Next Article in Journal
Prediction of Long-Term Health Risk from Radiocesium Deposited on Ground with Consideration of Land-Surface Properties
Next Article in Special Issue
A Soil-Dependent Approach for the Design of Novel Negative Stiffness Seismic Protection Devices
Previous Article in Journal
Discrete Nonlinear Schrödinger Systems for Periodic Media with Nonlocal Nonlinearity: The Case of Nematic Liquid Crystals
Previous Article in Special Issue
An Experimental Study on the Flexural Behavior of Precast Concrete Modular Beam Systems Using Inserted Steel Plates
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Experimental Investigation into the Seismic Performance of Prefabricated Reinforced Masonry Shear Walls with Vertical Joint Connections

1
School of Civil Engineering, Harbin Institute of Technology, Harbin 150090, China
2
Key Lab of Structures Dynamic Behavior and Control of the Ministry of Education, Harbin Institute of Technology, Harbin 150090, China
3
Key Lab Smart Prevention and Mitigation of Civil Engineering Disasters of the Ministry of Industry and Information Technology, Harbin Institute of Technology, Harbin 150090, China
*
Author to whom correspondence should be addressed.
Appl. Sci. 2021, 11(10), 4421; https://doi.org/10.3390/app11104421
Submission received: 23 April 2021 / Revised: 10 May 2021 / Accepted: 12 May 2021 / Published: 13 May 2021

Abstract

:
In this study, four single-story reinforced masonry shear walls (RMSWs) (two prefabricated and two cast-in-place) under reversed cyclic loading were tested to evaluate their seismic performance. The aim of the study was to evaluate the shear behavior of RMSWs with flanges at the wall ends as well as the effect of construction method. The test results showed that all specimens had a similar failure mode with diagonal cracking. However, the crack distribution was strongly influenced by the construction method. The lateral capacity of the prefabricated walls was 12% and 27% higher than that of the corresponding cast-in-place walls with respect to the rectangular and T-shaped cross sections. The prefabricated walls showed better post-cracking performance than did the cast-in-place wall. The secant stiffness of all the walls decreased rapidly to approximately 63% of the initial stiffness when the first major diagonal crack was observed. The idealized equivalent elastic-plastic system showed that the prefabricated walls had a greater displacement ductility of 3.2–4.8 than that of the cast-in-place walls with a displacement ductility value of 2.3–2.7. This proved that the vertical joints in prefabricated RMSWs enhanced the seismic performance of walls in shear capacity and ductility. In addition, the equivalent viscous damping of the specimens ranged from 0.13 to 0.26 for prefabricated and cast-in-place walls, respectively.

1. Introduction

Reinforced masonry shear walls (RMSWs) have been widely used in medium-height or high-rise buildings in low-seismicity regions in North America and China because of their high lateral strength, stiffness, ductility, and energy dissipation [1,2,3]. With the rapid development of the building industry, prefabricate RMSWs structures are adopted because of the advantages of high component quality, quick onsite construction, energy savings, reduced labor consumption, and environmental benefits compared with the traditional cast-in-place construction method. Prefabricated RMSWs are the main horizontal bearing components to resist lateral forces transferred from concrete slabs, which act as rigid diagrams during earthquakes. Therefore, for the past few decades many researchers have focused on the in-plane seismic behavior of RMSWs and the connection method between prefabricated walls.
Two distinct in-plane failure modes of RMSWs are flexural failure and shear failure [4,5]. Numerous experimental investigations have been carried out in recent decades. The results have demonstrated that the flexural failure can be well-defined and characterized by the tensile yielding of vertical reinforcement and compressive crushing at the toes of the walls. The lateral capacity can be precisely predicted based on the plane cross-section assumption [6,7,8,9]. Furthermore, the shear failure is characterized by the diagonal cracks with a brittle behavior, which represents a low energy dissipation capacity [10,11,12,13]. Due to the complexity of each component contributing to the lateral strength, there are some experimental programs concentrating on the design modes of RMSWs failing in the shear wall under reversed cyclic loading [14,15,16]. In addition, a few studies were carried out using artificial neural networks to predict the lateral capacity of reinforced masonry walls [17,18,19]. The results showed that the proposed models perform better than do existing equations. However, the models based on the artificial neural networks lack the mechanics theory and their accuracy depends on the experimental database.
Regarding the prefabricated RMSWs, the key problem is the connection of prefabricated members. Two main connection joints are horizontal joints and vertical joints in the shear wall structures. The crucial part of the horizontal joints is the connection of vertical reinforcement. Xu et al. [20,21] tested nine prefabricated RMSWs with horizontal joints to evaluate the seismic performance under lateral cyclic loading. The results show that prefabricated RMSWs have higher lateral capacity than do traditional walls. The paper explained that prefabricated RMSWs eliminate the cleaning-hole blocks at the bottom course of the wall because of the change of construction technique. This improvement changes the connection method of vertical reinforcement from overlapped to continuous. The continuous vertical rebar performs better than an overlapped one does as a shear wall component. With respect to the vertical joints in the prefabricated RMSWs, Zhang et al. [22] proposed an innovative vertical joint connection of prefabricated RMSWs [22]. The research variables were axial compressive stress, horizontal reinforcement ratio, and construction methods. The results show the proposed vertical joints enhanced the seismic performance of prefabricated RMSWs in shear capacity and ductility.
In addition, a few studies focused on the seismic performance of RMSWs with flanges or boundary conditions to enhance the ductility and energy dissipation [23,24,25,26]. Shedid et al. [24,25] tested seven RMSWs with different end configurations and aspect ratios under cyclic loading. The results showed that the ductility values of the walls that were flanged and end-confined were, respectively, 1.5 and 2 times those of their rectangular counterparts. To maintain the same lateral capacity, more than 40% in the amount of vertical reinforcement was saved by using the proposed methods. Omar et al. [26] tested six RMSWs with different end configurations. The test results showed that the displacement ductility value of the rectangular, flanged wall and the wall with boundary elements with low reinforcement ratios were almost similar. However, with higher reinforcement ratios, the attained displacement ductility value for the walls that had flanges or boundary elements were 33% and 40% higher than that of their counterparts, respectively. However, few studies were conducted on the seismic behavior of prefabricated RMSWs with flanges and vertical joints connections in prefabricated RMSWs, which are considered to be one of the most crucial parts of the reinforced masonry shear wall structural system.
To clarify and address this issue, an experimental study on the prefabricated RMSWs with flanges was conducted to evaluate the seismic performance. Four full-scale fully grouted RMSWs were designed under the Chinese code [27] and tested under reversed cyclic loading. The aim of the study was to evaluate the shear behavior of RMSWs with flanges at the wall ends as well as the effect of construction method on seismic performance. The experimental program and test results are summarized in this paper. The crack patterns, failure modes, and force–displacement responses were obtained. The influence of flanges and construction methods on the lateral capacity, displacement ductility, stiffness degradation, energy dissipation, and equivalent viscous damping was evaluated.

