Next Article in Journal
Performance Estimation of Intensity Accumulation Display by Computer-Generated Holograms
Next Article in Special Issue
A Low-Power, Low-Noise, Resistive-Bridge Microsensor Readout Circuit with Chopper-Stabilized Recycling Folded Cascode Instrumentation Amplifier
Previous Article in Journal
Radiation-Induced Stable Radicals in Calcium Phosphates: Results of Multifrequency EPR, EDNMR, ESEEM, and ENDOR Studies
Previous Article in Special Issue
Isomorphic Circuits of Independent Amplitude Tunable Voltage-Mode Bandpass Filters and Quadrature Sinusoidal Oscillators
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Carbon Dioxide Adsorption on Carbon Nanofibers with Different Porous Structures

1
Department of Mechanical Engineering, Yuan Ze University, Taoyuan 320, Taiwan
2
Fuel Cell Center, Yuan Ze University, Taoyuan 320, Taiwan
*
Author to whom correspondence should be addressed.
Appl. Sci. 2021, 11(16), 7724; https://doi.org/10.3390/app11167724
Submission received: 31 July 2021 / Revised: 17 August 2021 / Accepted: 20 August 2021 / Published: 22 August 2021
(This article belongs to the Special Issue Selected Papers from IMETI 2021)

Abstract

:
Electrospinning techniques have become an efficient way to produce continuous and porous carbon nanofibers. In view of CO2 capture as one of the important works for alleviating global warming, this study intended to synthesize polyacrylonitrile (PAN)-based activated carbon nanofibers (ACNFs) using electrospinning processes for CO2 capture. Different structures of PAN-based ACNFs were prepared, including solid, hollow, and porous nanofibers, where poly(methyl methacrylate) (PMMA) was selected as the sacrificing core or pore generator. The results showed that the PMMA could be removed successfully at a carbonization temperature of 900 °C, forming the hollow or porous ACNFs. The diameters of the ACNFs ranged from 500 to 900 nm, and the shell thickness of the hollow ACNFs was approximately 70–110 nm. The solid ACNFs and hollow ACNFs were microporous materials, while the porous ACNFs were characterized by hierarchical pore structures. The hollow ACNFs and porous ACNFs possessed higher specific surface areas than that of the solid ACNFs, while the solid ACNFs exhibited the highest microporosity (94%). The CO2 adsorption capacity on the ACNFs was highly dependent on the ratio of V<0.7 nm to Vt, the ratio of Vmi to Vt, and the N-containing functional groups. The CO2 adsorption breakthrough curves could be curve-fitted well with the Yoon and Nelson model. Furthermore, the 10 cyclic tests demonstrated that the ACNFs are promising adsorbents.

1. Introduction

Carbon fibers are of great significance in scientific and technological applications because of their high specific surface areas, high surface area to volume ratios, easy functionalization, superior mechanical properties, outstanding flexibility, etc., particularly when the carbon fibers are reduced to nanoscale. These superior properties make the carbon nanofibers show excellent performances in several applications (e.g., gas adsorption, gas storage, filter media, sensors, drug delivery, tissue engineering, protective clothing, etc.) [1,2,3]. Drawing [4,5], template synthesis [6,7], phase separation [8], self-assembly [9,10], and electrospinning [11,12] have all been investigated to produce nanofibers successfully. Compared with other methods, electrospinning is acknowledged as a simple, inexpensive, and efficient process to draw out polymers into continuous fibers with diameters ranging from submicrons to nanometers [3,13].
Despite this, the electrospinning process is very intricate, and can be described as the interactions of several physical instability processes [13,14], such as applied electrical voltage, tip-to-collector distance, and injection rate. The concentration and viscosity of the polymer solution have the most significant influence on the electrospinning process and the resultant fiber morphology [3]. In effect, the diameter of the electrospun nanofibers is influenced not only by the concentration of the polymer and the solution viscosity, but also by its molecular conformation [14,15]. In the dilute concentration range, the electrospinning of polymer solutions only forms polymer droplets, due to an insufficient chain overlap. As the concentration is increased, beaded fibers and further uniform fibers can be observed sequentially [16]. A fibrous structure is stabilized above a minimum concentration, but the fiber diameter increases with molecular weight and concentration [15]. For the polymers with higher molecular weights, uniform fibers can be formed at a lower polymer concentration compared with those having lower molecular weights [17]. Thus, the intermolecular entanglements play an important role in stabilizing the fibrous structure [18].
The co-electrospinning of polymer solutions from a spinneret set containing two coaxial capillaries has been developed to serve as an alternative technique for the fabrication of hollow fibers [19]. Using this method, co-electrospinning immiscible and miscible pairs of polymer solutions forms nanofibers with core/shell structures [19]. Subsequently, the core material can be removed by thermal decomposition [19,20] or extraction with mineral oil or solvent [21]. In general, it is suggested that the core-polymer capillary protrude ~1 mm below the end of the shell capillary to produce a good Taylor cone at the end of the nozzle [19,22]. Kaerkitcha et al. [22] found that good morphologies of polyacrylonitrile (PAN)/poly(methyl methacrylate) (PMMA) nanofibers were obtained from the coaxial nozzle electrospinning at 15 kV. For an applied voltage of 10 kV, the injection was retarded for a period until the electrostatic force was strong enough to inject the solution jet, and some of the nanofibers were fused together as a bundle of fibers. If the applied electrical voltage was greater than 20 kV, the extraction rate of the polymer solution was too fast to evaporate the solvent. Thus, wet nanofibers were fused together to form a bundle morphology.
Another type of PAN carbon nanofiber with a nanometer porous structure in individual electrospun nanofibers can be produced by blending a sacrificial polymer (e.g., PMMA) into a PAN solution [23]. After thermal treatment, the decomposition of the PMMA results in the formation of a porous structure. The use of PAN-based blends is recognized as an efficient way to create a hierarchical porous structure in carbon nanofibers. Gbewonyo et al. [23] observed that the introduction of PMMA and silica nanoparticles to PAN polymer solutions enabled the fabrication of a carbon nanofibrous mat with a unique hierarchical porous structure via the electrospinning process. However, it reduced thermal conductivity by 98% compared to the non-porous carbon film. Zhou et al. [24] proposed a new method to adopt a metal-free reversible addition–fragmentation chain-transfer polymerization of poly(acrylonitrile-block-methyl methacrylate), followed by electrospinning, stabilization, and carbonization. This new method produced porous nanofibers with a specific surface area of 503 m2/g, higher than those samples formed by traditional methods.
Porosity development in relation to a high specific surface area and micropore volume is very important for carbon nanofibers, depending on their application. Different structures (such as core/shell, hollow, and porous) of carbon nanofibers have been produced using electrospinning techniques, which have become a straightforward and convenient way to produce continuous and porous carbon nanofibers [12]. These porous nanofibers have great potential for use in drug delivery and as a scaffold for tissue engineering [25], in the capacitive deionization process for water treatment [26], or in energy [27,28,29,30]. However, there is very little application in gas adsorption. To reduce the impacts of global warming, the capture of carbon dioxide (CO2) is important. Moreover, the ultramicropore volume, specific surface area, and nitrogen-containing functional groups of adsorbents are regarded as the major features affecting the CO2 adsorption capacities of the adsorbents. Therefore, the aim of this study was to synthesize polyacrylonitrile (PAN)-based activated carbon nanofibers (ACNFs) using electrospinning processes for the capture of CO2. Using a sacrificing core or pore generator, i.e., poly(methyl methacrylate) (PMMA), solid, hollow, or porous ACNFs were prepared. Through electrospinning, followed by stabilization, carbonization, and activation, ACNFs were formed with different porous structures. Several properties of the ACNFs with different porous structures were characterized, and the CO2 adsorption on the ACNFs was investigated.

2. Materials and Methods

2.1. Preparation of Electrospun Nanofibers

Polyacrylonitrile (PAN)-based carbon nanofibers with different porous structures were prepared using electrospinning processes, including solid, hollow, and porous nanofibers. The hollow nanofibers were synthesized using a coaxial electrospinning process in which PAN (Mw = 150 kDa, Sigma–Aldrich, St. Louis, MO, USA) was the shell polymer and poly(methyl methacrylate) (PMMA) (Mw = 120 kDa, Sigma–Aldrich) was selected as the sacrifice core. Initially, PAN and PMMA were dissolved in N, N-dimethylacetamide (DMAc, Sigma–Aldrich) individually to form the polymer solutions with 10 wt.% PAN or 30 wt.% PMMA. The resulting solutions were subjected to magnetic stirring at 60 °C for 24 h in order to obtain homogeneous polymer solutions. The core–shell fibers were prepared using a coaxial spinneret system in an electrospinning unit (FES-COE, Falco Tech Enterprise Co., Ltd., New Taipei City, Taiwan). The inner diameter of the outer needle (18 gauge) was 0.96 mm, and the inner and outer diameters of the inner needle (21 gauge) were 0.52 and 0.82 mm, respectively. The electrospinning was carried out under an applied electrical voltage of 15 kV onto a metal drum collector (∅ 10 cm) covered with aluminum foil and rotated at 300 rpm, and a tip-to-collector distance of 20 cm was used. The shell and core solutions were pumped at a flow rate of 1.0 and 0.5 mL/h [22], respectively, and pushed by two syringe pumps (NE-1000, New Era Pump Systems, Inc., Farmingdale, NY, USA).
The core–shell fiber was stabilized in air from room temperature to 280 °C at a heating rate of 1 °C/min, then the temperature was held at 280 °C for 12 h to complete the cyclization and dehydrogenation reactions before the carbonization process to convert PAN from thermoplastic to a non-plastic compound [28,31,32]. The stabilized nanofibers were cooled down to room temperature and then carbonized in a nitrogen atmosphere with a flow of 100 sccm in a tubular furnace at 900 °C with a heating rate of 5° C/min, and maintained for 1 h [28] before the sample was cooled down to room temperature. After carbonization, activation of the samples was carried out by raising the temperature to 850 °C at a rate of 10° C/min under flowing nitrogen. CO2 was used as the activation agent with a flow rate of 100 sccm, switched in and held for 1 h. This sample was labeled as PANh15. For comparison, the PMMA (core polymer) was replaced with PAN, and the other conditions remained the same. This solid sample was the control sample and was denoted as PANf. Another type of core–shell fiber was synthesized under an applied electrical voltage of 12 kV, and the shell and core solutions were pumped at a flow rate of 0.7 and 0.3 mL/h, respectively. The other treatments remained the same, and this sample was denoted as PANh12.
In addition, the porous fibers were obtained from a copolymer that was electrospun using a traditional single spinneret system, where PMMA was selected as the pore generator. First, a mixture of PAN and PMMA was dissolved in DMAc by stirring for 24 h at 60 °C to obtain a blend solution for electrospinning. The blend ratio of PAN and PMMA was 2:1 (w/w), and the total polymer concentration was 15 wt.%. The blend solution was loaded into a syringe with a 21-gauge spinneret (0.52 mm inner diameter). The infusion rate of the solution in the syringe was 1.0 mL/h. The applied voltage was 15 kV, and a tip-to-collector distance of 15 cm was chosen. The follow-up processes remained the same, and this sample was labeled as PANp.

2.2. Characterizations

The morphology of the samples was observed using field emission scanning electron microscopy (FESEM) with a microscope (S-4700, Hitachi, Krefeld, Germany). The surface feature of the samples was deduced from N2 adsorption–desorption isotherms measured at –196 °C using an ASAP 2020 accelerated surface area and porosimetry system (Micromeritics, Norcross, GA, USA). Prior to the adsorption measurements, all samples were degassed at 350 °C for 24 h. The specific surface areas (SSAs) of the samples were measured in P/Po = 0.05 ~ 0.3 using the Brunauer–Emmett–Teller (BET) method. The micropore (<2.0 nm) surface area (Smi) was determined using the t-plot method. The single point total pore volume (Vt) was obtained at P/Po ≈ 0.99. The mesopore volume (Vme), micropore volume (Vmi), and ultramicropore (<0.7 nm) volume (V<0.7 nm) were calculated by applying a non-local density functional theory (NLDFT) model, where V<0.7 nm is part of Vmi. The pore size distribution curves were also obtained from a NLDFT model. X-ray photoelectron spectroscopy (XPS) was utilized to determine the number and type of functional groups present on the surface of the samples. The XPS spectra of all samples were collected using a spectrophotometer (PHI 5000 VersaProbe II, ULVAC-PHI, Kanagawa, Japan), in which a scanning X-ray monochromator (Al Anode, hν = 1401 eV) was used and the information on the elements within a few nanometers of the sample surface could be obtained. For calibration purposes, the C 1s electron binding energy (B.E.) that corresponds to graphitic carbon was set at 284.6 eV. A nonlinear least squares curve-fitting program (XPSPEAK software, version 4.1, The Chinese University of Hong Kong, Hong Kong, China) was used for the deconvolution of the XPS spectra.

2.3. CO2 Adsorption Isotherms

The CO2 adsorption isotherms on all the samples were measured using the Micromeritics ASAP 2020 system. Prior to measurement, a sample of approximately 0.05 g was outgassed at 350 °C for 24 h to remove the adsorbed contaminants. The equilibration interval for each pressure point was 45 s, and the CO2 pressure ranged from 0 to 123 kPa. The temperature during the CO2 adsorption process was maintained at 25, 40, or 55 °C using a circulating water bath thermostat. The interaction between the adsorbate molecules and the adsorbent lattice atoms can be predicted by the isosteric heat of adsorption ( Q s t ), which can be used as a measure of the energetic heterogeneity of a solid surface [33]. The Q s t can be estimated using the Clausius–Clapeyron equation, shown in Equation (1):
Q s t R = ( d ln P d   1 T ) ,
where Q s t (kJ/mol) is the isosteric heat of adsorption, R (=8.314 J/mol/K) is the gas constant, P (kPa) is the CO2 pressure, and T (K) is the adsorption temperature. A Pearson correlation analysis was performed to explore the relationships between the CO2 adsorption capacity and the surface features, and the nitrogen-containing functional groups of the adsorbents.

2.4. CO2 Adsorption Column Experiments

A fixed-bed reactor was utilized to carry out the adsorption column breakthrough curves of CO2 on all samples according to the ASTM D5160-95 method [34] at 25, 40, or 55 °C. A sample of 0.4–0.7 g was loaded into a glass tube with an inner diameter of 1 cm and a length of 20 cm, with a packed height of 10 cm. The glass tube was covered with a stainless steel sleeve on which a heating strip was wound to control the temperature of the fixed bed, and a thermocouple was positioned on the surface of the glass tube to monitor the temperature of the adsorption bed. Typical untreated flue gas compositions from a power plant burning low sulfur coal contain approximately 15–16% of CO2 [35,36]. Thus, the CO2 concentration was set at 15%, and was supplied by CO2 and N2 cylinders under appropriate mixing and quantified by gas chromatography with a thermal conductivity detector (GC/TCD). The total flow rate of the gas stream was 20 sccm. The CO2 concentration at the exit was measured using GC/TCD. When the exit concentration reached the inlet concentration, the adsorbent was heated to 150 °C to cause CO2 desorption and to regenerate the adsorbent in the nitrogen atmosphere. The Yoon and Nelson equation (Equation (2)) was used for data fitting, which is a semi-empirical gas adsorption model that could predict the whole breakthrough curve [37]:
C C 0 = 1 1 + e x p [ k ( τ t ) ] ,
where C is the outlet concentration at time t (mmol/cm3), C0 is the inlet concentration of CO2 (mmol/cm3), k is the rate coefficient (1/min), τ is the time at 50% breakthrough (min), and t is the breakthrough time (min). Adsorption–desorption cyclic tests were performed to evaluate the regeneration of the adsorbents. A total of 10 successive breakthrough experiments were conducted.

3. Results and Discussion

3.1. FESEM Images

In order to ensure that carbonization at 900 °C for 1 h was an appropriate process to cause the thermal decomposition of PMMA, the FESEM images were observed for the carbonized samples, as shown in Figure 1. These images clearly demonstrate the formation of hollow tubular structures for PANh15 (Figure 1a) and PANh12 (Figure 1b). Figure 1c is the cross-section of PANp, which displays several pores that were well distributed in the nanofibers. Since the pores were small and dispersed, a high magnification was needed to clearly identify the pores. These images show that the PMMA in the core or in the fibers experienced a variety of intrinsic thermal degradation processes, such as depolymerization, random scission, and side-group elimination, and finally formed volatile degradation products [19].
The surface morphology of all samples is illustrated in Figure 2A–D and their cross-sections are shown in Figure 2a–d. The nanofibers were randomly distributed with uniform sizes and little directionality. PANf was prepared using coaxial electrospinning with the same core and shell solutions. However, the resultant nanofibers were merged without demarcations. Although the surface of nanofibers in a lower magnification was smooth, the surface of nanofibers was, in fact, uneven (Figure 2a–d), especially for PANp. This evidently indicates that the evaporation of volatile compounds from PMMA and PAN in the carbonization and activation stages generated pores on the wall or fibers. The diameters of PANf and PANp from Figure 2a,d were approximately 500 and 900 nm, and the outer diameters of PANh15 (Figure 2b) and PANh12 (Figure 2c) were approximately 800 and 870 nm with a shell thickness of 77 and 106 nm, respectively. The results imply that the volatile compounds from the thermal decomposition of PMMA were expected to escape from the longitudinal and lateral directions of the nanotubes. It is believed that the removal of PMMA retarded or hindered the fiber shrinkage such that the hollow fibers and PANp possessed larger fiber sizes. In addition, comparing PANh15 with PANh12, the larger applied voltage and injection rates of polymers produced smaller fiber sizes and shell thickness. Figure 2d indicates that PMMA and PAN in copolymer solution were uniformly distributed during the electrospinning process.

3.2. ASAP Data

Figure 3a shows the N2 adsorption–desorption isotherms of all the samples at –196 °C. The adsorption isotherms for PANf, PANh15, and PANh12 were essentially type I according to the Brunauer–Emmett–Teller (BET) classification, and the desorption branch almost superimposed on the adsorption branch, which is indicative of microporosity. However, PANp exhibited a different pattern, in which the adsorption isotherm represented type IV features with a distinct hysteresis loop at a relative pressure between 0.42 and 1.0. This hysteresis loop was identified as H3 according to the International Union of Pure and Applied Chemistry (IUPAC) classification, indicating the existence of mesoporosity and microporosity. The pore size distributions in the 0.4–2 nm and 5–20 nm ranges are shown in Figure 3b,c, respectively, which were derived from the NLDFT model. The main micropores for all samples were at approximately 0.6 nm, and a peak occurring at 0.4–0.5 nm was also found on PANf and PANh15. Additionally, a large peak at around 0.6 nm was observed on PANh12. The above were classified as ultramicropores (pore size less than 0.7 nm). It is noted that PANp had significant pore volumes at 5–20 nm, in response to the hysteresis loop in the N2 isotherms.
Table 1 summarizes the surface features of the samples determined from the N2 adsorption–desorption isotherms. The BET specific surface areas (SSAs) of PANf, PANh15, PANh12, and PANp were 733, 1222, 884, and 825 m2/g. The micropore and ultramicropore volumes both followed the order PANh15 > PANh12 > PANp > PANf, though the total pore volume of PANh12 was less than that of PANp. The ratios of surface areas and pore volumes obtained from the N2 adsorption–desorption data at –196 °C for all samples are shown in Figure 4. PANp held a large amount of mesopore. Despite PANf having a smaller surface area and pore volume, its microporosity was conspicuous.

3.3. XPS Data

PAN is characterized with the C N group. In order to understand the change of nitrogen-containing functional groups undergoing subsequent electrospinning, stabilization, carbonization, and activation processes, XPS was conducted to explore the surface elemental compositions and their chemical states. The XPS survey scan spectra of the samples indicated that the major peaks were due to the C 1s, N 1s, and O 1s photoelectrons. Figure 5 shows the atomic ratios of C 1s, N 1s, and O 1s of the samples. The atomic ratio of N 1s followed the order PANp > PANf > PANh15 > PANh12, which indicated that a larger amount of nitrogen enabled the loss of the hollow nanofibers in the manufacture processes.
The curve-fitting for the high resolution XPS N 1s spectra [38,39,40] for all the samples is shown in Figure 6. The N 1s spectra were decomposed into, at most, seven identified components. Table 2 displays the percentages of nitrogen-containing functional groups. The peak at 395.7 eV was the aromatic N-imines; the peak at 398.4 eV represented the pyridine-type N; the peak at 400.1 eV was the pyrrole or pyridone; the peak at 401.2 eV showed the quarternary N; the peak at 402.4 eV indicated the pyridine-N oxides; and the peak at 404 eV was the shake-up satellites. The contribution of chemisorbed NO2 was assigned at 405 eV. PANf and PANh15 had a higher percentage of the pyrrole or pyridone (400.1 eV) and pyridine-type N (398.4 eV), while the pyridine-type N (398.4 eV) and the quarternary N (401.2 eV) were predominant on PANh12 and PANp. In summary, PANh15 had the highest percentage of pyrrole or pyridone of the five-member or six-member rings, and the pyridine-type N groups of the six-member rings were the primary functional groups on the others. In addition, PANh12 showed a higher percentage of the quarternary N and pyridine-N oxides in comparison with the others.

3.4. CO2 Adsorption Equilibrium

The adsorption equilibrium isotherms of CO2 on all samples at different temperatures (25, 40, and 55 °C) are shown in Figure 7. With increasing pressure and a decreasing temperature, the CO2 adsorbed amounts increased. This demonstrated that CO2 adsorption at 25 to 55 °C on the samples was exothermic. At 25 °C and 1 atm, the adsorption amounts of CO2 on PANf, PANh15, PANh12, and PANp were 2.95, 3.04, 3.16, and 2.86 mmol/g, respectively, which were superior to that of commercial activated carbon fibers with a fiber size of approximately 6.8 μm (1.92 mmol/g) [41]. The CO2 uptake at 25 °C and 0.15 atm (a typical untreated flue gas composition) followed the order PANf (0.97 mmol/g) > PANh12 (0.94 mmol/g) > PANp (0.88 mmol/g) > PANh15 (0.86 mmol/g). These data are also shown in Table 1. Table 3 summarizes the CO2 adsorption amounts in this work with various related adsorbents in the literature. Compared with our previous studies, the carbonization temperature in this work was higher in order to completely remove the PMMA. It is believed that the carbonization temperature was too high to get a high CO2 uptake.
The Qst values changing with the CO2 loading (0.2 to 1.2 mmol/g) are shown in Figure 8, where the Qst values log-linearly decreased with the CO2 loading. This phenomenon implies that the active sites on the surface of ACNFs were energetically heterogeneous for CO2 adsorption [42]. In addition, the enhanced micropore confinement or the interactions between CO2 molecules and the nitrogen-containing functional groups [43] could be responsible for the higher Qst values at a lower CO2 loading. According to the Qst values, almost lower than 40 kJ/mole, it was indicative of a typical physical adsorption for the CO2 adsorption on these adsorbents.
In addition, in investigating the important properties of adsorbents for the CO2 adsorption capacity, it was observed that the CO2 uptake at 0.15 atm had high correlation coefficients with chemisorbed NO2 and the ratio of V< 0.7 nm to Vt using the Pearson correlation analysis. Moreover, the CO2 uptake at 1 atm was highly related to pyridine-N oxides and the ratio of Vmi to Vt.

3.5. CO2 Adsorption Breakthrough Curves

Figure 9 shows the adsorption breakthrough curves of CO2 at different temperatures on the samples. The CO2 concentration was 15%. The Yoon and Nelson equation (Equation (2)) was adopted for breakthrough data fitting, which could predict the whole breakthrough curve. The fitting results are listed in Table 4 and also plotted in Figure 9. The values of R-squared suggest that the Yoon and Nelson equation fitted the data well in the whole range. The adsorption breakthrough wave was not sharp for PANf (at 25 °C) and PANh15 (at 25 and 40 °C), which could account for the larger pore diffusion resistance [50] due to smaller nanofiber sizes or a large micropore volume. This feature was in relation to the values of the rate coefficient, k’. The rate coefficients in this work did not exhibit large variations. Moreover, the highest rate coefficient took place on the curves at 40 °C except for PANh15, which implies that the pore diffusion resistance was weak at 40 °C. In order to determine the regeneration of these samples, PANh15 was selected as an example to carry out the adsorption–desorption runs 10 times. Successive cyclic adsorption breakthrough curves and the variation of time at C/C0 = 0.1 and 0.5 are shown in Figure 10. The data demonstrates that after 10 adsorption–desorption cyclic tests, this adsorbent maintained its CO2 adsorption capacities without appreciable degradation.

4. Conclusions

This study successfully fabricated hollow ACNFs and porous ACNFs using the electrospinning technique. The ACNFs with different pore structures displayed distinctive features of N2 isotherms. The carbonization at 900 °C was appropriate to completely decompose and remove the PMMA, but a high carbonization temperature decreases the CO2 uptake, compared with previous studies. The solid ACNFs exhibited the highest microporosity, while the hollow ACNFs and porous ACNFs displayed higher specific surface areas than that of the solid ACNFs. The CO2 adsorption of the ACNFs was an exothermic reaction, and the performance was highly related to the surface features and the nitrogen groups. The Yoon and Nelson equation could be adopted to fit well with the CO2 adsorption breakthrough data. The cyclic tests demonstrated that the breakthrough points in the curves were almost unchanged after 10 adsorption–desorption runs, which indicates that the hollow ACNFs are promising adsorbents. These ACNFs exhibited a good CO2 adsorption capacity and an excellent cyclic operation performance. These are the keys to CO2 capture in industrial applications.

Author Contributions

Conceptualization, Y.-C.C.; methodology, Y.-C.C.; software, C.-C.H.; validation, Y.-C.C.; investigation, W.-T.C.; data curation, C.-C.H. and W.-T.C.; writing—original draft preparation, Y.-C.C.; writing—review and editing, Y.-C.C.; visualization, Y.-C.C.; supervision, Y.-C.C.; project administration, Y.-C.C.; funding acquisition, Y.-C.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Ministry of Science and Technology, Taiwan, grant numbers MOST 107-2221-E-155-002- and MOST 108-2221-E-155-038-.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author. The data are not publicly available due to privacy restrictions.

Acknowledgments

The authors would like to thank the Instrumentation Center at NTU for performing the FESEM and EA analyses, the Department of Chemical Engineering at NTU for performing the N2 adsorption–desorption analysis, and the Instrumentation Center at NTHU for performing the XPS analysis.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Huang, Z.M.; Zhang, Y.Z.; Kotaki, M.; Ramakrishna, S. A review on polymer nanofibers by electrospinning and their applications in nanocomposites. Compos. Sci. Technol. 2003, 63, 2223–2253. [Google Scholar] [CrossRef]
  2. Nasouri, K.; Shoushtari, A.M.; Kaflou, A. Investigation of polyacrylonitrile electrospun nanofibres morphology as a function of polymer concentration, viscosity and Berry number. Micro Nano Lett. 2012, 7, 423–426. [Google Scholar] [CrossRef]
  3. Ondarçuhu, T.; Joachim, C. Drawing a single nanofiber over hundreds of microns. Eur. Phys. Lett. 1998, 42, 215–220. [Google Scholar] [CrossRef]
  4. Yang, X.; Liu, Y.; Li, J.; Zhang, X. Influence of thermal decomposition on morphologies and magnetic properties of iron nanofibres via electrospinning. Micro Nano Lett. 2011, 6, 967–970. [Google Scholar] [CrossRef]
  5. Xing, X.; Wang, Y.; Li, B. Nanofiber drawing and nanodevice assembly in poly(trimethylene terephthalate). Opt. Express 2008, 16, 10815–10822. [Google Scholar] [CrossRef]
  6. Feng, L.; Li, S.H.; Li, H.J.; Zhai, J.; Song, Y.; Jiang, L.; Zhu, D. Super hydrophobic surface of aligned polyacrylonitrile nanoflbers. Angew. Chem. Int. Edit. 2002, 41, 1221–1223. [Google Scholar] [CrossRef]
  7. Martín, J.; Maiz, J.; Sacristan, J.; Mijangos, C. Tailored polymer-based nanorods and nanotubes by “template synthesis”: From preparation to applications. Polymer 2012, 53, 1149–1166. [Google Scholar] [CrossRef] [Green Version]
  8. Ma, P.X.; Zhang, R. Synthetic nano-scale fibrous extracellular matrix. J. Biomed. Mater. Res. 1999, 46, 60–72. [Google Scholar] [CrossRef] [Green Version]
  9. Liu, G.; Ding, J.; Qiao, L.; Guo, A.; Dymov, B.P.; Gleeson, J.T.; Hashimoto, T.; Saijo, K. Polystyrene-block-poly(2-cinnamoylethyl methacrylate) nanofibers preparation, characterization, and liquid crystalline properties. Chem. Eur. J. 1999, 5, 2740–2749. [Google Scholar] [CrossRef]
  10. Wang, J.; Ouyang, Z.; Ren, Z.; Li, J.; Zhang, P.; Wei, G.; Su, Z. Self-assembled peptide nanofibers on graphene oxide as a novel nanohybrid for biomimetic mineralization of hydroxyapatite. Carbon 2015, 89, 20–30. [Google Scholar] [CrossRef]
  11. Doshi, J.; Reneker, D.H. Electrospinning process and applications of electrospun fibers. J. Electrostat. 1995, 35, 151–160. [Google Scholar] [CrossRef]
  12. Zhang, L.; Aboagye, A.; Kelkar, A.; Lai, C.; Fong, H. A review: Carbon nanofibers from electrospun polyacrylonitrile and their applications. J. Mater. Sci. 2014, 49, 463–480. [Google Scholar] [CrossRef]
  13. Greiner, A.; Wendorff, J.H. Electrospinning: A fascinating method for the preparation of ultrathin fibers. Angew. Chem. Int. Ed. 2007, 46, 5670–5703. [Google Scholar] [CrossRef]
  14. Ahmadian, A.; Shafiee, A.; Aliahmad, N.; Agarwal, M. Overview of nano-fiber mats fabrication via electrospinning and morphology analysis. Textiles 2021, 1, 206–226. [Google Scholar] [CrossRef]
  15. Koski, A.; Yim, K.; Shivkumar, S. Effect of molecular weight on fibrous PVA produced by electrospinning. Mater. Lett. 2004, 58, 493–497. [Google Scholar] [CrossRef]
  16. Gupta, P.; Elkins, C.; Long, T.E.; Wilkes, G.L. Electrospinning of linear homopolymers of poly(methyl methacrylate): Exploring relationships between fiber formation, viscosity, molecular weight and concentration in a good solvent. Polymer 2005, 46, 4799–4810. [Google Scholar] [CrossRef]
  17. Shenoy, S.L.; Bates, W.D.; Frisch, H.L.; Wnek, G.E. Role of chain entanglements on fiber formation during electrospinning of polymer solutions: Good solvent, non-specific polymer–polymer interaction limit. Polymer 2005, 46, 3372–3384. [Google Scholar] [CrossRef]
  18. Hsu, C.M.; Shivkumar, S. Nano-sized beads and porous fiber constructs of poly(1′-caprolactone) produced by electrospinning. J. Mater. Sci. 2004, 39, 3003–3013. [Google Scholar] [CrossRef]
  19. Zussman, E.; Yarin, A.L.; Bazilevsky, A.V.; Avrahami, R.; Feldman, M. Electrospun polyacrylonitrile/poly(methyl methacrylate)-derived turbostratic carbon micro-/nanotubes. Adv. Mater. 2006, 18, 348–353. [Google Scholar] [CrossRef]
  20. Xie, W.; Khan, S.; Rojas, O.J.; Parsons, G.N. Control of micro- and mesopores in carbon nanofibers and hollow carbon nanofibers derived from cellulose diacetate via vapor phase infiltration of diethyl zinc. ACS Sustain. Chem. Eng. 2018, 6, 13844–13853. [Google Scholar] [CrossRef]
  21. Zhang, L.; Hsieh, Y.L. Carbon nanofibers with nanoporosity and hollow channels from binary polyacrylonitrile systems. Eur. Polym. J. 2009, 45, 47–56. [Google Scholar] [CrossRef]
  22. Kaerkitcha, N.; Chuangchote, S.; Sagawa, T. Control of physical properties of carbon nanofibers obtained from coaxial electrospinning of PMMA and PAN with adjustable inner/outer nozzle-ends. Nanoscale Res. Lett. 2016, 11, 186. [Google Scholar] [CrossRef] [Green Version]
  23. Gbewonyo, S.; Carpenter, A.W.; Gause, C.B.; Mucha, N.R.; Zhang, L. Low thermal conductivity carbon fibrous composite nanomaterial enabled by multi-scale porous structure. Mater. Des. 2017, 134, 218–225. [Google Scholar] [CrossRef]
  24. Zhou, Z.; Liu, T.; Khan, A.U.; Liu, G. Block copolymer–based porous carbon fibers. Sci. Adv. 2019, 55, 6852. [Google Scholar] [CrossRef] [Green Version]
  25. Qu, H.; Wei, S.; Guo, Z. Coaxial electrospun nanostructures and their applications. J. Mater. Chem. A 2013, 1, 11513–11528. [Google Scholar] [CrossRef]
  26. El-Deen, A.G.; Barakat, N.A.M.; Khalild, K.A.; Kim, H.Y. Hollow carbon nanofibers as an effective electrode for brackish water desalination using the capacitive deionization process. New J. Chem. 2014, 38, 198–205. [Google Scholar] [CrossRef]
  27. Park, S.H.; Jung, H.R.; Lee, W.J. Hollow activated carbon nanofibers prepared by electrospinning as counter electrodes for dye-sensitized solar cells. Electrochim. Acta 2013, 102, 423–428. [Google Scholar] [CrossRef]
  28. Wu, Y.; Gao, M.; Li, X.; Liu, Y.; Pan, H. Preparation of mesohollow and microporous carbon nanofiber and its application in cathode material for lithium–sulfur batteries. J. Alloy. Compd. 2014, 608, 220–228. [Google Scholar] [CrossRef]
  29. Peng, Y.T.; Lo, C.T. Electrospun porous carbon nanofibers as lithium ion battery anodes. J. Solid State Electrochem. 2015, 19, 3401–3410. [Google Scholar] [CrossRef]
  30. Zhang, T.; Qu, H.; Sun, K. Development of polydopamine coated electrospun PAN/PMMA nanofibrous membrane as composite separator for Lithium-ion batteries. Mater. Lett. 2019, 245, 10–13. [Google Scholar] [CrossRef]
  31. Zhao, W.; Yamamoto, Y.; Tagawa, S. Regulation of the thermal reactions of polyacrylonitrile by c-irradiation. Chem. Mater. 1999, 11, 1030–1034. [Google Scholar] [CrossRef]
  32. Qin, X.H. Structure and property of electrospinning PAN nanofibers by different preoxidation temperature. J. Therm. Anal. Calorim. 2010, 99, 571–575. [Google Scholar] [CrossRef]
  33. Lee, J.S.; Kim, J.H.; Kim, J.T.; Suh, J.K.; Lee, J.M.; Lee, C.H. Adsorption equilibria of CO2 on zeolite 13X and zeolite X/activated carbon composite. J. Chem. Eng. Data 2002, 47, 1237–1242. [Google Scholar] [CrossRef]
  34. ASTM D5160-95. Standard Guide for Gas.-Phase Adsorption Testing of Activated Carbon; ASTM International: West Conshohocken, PA, USA, 2019. [Google Scholar]
  35. Granite, E.J.; Pennline, H.W. Photochemical removal of mercury from flue gas. Ind. Eng. Chem. Res. 2002, 41, 5470–5476. [Google Scholar] [CrossRef]
  36. Chou, C.T.; Chen, C.Y. Carbon dioxide recovery by vacuum swing adsorption. Sep. Purif. Technol. 2004, 39, 51–65. [Google Scholar] [CrossRef]
  37. Huang, Z.H.; Kang, F.; Liang, K.M.; Hao, J. Breakthrough of methyethylketone and benzene vapors in activated carbon fiber beds. J. Hazard. Mater. B 2003, 98, 107–115. [Google Scholar] [CrossRef]
  38. Biniak, S.; Szymanski, G.; Siedlewski, J.; Swiatkowski, A. The characterization of activated carbons with oxygen and nitrogen surface groups. Carbon 1997, 35, 1799–1810. [Google Scholar] [CrossRef]
  39. Pamula, E.; Rouxhet, P.G. Bulk and surface chemical functionalities of Type III PAN-based carbon fibers. Carbon 2003, 41, 1905–1915. [Google Scholar] [CrossRef]
  40. Raymundo-Pinero, E.; Cazorla-Amoros, D.; Linares-Solano, A. The role of different nitrogen functional groups on the removal of SO2 from flue gases by N-doped activated carbon powders and fibers. Carbon 2003, 41, 1925–1932. [Google Scholar] [CrossRef]
  41. Chiang, Y.C.; Hsu, W.L.; Lin, S.Y.; Juang, R.S. Enhanced CO2 adsorption on activated carbon fibers grafted with nitrogen-doped carbon nanotubes. Materials 2017, 10, 511. [Google Scholar] [CrossRef]
  42. Toth, J. Isotherm equations for monolayer adsorption of gases on heterogeneous solid surfaces. In Fundamentals of Adsorption; Myers, A., Belfort, G., Eds.; Engineering Foundation: New York, NY, USA, 1984; pp. 657–665. [Google Scholar]
  43. To, J.W.F.; He, J.; Mei, J.; Haghpanah, R.; Chen, Z.; Kurosawa, T. Hierarchical N-doped carbon as CO2 adsorbent with high CO2 selectivity from rationally designed polypyrrole precursor. J. Am. Chem. Soc. 2016, 38, 1001–1009. [Google Scholar] [CrossRef]
  44. Chiang, Y.C.; Lee, S.T.; Leo, Y.J.; Tseng, T.L. Importance of pore structure and surface chemistry in carbon dioxide adsorption on electrospun carbon nanofiber. Sens. Mater. 2020, 32, 2277–2288. [Google Scholar]
  45. Xiong, L.; Wang, X.F.; Li, L.; Jin, L.; Zhang, Y.G.; Song, S.L.; Liu, R.P. Nitrogen-enriched porous carbon fiber as CO2 adsorbent with superior CO2 selectivity by air activation. Energy Fuels 2019, 33, 12558–12567. [Google Scholar] [CrossRef]
  46. Heo, Y.J.; Zhang, Y.; Rhee, K.Y.; Park, S.J. Synthesis of PAN/PVDF nanofiber composites-based carbon adsorbents for CO2 capture. Composites B 2019, 156, 95–99. [Google Scholar] [CrossRef]
  47. Jeong, D.; Jie, W.; Adelodun, A.A.; Kim, S.; Jo, Y. Electrospun melamine-blended activated carbon nanofibers for enhanced control of indoor CO2. J. Appl. Polym. Sci. 2019, 136, 47747. [Google Scholar] [CrossRef]
  48. Ojeda-López, R.; Esparza-Schulz, J.M.; Pérez-Hermosillo, I.J.; Hernández-Gordillo, A.; Domínguez-Ortiz, A. Improve in CO2 and CH4 adsorption capacity on carbon microfibers synthesized by electrospinning of PAN. Fibers 2019, 7, 81. [Google Scholar] [CrossRef] [Green Version]
  49. Chiang, Y.C.; Wu, C.Y.; Chen, Y.J. Effects of activation on the properties of electrospun carbon nanofibers and their adsorption performance for carbon dioxide. Sep. Purif. Technol. 2020, 233, 116040. [Google Scholar] [CrossRef]
  50. Brasquet, C.; Cloirec, P.L. Adsorption onto activated carbon fibers: Applications to water and air treatments. Carbon 1997, 35, 1307–1313. [Google Scholar] [CrossRef]
Figure 1. FESEM images of the carbonized samples of: (a) PANh15; (b) PANh12; (c) PANp.
Figure 1. FESEM images of the carbonized samples of: (a) PANh15; (b) PANh12; (c) PANp.
Applsci 11 07724 g001
Figure 2. FESEM images of the ACNFs: (A,a) PANf; (B,b) PANh15; (C,c) PANh12; (D,d) PANp.
Figure 2. FESEM images of the ACNFs: (A,a) PANf; (B,b) PANh15; (C,c) PANh12; (D,d) PANp.
Applsci 11 07724 g002
Figure 3. N2 adsorption–desorption data at −196 °C for the ACNFs: (a) isotherms; (b) pore size distributions (0.4–2 nm); (c) pore size distributions (5–20 nm).
Figure 3. N2 adsorption–desorption data at −196 °C for the ACNFs: (a) isotherms; (b) pore size distributions (0.4–2 nm); (c) pore size distributions (5–20 nm).
Applsci 11 07724 g003
Figure 4. The ratios of surface areas and pore volumes obtained from N2 adsorption–desorption data at −196 °C for all samples.
Figure 4. The ratios of surface areas and pore volumes obtained from N2 adsorption–desorption data at −196 °C for all samples.
Applsci 11 07724 g004
Figure 5. The atomic ratios of C 1s, N 1s, and O 1s obtained from the X-ray photoelectron spectroscopy (XPS) of the samples.
Figure 5. The atomic ratios of C 1s, N 1s, and O 1s obtained from the X-ray photoelectron spectroscopy (XPS) of the samples.
Applsci 11 07724 g005
Figure 6. Results of the fits of the high resolution X-ray photoelectron spectroscopy (XPS) N 1s region: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp. The values were given in atomic ratio (%) of total intensity.
Figure 6. Results of the fits of the high resolution X-ray photoelectron spectroscopy (XPS) N 1s region: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp. The values were given in atomic ratio (%) of total intensity.
Applsci 11 07724 g006
Figure 7. Adsorption isotherms of CO2 of the ACNFs: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp.
Figure 7. Adsorption isotherms of CO2 of the ACNFs: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp.
Applsci 11 07724 g007
Figure 8. The isosteric heat of adsorption of CO2 on the samples.
Figure 8. The isosteric heat of adsorption of CO2 on the samples.
Applsci 11 07724 g008
Figure 9. Adsorption breakthrough curves of CO2 at different temperatures on the samples: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp. The lines are the fitted results using the Yoon and Nelson equation.
Figure 9. Adsorption breakthrough curves of CO2 at different temperatures on the samples: (a) PANf; (b) PANh15; (c) PANh12; (d) PANp. The lines are the fitted results using the Yoon and Nelson equation.
Applsci 11 07724 g009
Figure 10. (a) Successive cyclic adsorption breakthrough curves, and (b) the variation of time at C/C0 = 0.1 and 0.5.
Figure 10. (a) Successive cyclic adsorption breakthrough curves, and (b) the variation of time at C/C0 = 0.1 and 0.5.
Applsci 11 07724 g010
Table 1. Surface feature of the samples determined from N2 adsorption–desorption isotherms.
Table 1. Surface feature of the samples determined from N2 adsorption–desorption isotherms.
SampleSSA α
(m2/g)
Smi β
(m2/g)
Vt γ
(cm3/g)
Vma φ
(cm3/g)
Vme η
(cm3/g)
Vmi η
(cm3/g)
V<0.7 nm η
(cm3/g)
rp ξ
(nm)
q C O 2 φ (mmol/g)
at 25 °C
0.15 atm1 atm
PANf7336170.36160.01250.01060.33850.22270.4570.972.95
PANh1512229960.71210.04850.10380.55980.35580.4760.863.04
PANh128847090.48400.02990.04900.40500.26650.5030.943.16
PANp8256240.62930.02560.24150.36220.24290.7350.882.86
α SSA (specific surface area) was determined using the BET method. β Smi was determined using the t-plot method. γ Vt represented the single point total pore volume at P/Po ≈ 0.99. η Vme, Vmi, and V< 0.7 nm were determined using a non-local density functional theory (NLDFT) model. φ Vma was obtained by subtraction. ξ rp (average pore hydraulic radius) was determined using the micropore analysis (MP) method. ϕ qCO2 was the CO2 amount adsorbed on the samples determined using the ASAP2020 at 0.15 and 1 atm (298 K).
Table 2. Results of the fits of the XPS N1s region, values shown at. % of total intensity.
Table 2. Results of the fits of the XPS N1s region, values shown at. % of total intensity.
SampleBinding Energy (eV)
395.7398.4400.1401.2402.4404405
Aromatic
N-imines
Pyridine
-Type N
Pyrrole or
Pyridone
Quarternary NPyridine-
N oxides
Shake-Up
Satellites
NO2
PANf21.820.518.410.31.227.8
PANh158.020.629.116.711.913.7
PANh120.337.27.722.414.218.2
PANp6.232.215.319.59.42.814.7
Table 3. Comparisons of CO2 uptakes on the adsorbents in this study with various support materials using electrospinning in the literature.
Table 3. Comparisons of CO2 uptakes on the adsorbents in this study with various support materials using electrospinning in the literature.
AdsorbentPrecursorSSA (m2/g)Conc. of CO2Temp. (°C)CO2 Uptake (mmol/g)Reference
Hollow ACNFs αPAN8841 atm
0.15 atm
253.16
0.94
This study
ACNFsPAN8721 atm
0.15 atm
253.47
1.01
[44]
CNFs βPAN3061 atm
0.15 atm
252.52
1.11
[44]
ACNFsPAN4861 bar
0.15 bar
252.25
1.09
[45]
CNFsPAN121 bar250.55[46]
ACNFsPAN, polyvinylidene
fluoride
9251 bar252.21[46]
ACNFsPAN4121 bar250.92[47]
ACNFsPAN
Melamine
5471 bar251.44[47]
CNFsPAN9661 bar252.9[48]
ACNFsPAN8971 atm
0.15 atm
253.17
1.00
[49]
ACFs γPAN9661 atm252.33[41]
α ACNFs: activated carbon nanofibers; β CNFs: carbon nanofibers; γ ACFs: activated carbon fibers.
Table 4. Fitted parameters of the Yoon and Nelson equation for the CO2 adsorption breakthrough data on the samples at different temperatures.
Table 4. Fitted parameters of the Yoon and Nelson equation for the CO2 adsorption breakthrough data on the samples at different temperatures.
SampleTemp. (°C)τ (min)K′ (1/min)R2
PANf2516.400.5530.99009
4014.070.9040.99453
5510.520.6550.99294
PANh152513.010.5470.99352
4011.040.5150.99093
558.870.7790.99147
PANh122513.170.8950.99363
4010.540.9180.99206
558.140.8270.98918
PANp2519.650.9770.99107
4017.341.0570.99462
5514.800.9800.98692
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Chiang, Y.-C.; Huang, C.-C.; Chin, W.-T. Carbon Dioxide Adsorption on Carbon Nanofibers with Different Porous Structures. Appl. Sci. 2021, 11, 7724. https://doi.org/10.3390/app11167724

AMA Style

Chiang Y-C, Huang C-C, Chin W-T. Carbon Dioxide Adsorption on Carbon Nanofibers with Different Porous Structures. Applied Sciences. 2021; 11(16):7724. https://doi.org/10.3390/app11167724

Chicago/Turabian Style

Chiang, Yu-Chun, Chih-Cheng Huang, and Wei-Ting Chin. 2021. "Carbon Dioxide Adsorption on Carbon Nanofibers with Different Porous Structures" Applied Sciences 11, no. 16: 7724. https://doi.org/10.3390/app11167724

APA Style

Chiang, Y. -C., Huang, C. -C., & Chin, W. -T. (2021). Carbon Dioxide Adsorption on Carbon Nanofibers with Different Porous Structures. Applied Sciences, 11(16), 7724. https://doi.org/10.3390/app11167724

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop