has to be carefully controlled. In general, small sizes, high density, and homogenous distribution of α-Fe are beneficial for achieving large magnetization. In other words, nucleation of α-Fe should be stimulated, while its growth rate should be retarded.
  • Annealing usually tends to embrittle Fe-based MGs; the higher the annealing temperature, the more brittle the MGs would become. Therefore, precipitation of α-Fe at low temperatures is beneficial and preferred.
  • The stability of the residual amorphous matrix should be insufficiently high so that the formation of hard magnetic phases such as Fe3(B,C,P) can be avoided.
As elaborated above, as far as soft magnetic properties are considered, the thermal stability of both the α-Fe primary phase and the remaining amorphous matrix have to be controlled, which is closely related to the types of metalloid constituents and their total concentration in Fe-based MGs. From a standpoint of glass-forming ability (GFA), nevertheless, α-Fe precipitation needs to be retarded during undercooling, which somewhat conflicts with the requirements for obtaining decent soft magnetic properties. To solve this dilemma and manipulate primary crystallization of α-Fe, effects of metalloids including C, B, Si, and P on thermal stability and soft magnetic properties of Fe-based MGs have to be investigated in detail. Currently, no consensus in this regard has been reached, and some experimental findings even contradict each other. For example, by studying FINEMET alloy, Kim et al. reported that the addition of P increased the primary crystallization temperature and coarsened the grain size, which led to the increased coercivity [16]. However, Cui et al. found the grain size dramatically decreased from 200 to about 20 nm with addition of 4 at. % P to FeSiB alloy [17]. For the metalloid element Si, it was also noted that by Si substituting P, the GFA was increased in Fe70Al5Ga2P12.65−xC5.75B4.6Six alloys but decreased in Fe83P16−xSixCu1 alloys [18,19]. Moreover, effects of B and C are also not well understood; in many alloy systems such as (Fe, Cr)-metalloid (metalloid = C, B, or P) [20] and FePCB [21], B and C are effective at improving GFA. Nevertheless, it was reported that the increase of B in Fe-Zr-B amorphous alloys gave rise to the decrease of structural homogeneity in the bcc (body-centered-cubic) phase, resulting in the deterioration of soft magnetic properties [22].
In our previous work, an interesting series of FeCBSiPCu BMGs with high GFA and excellent soft magnetic properties [23] was developed. Unfortunately, formation of α-Fe overlapped with crystallization event of the residual amorphous matrix [i.e., formation of hard magnetic phase Fe3(B,C,P)]. Consequently, it is hard to obtain a uniform distribution of nanosized α-Fe particles without the formation of hard magnetic phases, which dramatically increase coercivity. In this paper, Fe79.3C3.1B6.9Si2.7P7.3Cu0.7 MG with a high Fe content was selected as a base alloy with which to scrutinize the effects of the metalloids on thermal stability and soft magnetic properties. The findings not only shed new insights into understanding nanocrystallization in amorphous solids, but also provide a useful guideline for developing novel soft magnetic amorphous alloys with a much wider annealing process window and better overall properties.

2. Materials and Methods

All alloy ingots with nominal compositions of Fe77.3+xC5.1−xB6.9Si2.7P7.3Cu0.7, Fe77.3+xC3.1B8.9−xSi2.7P7.3Cu0.7, Fe77.3+xC3.1B6.9Si4.7−xP7.3Cu0.7, and Fe77.3+xC3.1B6.9Si2.7P9.3−xCu0.7 (X = 0, 1,2,3, and 4 at. %) were prepared by arc-melting mixtures of Fe (99.99 wt. %), Si (99.99 wt. %), B (99.9 wt. %), Cu (99.99 wt. %), and industrial Fe-P master alloys (P: 24.81, Si: 1.4, C: 0.028, S: 0.034, Cr: 0.14, Mn: 2.24, Ti: 1.37, B: 0.0075, Al: 0.21, wt. %) in a high purity argon atmosphere. Amorphous ribbons, typically 1–1.5 mm wide and 25–30 μm thick, were produced by the melt-spinning technique with a surface speed of 40 m/s.
Thermal properties of all as-spun amorphous ribbons were evaluated using differential scanning calorimetry (DSC) at a heating rate of 0.33 K/s with argon as purging gas. According to the corresponding DSC curves, the amorphous specimens were annealed at different temperatures for 600 s under argon atmosphere. Microstructures of the as-spun and annealed ribbons were identified by X-ray diffraction (XRD) with Cu Kα radiation. Some ribbons with representative compositions and magnetic properties were further investigated by transmission electron microscopy (TEM). The MS values of all the as-spun and some annealed ribbons were characterized with a vibrating sample magnetometer (VSM) under a applied field of −800 to 800 kA/m. Coercivity (HC) was measured by using a B–H loop tracer under a field of 1000 A/m.

3. Results and Discussion

3.1. Thermal Stability

XRD patterns for all as-spun ribbon samples are shown in Figure 1. Clearly, all specimens exhibit a diffuse peak, indicative of their fully amorphous nature. Figure 2 demonstrates the corresponding DSC curves of these as-prepared Fe-based MGs at a heating rate of 0.33 K/s. Similar crystallization behavior showing two main exothermic peaks was observed for all the selected compositions. TC, Tx1, and Tx2 correspond to Curie temperature, and crystallization temperature of the 1st and 2nd peak, respectively. All the related thermal stability parameters are summarized in Table 1.
As can been seen from Figure 2a, with the increase of the C content, the first peak shifts gradually toward higher temperatures, while the second peak keeps almost unchanged. The first peak temperature (Tx1) and the second peak temperature (Tx2) as a function of C content are listed in Table 1. As demonstrated in Figure 2b, the addition of B in these alloys has similar effects on their crystallization behavior, i.e., the first peak temperature shifts toward higher temperatures, while the second peak position is the same. All these observations reveal that increasing the content of either C or B can appreciably suppress the precipitation of primary phase during annealing process but has little impact on the crystallization of residual amorphous phase.
The influence of Si addition on the crystallization behavior of the current Fe-based MGs is presented in Figure 2c. From the DSC curves, it is known that increasing the Si content shifts both crystallization peaks to higher temperatures, but rise of the first peak temperature is much larger than the second peak temperature (see Table 1 as well). These results uncover that increasing Si in the alloys could retard both crystallization stages, but is more pronounced on the crystallization of primary phase.
Figure 2d displays effects of P on the crystallization behavior of Fe-based MGs. Surprisingly, the two exothermic peaks move closer as the P content is raised. As also tabulated in Table 1, when P increases from 5.3 to 9.3 at. %, the first peak temperature Tx1 increases from 697 to 760 K, while the second peak temperature Tx2 decreases from 807 to 785 K. It is clear that addition of P could retard the crystallization of primary phase but destabilizes the residual amorphous phase.
As shown in Table 1, Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy has the largest ΔTx—(Tx2 − Tx1) of 108 K among all the alloys investigated, which provides the widest annealing window for subsequent heat treatment. Thus, it is much easier to control the precipitation of α-Fe and Fe3P(C,B) by annealing in such a wider temperature range. To investigate detailed crystallization process associated with these exothermic events, TEM characterization of the specimens annealed at certain temperatures for 10 mins, i.e., the temperature after the 1st and 2nd peak were conducted for as-spun ribbons. As an example, Figure 3 shows the bright-field TEM images, selected area electron diffraction (SAED) patterns, and high resolution microstructures for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloys of as-cast and annealed at different temperatures. Figure 3b shows that nano-scale α-Fe grains embedded in residual amorphous matrix uniformly for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy annealed at 743 K for 10 min, which corresponds to the SAED pattern consisting of both a diffused halo ring pattern produced by residual amorphous matrix and distinct spot rings generated by the nanocrystalline α-Fe. Figure 3c–e shows the SAED pattern and high resolution microstructures for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy annealed at 843 K for 10 min. It can be seen clearly that complex phase forms in residual amorphous matrix. According to the high resolution microstructures, the new phase is Fe3P(C,B), which is consistent with the XRD results. So Tx2 corresponds to the formation of phosphorus-enriched phase Fe3P(C,B).
As elaborated above, the first crystallization peak corresponds to precipitation of the α-Fe phase, while the second at higher temperatures related to crystallization event of the remaining amorphous phase can be confirmed by TEM characterization shown in Figure 3. Based on the above experimental data, adjusting the type or/and concentration of metalloid elements could manipulate crystallization behavior of Fe-based MGs so that desirable characteristics of α-Fe particles and a wide annealing process window (i.e., the temperature span between the two crystallization peaks) can be achieved. It is clear that addition of all the metalloid elements investigated, i.e., P, C, B, and Si, can effectively retard the precipitation process of α-Fe during reheating of the Fe-based MGs. According to phase diagrams, the solid solution limit of α-Fe with C, B, Si, and P is 0.1, 0, 19.6, and 4.9 at. %, respectively. Thus, during the primary crystallization of α-Fe, long-range diffusion of the metalloids is necessary because of their limited solubility in Fe. Rejection of these metalloids suppresses formation of α-Fe, shifting the crystallization event to higher temperature remarkably, i.e., increasing the Tx1 value. In general, glass formation is virtually to avoid formation of any crystalline phases; suppression of α-Fe would usually result in large GFA.
As revealed in Figure 3, this late crystallization stage is mainly related to formation of Fe3P(C, B). Note that, according to Miedema’s theory [24], formation enthalpy of Fe3C, Fe3B, Fe3Si, and Fe3P were calculated to be −1.4, −23, −21, and −50 kJ/mol, respectively. The estimated standard formation enthalpy of Fe3P is much larger than that of Fe3C, Fe3B, and Fe3Si, suggesting that Fe3P can form much easier than Fe3C, Fe3B, and Fe3Si. Therefore, phosphorus-enriched phase tends to be formed with the solution of other metalloids like C, B, and Si. As phosphorus-enriched phase is formed easier than the other three phases, so Tx2 is mainly affected by formation of this phase. Thus, as presented by Figure 2, decreasing carbon content leads to few changes of Tx2. The invariant of Tx2 results from the constant level of P content. Namely, decreasing carbon content has nearly no remarkable influence on the precipitation of phosphorus-enriched phase. Additionally, increasing boron content is similar to that of C. However, influence of Si on Tx2 of all alloys is different: for the increasing of Si content, the Tx2 moves to higher temperature. Part of Si is solute in α-Fe, with rest of it remaining in residual amorphous matrix. Thus, by increasing Si content, residual amorphous matrix could be more stable and leads Tx2 to higher temperature. Effects of P on thermal stability are different from those of other metalloids. According to Fe-P phase diagram, it can be seen that the liquidus tend to move to lower temperature by increasing P content, which leads to the process of crystalline changing from hypoeutectic type to eutectic type consistent with DSC results.

3.2. Soft Magnetic Properties

Figure 4a shows the MS measured with VSM of Fe77.3+xC5.1−xB6.9Si2.7P7.3Cu0.7, Fe77.3+xC3.1B8.9−xSi2.7P7.3Cu0.7, Fe77.3+xC3.1B6.9Si4.7−xP7.3Cu0.7, and Fe77.3+xC3.1B6.9Si2.7P9.3−xCu0.7 (X = 0, 2 and 4) amorphous as-spun ribbons, respectively. When the content of metalloid elements is decreased, MS has an increasing trend for all as-prepared ribbons. Specifically, the MS increases gradually from 1.45 T to 1.58 T, 1.43 T to 1.63 T, 1.40 T to1.55 T, and 1.43 T to 1.61 T when the content of C, B, Si and P is decreased. Due to the large negative mixing heat between Fe and metalloid elements, the addition of metalloid elements tends to generate Fe-metalloid atomic pairs. It should consider the electron interactions of Fe and metalloid elements. For C, B, Si, P elements, which all have p electrons, the p orbitals interact with 3d electrons of Fe, which would lead to the reduction of the effective magneton number. As a result, with the addition of metalloid elements, the saturated magnetization tends to be decreased, which is consistent with previous work [16,22].
Figure 4b shows the composition dependence of Curie temperature for all investigated FeCBSiPCu MGs. As can be seen in Figure 4b, each curve shows a decline trend, indicating that the Curie temperature declines gradually by decreasing metalloid elements. For Fe77.3+xC3.1B8.9−xSi2.7P7.3Cu0.7 (X = 0, 1, 2, 3, 4) alloys, the TC shifts from 632 to 601 K, which is the maximum decrease compared with that of adjusting C, Si, and P contents. It is obvious that all curves have plateaus, especially for Fe77.3+xC3.1B6.9Si2.7P9.3−xCu0.7 (X = 0, 1, 2, 3, 4) alloys; the Curie temperature even keeps as a constant value when P content is more than 7.3%, indicating that effects of metalloid elements on Curie temperature of FeCBSiPCu amorphous alloys are not remarkable if the content of metalloid elements reach to relative high value. According to molecular field theory, Curie temperature is proportional to exchange-integral constant A, which is affected by type of alloying element and distance between magnetic element. For FeCBSiPCu amorphous alloys, exchange-integral constant A is only related to Fe-Fe interaction, since there exists only one type of magnetic element Fe in FeCBSiPCu alloy system. For FeCBSiPCu amorphous alloys, AFe-Fe increases, since the addition of metalloid elements such as C, B, Si, and P increases distance between two Fe atoms, which results in the increasing of Curie temperature.
Moreover, effects of metalloid elements on coercivity (HC) of the current FeCBSiPCu MGs were also investigated. Coercivity as a function of the content of metalloid elements is shown in Figure 4c for the as-prepared Fe-based amorphous ribbons. It is of importance to point out that the lowest HC value was achieved at the alloy with 4.1 at. % C and 7.9 at. % B, respectively. However, Si and P have different effects on the coercivity. It can be seen that for the alloy with 3.7 at. % Si, HC is much higher than that of the rest alloys with 4.7, 2.7, 1.7, and 0.7 at. % Si. By decreasing the P content, HC seems to be quite stable. When the P content decreases to 5.3 at. %, HC increases sharply from 8.6 to 23.4 A/m. The influence of metalloid elements on HC may be related to the GFA. It is generally accepted that the alloys with higher GFA have a more homogeneous structure, usually resulting in lower HC [25]. For example, excessive or too little addition of C and B could deteriorate the GFA and lead to the higher HC. As mentioned eariler, P has a relatively high solute limit with Fe and addition of P is beneifical for glass formation. As a result, the alloys with a high amount of P have a low coercivity value, but once the P content is lowered to 5.3 at. %, HC sharply increases, suggesting that too little addition of P leads to the deterioration of GFA.

4. Conclusions

Partial subsititution of metalloid elements with various contents of iron in the Fe77.3+xC5.1−x B6.9Si2.7P7.3Cu0.7, Fe77.3+xC3.1B8.9−xSi2.7P7.3Cu0.7, Fe77.3+xC3.1B6.9Si4.7−xP7.3Cu0.7, and Fe77.3+xC3.1B6.9Si2.7P9.3−xCu0.7 (X = 0, 1, 2, 3 and 4) alloy system has been conducted, and the effects of metalloid elements on the thermal stability and soft magnetic properties of our FeCBSiPCu MGs has been investigated. The main conclusions are as follows:
  • C and B have similar influences on the crystallization behavior of investigated alloys. Increasing C or B leads to the increasing of Tx1, while the Tx2 remains unchanged. Increasing Si content results in the increasing of both Tx1 and Tx2. However, the increase of P content enhances Tx1 and makes Tx2 shift to lower temperature.
  • When the content of the metalloid elements is increased, MS has a decreasing trend for all as-prepared ribbons. The dependence of MS on the metalloid elements contents could be explained from the standpoint of the interactions between sp orbitals of metalloid elements and 3d electrons of Fe by increasing the content of metalloid elements.
  • For FeCBSiPCu MGs, Curie temperature declines gradually by decreasing the metalloid elements. However, the effects of metalloid elements on the Curie temperature of FeCBSiPCu MGs are not remarkable if the content of metalloid elements reaches a relatively high value.
  • The effects of metalloids on coercivity are closely related to their roles on the GFA. If their addition is beneficial for glass formation, then the coercivity value of the resultant glassy alloys will be reduced.

Acknowledgments

This research was supported by National Natural Science Foundation of China (Nos. 51671018, 51531001, 51422101, 51371003, 51271212 and 51671021), 111 Project (B07003), International S&T Cooperation Program of China (2015DFG52600), Program for Changjiang Scholars and Innovative Research Team in University of China(IRT_14R05), and the Projects of SKL-AMM-USTB (2016Z-04,2016-09, 2016Z-16). Hongxiang Li thanks the financial support from Beijing Natural Science Foundation (No. 2142022), and Program for Excellent Talents in Beijing Municipality (No. 2013D009006000004).

Author Contributions

Zhichao Lu, Hongxiang Li, Zhifeng Lei, and Zhaoping Lu conceived and designed the experiments; Zhichao Lu performed the experiments; Zhichao Lu and Zhifeng Lei analyzed the data; Chuntao Chang and Xianzhen Wang contributed analysis tools; and Zhichao Lu wrote the paper under the guidance of Hongxiang Li and Zhaoping Lu.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Inoue, A.; Zhang, T.; Takeuchi, A. Bulk amorphous alloys with high mechanical strength and good soft magnetic properties in Fe–TM–B (TM = IV–VIII group transition metal) system. Appl. Phys. Lett. 1997, 71, 464–466. [Google Scholar] [CrossRef]
  2. Borrego, J.M.; Conde, A.; Roth, S.; Eckert, J. Glass-forming ability and soft magnetic properties of FeCoSiAlGaPCB amorphous alloys. J. Appl. Phys. 2002, 92, 2073–2078. [Google Scholar] [CrossRef]
  3. Jiao, Z.B.; Li, H.X.; Gao, J.E.; Wu, Y.; Lu, Z.P. Effects of alloying elements on glass formation, mechanical and soft-magnetic properties of Fe-based metallic glasses. Intermetallics 2011, 19, 1502–1508. [Google Scholar] [CrossRef]
  4. Yang, X.H.; Ma, X.H.; Li, Q.; Guo, S.F. The effect of Mo on the glass forming ability, mechanical and magnetic properties of FePC ternary bulk metallic glasses. J. Alloys Compd. 2013, 554, 446–449. [Google Scholar] [CrossRef]
  5. Onodera, R.; Kimura, S.; Watanabe, K.; Yokoyama, Y.; Makino, A.; Koyama, K. Nucleation control for fine nano crystallization of Fe-based amorphous alloy by high-magnetic-field annealing. J. Alloys Compd. 2015, 637, 213–218. [Google Scholar] [CrossRef]
  6. Figueroa, E.; Lundgren, L.; Beckman, O.; Bhagat, S.M. The anomalous magnetization of amorphous metglas 2826-A. Solid State Commun. 1976, 20, 961–964. [Google Scholar] [CrossRef]
  7. Yoshizawa, Y.; Oguma, S.; Yamauchi, K. New Fe-based soft magnetic alloys composed of ultrafine grain structure. J. Appl. Phys. 1988, 64, 6044–6046. [Google Scholar] [CrossRef]
  8. Suzuki, K.; Kataoka, N.; Inoue, A.; Makino, A.; Masumoto, T. High saturation magnetization and soft magnetic properties of bcc Fe–Zr–B alloys with ultrafine grain structure. Mater. Trans. JIM 1990, 31, 743–746. [Google Scholar] [CrossRef]
  9. Willard, M.A.; Laughlin, D.E.; McHenry, M.E.; Thoma, D.; Sickafus, K.; Cross, J.O.; Harris, V.G. Structure and magnetic properties of (Fe0.5Co0.5)88Zr7B4Cu1 nanocrystalline alloys. J. Appl. Phys. 1998, 84, 6773–6777. [Google Scholar] [CrossRef]
  10. Takenaka, K.; Nishiyama, N.; Setyawan, A.D.; Sharma, P.; Makino, A. Performance of a prototype power transformer constructed by nanocrystalline Fe-Co-Si-B-P-Cu soft magnetic alloys. J. Appl. Phys. 2015, 117, 17D519. [Google Scholar] [CrossRef]
  11. Hasegawa, R. Applications of amorphous magnetic alloys in electronic devices. J. Non-Cryst. Solids 2001, 287, 405–412. [Google Scholar] [CrossRef]
  12. Matsumoto, H.; Urata, A.; Yamada, Y.; Inoue, A. FePBNbCr soft-magnetic glassy alloys with low loss characteristics for inductor cores. J. Alloys Compd. 2010, 504, S139–S141. [Google Scholar] [CrossRef]
  13. Nishiyama, N.; Tanimoto, K.; Makino, A. Outstanding efficiency in energy conversion for electric motors constructed by nanocrystalline soft magnetic alloy “NANOMET®” cores. AIP Adv. 2016, 6, 055925. [Google Scholar] [CrossRef]
  14. Lei, C.; Lei, J.; Yang, Z.; Zhou, Y. Improved micro fluxgate sensor with double-layer Fe-based amorphous core. Microsyst. Technol. 2013, 19, 167–172. [Google Scholar] [CrossRef]
  15. Matsumoto, H.; Urata, A.; Yamada, Y.; Ioune, A. Novel FePBNbCr glassy alloys “SENNTIX” with good soft-magnetic properties for high efficiency commercial inductor cores. J. Alloys Compd. 2011, 509, S193–S196. [Google Scholar] [CrossRef]
  16. Sun, D.S.; Hong, S.M.; Jin, H.M.; Jin, L.; Kim, C.G.; Kim, C.O. Effect of P addition on microstructure and soft magnetic properties of Fe73.5−XNb3Cu1PXSi13.5B9 alloys. J. Magn. Magn. Mater. 2006, 304, e198–e200. [Google Scholar] [CrossRef]
  17. Cui, L.Y.; Men, H.; Makino, A.; Kubota, T.; Yubuta, K.; Qi, M. Effect of Cu and P on the crystallization behavior of Fe-rich hetero-amorphous FeSiB alloy. Mater. Trans. 2009, 50, 2515–2520. [Google Scholar] [CrossRef]
  18. Mizushima, T.; Makino, A.; Inoue, A. Influence of Si addition on thermal stability and soft magnetic properties for Fe–Al–Ga–P–C–B glassy alloys. J. Appl. Phys. 1998, 83, 6329–6331. [Google Scholar] [CrossRef]
  19. Chen, F.G.; Wang, Y.G. Investigation of glass forming ability, thermal stability and soft magnetic properties of melt-spun Fe83P16−xSixCu1 (x= 0, 1, 2, 3, 4, 5) alloy ribbons. J. Alloys Comps. 2014, 584, 377–380. [Google Scholar] [CrossRef]
  20. Suzuki, K.; Makino, A.; Kataoka, N.; Inoue, A.; Masumoto, T. High saturation magnetization and soft magnetic properties of bcc Fe–Zr–B and Fe–Zr–B–M (M = transition metal) alloys with nanoscale grain size. Mater. Trans. JIM 1991, 32, 93–102. [Google Scholar] [CrossRef]
  21. Wu, Y.; Hui, X.D.; Lu, Z.P.; Liu, Z.Y.; Liang, L.; Chen, G.L. Effects of metalloid elements on the glass-forming ability of Fe-based alloys. J. Alloys Comps. 2009, 467, 187–190. [Google Scholar] [CrossRef]
  22. Demetriou, M.D.; Kaltenboeck, G.; Suh, J.Y.; Garrett, G.; Floyd, M.; Crewdson, C.; Hofmann, D.C.; Kozachkov, H.; Wiest, A.; Schramm, J.P.; et al. Glassy steel optimized for glass-forming ability and toughness. Appl. Phys. Lett. 2009, 95, 041907. [Google Scholar] [CrossRef]
  23. Li, H.X.; Gao, J.E.; Wu, Y.; Jiao, Z.B.; Ma, D.; Stoica, A.; Wang, X.L.; Ren, Y.; Miller, M.K.; Lu, Z.P.; et al. Enhancing glass-forming ability via frustration of nano-clustering in alloys with a high solvent content. Sci. Rep. 2013, 3, 1983. [Google Scholar] [CrossRef] [PubMed]
  24. Miedema, A.R.; de Chatel, P.F.; de Boer, F.R. Cohesion in alloys—Fundamentals of a semi-empirical model. Phys. B+C 1980, 100, 1–28. [Google Scholar] [CrossRef]
  25. Lee, S.; Kato, H.; Kubota, T.; Yubuta, K.; Makino, A.; Inoue, A. Excellent thermal stability and bulk glass forming ability of Fe-B-Nb-Y soft magnetic metallic glass. Mater. Trans. 2008, 49, 506–512. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of as-prepared FeCBSiPCu MGs.
Figure 1. XRD patterns of as-prepared FeCBSiPCu MGs.
Metals 08 00283 g001
Figure 2. DSC curves of as-prepared FeCBSiPCu MGs at a heating rate of 0.33 K/s.
Figure 2. DSC curves of as-prepared FeCBSiPCu MGs at a heating rate of 0.33 K/s.
Metals 08 00283 g002
Figure 3. TEM images for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloys of as-cast (a), annealed at 743 K (b), and annealed at 843 K (c) for 10 min; HRTEM images for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy annealed at 843 K for 10 min (d,e) and XRD patterns of Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy as-cast and annealed at different temperatures (f).
Figure 3. TEM images for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloys of as-cast (a), annealed at 743 K (b), and annealed at 843 K (c) for 10 min; HRTEM images for Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy annealed at 843 K for 10 min (d,e) and XRD patterns of Fe81.3C3.1B4.9Si2.7P7.3Cu0.7 alloy as-cast and annealed at different temperatures (f).
Metals 08 00283 g003
Figure 4. Changes of MS (a), changes of Curie temperature (b), and coercivity (c) for all as-prepared FeCBSiPCu MGs as a function of content of metalloid elements.
Figure 4. Changes of MS (a), changes of Curie temperature (b), and coercivity (c) for all as-prepared FeCBSiPCu MGs as a function of content of metalloid elements.
Metals 08 00283 g004
Table 1. Thermal stability and magntic properties of FeCBSiPCu MGs.
Table 1. Thermal stability and magntic properties of FeCBSiPCu MGs.
AlloysXThermal StabilitySoft Magnetic Properties
Tx1 (K)Tx2 (K)ΔTx (K)MS (T)TC (K)HC (A/m)
Fe77.3+xC5.1−xB6.9Si2.7P7.3Cu0.70746795491.456309.8
172679266 6318.0
2709791821.5162811.1
369879395 62115.9
4691788971.5861021.4
Fe77.3+xC3.1B8.9−xSi2.7P7.3Cu0.70745793481.4363211.0
172979465 6315.8
2709791821.5162811.1
369979394 61012.0
46837911081.6360120.2
Fe77.3+xC3.1B6.9Si4.7−xP7.3Cu0.70752802501.4063811.5
172879668 63426.2
2709791821.5162811.1
369678185 6208.4
4682773911.556087.3
Fe77.3+xC3.1B6.9Si2.7P9.3−xCu0.70746774281.436285.4
172178362 6288.2
2709791821.5162811.1
369679599 6188.6
4686799821.6161823.4

Share and Cite

MDPI and ACS Style

Lu, Z.; Li, H.; Lei, Z.; Chang, C.; Wang, X.; Lu, Z. The Effects of Metalloid Elements on the Nanocrystallization Behavior and Soft Magnetic Properties of FeCBSiPCu Amorphous Alloys. Metals 2018, 8, 283. https://doi.org/10.3390/met8040283

AMA Style

Lu Z, Li H, Lei Z, Chang C, Wang X, Lu Z. The Effects of Metalloid Elements on the Nanocrystallization Behavior and Soft Magnetic Properties of FeCBSiPCu Amorphous Alloys. Metals. 2018; 8(4):283. https://doi.org/10.3390/met8040283

Chicago/Turabian Style

Lu, Zhichao, Hongxiang Li, Zhifeng Lei, Chuntao Chang, Xianzhen Wang, and Zhaoping Lu. 2018. "The Effects of Metalloid Elements on the Nanocrystallization Behavior and Soft Magnetic Properties of FeCBSiPCu Amorphous Alloys" Metals 8, no. 4: 283. https://doi.org/10.3390/met8040283

APA Style

Lu, Z., Li, H., Lei, Z., Chang, C., Wang, X., & Lu, Z. (2018). The Effects of Metalloid Elements on the Nanocrystallization Behavior and Soft Magnetic Properties of FeCBSiPCu Amorphous Alloys. Metals, 8(4), 283. https://doi.org/10.3390/met8040283

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.