2. Materials and Methods

2.1. Test Specimens

In this study, four single-story, full-scale, fully grouted RMSWs were tested to evaluate the seismic performance. Table 1 summarizes the dimensions, reinforcement details, and studied parameters of the specimens. The configuration details of the specimens are illustrated in Figure 1. The research parameters of this study were construction method and type of cross section. All the specimens were vertically loaded with an axial compressive stress of 1.05 MPa, which is 5% of the masonry compressive strength. The horizontal reinforcement was uniformly embedded in bond beams with a spacing of 400 mm along the wall height and terminated with 90 degree hooks at the ends of the walls. The horizontal reinforcement ratio of the specimens was 0.132% based on the gross area. The walls were denoted as PCMW, CMW, PCMWT, and CMWT, respectively. PCMW denoted the masonry walls constructed with a prefabricated technique and CMW denoted cast-in-place masonry walls. Compared to the rectangular cross-sectional walls (PCMW and CMW), the T-shaped section specimens (PCMWT and CMWT) had one flange at each end of the wall. The vertical joint was designed at the middle of the specimen. The reinforcement configuration at the vertical joint was comprised of four vertical reinforcement and distributed stirrups, which were designed to satisfy the requirements of strong connection and weak member according to [28]. Spiral stirrups were placed at the ends of the walls with a height of five courses, as shown in Figure 1a–d.
Considering the lab conditions, including the lab space, capacity of the actuator, and predicted shear-dominated failure mode, all the walls were heavily reinforced in the vertical direction with a vertical reinforcement ratio from 0.330% to 0.443%. The distributed vertical reinforcement was located at the center of vertical cell. As a result, the ratio of theoretical flexural strength and shear strength based on the equation proposed by GB 50003-2011 was approximately 1.2 for the rectangular walls and 1.4 for the T-shaped walls. The vertical reinforcements were anchored to the foundation and bottom concrete beams with a sufficient length to prevent anchoring failure.

2.2. Specimen Construction

All the test walls were constructed by the same experienced mason under professional supervision. The entire construction process using a prefabricated technique is divided into four steps and illustrated in Figure 2. The construction process is described as follows: (1) The foundation concrete walls with the vertical reinforcement anchors were constructed on site. In the meantime, the prefabricated walls were constructed on the yellow steel beams to allow for clean up the redundant mortar from vertical cells during the laying of the units, as shown in Figure 2a,b; (2) After the hollow units were cured to a specified strength that met the requirement of lifting, the wall segments were hoisted safely to the assigned locations and supported by steel tubes as shown in Figure 2c,d; (3) The hollow walls were grouted with pre-mixed fine concrete before installing the vertical joint reinforcement cage and templates; (4) The top reinforced concrete beam was constructed to transfer the loads from the actuators and provide the fixed boundary condition.
With respect to the cast-in-place walls, there were mainly two aspects different from the prefabricated walls. First, no vertical connection joints existed. Second, the first course units of the cast-in-place walls were cleaning holes where the vertical reinforcement overlapped.

2.3. Material Properties

Two main types of units were used in the test as shown in Figure 3, which were bond-beam units and cleaning-hole units, respectively. The overall dimensions of the two kinds of units were the same: 390 mm (length) × 190 mm (height) × 190 mm (thickness). The ratio of the vertical cell to the entire volume of the unit was 47%. The face shell of the unit was 30 mm. Bond-beam units have the advantages of grouting continuity in both the vertical and horizontal directions. The cleaning-hole units were only constructed in the first course of the cast-in-place specimens where the redundant mortar was first eliminated and then the vertical reinforcement was overlapped. The material test was conducted on the same day as the wall test.
The average compressive strength of the units was 17.4 MPa (c.o.v. = 8.3%) based on the gross area. The mortar cubes with dimensions of 70.7 mm × 70.7 mm × 70.7 mm had an average 28-day compressive strength of 13.1 MPa (c.o.v. = 4.8%). The dimension of grout samples was 100 mm × 100 mm × 100 mm. The premixed fine grout had a slump of 200 ± 20 mm and was added with 5% volume of expanding agent, which satisfies [29]. The average compressive stress of grout was 45.0 MPa (c.o.v. = 4.0%). In addition to the above-mentioned material test, the prism test was also carried out because of the material complexity of masonry. The dimension of the prism was 590 mm (length) × 990 mm (height) × 190 mm (thickness). The average compressive strength of the prisms was 21.0 MPa (c.o.v. = 8.2%). All the samples were cured in the same conditions as the test walls. The average yield strength of the D8, D14, and D16 bars were 452 MPa, 463 MPa, and 455 MPa, respectively. The average ultimate strength of the D8, D14, and D16 bars were 637 MPa, 652 MPa, and 612 MPa, respectively. The number of samples for each size of reinforcement was three.

2.4. Test Setup and Instrumentation

Figure 4 shows the test set-up of the test. The lateral reversed loads and constant vertical loads were exerted by three MTS hydraulic actuators with a capacity of 1300 kN. An L-shaped steel beam was designed to transfer the lateral and axial loads from the actuators to the test specimens.
The L-shaped steel beam was bolted to three actuators that were anchored to the rigid reaction floor. To prevent the wall from moving out of plane, two bracing rollers were placed on each side of the specimens. During the test, the two vertical actuators were operated by assigned instruction to provide constant axial loads and constrain the rotation of the specimen. The foundation concrete beam of the specimen was anchored to the laboratory floor by six bolts to prevent slide and uplift, which was considered as a fixed boundary condition. Hence, the boundary conditions of all the specimens were fixed-fixed with a shear span-to-depth ratio of 0.58.
As shown in Figure 2, a total of six linear variable differential transformers (LVDTs) at different heights of the wall were used to measure the lateral displacement relative to the foundation floor of the specimen. Two LVDTs were used to monitor the uplift of foundation beam. All the data including the loads from three actuators and displacements from LVDTs were recorded automatically by the acquisition system at a specified frequency.

2.5. Loading Protocol

A force–displacement hybrid control loading protocol was applied to attain the strength and stiffness degradation according to JGJ/T 101-2015. The loading protocol is shown in Figure 5. At the beginning of the test, the vertical load was gradually applied to the designed value to the specimen through the L-shaped loading beam from the two vertical actuators. Then, the lateral cyclic loading began with a force-controlled stage. The lateral load was cycled once starting with approximately 20% of the predicted cracking capacity until the first major diagonal crack was observed. The displacement at first major diagonal crack was defined as ∆. Afterwards, the displacement-controlled loading stage was applied. The lateral load was cycled twice until the lateral capacity dropped to 85% of the peak strength according to JGJ/T 101-2015. The loading protocol in this study was used in previous experimental programs [22,30].

3. Results and Discussion

3.1. Crack Pattern and Failure Mode

Figure 6 shows the crack patterns and failure modes of the four tested walls. The drift ratio was computed as the horizontal displacement divided by the actual height of the wall (2790 mm). PCMW was a rectangular wall with a prefabricated construction technique. Several stepped mortar joint cracks were observed at both segments at the load of 420 kN with a 0.09% drift loading cycle. No cracks were seen at the vertical joint. The first major diagonal crack was visible at 6 mm with a 0.21% drift loading cycle and extended to the right toe of the wall. A few stepped mortar joint cracks were seen over the lower five courses above the foundation at a distance about 600 mm from both wall ends. During the loading cycle at 12 mm with a 0.43% drift cycle, the wall reached its lateral capacity of +624 kN and −675 kN for both directions. As the test continued, progressive penetration of the diagonal cracks extended to the full height of the wall at 18 mm with a 0.64% drift loading cycle. The cracks were distributed on the entire wall. The major diagonal crack became wider and the mortar at the interaction of the bed and head joints expanded outwards, which led to a separation between mortar and units at 24 mm with a 0.86% drift loading cycle. The wall lost 8% of its lateral strength. During the loading cycle at 30 mm with a 1.07% drift top wall displacement, face shell spalling of units along the major diagonal crack occurred. Vertical cracks at the wall toes over the lower three courses above the foundation reinforced concrete beam widened and resulted in a face shell separation. Furthermore, damage in both sides of the segments was more severe than in the vertical joint with respect to the width and quantity of the diagonal cracks. The test ended with the strength decreasing to 74% of peak load.
PCMWT was a flanged wall with a prefabricated construction technique. A similar crack pattern was observed in both PCMWT and PCMW. PCMWT showed elastic behavior until the loading reached 660 kN. The first slight cracks were observed in the positive loading direction at a lateral load of +720 kN and a top lateral load of 3.64 mm with a 0.13% drift. The first visible cracks were composed of a combination of several stepped cracks along the mortar bed joints and head joints as well as diagonal cracks penetrating through the masonry units at the lower half of the wall. As the imposed lateral displacement increased, the first major diagonal crack appeared and simultaneously extended to the full height of the wall at the 4 mm with a 0.14% drift loading cycle. With further loading, the wall reached its lateral capacity of 906 kN for the positive direction at 8 mm with a 0.29% drift loading cycle. During this loading circle, horizontal mortar cracks were observed at webs of the flanges up to the fifth course. The wall reached an ultimate resistance of −857 kN for the negative direction at 12 mm with a 0.43% drift loading cycle. Diagonal cracks parallel to the major ones in both directions were observed and constantly extended to the ends of the walls at approximately 45 degrees. Vertical cracks in both flanged end zones extending to the fourth course were also seen. During the loading cycle at 20 mm with a 0.71% drift top wall displacement, extensive diagonal cracks extended into wall toes and distributed on the entire wall. The crack width continued to increase. The wall lost about 18% of its capacity. The major diagonal crack gradually became distinct with a width of 6 mm at 24 mm with a 0.86% drift loading circle. Spalling of the face shells along the major diagonal crack at both segments occurred as the crack continued to widen. At the end of the test and at 32 mm with 1.14% drift loading cycle, vertical cracks at the flanged end zone and the major diagonal crack became wider. A significant face shell spalling in these regions led to a loss of 38% of the wall capacity.
CMW was a rectangular wall with a traditional construction technique. Compared to the prefabricated walls, CMW showed a different crack propagation and distribution. The first major diagonal crack was observed in the positive loading direction, which extended to the entire height of the wall at 6 mm with a 0.21% drift loading cycle. During the loading cycle at 9 mm with a 0.32% drift top wall displacement, the wall reached its lateral capacity of +675 kN and −628 kN for both directions. Diagonal cracks in the negative directions extended to the entire height of the wall. Horizontal cracks were observed at both wall ends at the lower six courses above the foundation with a length of 200 mm at 12 mm with a 0.43% drift loading cycle. During the 18 mm with 0.64% drift loading cycle, diagonal cracks became wider. An 8 mm wide major diagonal crack led to a face shell separation in this region. Most of the damage was limited to the major diagonal cracks and the first course of the wall. Less damage was observed at the middle top of the wall. At the end of the test at 32 mm with a 1.14% drift loading cycle, the strength dropped to 70% of the peak load.
CMWT was a flanged wall with a traditional construction technique. During the loading cycle at 8 mm with a 0.29% drift, stepped mortar cracks at the ends of wall web were observed over the lower four courses above the foundation. The horizontal cracks at the webs of the flanges were also seen. Vertical cracks at the flanged end zones extending to the second course were also observed. Diagonal cracks were observed in the middle third of the wall height in the positive loading direction at 20 mm with a 0.71% drift loading cycle. The wall reached ultimate resistances of +728 kN and −662 kN for both directions at the loading cycle of 24 mm with a 0.86% drift top displacement. The first major diagonal crack extended from the wall toes to the top of the wall. The diagonal cracks in the positive loading direction became wider. Extensive diagonal cracks in both directions were observed during the loading cycle at 32 mm with a 1.14% drift. The damage was mainly distributed in the lower half height of the wall. The diagonal crack was incrementally widened, which led to a significant face shell spalling at the lower two courses of the wall. The vertical reinforcement buckled in this region when removing the crumbling grout columns. The wall lost about 25% of its resistance.
All the walls presented diagonal shear failure. Two main types of diagonal cracking were observed. The first type included stepped cracks along the bed joints and vertical joints. This can be explained that the principal stress exceeded the bond strength between the units and mortar where the material was the weakest in the specimen. The second type included diagonal cracks crossing the units and mortars. This indicated the principal stress exceeded the tensile strength of the material.
In addition, the diagonal cracks parallel to each other occurred at approximately 45° relative to the floor, which is perpendicular to the angle of principal stress. At the post-peak stage, the face shell spalling was observed because of the increasing width of the cracks. The first sets of visible diagonal cracks in the prefabricated walls (PCMW and PCMWT) were located at both segments at the wall ends. In addition, compared to both segments, the vertical joint in the middle of the specimen had less damage. This is because the material strength of grout in the vertical joint is higher than the masonry strength, despite the shear stress being highest in the middle of the wall.
Furthermore, the cracks in the cast-in-place specimens (CMW and CMWT) were mainly distributed in the lower half of the walls. This is because the connection methods of the vertical reinforcements were continuous on the top and overlapped on the bottom of the specimens, respectively. The grout in the first course of the wall peeled off because of the lack of protection from unit face shells where the vertical rebar overlapped. It illustrated that the use of cleaning-hole units and overlapped reinforcement changed the crack distribution. However, the proposed prefabricated construction method solved the abovementioned problems and consequently attained a uniformly distributed cracking pattern.

3.2. Force–Displacement Response

Figure 7 shows the hysteretic behavior of the tested walls. The skeleton curves of the specimens are shown in Figure 8. PCMW, PCMWT, and CMWT displayed symmetric behavior during the test. However, CMW showed asymmetric curves at the post-peak stage. This was because the first major diagonal crack in the positive direction was earlier than that in the negative direction. The pinching effect in prefabricated walls was more obvious than it was in cast-in-place walls. All the walls displayed elastic behavior before the first major diagonal crack occurred. The hysteretic loop was narrow, which illustrates low energy dissipation capacity. As the imposed displacement increased, the loop enlarged rapidly, which also indicates a high level of energy dissipation at the post-peak phase.
The bearing capacity of the prefabricated walls PCMW and PCMWT decreased slowly, which indicates a ductile failure process. However, the cast-in-place ones exhibited a rapid capacity degradation, which indicates a brittle failure mode.
All the tested walls had the same level of axial compressive stress and horizontal reinforcement ratio. The differences between the walls were mainly in the types of cross sections and construction methods. The lateral capacity of PCMWT and CMWT with a T-shaped section was 21% and 7% higher than that of the corresponding rectangular sections of PCMW and CMW, respectively. This illustrated that the flanges of the wall enhanced the bearing capacity in compression. However, the lateral resistance of the T-shaped walls dropped more rapidly than that of the rectangular section walls. This illustrated that increasing the compression area of the wall did not improve the post-peak strength or ductility of the wall. Regarding the construction method, the lateral capacity of PCMW and PCMWT was 12% and 27% higher than that of the corresponding cast-in-place walls, CMW and CMWT, respectively. This indicates that the vertical joint enhanced the shear capacity of the wall. The residual dropping mortars during the construction weakened the bond strength and friction at the interface of the walls and the bottom of the concrete beam. The continuous vertical reinforcement in PCMW and PCMWT performed better than that in CMWT and CMW where the vertical reinforcement was overlapped. The experiment results are summarized in Table 2 for a quantitative comparison of the specimen deformation characteristics at the stages of the first diagonal crack, peak load, and 15% strength degradation.

3.3. Displacement Ductility

Displacement ductility is a key seismic parameter that reflects the inelastic deformation capacity of specimens without significant strength degradation in the post-yield phase. The methodology adopted in this study was based on an equal-energy system proposed by Tomaževič [31]. Figure 9 describes the idealized elastic-plastic envelop and experimental curve. The parameters used in the idealized elastic-plastic envelop and equivalent displacement ductility are summarized in Table 3. The idealized lateral capacity can be computed by Equation (1).
V ideal = K e × ( 0.85 u 0.85 u 2 2 A env K e )
where 0.85 u is the lateral strength dropped to 85% of the peak resistance; A nev is the area under the experimental resistance envelope.
Table 2 shows the experimental displacement ductility ( μ exp ), which is defined as the ratio between the lateral displacements when the lateral capacity dropped to 85% of the maximum load and when the first major diagonal crack occurred. The experimental displacement ductility ranged from 2.6 to 4.3, and the equivalent displacement ductility ( μ ideal ) ranged from 2.3 to 3.8. It is obvious that the calculated equivalent displacement ductility was about 12% lower than the experiment displacement ductility. However, the ductility results from two methods displayed a consistent trend regarding the studied parameters.
The displacement ductility of prefabricated walls was 41% and 39% higher than that of cast-in-place walls regarding flanged and rectangular cross sections, respectively. This implies that the existence of vertical joints and continuous vertical reinforcement connections enhanced the deformability of the walls in the post-peak phase. This is also evidenced by the observation of uniformly distributed crack patterns in the prefabricated walls (PCMW and PCMWT). Nevertheless, the cracks of the cast-in-place walls were distributed mainly at the bottom of the wall. With respect to the cross section, the displacement ductility of the flanged walls was 19% and 17% higher than that of rectangular walls for prefabricated and traditional construction techniques, respectively. The reason for the higher displacement ductility was the configuration of the flanges, which lead to a larger compression area and enabled maintaining the lateral resistance at high drift levels. This was also found in a previous study [26].

3.4. Stiffness Degradation

The secant stiffness at each load cycle can be calculated by Equation (2):
K si = V max , i V min , i δ max , i δ min , i
where V max , i and V min , i are the maximum loads at cycle i ; δ max , i and δ min , i are the lateral displacements corresponding to V max , i and V min , i . The initial stiffness of wall K e was computed at the lateral load corresponding to 20% of the predicted cracking strength for masonry walls, where it is considered that the wall still maintains elastic behavior.
PCMWT and CMWT had an initial stiffness ( K 0 ) of 630.7 and 630.6 kN/mm, respectively. PCMW and CMW had an initial stiffness fo 388.8 and 386.8 kN/mm, respectively. This indicated that a T-shaped cross section increased the initial stiffness of the specimens by 62% compared to that of rectangular walls. However, the construction method had no influence on that. This is because the initial stiffness is related to the cross-sectional inertia moment.
Figure 10 shows the normalized stiffness degradation with respect to K 0 . In general, the secant stiffness decreased sharply at low values of drift and then dropped slowly at high values of drift. The secant stiffness dropped to 30% of the initial stiffness at 0.21% drift when the first major diagonal crack was observed. At the ultimate loading, the stiffness was approximately 5% of the initial stiffness. The stiffness of specimens PCMWT and CMWT with flanges decreased rapidly compared to that of the cast-in-place walls until the first major diagonal crack occurred. This illustrated that the flange of the wall increased the initial stiffness but lead to a rapid stiffness degradation.

3.5. Energy Dissipation

Energy dissipation is an important index for evaluating the seismic performance of a structural member. A high energy dissipation capacity can reduce the seismic response and demands. The energy dissipation was estimated by calculating the enclosed area of the hysteretic loops. Figure 11 shows the single circle and cumulative energy dissipation versus lateral displacement. The capacity of energy dissipation for all test walls was basically same until the lateral displacement reached 3 mm (0.11% drift). The slope had an obvious increase when the first major diagonal crack occurred, which implied the horizontal reinforcement worked to dissipate energy. Regarding the construction method, the cast-in-place walls had higher energy dissipation capacity than did the prefabricated ones at the same lateral drift. This indicated that the energy dissipation was related to the location and direction of the diagonal cracks. A larger compression zone in the cast-in-place walls contributed to better energy dissipation than in the prefabricated ones. With respect to cross section, the T-shaped cross section improved the energy dissipation capacity compared to that of the rectangular section. This is because the boundary flange increased the compression area of the wall, which improved the lateral capacity. Therefore, walls with a T-shaped section had a higher lateral capacity at the same lateral displacement.

3.6. Equivalent Viscous Damping

As shown in Figure 12, the equivalent damping ratio can be computed by Equation (3):
ξ eq = 1 2 π × S ( ABC + CDA ) S ( OBE + ODF )
where S ( ABC + CDA ) denotes the area enclosed by the hysteretic loop and S ( OBE + ODF ) denotes the area of triangles that represents the rigid, perfectly plastic curve.
The equivalent damping ratio versus lateral drift is plotted in Figure 13. At the beginning of the test, the equivalent damping ratio was high, ranging from 0.26 to 0.45. Then, the equivalent damping ratio dropped rapidly to approximately 0.10 at the lateral displacement of 3 mm. As the lateral displacement increased, the equivalent damping ratio increased to a steady value of 0.26 and 0.13 for prefabricated walls and cast-in-place walls, respectively. However, the equivalent viscous damping of reinforced concrete masonry structures was assumed, ranging from 0.07 to 0.10. This indicated that the structures with RMSWs can provide a high level of damping and, hence, reduce the seismic demand. Regarding to the construction method, the equivalent damping ratios of cast-in-place walls were higher than those of prefabricated walls, which was also found in previous literature [21].

4. Conclusions

This paper presents a comparative study on the in-plane seismic behavior of four single-story RMSWs under reversed cyclic loading. The effects of construction method and cross section on the seismic performance were evaluated according to displacement ductility, stiffness degradation, energy dissipation, and equivalent viscous damping. The following conclusions can be drawn:
(1)
All the walls presented diagonal shear failure. The stepped cracks along the bed joints and vertical joints and diagonal crack crossing the units and mortars were observed. The first sets of visible diagonal cracks in the prefabricated walls were located at both segments at the wall ends. Furthermore, the cracks in the cast-in-place specimens were mainly distributed in the lower half of the walls. The grout in the first course of the wall peeled off because of the lack of protection from unit face shells where the vertical rebar overlapped. This illustrated that the use of cleaning-hole units and overlapped reinforcement changed the crack distribution.
(2)
All the test specimens displayed symmetric behavior until the peak load. The lateral capacity of PCMWT and CMWT with a T-shaped section was 21% and 7% higher than that of the corresponding rectangular sections of PCMW and CMW, respectively. Regarding the construction method, the lateral capacity of PCMW and PCMWT was 12% and 27% higher than that of the corresponding cast-in-place walls, CMW and CMWT, respectively.
(3)
The equivalent displacement ductility varied between 2.3 and 3.8, which is related to the studied parameters of construction method and cross section. The displacement ductility of prefabricated walls was 41% and 39% higher than that of the cast-in-place walls regarding flanged and rectangular cross sections, respectively. Furthermore, the displacement ductility of the flanged walls was 19% and 17% higher than that of rectangular walls for prefabricated and traditional construction techniques, respectively.
(4)
The initial stiffness of the test walls in this study was predominantly influenced by the cross section. The T-shaped cross section increased the initial stiffness of the specimens by 62% compared to that of rectangular walls. The secant stiffness decreased sharply at low values of drift and then dropped slowly at high values of drift. Additionally, the stiffness of specimens with flanges decreased more rapidly than did that of cast-in-place walls until the first major diagonal crack occurred.
(5)
The slope had an obvious increase when the first major diagonal crack occurred. The cast-in-place walls had higher energy dissipation capacity than did the prefabricated ones at the same lateral drift. The T-shaped cross section improved the energy dissipation capacity compared to that of the rectangular section. Then, the equivalent damping ratio dropped rapidly to approximately 0.10 and finally remained stable at a value of 0.13 and 0.26 for prefabricated and cast-in-place walls, respectively.

Author Contributions

Formal analysis, Z.Z.; methodology, Z.Z.; writing—original draft preparation, Z.Z.; writing—review and editing, F.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Acknowledgments

The present work was conducted with the financial support of the National Key R&D Plan-China (Grant No. 2016YFC0701502-3).

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

A nev the area under the experimental resistance envelope
dthickness of the wall
Hheight of the wall
Llength of the wall
K e secant stiffness at first diagonal crack state
K s i secant stiffness at loading cycle i
V e shear force at first diagonal crack state
V i d e a l the idealized lateral capacity under the equal-energy system
V u shear force at peak state
V 0.85 u shear   force   at   final   state   when   the   shear   capacity   dropped   to   85 %   of   V u
ρ h horizontal reinforcement ratio
ρ v vertical reinforcement ratio
σ n axial stress
e displacement at first diagonal crack state
i d e a l the idealized displacement under the equal-energy system
u displacement at peak state
0.85 u displacement   at   final   state   when   the   shear   capacity   dropped   to   85 %   of   V u
ξ eq equivalent damping ratio
μ exp experimental displacement ductility
μ ideal equivalent displacement ductility

References

  1. Wang, F.L.; Zhang, X.C.; Zhu, F. Research progress and low-carbon property of reinforced concrete block masonry structures in China. In Proceedings of the 16th International Brick and Block Masonry Conference, Padova, Italy, 26–30 June 2016; Taylor & Francis Group: London, UK, 2016. [Google Scholar]
  2. Corrêa, M.R. The evolution of the design and construction of masonry buildings in Brazil. Gestão Tecnol. Proj. 2012, 7, 3–11. [Google Scholar] [CrossRef] [Green Version]
  3. El-Dakhakhni, W.; Ashour, A. Seismic Response of Reinforced-Concrete Masonry Shear-Wall Components and Systems: State of the Art. J. Struct. Eng. 2017, 143, 03117001. [Google Scholar] [CrossRef]
  4. Shing, P.B.; Noland, J.L.; Klamerus, E.; Spaeh, H. Inelastic behavior of concrete masonry shear walls. J. Struct. Eng. 1989, 115, 2204–2225. [Google Scholar] [CrossRef]
  5. Shing, P.B.; Schuller, M.; Hoskere, V.S. In-Plane Resistance of Reinforced Masonry Shear Walls. J. Struct. Eng. 1990, 116, 619–640. [Google Scholar] [CrossRef]
  6. Shedid, M.T.; Drysdale, R.G.; El-Dakhakhni, W.W. Behavior of Fully Grouted Reinforced Concrete Masonry Shear Walls Failing in Flexure: Experimental Results. J. Struct. Eng. 2008, 134, 1754–1767. [Google Scholar] [CrossRef]
  7. Shedid, M.T.; El-Dakhakhni, W.W.; Drysdale, R.G. Behavior of fully grouted reinforced concrete masonry shear walls failing in flexure: Analysis. Eng. Struct. 2009, 31, 2032–2044. [Google Scholar] [CrossRef]
  8. Priestley, M.J.N. Seismic design of concrete masonry shear walls. Amer. Concr. Inst. Struct. J. 1986, 83, 58–68. [Google Scholar] [CrossRef]
  9. Ibrahim, K.S.; Suter, G.T. Ductility of concrete masonry shear walls subjected to cyclic loading. In Proceedings of the 8th North American Masonry Conference, Austin, TX, USA, 6–9 June 1999; The Masonry Society: Longmont, CO, USA, 1999. [Google Scholar]
  10. Zou, X.; Feng, P.; Wang, J.; Wu, Y.; Fan, Y. FRP stay-in-place form and shear key connection for FRP-concrete hybrid beams/decks. Compos. Struct. 2018, 192, 489–499. [Google Scholar] [CrossRef]
  11. Funari, M.F.; Greco, F.; Lonetti, P. A coupled ALE-Cohesive formulation for layered structural systems. Procedia Struct. Integr. 2017, 3, 362–369. [Google Scholar] [CrossRef]
  12. El-Dakhakhni, W.W.; Banting, B.R.; Miller, S.C. Seismic Performance Parameter Quantification of Shear-Critical Reinforced Concrete Masonry Squat Walls. J. Struct. Eng. 2013, 139, 957–973. [Google Scholar] [CrossRef]
  13. Eldin, H.M.S.; Galal, K. In-Plane Seismic Performance of Fully Grouted Reinforced Masonry Shear Walls. J. Struct. Eng. 2017, 143, 04017054. [Google Scholar] [CrossRef]
  14. Eldin, H.M.S.; Ashour, A.; Galal, K. Seismic performance parameters of fully grouted reinforced masonry squat shear walls. Eng. Struct. 2019, 187, 518–527. [Google Scholar] [CrossRef]
  15. ElDin, H.M.S.; Aly, N.; Galal, K. In-plane shear strength equation for fully grouted reinforced masonry shear walls. Eng. Struct. 2019, 190, 319–332. [Google Scholar] [CrossRef]
  16. Masoud, S.; Ehsan, A.; Mohammad, M.K. Micromechanical modeling of mortar joints and brick-mortar interfaces in masonry Structures: A review of recent developments. Structures 2020, 23, 831–844. [Google Scholar]
  17. Aguilar, V.; Sandoval, C.; Adam, J.M.; Garzón-Roca, J.; Valdebenito, G. Prediction of the shear strength of reinforced masonry walls using a large experimental database and artificial neural networks. Struct. Infrastruct. Eng. 2016, 12, 1663–1676. [Google Scholar] [CrossRef]
  18. Hung, J.; Cruz, C.; Sandoval, C.; Banting, B. Analysis of partially grouted masonry shear walls using artificial neural networks. In Proceedings of the 10th International Masonry Conference, Milan, Italy, 9–11 July 2018. [Google Scholar]
  19. Vidal, V.A. Estimation of Shear Strength of Reinforced Masonry Walls. Comparative Study and Use of Artificial Neural Networks. PhD Thesis, Austral University of Chile, Valdivia, Chile, 2013. [Google Scholar]
  20. Xu, W.; Yang, X.; Wang, F.; Chi, B. Experimental and numerical study on the seismic performance of prefabricated reinforced masonry shear walls. Appl. Sci. 2018, 8, 1856. [Google Scholar] [CrossRef] [Green Version]
  21. Xu, W.; Yang, X.; Wang, F.L. Experimental investigation on the seismic behavior of newly-developed precast reinforced concrete block masonry shear walls. Appl. Sci. 2018, 8, 1071. [Google Scholar] [CrossRef] [Green Version]
  22. Zhang, Z.; Wang, F.; Chi, B. Seismic performance of shear-critical prefabricated reinforced masonry shear walls with innovative vertical joint connections. Eng. Struct. 2020, 219, 110958. [Google Scholar] [CrossRef]
  23. Robazza, B.; Yang, T.; Brzev, S.; Elwood, K.; Anderson, D.; McEwen, W. Response of slender reinforced masonry shear walls with flanged boundary elements under in-plane lateral loading: An experimental study. Eng. Struct. 2019, 190, 389–409. [Google Scholar] [CrossRef]
  24. Shedid, M.T.; El-Dakhakhni, W.W.; Drysdale, R.G. Characteristics of Rectangular, Flanged, and End-Confined Reinforced Concrete Masonry Shear Walls for Seismic Design. J. Struct. Eng. 2010, 136, 1471–1482. [Google Scholar] [CrossRef]
  25. Shedid, M.T.; El-Dakhakhni, W.W.; Drysdale, R.G. Alternative Strategies to Enhance the Seismic Performance of Reinforced Concrete-Block Shear Wall Systems. J. Struct. Eng. 2010, 136, 676–689. [Google Scholar] [CrossRef]
  26. El-Azizy, O.A.; Shedid, M.T.; El-Dakhakhni, W.W.; Drysdale, R.G. Experimental evaluation of the seismic performance of reinforced concrete structural walls with different end configurations. Eng. Struct. 2015, 101, 246–263. [Google Scholar] [CrossRef]
  27. Standardization Administration of China. GB 50003-2011: Code for Design of Masonry Structure; Standardization Administration of China: Beijing, China. (In Chinese)
  28. Standardization Administration of China. GB 50011-2010: Code for Seismic Design of Buildings; Standardization Administration of China: Beijing, China, 2010. (In Chinese)
  29. Standardization Administration of China. JC861-2008: Grout for Concret Unit Masonry; Standardization Administration of China: Beijing, China, 2008. (In Chinese)
  30. Chi, B.; Yang, X.; Wang, F.; Zhang, Z.; Quan, Y. Experimental investigation of effect of section configuration on seismic performance of an innovative integrated concrete masonry wall system. Eng. Struct. 2020, 206, 110163. [Google Scholar] [CrossRef]
  31. Tomaževič, M. Earthquake-Resistant Design of Masonry Buildings; Imperial College PR: London, UK, 1999. [Google Scholar]
Figure 1. Configuration and reinforcement details of test specimens: (a) Front view of PCMW; (b) Front view of CMW; (c) Front view of PCMWT; (d) Front view of CMWT; (e) Reinforcement configuration of PCMW; (f) Reinforcement configuration of CMW; (g) Reinforcement configuration of PCMWT; (h) Reinforcement configuration of CMWT.
Figure 1. Configuration and reinforcement details of test specimens: (a) Front view of PCMW; (b) Front view of CMW; (c) Front view of PCMWT; (d) Front view of CMWT; (e) Reinforcement configuration of PCMW; (f) Reinforcement configuration of CMW; (g) Reinforcement configuration of PCMWT; (h) Reinforcement configuration of CMWT.
Applsci 11 04421 g001aApplsci 11 04421 g001b
Figure 2. Construction details of test specimens with the prefabricated technique: (a) reinforcement configuration of hollow wall; (b) completion of hollow wall construction; (c) lifting of hollow wall; (d) adjustment and support of the wall.
Figure 2. Construction details of test specimens with the prefabricated technique: (a) reinforcement configuration of hollow wall; (b) completion of hollow wall construction; (c) lifting of hollow wall; (d) adjustment and support of the wall.
Applsci 11 04421 g002
Figure 3. Dimensions of the (a) bond-beam units and (b) cleaning-hole units (mm).
Figure 3. Dimensions of the (a) bond-beam units and (b) cleaning-hole units (mm).
Applsci 11 04421 g003
Figure 4. Test setup and instrumentation.
Figure 4. Test setup and instrumentation.
Applsci 11 04421 g004
Figure 5. Loading procedure.
Figure 5. Loading procedure.
Applsci 11 04421 g005
Figure 6. Failure modes of the specimens: (a) PCMW, (b) PCMWT, (c) CMW, and (d) CMWT.
Figure 6. Failure modes of the specimens: (a) PCMW, (b) PCMWT, (c) CMW, and (d) CMWT.
Applsci 11 04421 g006
Figure 7. Hysteresis curves of the specimens: (a) PCMW, (b) CMW, (c) PCMWT, and (d) CMWT.
Figure 7. Hysteresis curves of the specimens: (a) PCMW, (b) CMW, (c) PCMWT, and (d) CMWT.
Applsci 11 04421 g007
Figure 8. Skeleton curves of the test walls.
Figure 8. Skeleton curves of the test walls.
Applsci 11 04421 g008
Figure 9. Idealized equivalent elastic-plastic system.
Figure 9. Idealized equivalent elastic-plastic system.
Applsci 11 04421 g009
Figure 10. Normalized stiffness degradation of specimens.
Figure 10. Normalized stiffness degradation of specimens.
Applsci 11 04421 g010
Figure 11. Energy dissipation: (a) single cycle and (b) cumulative.
Figure 11. Energy dissipation: (a) single cycle and (b) cumulative.
Applsci 11 04421 g011
Figure 12. Schematic of the load–deformation hysteresis curve.
Figure 12. Schematic of the load–deformation hysteresis curve.
Applsci 11 04421 g012
Figure 13. Equivalent viscous damping of the tested walls.
Figure 13. Equivalent viscous damping of the tested walls.
Applsci 11 04421 g013
Table 1. Dimensions and reinforcement details of the test walls.
Table 1. Dimensions and reinforcement details of the test walls.
Wall IDH (mm)L (mm)d (mm)Flange (mm)Reinforcement DetailsAxial StressConstruction Method
Horizontal ρ h   ( % ) Vertical ρ v   ( % ) σ n   ( MPa )
PCMW27902390190-2C8@4000.1326C16 + 4C8 + 4C140.4431.05Prefabricated
CMW27902390190-2C8@4000.1326C16 + 6C80.3301.05Cast-in-place
PCMMT279023901905902C8@4000.1326C16 + 4C8 + 4C140.4151.05Prefabricated
CMWT279023901905902C8@4000.1328C16 + 8C80.3301.05Cast-in-place
Table 2. Test results and experimental displacement ductility.
Table 2. Test results and experimental displacement ductility.
Wall IDDirectionFirst Crack StatePeak StateFinal State μexp μ ¯ e x p
V e
(kN)
Δ e
(mm)
V u
(kN)
u
(mm)
V 0.85 u
(kN)
0.85 u
(mm)
PCMW(+)6245.973111.962126.74.53.8
(−)−675−8.9−723−12.0−615−26.73.0
CMW(+)6515.96758.957414.52.52.6
(−)−577−5.9−628−9.0−534−15.72.7
PCMWT(+)7904.09068.177023.35.84.3
(−)−848−8.0−857−11.8−729−21.72.7
CMWT(+)66011.172823.461931.92.92.8
(−)−601−11.4−662−23.9−563−30.82.7
Table 3. Idealized elastic-plastic envelope parameters and equivalent displacement ductility.
Table 3. Idealized elastic-plastic envelope parameters and equivalent displacement ductility.
Wall IDDirection K e
(kN/mm)
A e n v
(kN•mm)
0.85 u
(mm)
V i d e a l
(kN)
i d e a l
(mm)
μ i d e a l μ ¯ i d e a l
PCMW(+)105.117,13526.77397.03.83.2
(−)75.716,623−26.7−76910.22.6
CMW(+)111.0817114.57286.62.22.3
(−)97.48201−15.7−6686.92.3
PCMWT(+)199.618,75123.38904.55.23.8
(−)105.516,270−21.79459.0−2.4
CMWT(+)56.319,83631.985510.62.92.7
(−)51.216,646−30.883411.2−2.5
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zhang, Z.; Wang, F. Experimental Investigation into the Seismic Performance of Prefabricated Reinforced Masonry Shear Walls with Vertical Joint Connections. Appl. Sci. 2021, 11, 4421. https://doi.org/10.3390/app11104421

AMA Style

Zhang Z, Wang F. Experimental Investigation into the Seismic Performance of Prefabricated Reinforced Masonry Shear Walls with Vertical Joint Connections. Applied Sciences. 2021; 11(10):4421. https://doi.org/10.3390/app11104421

Chicago/Turabian Style

Zhang, Zhiming, and Fenglai Wang. 2021. "Experimental Investigation into the Seismic Performance of Prefabricated Reinforced Masonry Shear Walls with Vertical Joint Connections" Applied Sciences 11, no. 10: 4421. https://doi.org/10.3390/app11104421

APA Style

Zhang, Z., & Wang, F. (2021). Experimental Investigation into the Seismic Performance of Prefabricated Reinforced Masonry Shear Walls with Vertical Joint Connections. Applied Sciences, 11(10), 4421. https://doi.org/10.3390/app11104421

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop