Next Article in Journal
In-Life Range Modularity for Electric Vehicles: The Environmental Impact of a Range-Extender Trailer System
Next Article in Special Issue
Effect of Additional Shielding Gas on Welding Seam Formation during Twin Wire DP-MIG High-Speed Welding
Previous Article in Journal
Design and Experimental Validation of a Cooperative Adaptive Cruise Control System Based on Supervised Reinforcement Learning
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Fatigue Strength Assessment of Steel Rollers: On the Reliability of the Strain Energy Density Approach on Real Components

1
Rulli Rulmeca S.P.A, 24011 Almè (BG), Italy
2
Department of Industrial and Mechanical Engineering, Norwegian University of Science and Technology, Richard Birkelands vei 2b, 7034 Trondheim, Norway
*
Author to whom correspondence should be addressed.
Appl. Sci. 2018, 8(7), 1015; https://doi.org/10.3390/app8071015
Submission received: 7 June 2018 / Revised: 14 June 2018 / Accepted: 18 June 2018 / Published: 21 June 2018
(This article belongs to the Special Issue Welding of Steels)

Abstract

:
Welded joints are one of the most widely applied methods to join different steel components. However, they introduce stress concentrators that are commonly known to reduce the fatigue strength of structures. Several methods have been developed to assess the fatigue behavior of welded components, such as the Notch Stress Intensity Factors (NSIFs) approach. However, this approach has been reported to be geometry dependent, and does not allow for a direct comparison of failures occurring at the weld toes with those occurring at the weld roots. This drawback has been overcame by considering the value of the strain energy density (SED) range averaged in a control volume ahead of the notch tip. More than 900 fatigue data of welded joints have been summarized within a single scatter band ΔW-N (strain energy range–umber of cycles to failure) using this approach. The reliability of the just mentioned scatter band in summarizing the fatigue data of real components such as steel welded rollers produced by Rulmeca is herein evaluated. The results prove the reliability of the SED approach to assess the fatigue behavior of welded rollers, paving the way to its diffusion in assessing real components.

1. Introduction

Welding procedures have allowed the simple realization of many complex structural connections in several different applications, such as bridges, cranes, offshore structures, and buildings [1]. Besides the optimization of the process parameters [2,3,4], researchers have focused on the fatigue behavior of welded components. All the aforementioned applications are in fact subjected to repetitive loading and hence the fatigue of welded structures has become one of the greatest matters of concern [5]. Welds represent local regions of higher stresses (i.e., stress concentrators) and fatigue failure is widely known to be sensitive to local peak stresses. Thus, over the years, several methods have been developed to assess the fatigue behavior of welds, and among these the Notch Stress Intensity Factor (NSIF) approach is worth mentioning [6,7,8]. In fact, since experimental observations have revealed that the most used welding procedures, such as arc and laser welding, are characterized by a very small weld toe radius, it is acceptable to model it as a sharp notch and the fatigue behavior can thus be correlated to the NSIFs [9,10]. Fatigue life can be divided into two different phases; i.e., nucleation and growth of cracks—and NSIFs were found to be able to predict either the initiation phase or the whole fatigue life [11,12,13,14]. This holds when the majority of the propagation phase has been spent within the region governed by the stress singularity. Several studies proved this behavior. Lassen demonstrated that in transverse, non-load-carrying joints manufactured via different welding procedures the nucleation of a 0.1 mm long crack required up to 40% of the whole fatigue life [15]. In addition, Singh et al. reported that in load-carrying AISI 304L fillet joints up to 70% of the fatigue life was spent propagating the original lack of a penetration crack of 0.5 mm [16,17]. However, the results are highly dependent of the on the stress distribution ahead of the point of singularity and, since time consuming FE analyses are required, this has limited the diffusion of the NSIFs approach in the assessment of real structures. Furthermore, the main limitation of this method consists in its geometry dependency. Its unit depends in fact on the notch opening angle according to Williams’ formulations [18]. Different notch geometries are not thus comparable but ad-hoc material properties are required for each geometry. A breakthrough in the fatigue assessment of welded joints is represented by the strain energy density (SED) method, capable of overcoming all the limitations of the NSIFs approach [19]. The SED is evaluated averaging the range value of the strain energy in a cylindrical volume sector of radius Rc centered at the notch tip. According to this approach, fatigue failure occurs then this scalar quantity reaches its critical value ΔWc. Both the radius Rc and the critical energy range ΔWc. depend only on material properties [11] and shall be assumed to be independent of the load mode. Using this approach, Livieri and Lazzarin [20] summarized more than 600 experimental data obtained from different welded joints within a single narrow SED scatter-band. Failures occurred either at the weld root or at the weld toe. This work has then been extended by Berto and Lazzarin [21], including hollow section joints, and now more than 900 fatigue data are summarized in a single scatter band as depicted in Figure 1.
Moreover, the SED approach has been also reported to be a reliable tool in multi-axial fatigue assessment. Berto and Lazzarin [22] in fact resumed several experimental fatigue data obtained for structural steel within a single scatter band, drawn according to the following two assumptions: First, the critical value of strain energy density is considered to be independent from the type of loading in the high-cycle fatigue regime, and its value at 2 × 106 cycles has thus been imposed equal to that obtained for welded joints under uniaxial loading; a slope equal to 5/2 as suggested in Ref. [23] has been used. The approach has then been successfully applied to either the tensile or fatigue assessment of several notched materials, from metals [24,25,26,27,28,29,30,31,32] to polymers [33,34,35] and ceramics [36,37].
Recently, the SED approach was also preliminarily applied to the fatigue assessment of real components, such as rollers (Figure 2) produced by Rulmeca [38]. Besides surface pitting due to contact fatigue [39,40], rollers are in fact affected by fatigue failures at the weld root. The bearing housings of the rollers are joint to the tube body by means of welding procedures. Although the connection between the bearing housings and the tube body is fundamental in preventing any imbalance in the roller, it is responsible to the fatigue failure of the rollers due to the lack of penetration at the weld root.
This work aims to further analyze the problem of fatigue failure at the weld root and to assess the reliability of the SED scatter band reported in Figure 1 in their assessment. Hence, firstly, new fatigue data sets have been obtained for three different roller types; i.e., PSV2, PSV4 and PSV5—and each roller type was characterized by different dimensions. Then, the new fatigue data together with those reported in Ref. [38] were analyzed in terms of SED, and they have been shown to be satisfactorily resumed by the scatter band obtained in Ref. [21]. This represents a breakthrough in the fatigue design of rollers, and in general of welded structures, since the SED scatter band reported in Figure 1 can be reliably used to predict the fatigue behavior of real components, whether they fail at the weld root or at the weld toe.

2. A Brief Description of the Strain Energy Density Approach

Considering the SED criterion [19] statements for dynamic loadings, fatigue failure occurs when the strain energy range Δ W ¯ averaged in a control volume of radius Rc ahead of the crack tip reaches its critical value ΔWc. Simple analytical formulations have been obtained in Ref. [19] for the assessment of the critical value of the strain energy density range ΔWc (Equation (1)) and of the critical radius Rc (Equation (2)):
Δ W C = Δ σ A 2 2 E
R C = ( 2 e 1 Δ K 1 A Δ σ A ) 1 1 λ 1
where ΔσA is the fatigue limit of the material without geometric singularities, E is the Young's modulus of the material, λ1 is Williams’ eigenvalue for mode 1 [18], Δ K 1 A N is the amplitude of the Notch Stress Intensity Factors (NSIF) fatigue threshold, and e1 is a parameter dependent either on geometrical parameters (the notch opening angle 2α) or on material properties (the Poisson’s ratio ν). The reader should refer to Ref. [19] for e1 formulation. Dealing with rollers, the control volume is a circle centered at the weld root tip (blue circle in Figure 3), and its radius, as well as the critical strain energy density range value, is only dependent on the material [11].
The value of the critical radius has been obtained by leveraging on previously published data either for failures at the weld root or at the weld toe. Concerning the former, considering the value of 211 MPa mm0.326 for the amplitude of the Notch Stress Intensity Factors Δ K 1 A N obtained by Livieri and Lazzarin [41] for the transverse non-load carrying fillet welded joints, and that of 153 MPa for the fatigue strength ΔσA of butt ground welds obtained by Taylor at al. [42], the critical value Rc for steel welded joints corresponds to 0.28 mm. Dealing with the case of failure to occur at the weld root, instead, considering Δ K 1 A N = 180 MPa mm0.5, Equation (2) gives a critical value of the radius equal to 0.36 mm. However, being on the safe side, an Rc value of 0.28 mm has been used in this work also for failures occurring at the weld roots.

3. Geometry

In this report rollers belonging to the series PSV were studied. Representing the state of the art of Rulmeca’s production [34], these rollers are widely required for conveyors in applications characterized by high working load and by the need to convey large lump size materials. The main components of the roller are reported in Figure 2 and their functions are widely described in Ref. [38]. Among them, the feature investigated in this work is the joint between the roller shell (tube) and the bearing housing, where the failure occurs. Joining these two features optimizes the roller performance, avoiding any imbalance in the rollers and allowing their use at the highest speeds. However, although weldment is of utmost importance for a proper roller operation, it represents the weakest point of the structure considering fatigue behavior, since the lack of penetration at the weld root (Figure 4) leads to the final failure of the roller (Figure 4b,c).
The length of the lack of penetration, indicated as c in Figure 3, has been determined carrying out micrographic analyses on the welded rollers, resulting in a value of c in the range between 0.6 and 1.0 mm. As reported in Ref. [38], the SED value is slightly affected by a variation of c in this range, and thus the length c = 1 mm is set in all the analyses.
The rollers tested in this work belong to three different types of rollers; i.e., PSV2, PSV4 and PSV5. The geometrical parameters are listed in Table 1 in addition to the rollers tested in Ref. [38]; i.e., PSV4 133 315 and PSV4 159 530. See Figure 5 for an explanation of the meaning of the geometrical details.

4. Results

Seven different roller geometries have been tested under fatigue; i.e., PSV2 133 315, PSV2, PSV2 133 600, PSV2 159 380, PSV2 159 600, PSV4 159 530, PSV5 133 315, PSV5 159 530. The test system mimicking the in-service conditions of the rollers was developed by the authors. An external counter-roll presses the tested roller, which rotates with a constant speed, with a constant pressure, applying the load. Further details about the test system can be found in Ref. [38]. The fatigue results for each geometry are reported in Table 2, Table 3, Table 4, Table 5, Table 6, Table 7 and Table 8. In Table 6 the fatigue results obtained in Ref. [38] are also reported. In addition, in Table 9 the experimental data obtained in Ref. [38] for PSV4 133 315 are resumed.
The fatigue data reported in Table 2, Table 3, Table 4, Table 5, Table 6, Table 7, Table 8 and Table 9 have been analyzed in terms of the SED range by means of FE analyses (details on FE models can be found in Ref. [38]). The results have been compared with the scatter band presented in Ref. [21]. It is worth mentioning that the just mentioned scatter band has been obtained by mostly considering welded joints that fail at the weld toes (Figure 6). It can be seen that the scatter band previously obtained allows reliable predictions of fatigue strength of different roller geometries that fail at the weld root. Therefore, the aforementioned scatter band has revealed to be a reliable tool for the assessment of the fatigue failure of the welded joints regardless of the location of the failure.

5. Conclusions

The SED approach has been herein used to assess the fatigue behavior of different types of PSV rollers, representing the state of the art of Rulmeca’s production. These rollers are subjected to fatigue failures because of a lack of penetration of the weld root connecting the bearing housings to the tube body. Fatigue tests on seven different roller geometries have been carried out and the results have been analyzed in terms of SED. Together with the data obtained in Ref. [38], they have been reported to fall within the scatter band ΔW-N (strain energy range–number of cycles to failure) obtained in Ref. [21] that summarizes about 900 fatigue data obtained from welded joints characterized by different main plate thicknesses, different transverse plates, and different bead flanks. Although this scatter band was obtained with the majority of the failures occurring at the weld toes, it provides reliable predictions of the fatigue behavior of welded joints with failures from the notch root; i.e., the considered roller geometries.

Author Contributions

F.C. performed the experimental tests and analyzed the data; M.P. wrote the manuscript and partially analyzed the data; L.M.V. partially wrote the manuscript; F.B. and T.W. provided scientific guidance.

Funding

This research received no external funding.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Liu, H.; Wang, P.; Wei, X.; Xiao, J.; Chen, R. Longitudinal Seismic Response of Continuously Welded Track on Railway Arch Bridges. Appl. Sci. 2018, 8, 775. [Google Scholar] [CrossRef]
  2. Stadler, M.; Freton, P.; Gonzalez, J.-J. Influence of Welding Parameters on the Weld Pool Dimensions and Shape in a TIG Configuration. Appl. Sci. 2017, 7, 373. [Google Scholar] [CrossRef]
  3. Jin, L.; Xue, J.; Zhang, Z.; Hu, Y. Effects of Thermal Frequency on Microstructures, Mechanical and Corrosion Properties of AA6061 Joints. Appl. Sci. 2018, 8, 540. [Google Scholar] [CrossRef]
  4. Ikram, A.; Chung, H. The Effect of EN Ratio and Current on Microstructural and Mechanical Properties of Weld Joined by AC-GMAW on Square Groove Butt Joints. Appl. Sci. 2017, 7, 261. [Google Scholar] [CrossRef]
  5. Schijve, J. Fatigue of Welded Joints. In Fatigue of Structures and Materials; Springer: Dordrecht, The Netherlands, 2009; pp. 535–558. [Google Scholar]
  6. Atzori, B.; Lazzarin, P.; Meneghetti, G. Fatigue strength assessment of welded joints: From the integration of Paris’ law to a synthesis based on the notch stress intensity factors of the uncracked geometries. Eng. Fract. Mech. 2008, 75, 364–378. [Google Scholar] [CrossRef]
  7. Peron, M.; Razavi, S.M.J.; Berto, F.; Torgersen, J. Notch stress intensity factor under mixed mode loadings: An overview of recent advanced methods for rapid calculation. Fract. Integr. Struct. 2017, 42, 196–204. [Google Scholar]
  8. Ferro, P.; Peron, M.; Razavi, S.M.J.; Berto, F.; Torgersen, J. The fatigue behavior of V-notches in presence of residual stresses: Recent developments and future outcomes. Fract. Integr. Struct. 2017, 42, 189–195. [Google Scholar]
  9. Dunn, M.L.; Suwito, W.; Cunningham, S.; May, C.W. Fracture initiation at sharp notches under mode I, mode II, and mild mixed mode loading. Int. J. Fract. 1997, 84, 367–381. [Google Scholar] [CrossRef]
  10. Dunn, M.L.; Suwito, W.; Cunningham, S. Fracture initiation at sharp notches: Correlation using critical stress intensities. Int. J. Solids Struct. 1997, 34, 3873–3883. [Google Scholar] [CrossRef]
  11. Berto, F.; Lazzarin, P. Recent developments in brittle and quasi-brittle failure assessment of engineering materials by means of local approaches. Mater. Sci. Eng. R 2014, 75, 1–48. [Google Scholar] [CrossRef]
  12. Ferro, P. The local strain energy density approach applied to pre-stressed components subjected to cyclic load. Fatigue Fract. Eng. Mater. Struct. 2014, 37, 1268–1280. [Google Scholar] [CrossRef]
  13. Radaj, D. State-of-the-art review on the local strain energy density concept and its relation to the J-integral and peak stress method. Fatigue Fract. Eng. Mater. Struct. 2015, 38, 2–28. [Google Scholar] [CrossRef]
  14. Radaj, D. State-of-the-art review on extended stress intensity factor concepts. Fatigue Fract. Eng. Mater. Struct. 2014, 37, 1–28. [Google Scholar] [CrossRef]
  15. Lassen, T. The Effect of the Welding Process on the Fatigue Crack Growth. Weld J. 1990, 69, 75–81. [Google Scholar]
  16. Singh, P.J.; Guha, B.; Achar, D.R. Fatigue life improvement of AISI 304L cruciform welded joints by cryogenic treatment. Eng. Fail. Anal. 2003, 10, 1–12. [Google Scholar] [CrossRef]
  17. Singh, P.J.; Achar, D.R.; Guha, B.; Nordberg, H. Fatigue life prediction of gas tungsten arc welded AISI 304L cruciform joints with different LOP sizes. Int. J. Fatigue 2003, 25, 1–7. [Google Scholar] [CrossRef]
  18. Williams, M.L. Stress singularities resulting from various boundary conditions in angular corners on plates in extension. J. Appl. Mech. 1952, 19, 526–528. [Google Scholar]
  19. Lazzarin, P.; Zambardi, R. A finite-volume-energy based approach to predict the static and fatigue behavior of components with sharp V-shaped notches. Int. J. Fract. 2001, 112, 275–298. [Google Scholar] [CrossRef]
  20. Livieri, P.; Lazzarin, P. Fatigue strength of steel and aluminium welded joints based on generalised stress intensity factors and local strain energy values. Int. J. Fract. 2005, 133, 247–276. [Google Scholar] [CrossRef]
  21. Berto, F.; Lazzarin, P. A review of the volume-based strain energy density approach applied to V-notches and welded structures. Theor. Appl. Fract. Mech. 2009, 52, 183–194. [Google Scholar] [CrossRef]
  22. Berto, F.; Lazzarin, P. Fatigue strength of structural components under multi-axial loading in terms of local energy density averaged on a control volume. Int. J. Fatigue 2011, 33, 1055–1065. [Google Scholar] [CrossRef]
  23. Lazzarin, P.; Sonsino, C.M.; Zambardi, R. A notch stress intensity approach to assess the multiaxial fatigue strength of welded tube-to-flange joints subjected to combined loadings. Fatigue Fract. Eng. Mater. Struct. 2004, 27, 127–140. [Google Scholar] [CrossRef]
  24. Peron, M.; Torgersen, J.; Berto, F. Rupture Predictions of Notched Ti-6Al-4V Using Local Approaches. Materials 2018, 11, 663. [Google Scholar] [CrossRef] [PubMed]
  25. Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F.; Welo, T. 40CrMoV13.9 notched specimens under multiaxial fatigue: An overview of recent results. Fract. Integr. Struct. 2017, 41, 440–446. [Google Scholar]
  26. Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F.; Mutignani, F. Effect of hot dip galvanization on the fatigue strength of steel bolted connections. Fract. Integr. Struct. 2017, 41, 432–439. [Google Scholar]
  27. Gallo, P.; Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F. Creep behavior of V-notched components. Fract. Integr. Struct. 2017, 41, 456–463. [Google Scholar]
  28. Razavi, S.M.J.; Peron, M.; Mutignani, F.; Torgersen, J.; Berto, F. Fatigue Strength of Hot-Dip Galvanized Welded Steel Connections. Key Eng. Mater. 2017, 754, 244–247. [Google Scholar] [CrossRef]
  29. Peron, M.; Razavi, S.M.J.; Berto, F.; Torgersen, J.; Colussi, M. Fracture assessment of magnetostrictive materials. Fract. Integr. Struct. 2017, 42, 223–230. [Google Scholar]
  30. Campagnolo, A.; Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F. Mode II brittle fracture: Recent developments. Fract. Integr. Struct. 2017, 42, 181–188. [Google Scholar]
  31. Peron, M.; Razavi, S.M.J.; Berto, F.; Torgersen, J.; Mutignani, F. Local strain energy density for the fatigue assessment of hot dip galvanized welded joints: Some recent outcomes. Fract. Integr. Struct. 2017, 42, 205–213. [Google Scholar]
  32. Razavi, S.M.J.; Peron, M.; Mutignani, F.; Torgersen, J.; Berto, F. A Study on the Fatigue Behavior of Hot Dip Galvanized Steel Connections. Key Eng. Mater. 2017, 754, 241–243. [Google Scholar] [CrossRef]
  33. Peron, M.; Razavi, S.; Torgersen, J.; Berto, F. Fracture Assessment of PEEK under Static Loading by Means of the Local Strain Energy Density. Materials 2017, 10, 14–23. [Google Scholar]
  34. Peron, M.; Razavi, S.M.J.; Berto, F.; Torgersen, J.; Marsavina, L. Local strain energy density for the fracture assessment of polyurethane specimens weakened by notches of different shape. Fract. Integr. Struct. 2017, 42, 214–222. [Google Scholar]
  35. Berto, F.; Cendon, D.A.; Lazzarin, P.; Elices, M. Fracture behaviour of notched round bars made of PMMA subjected to torsion at −60 °C. Eng. Fract. Mech. 2013, 102, 271–287. [Google Scholar] [CrossRef] [Green Version]
  36. Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F. Static Multiaxial Fracture Behavior of Graphite Components: A Review of Recent Results. Key Eng. Mater. 2017, 754, 35–38. [Google Scholar] [CrossRef]
  37. Razavi, S.M.J.; Peron, M.; Torgersen, J.; Berto, F. Notched graphite under multiaxial loading. Fract. Integr. Struct. 2017, 41, 424–431. [Google Scholar]
  38. Berto, F.; Campagnolo, A.; Chebat, F.; Cincera, M.; Santini, M. Fatigue strength of steel rollers with failure occurring at the weld root based on the local strain energy values: Modelling and fatigue assessment. Int. J. Fatigue 2016, 82, 643–657. [Google Scholar] [CrossRef]
  39. Seki, M.; Nishie, N.; Kozai, S.; Kakuda, M.; Soyama, H.; Naito, A.; Fujii, M. Fatigue Strength of Steel Rollers and Gears Treated by Cavitation Peening with Short Processing Time (A Case of Processing Time of 1 min and 5 min). J. Adv. Mech. Des. Syst. Manuf. 2012, 6, 33–43. [Google Scholar] [CrossRef]
  40. Fujita, K.; Yoshida, A. Surface fatigue failure of nitride-hardened aluminium-chromium-molybdenum steel rollers under pure rolling and sliding-rolling contacts. Wear 1979, 53, 61–68. [Google Scholar] [CrossRef]
  41. Lazzarin, P.; Livieri, P. Notch stress intensity factors and fatigue strength of aluminium and steel welded joints. Int. J. Fatigue 2001, 23, 225–232. [Google Scholar] [CrossRef]
  42. Taylor, D.; Barrett, N.; Lucano, G. Some new methods for predicting fatigue in welded joints. Int. J. Fatigue 2002, 24, 509–518. [Google Scholar] [CrossRef]
Figure 1. Fatigue behavior of welded joints as a function of the averaged local strain energy density range ΔW; R is the nominal load ratio.
Figure 1. Fatigue behavior of welded joints as a function of the averaged local strain energy density range ΔW; R is the nominal load ratio.
Applsci 08 01015 g001
Figure 2. Typical roller assembly.
Figure 2. Typical roller assembly.
Applsci 08 01015 g002
Figure 3. Schematic representation of the weld root, characterized by a weld root length “c”, and the control volume of the strain energy density (SED) approach (blue circle).
Figure 3. Schematic representation of the weld root, characterized by a weld root length “c”, and the control volume of the strain energy density (SED) approach (blue circle).
Applsci 08 01015 g003
Figure 4. Lack of penetration at the weld root (a), a detail of the crack through the welded zone (b) and typical roller failure (c).
Figure 4. Lack of penetration at the weld root (a), a detail of the crack through the welded zone (b) and typical roller failure (c).
Applsci 08 01015 g004aApplsci 08 01015 g004b
Figure 5. Geometry of the rollers.
Figure 5. Geometry of the rollers.
Applsci 08 01015 g005
Figure 6. Synthesis of fatigue data for different roller geometries in terms of local SED and a comparison with the scatter band shown in Figure 1.
Figure 6. Synthesis of fatigue data for different roller geometries in terms of local SED and a comparison with the scatter band shown in Figure 1.
Applsci 08 01015 g006
Table 1. Geometrical parameters of the rollers considered in the present investigation and in Ref. [38] (*).
Table 1. Geometrical parameters of the rollers considered in the present investigation and in Ref. [38] (*).
Model NameLength of the Roller [mm]Diameter of the Roller [mm]Tube Thickness [mm]Bearing Type
PSV2 133 31531513346205
PSV2 133 60060013346205
PSV2 159 3803801594.56205
PSV2 159 6006001594.56205
PSV4 133 315 *31513346206
PSV4 159 530 *5301594.56206
PSV5 133 31531513346306
PSV5 159 5305301594.56306
Table 2. Fatigue data for the roller PSV2 133 315.
Table 2. Fatigue data for the roller PSV2 133 315.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV2 133 31515415452,151,3880.101
25125451,343,3130.091
34665455,328,1210.075
44575452,440,8520.072
545154511,468,4290.071
642054510,198,9550.061
73805918,620,1790.050
Table 3. Fatigue data for the roller PSV2 133 600.
Table 3. Fatigue data for the roller PSV2 133 600.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV2 133 60015456536,478,4320.091
25316536,373,9310.086
352264810,132,7400.083
448464110,699,3960.072
546164110,722,2690.065
639549310,075,9940.048
Table 4. Fatigue data for the roller PSV2 159 380.
Table 4. Fatigue data for the roller PSV2 159 380.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV2 159 38011231534259,4630.517
2899534416,9560.276
3856534695,1040.250
4814534534,4080.226
5745534557,3650.189
65405341,556,2430.099
744853410,752,5320.068
84315345,451,9230.063
93975347,611,4440.054
103445345,958,0360.040
1129853410,612,4490.030
1223853414,382,7850.019
Table 5. Fatigue data for the roller PSV2 159 600.
Table 5. Fatigue data for the roller PSV2 159 600.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV2 159 60015615342,119,2580.101
25275343,983,7690.089
35025342,452,6180.081
44715342,809,7800.071
542453410,434,3900.058
640253410,224,2240.052
737353411,459,0750.045
835153414,488,2770.039
932453410,663,6030.034
1030254412,563,4050.029
1128354410,665,6270.026
1225454410,159,4360.021
Table 6. Fatigue data for the roller PSV4 159 530.
Table 6. Fatigue data for the roller PSV4 159 530.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV4 159 5301 *1262541363,2340.278
2 *1251541370,4320.274
3 *994541677,2790.173
4 *992541747,5480.172
5 *991541598,3900.172
6 *990541619,3440.171
77685456,140,0030.103
87155453,352,6510.089
9 *7085452,749,3330.088
1068154515,139,9280.081
116215455,433,7420.067
1258554510,065,5720.060
1353654510,791,7890.050
14 *5235459,962,1790.048
1548054510,690,4990.040
1645654511,909,3100.036
1742854511,221,8940.032
1840154515,489,4170.028
1938854511,608,3280.026
2034054510,967,6920.020
Data characterized by * were already presented in Ref. [38].
Table 7. Fatigue data for the roller PSV5 133 315.
Table 7. Fatigue data for the roller PSV5 133 315.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV5 133 31511251643306,2210.230
21245643605,9330.228
312006431,399,8670.212
4815638910,1640.098
5807638231,33600.096
67956382,089,0120.093
77766384,078,1980.089
875263810,913,6770.083
97136385,059,1600.075
1069563812,802,3530.071
116786383,863,8920.068
1265764314,832,9670.064
135936414,625,7830.052
1455664112,891,3170.045
1550864111,974,0270.038
Table 8. Fatigue data for the roller PSV5 159 530.
Table 8. Fatigue data for the roller PSV5 159 530.
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV5 159 53019195431,500,1120.124
28835431,368,1800.114
38325432,351,6320.101
47825433,250,5680.090
57365433,463,9290.079
67275433,203,4780.077
77105434,187,8250.074
86985433,082,7480.071
96605433,361,2710.064
106595433,086,5490.064
116285432,994,2510.058
1261554310,945,9830.055
Table 9. Fatigue data for the roller PSV4 133 315 from [38].
Table 9. Fatigue data for the roller PSV4 133 315 from [38].
SamplesLoad [Kg]RPMCyclesSED [MJ/mm3]
PSV4 133 31511700617110,0000.442
21675617155,5000.429
312456431,680,0000.237
41245643521,6580.237
58136383,687,6210.101
678663813,484,7450.094
776063810,728,3610.088
875263810,685,5830.086
97136381,044,0410.078
1064763810,164,9480.064
1161063811,055,2350.057
1255364610,479,3120.047
1351064610,615,3670.040
1440464611,446,9340.025

Share and Cite

MDPI and ACS Style

Chebat, F.; Peron, M.; Viespoli, L.M.; Welo, T.; Berto, F. Fatigue Strength Assessment of Steel Rollers: On the Reliability of the Strain Energy Density Approach on Real Components. Appl. Sci. 2018, 8, 1015. https://doi.org/10.3390/app8071015

AMA Style

Chebat F, Peron M, Viespoli LM, Welo T, Berto F. Fatigue Strength Assessment of Steel Rollers: On the Reliability of the Strain Energy Density Approach on Real Components. Applied Sciences. 2018; 8(7):1015. https://doi.org/10.3390/app8071015

Chicago/Turabian Style

Chebat, Francesco, Mirco Peron, Luigi Mario Viespoli, Torgeir Welo, and Filippo Berto. 2018. "Fatigue Strength Assessment of Steel Rollers: On the Reliability of the Strain Energy Density Approach on Real Components" Applied Sciences 8, no. 7: 1015. https://doi.org/10.3390/app8071015

APA Style

Chebat, F., Peron, M., Viespoli, L. M., Welo, T., & Berto, F. (2018). Fatigue Strength Assessment of Steel Rollers: On the Reliability of the Strain Energy Density Approach on Real Components. Applied Sciences, 8(7), 1015. https://doi.org/10.3390/app8071015

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop