Next Article in Journal
Data Hiding and Its Applications: Digital Watermarking and Steganography
Next Article in Special Issue
A Porous Tungsten Substrate for Catalytic Reduction of Hydrogen by Dealloying of a Tungsten–Rhenium Alloy in an Aqueous Solution of Hydrochloric Acid
Previous Article in Journal
On the Spectral Efficiency for Distributed Massive MIMO Systems
Previous Article in Special Issue
Using the Instrumented Indentation Technique to Determine Damage in Sintered Metal Matrix Composites after High-Temperature Deformation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Electrochemical Synthesis of Nano-Sized Silicon from KCl–K2SiF6 Melts for Powerful Lithium-Ion Batteries

1
Scientific Laboratory of the Electrochemical Devices and Materials, Ural Federal University, Mira St. 28, 620002 Yekaterinburg, Russia
2
Institute of High-Temperature Electrochemistry, Ural Branch, The Russian Academy of Sciences, Academicheskaya St. 20, 620137 Yekaterinburg, Russia
*
Author to whom correspondence should be addressed.
Appl. Sci. 2021, 11(22), 10927; https://doi.org/10.3390/app112210927
Submission received: 25 October 2021 / Revised: 12 November 2021 / Accepted: 16 November 2021 / Published: 19 November 2021

Abstract

:
Currently, silicon and silicon-based composite materials are widely used in microelectronics and solar energy devices. At the same time, silicon in the form of nanoscale fibers and various particles morphology is required for lithium-ion batteries with increased capacity. In this work, we studied the electrolytic production of nanosized silicon from low-fluoride KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts. The effect of SiO2 addition on the morphology and composition of electrolytic silicon deposits was studied under the conditions of potentiostatic electrolysis (cathode overvoltage of 0.1, 0.15, and 0.25 V vs. the potential of a quasi-reference electrode). The obtained silicon deposits were separated from the electrolyte residues, analyzed by scanning electron microscopy and spectral analysis, and then used to fabricate a composite Si/C anode for a lithium-ion battery. The energy characteristics of the manufactured anode half-cells were measured by the galvanostatic cycling method. Cycling revealed better capacity retention and higher coulombic efficiency of the Si/C composite based on silicon synthesized from KCl–K2SiF6–SiO2 melt. After 15 cycles at 200 mA·g−1, material obtained at 0.15 V overvoltage demonstrates capacity of 850 mAh·g−1.

1. Introduction

Currently, silicon and silicon-based composite materials are widely used in microelectronics, solar energy devices, as well as in the manufacture of portable energy storage devices [1,2,3]. In particular, a new lithium-ion battery (LIB) with a silicon-based anode is being actively developed. The theoretical capacity of such an anode (4200 mAh·g−1) is an order of magnitude higher than the widely used graphite anode [3,4]. However, during cycling, silicon is subject to huge volumetric expansion (up to 400% [5]), which leads to mechanical destruction of the electrode and significant loss of the original capacity. To avoid this, it is recommended to use anodes based on nanosized silicon particles. Nanosized silicon cannot be obtained by the existing methods of the carbothermal reduction of quartz to silicon with subsequent purification of the silicon by hydrogenation–dehydrogenation [6]. The use of nanosized silicon particles, mainly fibers and tubes within composite materials, can significantly reduce the problem of volumetric expansion. Suitable polymer binders also reduce mechanical degradation of the electrode, but they do not affect the silicon expansion [7,8]. Another method that can improve silicon’s performance is the coating (mainly carbon based) of silicon particles and creation of a “core-shell” structure [9,10]. Doped silicon anodes have also shown improved electrochemical performance and cyclic resistance in comparison with pure silicon [11,12,13].
Methods for preparing silicon nanofibers can be divided into two groups. The first group comprises methods based on removing excess material-laser ablation [14], ion etching [15], chemical etching [16,17]. These methods allow one to obtain high-purity components with the required sizes. However, they require expensive equipment, catalysts (gold is most often used) and are poorly suited for industrial scale production. The second group of methods includes silicon deposition on the substrates. Among these, the most commonly used method is the vapor–liquid–crystal deposition [18,19]. Silane is usually used as a source of silicon. The disadvantages of these methods also include the use of gold as a catalyst and the difficulty in scaling and hardware design of the process. To obtain silicon suitable for microelectronics, several stages of purification are needed, one of which is represented by a group of methods based on zone crystallization from molten silicon [20].
One of the cheapest and promising methods for producing nanosized silicon is electrolytic reduction from molten salts. To date, many studies have been carried out aimed at the electrolytic production of silicon from various molten electrolytes with K2SiF6, Na2SiF6, SiO2, and SiCl4 additives in a temperature range mainly from 550 °C to 750 °C [21,22,23,24,25,26,27,28,29,30,31,32,33,34,35,36,37,38,39]. All these studies show the fundamental possibility of using electroreduction for the production of silicon deposits of various morphologies, including continuous coatings up to 1 mm thick, submicron films (0.5–1 μm), micro-sized dendrites, nano- and micro-sized disordered fibers.
One of the most promising electrolytes for silicon production is the KCl–KF melt with a KF molar fraction of up to 66% [27,28,29,30,31], which is a good solvent for K2SiF6 and SiO2 and is water soluble. However, this system also has a number of disadvantages, including relatively high aggressiveness of KF to reactor materials, the need to remove impurities such as H2O and HF from KF when preparing a molten KCl–KF mixture, and a good solubility of oxides. Despite the positive results of the work performed, all of the above factors can impede the deposition of high-purity silicon, especially without oxygen inclusions.
To eliminate these drawbacks, alternative media with the reduced or zero fluoride content for the production of silicon are being investigated. In particular, this concerns the KCl–KI–KF–K2SiF6 [32,33] and CaCl2–CaO–SiO2 melts [34,35,36,37], although their use also implies the absence of moisture in the reactor and increased requirements for the preparation of molten electrolytes and instrumentation. In previous works, we have shown the fundamental possibility of obtaining nanosized silicon fibers by electrolytic refining of silicon in a low-fluoride KCl–K2SiF6 system [38,39]. The advantage of this system is that its anionic composition virtually does not change. That provides stabilization of the energy characteristics of silicon-containing electroactive ions and possibility of controlling the morphology of silicon deposits. Preliminary electrolysis tests [38,39] show that it is difficult to obtain nanosized silicon deposits from molten salts. In particular, this is due to the varied concentration of silicon-containing ions in the melt, the semiconducting nature of silicon, and increased sensitivity of the deposit morphology to oxygen impurities.
Despite the active interest in Si-based anodes for LIBs [3,4,6,7,8,9,10,11,12,13,14,15,16,17,18,19,40], the works devoted to the utilization of electrolytic silicon deposits as the LIB anode material are limited [41,42,43,44,45,46]. The highest characteristics for silicon obtained by electrodeposition are on carbon cloth. The capacity was more than 1100 mAh·g−1 by the 200th cycle at a discharge current of 500 mA·g−1, while the silicon nanopowder itself, without the use of carbon fabric, demonstrates very low capacity—less than 500 mAh·g−1 by the 5th cycle and less than 200 mAh·g−1 by 200th cycle [40]. In recent years, most researchers are focused on silicon electrodeposition from CaCl2-based melts. In work [42] carried out by researchers from the USA and China, electrodeposited nanofibers in LIB demonstrate a capacity of 714 mAh·g−1 after 500 cycles at C/2 current. According to [45], China launched a large-scale test production of electrodeposited silicon with capacity more than 2000 mAh·g−1 after 70 cycles at a current of 0.1 C; capacity at a current of 5 C is about 1600 mAh·g−1. It is noted that for practical use of the produced silicon they made Si/graphite mixture with a total capacity of 650 mAh·g−1 [47].
In this regard, in this work, we studied the effect of SiO2 on the morphology of nanosized silicon deposits during the electrolysis of KCl–K2SiF6 melts. For this, silicon deposits were obtained from the KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts at different cathode overvoltage. Obtained deposits were analyzed and tested on their electrochemical characteristics as a part of an Si-based anode of a LIB.

2. Materials and Methods

Melt preparation. The investigated KCl electrolytes with additions of K2SiF6 and SiO2 were prepared by mixing individual salts of a chemically pure grade (Reakhim, Russia) and then melting them in a glassy carbon crucible immediately before the experiments. In a previous study [48], it was shown that the purity of KCl used is close to that of the recrystallized salt; therefore, additional purification of the prepared melt from electropositive impurities was not carried out. The K2SiF6 salt was preliminarily purified from oxygen impurities by HF fluorination. For this, K2SiF6 was mixed with NH4F and heated in stages to a temperature of 450 °C according to a previously described procedure [49]. SiO2 was added to the melt in an amount of 0.34 wt.%. The KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts were held for an hour at the operating temperature to establish equilibrium between silicon ions [50,51]. Then, the melt samples were taken for analysis, and electrolysis was started.
Experimental setup. Electrolysis tests were carried out in a sealed quartz retort with a high-purity argon atmosphere at a temperature of 790 °C (Figure 1). A glassy carbon crucible with the melt was placed at the bottom of the retort, which was hermetically closed with a fluoroplastic cap. The inner walls of the retort were additionally shielded with nickel plates to protect against fluorine-containing sublimates. Holes with fittings were made in the cap, in which a working electrode (glassy carbon), a glassy carbon counter electrode, and a silicon QRE were placed. In addition, holes were provided for an additional working electrode, thermocouple, and a tube for gas supply and loading of silicon-containing additives. During the experiments, the temperature was controlled within ±2 °C by a Pt/PtRh thermocouple and a thermocouple module USB-TC01 (National Instruments, Austin, TX, USA).
Electrochemical measurements and electrodeposition. To establish the effect of SiO2 on the kinetics of silicon electrodeposition, voltammograms were obtained by the cyclic chronovoltammetry. Before measurement, the electrodes were kept in the melt for 30 min to establish a stable (within ± 5 mV) potential difference between the working electrode and the quasi-reference electrode (QRE). In order to determine and compensate the ohmic voltage drop in the measuring circuit, impedance spectroscopy and current interruption (I-Interrupt) technique were used.
The electrodeposition of silicon was carried out on glassy carbon plates with an area of 2 cm2 at different cathode overvoltage for one hour. The electrolysis time was selected based on the results of preliminary electrolysis tests [24,25]. For electrochemical measurements and electrolysis, PGSTAT AutoLAB 302N with Nova 1.11 software (MetrOhm, Herisau, Switzerland) was used. Glassy carbon plates were used as anodes.
At the end of the electrolysis, the electrode was raised above the melt for 20–30 min in order to remove excess salts included in the cathode deposit. Then, the electrode was raised to the cold zone of the retort and, after cooling in an inert atmosphere, was removed.
Separation of the cathode deposit. The obtained silicon deposits were washed in acidic (HCl) water solution; the pH of the solution for washing varies in the range of 2 to 4. An ultrasonic homogenizer SONOPULS UW mini 20 was used to disperse the deposits. Dispersion was carried out in a periodic mode at a given power of 0.995 kJ with a pulse duration of 90 s. After washing, the deposits were dried in a vacuum oven at 80 °C for 18 h.
Analysis of the morphology and composition. The elemental composition of the melt and the obtained silicon deposits was analyzed by atomic emission spectroscopy with inductively coupled plasma (AES-ICP) using an iCAP 6300 Duo Spectrometer (Thermo Scientific, Waltham, MA, USA). The morphology and elemental composition of the obtained deposits were studied using a Tescan Vega 4 (Tescan, Kohoutovice, Czech Republic) scanning electron microscope with an Xplore 30 EDS detector (Oxford, UK).
Electrochemical performance. Silicon performance was investigated in a 3-electrode half-cell. The anode composition was 10 wt.% polyvinylidene difluoride dissolved in N-methyl-2-pyrollidone, 10 wt.% carbon black, and 80 wt.% silicon. LIB fabrication was performed in an argon-filled glove box (O2, H2O < 0.1 ppm). Stainless steel mesh with applied composite anode was used as the working electrode and two separate lithium strips as the counter and reference electrodes. All electrodes were divided by two layers of separator and tightly placed in the cell. The cell was flooded with 1 mL of electrolyte—1 M LiPF6 in a mixture of ethylene carbonate/dimethyl carbonate/diethyl carbonate (1:1:1 by volume). Cycling experiments were performed using a Zive-SP2 potentiostat (WonATech, Seoul, Korea).

3. Results

3.1. Electrolysis Test Results

According to ICP, the silicon contents in the KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts before electrolysis tests were 0.05 and 0.15 wt.%, respectively. The deposits were obtained at cathode overvoltage of 0.1, 0.15, and 0.25 V relative to the QRE potential. For the KCl–K2SiF6 melt (0.05 wt.% of silicon), the obtained deposits are shown in Figure 2. It can be seen that the growth of deposits occurs with the formation of silicon-salt mixtures. In this case, with a decrease in the cathode overvoltage, the deposits change color from gray to light brown. This can be associated both with a change in the crystalline structure of silicon to amorphous, and with a change in the size of silicon particles [31,38].
Electrolysis tests in the KCl–K2SiF6 melt with the addition of SiO2 (0.15 wt.% of silicon) at the same cathode overvoltages of 0.1, 0.15, and 0.25 V vs. QRE potential were performed. As a result, cathodic deposits were obtained, photographs of which are shown in Figure 3. It can be noted that during electrolysis of the melt with the addition of SiO2, more volumetrically uniform deposits are obtained, while the color of the precipitates remains the same in all tests.

3.2. Effect of SiO2 on the Morphology of Silicon Deposits

For more detailed analysis of the effect of SiO2 on the morphology of the silicon, SEM images were made. Figure 4 shows the corresponding micrographs of the deposits. It can be seen that in the KCl–K2SiF6 system, silicon was deposited in the form of disordered fibers with an average diameter of 300–400 nm, while the effect of cathode overvoltage on the morphology of the deposit is not clearly observed. Such a result is probably due to the limiting stage of the preceding chemical reaction of silicon-containing ion dissociation.
When SiO2 is added in the melt, silicon is predominantly deposited in the form of nano-sized tubes and needles, the length of which varies in the range of 30–60 μm, and the diameter varies in the range of 200 nm to 400 nm. This effect can be interpreted as the mutual influence of several factors:
(1)
a change in the composition of silicon-containing electroactive particles, namely the inclusion of oxygen atoms in their composition, leading to a decrease in binding energy of silicon atoms [51] and facilitation of the charge transfer stage;
(2)
a decrease in electrical conductivity (increase in resistance) of the near-cathode layer melt, which will redistribute the current lines among the cathode surface. Namely, silicon electrodeposition will occur at the tips of the deposit, rather than on the lateral surfaces;
(3)
a change in the composition of silicon-containing electroactive ions, as a result the ions activity and the rate constant of the possible preceding chemical reaction in the melt change.
Taking into account the weak effect of the cathode overvoltage on the morphology of silicon deposits, the effect of SiO2 addition can be associated with the last two factors. It can be noted that the average size of silicon particles decreases with the addition of SiO2 to the melt. A similar effect was observed in other works [31,41].
According to EDX analysis, the average oxygen content in the fibers obtained during the electrolysis of the KCl–K2SiF6 melt was 2.1–4.3 wt.%, and the average oxygen content in nano-sized tubes and needles obtained during the electrolysis of this melt with the addition of SiO2 was 2.7–5.1 wt.%. The appearance of oxygen in the deposits can be caused both by the use of a quartz retort as a reactor container and after-electrolysis silicon treatment. It is important to note that the addition of SiO2 does not significantly increase oxygen content in silicon deposits, which is important from the point of the electrochemical characteristics as the anode of LIB.

3.3. Effect of SiO2 on the Kinetics of Silicon Electrodeposition

To check the effect of SiO2 addition on the silicon electroreduction, voltammograms were recorded in the KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts at a temperature of 790 °C. Figure 5 shows that the electroreduction of silicon-containing electroactive ions from the KCl–K2SiF6 melt occurs at a potential more negative than 0.1 V, with the formation of a cathodic peak Si [27,32] at a potential of –0.1 V, relative to the QRE potential (Figure 5, black line).
For the SiO2-containing melt, additional Si-O cathode waves appeared on the voltammogram at the potentials of about 0.1 and 0 V relative to the QRE potential (Figure 5, red line). Those waves can be associated with the discharge of different oxygen-containing electroactive Si-O-Cl-F anions, which appear in the melt during SiO2 dissolution [50,51]. A similar effect was observed in the works, aimed at the electroreduction of silicon and other elements from halide-oxide melts [52,53,54]. In the KCl–K2SiF6–SiO2 melt, an increase of the silicon electroreduction current was observed, since the silicon content has been increased. In the anode region, peak Si′ and a wave (Si-O)′ at a potential of 0.1 and 0.33 V relative to the QRE potential were detected. We assume that the peak Si′ is associated with silicon dissolution [27,32], and the additional wave (Si-O)′ can be caused by oxidation of a reduced form of the silicon electroactive ion. To obtain a more detailed picture, further study of the cathodic process in KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts is required.

3.4. Electrochemical Characteristics of the Obtained Silicon Deposits

The obtained silicon deposits were studied as a composite Si/C anode for a lithium-ion battery. In the first charge/discharge cycle (Figure 6), the capacity of Si/C composite prepared on the base of silicon electrodeposited from KCl–K2SiF6 was between 1450 and 3000 mAh·g−1 during lithiation, and between 950 and 1670 mAh·g−1 during delithiation. Despite of the similar morphology and size of silicon fibers synthesized at different overpotentials, their energy characteristics are different. As can be seen from Figure 6, samples 2 and 3 synthesized at 0.15 and 0.25 V show similar charging times, although the initial period associated with electrolyte reduction and solid electrolyte interphase formation is quite different. Silicon synthesized at 0.1 V demonstrates 60% lower capacity, and the highest initial coulombic efficiency of 65.5%.
After 15 cycles at 200 mA·g−1 (Figure 7a), the capacitance for the best sample of silicon fibers was 750 mAh·g−1 for sample 3 synthesized at 0.25 V overvoltage. The coulombic efficiency of the anode half-cell with silicon fibers in this case increased from 59% up to 92%. Silicon synthesized at 0.15 V (sample 2) demonstrates a similar capacity fade rate as sample 3, but a lower overall capacity. However, these samples have different coulombic efficiency during the first 10 cycles. Sample 1, while having a much lower capacity, demonstrates better capacity retention, with −50.7% of the initial capacity after 15 cycles.
For silicon samples obtained from the KCl–K2SiF6–SiO2 melt, the anode capacity was between 920 and 2430 mAh·g−1 for charging and between 600 and 1300 mAh·g−1 during discharge. As can be seen from Figure 6, the behavior of these samples is similar to the ones synthesized without the addition of SiO2 to the melt, but lower capacities are achieved for all the samples. The highest capacity value was observed for the sample 5 synthesized at 0.15 V overvoltage. The initial coulombic efficiency of the silicon needles/tubes was 44–65%, lower than for the samples 1–3. Sample 4 demonstrates much higher delithiation potential than all other samples, probably due to the higher C-rate in comparison to other samples. After 15 cycles (Figure 7b), samples synthesized from the melt with SiO2 addition demonstrate higher coulombic efficiency—between 93.5% and 96.1%—and better capacity retention rate. Remaining capacity of the sample 5 is 850 mAh·g−1, which is 74.5% of the initial capacity.
It is probable that such a difference in capacity fade rate is caused by different silicon structures or surface layer composition; however, the reasons for drastic capacity difference among the samples with similar morphology synthesized at different deposition overpotential is not clear. The results obtained indicate that further research is promising, aimed both at optimizing the conditions for obtaining silicon deposits from the investigated molten electrolytes, and at improving the performance of a lithium-ion battery with a composite anode based on the obtained silicon.

4. Conclusions

In this work, we studied the effect of cathode overvoltage and the addition of SiO2 on the morphology of silicon electrolytic deposits obtained from KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts at a temperature of 790 °C. Using scanning electron microscopy, it was shown that during electrolysis of the KCl–K2SiF6 melt, nano-sized disordered fibers (300–400 nm in diameter) are formed on the cathode, while the addition of SiO2 to the melt leads to an ordered growth of silicon deposit in the form of nano-sized needles and tubes (diameter 200–400 nm, length 30–60 µm). At the same time, it was noted that an increase in cathode overvoltage during the electrolysis of the studied molten electrolytes has virtually no effect on the morphology and size of the deposit, which may be associated with the course of the process under the conditions of a slowed-down preceding chemical reaction of the silicon-containing ion dissociation.
According to EDX analysis, the average oxygen content in silicon deposits obtained during the electrolysis of the KCl–K2SiF6 melt was 2.1–4.3 wt.%, and in the deposits obtained during the electrolysis of this melt with the addition of SiO2, the average oxygen content was 2.7–5.1 wt.%.
The resulting deposits were used for the manufacture of composite Si/C anode half-cells of lithium-ion batteries. All the synthesized samples have similar initial charge/discharge curves, although the capacity is different. Samples synthesized at 0.1 V show much lower capacity than the ones synthesized at 0.15 and 0.25 V overvoltage. Although the first cycle capacity of silicon synthesized with SiO2 addition is lower than that of silicon obtained without additive, further cycling results in higher capacity and much higher capacity retention for all samples. For silicon deposited from KCl–K2SiF6, the highest capacity value is 750 mAh·g−1 with capacity retention of 46.6 % and coulombic efficiency of 92.7%. The best results are achieved for silicon synthesized from KCl–K2SiF6–SiO2 at 0.15 V overvoltage; its capacity was 850 mAh·g−1 after 15 cycles at a current of 200 mA·g−1 and capacity retention of 74.5% with coulombic efficiency of 96.1%. Such differences in the capacity retention for the samples synthesized with and without SiO2 addition is not clear and requires further investigation.

Author Contributions

Conceptualization, T.G. and A.S.; methodology; T.G., S.Z., N.L., A.L. and A.T.; validation, T.G. and A.S.; formal analysis, A.S. and A.T.; investigation, T.G., S.Z., N.L., A.L. and A.T.; writing—original draft preparation, T.G. and A.S.; writing—review and editing, T.G. and A.S.; supervision, A.S. and Y.Z.; project administration, A.T. and A.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Acknowledgments

This work is performed in the frame of the State Assignment number 075-03-2020-582/1, dated 18 February 2020 (the theme number 0836-2020-0037).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Cohen, U. Some prospective applications of silicon electrodeposition from molten fluorides to solar cell fabrication. J. Electron. Mater. 1977, 6, 607–643. [Google Scholar] [CrossRef]
  2. Liu, Z.; Sofia, S.E.; Laine, H.S.; Woodhouse, M.; Wieghold, S.; Peters, I.M.; Buonassisi, T. Revisiting thin silicon for photovoltaics: A technoeconomic perspective. Energy Environ. Sci. 2020, 13, 12–23. [Google Scholar] [CrossRef] [Green Version]
  3. Feng, K.; Li, M.; Liu, W.; Kashkooli, A.G.; Xiao, X.; Cai, M.; Chen, Z. Silicon-based anodes for lithium-ion batteries: From fundamentals to practical applications. Small 2018, 14, 1702737. [Google Scholar] [CrossRef] [PubMed]
  4. Galashev, A.Y.; Suzdaltsev, A.V.; Ivanichkina, K.A. Design of the high performance microbattery with silicene anode. Mater. Sci. Eng. 2020, 261, 114718. [Google Scholar] [CrossRef]
  5. Schmidt, H.; Jerliu, B.; Hüger, E.; Stahnc, J. Volume expansion of amorphous silicon electrodes during potentiostatic lithiation of Li-ion batteries. Electrochem. Commun. 2020, 115, 106738. [Google Scholar] [CrossRef]
  6. Wu, J.J.; Chen, Z.; Ma, W.; Dai, Y. Thermodynamic estimation of silicon tetrachloride to trichlorosilane by a low temperature hydrogenation technique. Silicon 2017, 9, 69–75. [Google Scholar] [CrossRef]
  7. Zhang, C.; Wang, F.; Han, J.; Bai, S.; Tan, J.; Liu, J.; Li, F. Challenges and recent progress on silicon-based anode materials for next-generation lithium-ion batteries. Small Struct. 2021, 2, 2100009. [Google Scholar] [CrossRef]
  8. Zhao, Y.; Yue, F.; Li, S.; Zhang, Y.; Tian, Z.; Xu, Q.; Xin, S.; Guo, Y. Advances of polymer binders for silicon-based anodes in high energy density lithium-ion batteries. InfoMat 2021, 3, 460–501. [Google Scholar] [CrossRef]
  9. Liu, X.; Zhu, X.; Pan, D. Solutions for the problems of silicon–carbon anode materials for lithium-ion batteries. R. Soc. Open Sci. 2018, 5, 172370. [Google Scholar] [CrossRef] [Green Version]
  10. Azam, M.A.; Safie, N.E.; Ahmad, A.S.; Yuza, N.A.; Adilah Zulkifli, N.S. Recent advances of silicon, carbon composites and tin oxide as new anode materials for lithium-ion battery: A comprehensive review. J. Energy Storage 2021, 33, 102096. [Google Scholar] [CrossRef]
  11. Salah, M.; Hall, C.; Murphy, P.; Francis, C.; Kerr, R.; Stoehr, B.; Rudd, S.; Fabretto, M. Doped and reactive silicon thin film anodes for lithium ion batteries: A review. J. Power Sources 2021, 506, 230194. [Google Scholar] [CrossRef]
  12. Cho, S.; Jung, W.; Jung, G.Y.; Eom, K.S. High-performance boron-doped silicon micron-rod anode fabricated using a mass-producible lithography method for a lithium ion battery. J. Power Sources 2020, 454, 227931. [Google Scholar] [CrossRef]
  13. Chen, M.; Li, B.; Liu, X.; Zhou, L.; Yao, L.; Zai, J.; Qian, X.; Yu, X. Boron-doped porous Si anode materials with high initial coulombic efficiency and long cycling stability. J. Mater. Chem. 2018, 6, 3022. [Google Scholar] [CrossRef]
  14. Fukata, N.; Oshima, T.; Tsuruid, T.; Itod, S.; Murakami, K. Synthesis of silicon nanowires using laser ablation method and their manipulation by electron beam. Sci. Techn. Adv. Mater. 2005, 6, 628–632. [Google Scholar] [CrossRef] [Green Version]
  15. Hung, Y.-J.; Lee, S.-L.; Thibeault, B.J.; Coldren, L.A. Fabrication of highly-ordered silicon nanowire arrays with controllable sidewall profiles for achieving low surface reflection. IEEE J. Sel. Top. Quantum Electron. 2011, 17, 869–877. [Google Scholar] [CrossRef]
  16. Epur, R.; Hanumantha, P.J.; Datta, M.K.; Hong, D.; Gattu, B.; Kumta, P.N. A simple and scalable approach to hollow silicon nanotube (h-SiNT) anode architectures of superior electrochemical stability and reversible capacity. J. Mater. Chem. 2015, 3, 11117–11129. [Google Scholar] [CrossRef]
  17. Wendisch, F.J.; Rey, M.; Vogel, N.; Bourret, G.R. Large-scale synthesis of highly uniform silicon nanowire arrays using metal-assisted chemical etching. Chem. Mater. 2020, 32, 9425–9434. [Google Scholar] [CrossRef]
  18. Demami, F.; Ni, L.; Rogel, R.; Salaun, A.C.; Pichon, L. Silicon nanowires synthesis for chemical sensor applications. Procedia Eng. 2010, 5, 351–354. [Google Scholar] [CrossRef] [Green Version]
  19. Prosini, P.P.; Rufoloni, A.; Rondino, F.; Santoni, A. Silicon nanowires used as the anode of a lithium-ion battery. AIP Conf. Proc. 2015, 1667, 020008. [Google Scholar] [CrossRef] [Green Version]
  20. Parr, N.L.; Mech, E. Zone Refining and Allied Techniques; George Newnes Ltd.: London, UK, 1960. [Google Scholar]
  21. Zaykov, Y.P.; Zhuk, S.I.; Isakov, A.V.; Grishenkova, O.V.; Isaev, V.A. Electrochemical nucleation and growth of silicon in the KF-KCl-K2SiF6 melt. J. Solid State Electrochem. 2015, 19, 1341–1345. [Google Scholar] [CrossRef]
  22. Rao, G.M.; Elwell, D.; Feigelson, R.S. Electrodeposition of silicon onto graphite. J. Electrochem. Soc. 1981, 128, 1708–1711. [Google Scholar] [CrossRef]
  23. Bieber, A.L.; Massot, L.; Gibilaro, M.; Cassayre, L.; Taxil, P.; Chamelot, P. Silicon electrodeposition in molten fluorides. Electrochim. Acta 2012, 62, 282–289. [Google Scholar] [CrossRef] [Green Version]
  24. Kuznetsova, S.V.; Dolmatov, V.S.; Kuznetsov, S.A. Voltammetric study of electroreduction of silicon complexes in a chloride–fluoride melt. Russ. J. Electrochem. 2009, 45, 742–748. [Google Scholar] [CrossRef]
  25. Cai, Z.; Li, Y.; Tian, W. Electrochemical behavior of silicon compound in LiF–NaF–KF–Na2SiF6 molten salt. Ionics 2011, 17, 821–826. [Google Scholar] [CrossRef]
  26. Juzeliunas, E.; Fray, D.J. Silicon electrochemistry in molten salts. Chem. Rev. 2020, 120, 1690–1709. [Google Scholar] [CrossRef]
  27. Maeda, K.; Yasuda, K.; Nohira, K.T.; Hagiwara, R.; Homma, T. Silicon electrodeposition in water-soluble KF–KCl molten salt: Investigations on the reduction of Si(IV) ions. J. Electrochem. Soc. 2015, 162, D444–D448. [Google Scholar] [CrossRef]
  28. Zhuk, S.I.; Isakov, A.V.; Apisarov, A.P.; Grishenkova, O.V.; Isaev, V.A.; Vovkotrub, E.G.; Zaykov, Y.P. Electrodeposition of continuous silicon coatings from the KF–KCl–K2SiF6 melts. J. Electrochem. Soc. 2017, 164, H5135–H5138. [Google Scholar] [CrossRef]
  29. Zhuk, S.I.; Isaev, V.A.; Grishenkova, O.V.; Isakov, A.V.; Apisarov, A.P.; Zaykov, Y.P. Silicon electrodeposition from chloride-fluoride melts containing K2SiF6 and SiO2. J. Serb. Chem. Soc. 2017, 82, 51–62. [Google Scholar] [CrossRef]
  30. Yasuda, K.; Maeda, K.; Hagiwara, R.; Homma, T.; Nohira, T. Silicon electrodeposition in a water-soluble KF–KCl molten salt: Utilization of SiCl4 as Si source. J. Electrochem. Soc. 2017, 164, D67–D71. [Google Scholar] [CrossRef]
  31. Zaykov, Y.P.; Isakov, A.V.; Apisarov, A.P.; Chemezov, O.V. Production of silicon by electrolysis of halide and oxide-halide melts. Tsvetnye Met. 2013, 2013, 58–62. [Google Scholar]
  32. Laptev, M.V.; Isakov, A.V.; Grishenkova, O.V.; Vorob'ev, A.S.; Khudorozhkova, A.O.; Akashev, L.A.; Zaikov, Y.P. Electrodeposition of thin silicon films from the KF–KCl–KI–K2SiF6 melt. J. Electrochem. Soc. 2020, 167, 042506. [Google Scholar] [CrossRef]
  33. Khudorozhkova, A.O.; Isakov, A.V.; Kataev, A.A.; Redkin, A.A.; Zaykov, Y.P. Density of KF–KCl–KI melts. Rus. Met. (Metally) 2020, 2020, 918–924. [Google Scholar] [CrossRef]
  34. Cho, S.K.; Lim, T. Catalyst-mediate d doping in electrochemical growth of solar silicon. Electrochim. Acta 2021, 367, 137472. [Google Scholar] [CrossRef]
  35. Xie, H.; Zhao, H.; Liao, J.; Yin, H.; Bard, A.J. Electrochemically controllable coating of a functional silicon film on carbon materials. Electrochim. Acta 2018, 269, 610–616. [Google Scholar] [CrossRef]
  36. Zou, X.; Ji, L.; Yang, X.; Lim, T.; Yu, E.T.; Bard, A.J. Electrochemical formation of a p−n junction on thin film silicon deposited in molten salt. J. Amer. Chem. Soc. 2017, 139, 16060–16063. [Google Scholar] [CrossRef]
  37. Yasuda, K.; Nohira, T.; Hagiwara, R.; Ogata, Y.H. Direct electrolytic reduction of solid SiO2 in molten CaCl2 for the production of solar grade silicon. Electrochim. Acta 2007, 53, 106–110. [Google Scholar] [CrossRef]
  38. Gevel, T.A.; Zhuk, S.I.; Ustinova, Y.A.; Suzdaltsev, A.V.; Zaikov, Y.P. Silicon electroreduction from the KCl–K2SiF6 melt. Rasplavy 2021, 2021, 187–198. [Google Scholar] [CrossRef]
  39. Gevel, T.; Zhuk, S.; Suzdaltsev, A.; Zaikov, Y. Silicon electrodeposition from the KCl-K2SiF6 melt. SSRN Electron. J. 2021. [Google Scholar] [CrossRef]
  40. Liang, B.; Liu, Y.; Xu, Y. Silicon-based materials as high capacity anodes for next generation lithium ion batteries. J. Power Sources 2014, 267, 469–490. [Google Scholar] [CrossRef]
  41. Chemezov, O.V.; Isakov, A.V.; Apisarov, A.P.; Brezhestovsky, M.S.; Bushkova, O.V.; Batalov, N.N.; Zaikov, Y.P.; Shashkin, A.P. Electrolytic production of silicon nanofibers from the KCl–KF–K2SiF6–SiO2 melt for composite anodes of lithium-ion batteries. Electrochem. Energetics 2013, 13, 201–204. [Google Scholar]
  42. Dong, Y.; Slade, T.; Stolt, M.J.; Li, L.; Girard, S.N.; Mai, L.; Jin, S. Low-temperature molten-salt production of silicon nanowires by the electrochemical reduction of CaSiO3. Angew. Chem. 2017, 129, 14645–14649. [Google Scholar] [CrossRef]
  43. Yuan, Y.; Xiao, W.; Wang, Z.; Fray, D.J.; Jin, X. Efficient nanostructuring of silicon by electrochemical alloying / dealloying in molten salts for improved lithium storage. Angew. Chem. 2018, 130, 15969–15974. [Google Scholar] [CrossRef]
  44. Hamedani, A.A.; Ow-Yang, C.W.; Soytas, S.H. Mechanisms of Si nanoparticle formation by molten salt magnesiothermic reduction of silica for lithium-ion battery anodes. ChemElectroChem 2021, 8, 3181–3191. [Google Scholar] [CrossRef]
  45. Yu, Z.; Wang, N.; Fang, S.; Qi, X.; Gao, Z.; Yang, J.; Lu, S. Pilot-plant production of high-performance silicon nanowires by molten salt electrolysis of silica. Ind. Eng. Chem. Res. 2020, 59, 1–8. [Google Scholar] [CrossRef]
  46. Yu, Z.; Fang, S.; Wang, N.; Shi, B.; Hu, Y.; Shi, Z.; Shi, D.; Yang, J. In-situ growth of silicon nanowires on graphite by molten salt electrolysis for high performance lithium-ion batteries. Mater. Lett. 2020, 273, 127946. [Google Scholar] [CrossRef]
  47. Hou, Y.; Yang, Y.; Meng, W.; Lei, B.; Ren, M.; Yang, X.; Wang, Y.; Zhao, D. Core-shell structured Si@Cu nanoparticles encapsulated in carbon cages as high-performance lithium-ion battery anodes. J. Alloys Compd. 2021, 874, 159988. [Google Scholar] [CrossRef]
  48. Nikolaev, A.Y.; Suzdaltsev, A.V.; Zaikov, Y.P. High temperature corrosion of ZrN powder in molten LiCl with additions of PbCl2, KCl, Li2O, H2O, and LiOH. J. Electrochem. Soc. 2019, 166, C147–C152. [Google Scholar] [CrossRef]
  49. Nikolaev, A.; Suzdaltsev, A.; Zaikov, Y. Cathode process in the KF–AlF3–Al2O3 melts. J. Electrochem. Soc. 2019, 166, D784–D791. [Google Scholar] [CrossRef]
  50. Zaykov, Y.P.; Isakov, A.V.; Zakiryanova, I.D.; Reznitskikh, O.G.; Chemezov, O.V.; Redkin, A.A. Interaction between SiO2 and a KF–KCl–K2SiF6 melt. J. Phys. Chem. 2014, 118, 1584–1588. [Google Scholar] [CrossRef]
  51. Vorob'ev, A.S.; Isakov, A.V.; Kazakovtseva, N.A.; Khudorozhkova, A.O.; Galashev, A.E.; Zaikov, Y.P. Calculations of silicon complexes in KF–KCl–KI–K2SiF6 and KF–KCl–KI–K2SiF6–SiO2 molten electrolytes. AIP Conf. Proc. 2019, 2174, 020072. [Google Scholar] [CrossRef]
  52. Li, H.; Liang, J.; Xie, S.; Reddy, R.G.; Wang, L. Electrochemical and phase analysis of Si(IV) on Fe electrode in molten NaCl–NaF–KCl–SiO2 system. High Temp. Mater. Proc. 2018, 37, 921–928. [Google Scholar] [CrossRef]
  53. Pershin, P.; Suzdaltsev, A.; Zaikov, Y. Synthesis of silumins in KF–AlF3–SiO2 melt. J. Electrochem. Soc. 2016, 163, D167–D170. [Google Scholar] [CrossRef]
  54. Dolmatov, V.S.; Kuznetsov, S.A. Electroreduction of tantalum oxofluoride complexes in equimolar mixture of sodium and potassium chlorides. Rasplavy 2016, 2016, 322–332. [Google Scholar] [CrossRef]
Figure 1. Experimental setup. 1—working electrode; 2—gas inlet; 3—quartz cell; 4 —counter electrode; 5—quasi-reference electrodes; 6—glassy carbon crucible.
Figure 1. Experimental setup. 1—working electrode; 2—gas inlet; 3—quartz cell; 4 —counter electrode; 5—quasi-reference electrodes; 6—glassy carbon crucible.
Applsci 11 10927 g001
Figure 2. Photographs of the cathode deposits obtained after the electrolysis of the KCl–K2SiF6 melt at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE potential.
Figure 2. Photographs of the cathode deposits obtained after the electrolysis of the KCl–K2SiF6 melt at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE potential.
Applsci 11 10927 g002
Figure 3. Photographs of the cathode deposits obtained after the electrolysis of the KCl–K2SiF6–SiO2 melt at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE potential.
Figure 3. Photographs of the cathode deposits obtained after the electrolysis of the KCl–K2SiF6–SiO2 melt at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE potential.
Applsci 11 10927 g003
Figure 4. Micrographs of the cathode deposits obtained during the electrolysis of KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE.
Figure 4. Micrographs of the cathode deposits obtained during the electrolysis of KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts at a temperature of 790 °C and cathode overvoltage of 0.25, 0.15, and 0.1 V vs. QRE.
Applsci 11 10927 g004
Figure 5. Cyclic voltammograms for the KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts with a total silicon content of 0.05 and 0.15 wt.%, respectively. Potential sweep rate is 0.4 V s−1.
Figure 5. Cyclic voltammograms for the KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts with a total silicon content of 0.05 and 0.15 wt.%, respectively. Potential sweep rate is 0.4 V s−1.
Applsci 11 10927 g005
Figure 6. First charge/discharge cycle curves of Si/C composites based on electrodeposited silicon at 50 mA g−1. Solid lines represent silicon deposited from molten KCl–K2SiF6; dashed lines represent silicon deposited from molten KCl–K2SiF6–SiO2.
Figure 6. First charge/discharge cycle curves of Si/C composites based on electrodeposited silicon at 50 mA g−1. Solid lines represent silicon deposited from molten KCl–K2SiF6; dashed lines represent silicon deposited from molten KCl–K2SiF6–SiO2.
Applsci 11 10927 g006
Figure 7. Cycling performance and the coulombic efficiency of the Si/C made from silicon electrodeposited from (a) KCl–K2SiF6 (samples 1–3) and (b) KCl–K2SiF6–SiO2 (samples 4–6) at the cathode overvoltages of –0.1, –0.15, and –0.25 V. Diamonds-coulombic efficiency; squares-capacity.
Figure 7. Cycling performance and the coulombic efficiency of the Si/C made from silicon electrodeposited from (a) KCl–K2SiF6 (samples 1–3) and (b) KCl–K2SiF6–SiO2 (samples 4–6) at the cathode overvoltages of –0.1, –0.15, and –0.25 V. Diamonds-coulombic efficiency; squares-capacity.
Applsci 11 10927 g007
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Gevel, T.; Zhuk, S.; Leonova, N.; Leonova, A.; Trofimov, A.; Suzdaltsev, A.; Zaikov, Y. Electrochemical Synthesis of Nano-Sized Silicon from KCl–K2SiF6 Melts for Powerful Lithium-Ion Batteries. Appl. Sci. 2021, 11, 10927. https://doi.org/10.3390/app112210927

AMA Style

Gevel T, Zhuk S, Leonova N, Leonova A, Trofimov A, Suzdaltsev A, Zaikov Y. Electrochemical Synthesis of Nano-Sized Silicon from KCl–K2SiF6 Melts for Powerful Lithium-Ion Batteries. Applied Sciences. 2021; 11(22):10927. https://doi.org/10.3390/app112210927

Chicago/Turabian Style

Gevel, Timofey, Sergey Zhuk, Natalia Leonova, Anastasia Leonova, Alexey Trofimov, Andrey Suzdaltsev, and Yuriy Zaikov. 2021. "Electrochemical Synthesis of Nano-Sized Silicon from KCl–K2SiF6 Melts for Powerful Lithium-Ion Batteries" Applied Sciences 11, no. 22: 10927. https://doi.org/10.3390/app112210927

APA Style

Gevel, T., Zhuk, S., Leonova, N., Leonova, A., Trofimov, A., Suzdaltsev, A., & Zaikov, Y. (2021). Electrochemical Synthesis of Nano-Sized Silicon from KCl–K2SiF6 Melts for Powerful Lithium-Ion Batteries. Applied Sciences, 11(22), 10927. https://doi.org/10.3390/app112210927

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop