Next Article in Journal
The Genus Gnaphalium L. (Compositae): Phytochemical and Pharmacological Characteristics
Next Article in Special Issue
Palladium and Organocatalysis: An Excellent Recipe for Asymmetric Synthesis
Previous Article in Journal
Differential Growth Inhibitory Effects of Highly Oxygenated Guaianolides Isolated from the Middle Eastern Indigenous Plant Achillea falcata in HCT-116 Colorectal Cancer Cells
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Enhanced Stability of CaO and/or La2O3 Promoted Pd/Al2O3 Egg-Shell Catalysts in Partial Oxidation of Methane to Syngas

1
Ningbo Institute of Materials Technology & Engineering, Chinese Academy of Sciences, Ningbo 315201, China
2
Shanghai Key Laboratory of Atmospheric Particle Pollution and Prevention (LAP3), Department of Environmental Science and Engineering, Fudan University, Shanghai 200433, China
*
Authors to whom correspondence should be addressed.
Molecules 2013, 18(7), 8289-8297; https://doi.org/10.3390/molecules18078289
Submission received: 17 June 2013 / Revised: 5 July 2013 / Accepted: 9 July 2013 / Published: 15 July 2013
(This article belongs to the Special Issue Palladium Catalysts)

Abstract

:
An egg-shell Pd/Al2O3 catalyst showed higher activity than a regular Pd/Al2O3 catalyst in the partial oxidation of methane to syngas, but a common problem of this reaction is the catalyst deactivation on stream. We attempted to modify the egg-shell catalyst via impregnation with some metal oxide additives. Although the addition of MgO did not show any beneficial effect, the addition of CaO and/or La2O3 significantly improved the stability due to the suppression of carbon deposition and phase transformation of the Al2O3 support. The catalysts were characterized by X-ray diffraction (XRD), N2 adsorption-desorption, and thermogravimetric analysis (TGA).

Graphical Abstract

1. Introduction

Synthesis gas, a valuable feedstock for the synthesis of ammonia, methanol, dimethyl ether, acetic acid, etc., is mainly produced by steam reforming of methane [1,2,3]. In recent years, increasing attention has been paid to the catalytic partial oxidation of methane (POM) for syngas production because of less energy consumption, lower investment, and more desirable H2/CO ratio for some downstream processes [4,5].
The catalysts investigated in the POM processes are mainly supported Ni catalysts and noble metal (e.g., Rh, Pt, Ru, Pd, or Ir) catalysts [6,7]. Ni-based catalysts are cheap, but they deactivate easily due to carbon deposition and sintering above 700 °C [8]. Noble metal-based catalysts have much higher activity, and are less susceptible to catalyst deactivation [9,10].
Among noble metal catalysts, Pd catalysts supported on Al2O3, SiO2, MgO, CaO, and rare earth metal oxides have been used in POM [11,12]. The catalytic activity and stability can be improved by adding some promoters. For instance, Ryu et al. investigated the addition of CeO2, BaO, and SrO on the catalytic performance of Pd/Al2O3 for POM, and found that the optimum catalyst was a triply promoted Pd catalyst, namely Pd(2)/CeO2(23)/BaO(11)/SrO(0.8)/Al2O3 [13].
Because POM is performed under very high space velocity, the inner diffusion and reaction inside the pores of the catalysts are limited [14]. Therefore, it is desirable to disperse the active species on the outer surface of the catalyst as far as possible. Egg-shell catalysts can satisfy such a need. Besides, the cost of catalysts can be significantly lowered when adopting the egg shell design. In recent years, Rh [15,16] and Ni [14,17,18] egg-shell catalysts have been investigated in POM. For instance, Chen and co-workers compared the performance of egg-shell and uniform Ni/Al2O3 catalysts in POM, and found that egg-shell Ni/Al2O3 was more active due to the distribution of nickel component in the outer region of particles [17].
Herein, a Pd/Al2O3 egg-shell catalyst and its modified versions were tested in POM. The Pd/Al2O3 egg-shell catalyst showed higher activity than a conventional Pd/Al2O3, and the addition of CaO and/or La2O3 additives can significantly improve the stability on stream due to suppressed carbon deposition and phase transformation of the Al2O3 support.

2. Results and Discussion

Figure 1 shows the photos of the prepared egg-shell catalysts before reduction, highlighting the cross section.
Figure 1. Photos showing the cross section of the prepared egg-shell catalysts. Left: PdO/Al2O3; Right: PdO/La2O3/CaO/Al2O3.
Figure 1. Photos showing the cross section of the prepared egg-shell catalysts. Left: PdO/Al2O3; Right: PdO/La2O3/CaO/Al2O3.
Molecules 18 08289 g001
The outer surface was dark brown and the inner part of the particles was white, suggesting the accumulation of Pd species on the catalyst surface. The average thickness of the Pd-rich eggshell was approximately 0.2 mm. The catalysts after reduction also showed the egg-shell structure, as seen from the grey-pale black color of the shell while white color at the center.
Table 1 summarizes the specific surface areas of support (calcined at 1,000 °C) and egg-shell catalyst samples reduced at 750 °C. The surface area of Pd/Al2O3 egg-shell catalyst was lower than its corresponding Al2O3 support, probably due to the blockage of the pores by loading Pd as well as some degradation of the support as a result of the catalyst preparation procedure [19]. The addition of MgO, CaO, La2O3, or CaO and La2O3 into Pd/Al2O3 could retain a higher surface area.
Table 1. Specific surface areas of support (calcined at 1,000 °C) and egg-shell catalyst samples reduced at 750 °C.
Table 1. Specific surface areas of support (calcined at 1,000 °C) and egg-shell catalyst samples reduced at 750 °C.
SampleSpecific surface area (m2/g)
Al2O3118
Pd/Al2O358
Pd/MgO/Al2O399
Pd/CaO/Al2O378
Pd/La2O3/Al2O378
Pd/La2O3/CaO/Al2O3102
Figure 2 shows the performance of Pd/Al2O3 egg-shell catalyst in POM reaction as a function of reaction temperature.
Figure 2. Catalytic performance of Pd/Al2O3 egg-shell catalyst in POM reaction at different temperatures.
Figure 2. Catalytic performance of Pd/Al2O3 egg-shell catalyst in POM reaction at different temperatures.
Molecules 18 08289 g002
The CH4 conversion increased with the reaction temperature and reached 72% at 750 °C. For comparison, the CH4 conversion on a regular Pd/Al2O3 catalyst with the same Pd loading (0.2%) was 49% at 750 °C, demonstrating the advantage of the egg shell design. The CH4 conversion on Pd/Al2O3 egg-shell catalyst decreased when the reaction temperature was above 750 °C, due to the accelerated carbon deposition at high temperatures.
Figure 3 shows the CH4 conversion on various egg-shell catalysts at 750 °C as a function of time on stream. The initial CH4 conversions on these catalysts were comparable, ranging from 67% to 73%. However, the deactivation behaviors were quite different. Pd/Al2O3 egg-shell catalyst deactivated quickly on stream, as seen by the dropping of CH4 conversion from 72% to 40% after operation for 10 h. The addition of MgO barely changed the quick deactivation, whereas the addition of CaO and/or La2O3 significantly suppressed the deactivation. In particular, Pd/La2O3/CaO/Al2O3 egg-shell catalyst showed the best stability: the CH4 conversion changed from 70% to 62% after operation for 10 h.
Figure 3. Performance of the egg-shell catalysts as a function of time on stream in POM reaction. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Figure 3. Performance of the egg-shell catalysts as a function of time on stream in POM reaction. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Molecules 18 08289 g003
Figure 4. Selectivity to CO and H2 on Pd/La2O3/CaO/Al2O3 egg-shell catalyst in POM reaction.
Figure 4. Selectivity to CO and H2 on Pd/La2O3/CaO/Al2O3 egg-shell catalyst in POM reaction.
Molecules 18 08289 g004
Figure 4 shows the H2 selectivity and CO selectivity on Pd/La2O3/CaO/Al2O3 egg-shell catalyst as a function of time on stream. The H2 selectivity and CO selectivity were about 85% and 91%, respectively.
One reason for catalyst deactivation in the POM process is the deposition of carbon [20]. Indeed, the outer surface of the spent catalysts turned into black, indicating the deposition of carbon during the course of reaction. Therefore, TGA was employed to characterize the spent catalysts. As shown in Figure 5, all the samples showed an obvious weight loss from ca. 600 °C to 750 °C, attributing to the oxidation of deposited carbon, most likely graphitic carbon [21]. Interestingly, the amounts of deposited coke were different with different spent egg-shell catalysts: those on Pd/CaO/Al2O3 (4.3%), Pd/La2O3/Al2O3 (3.4%), and Pd/La2O3/CaO/Al2O3 (2.0%) were much less than those on Pd/Al2O3 (10.7%) and Pd/MgO/Al2O3 (12.1%), correlating nicely with the deactivation behaviors.
Figure 5. TG curves of the spent egg-shell catalysts collected after operation for 10 h. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Figure 5. TG curves of the spent egg-shell catalysts collected after operation for 10 h. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Molecules 18 08289 g005
Another reason for catalyst deactivation in POM process is the phase transformation of Al2O3 [22]. Figure 6 shows the XRD patterns of the support (calcined at 1,000 °C) and egg-shell catalysts reduced at 750 °C. The characteristic diffraction peaks of Al2O3 support calcined at 1,000 °C (Figure 6a) were at 31.5°, 32.9°, 36.8°, 39.8°, 45.6°, and 67.3°, corresponding to δ phase (JCPDS 4-877). For Pd/Al2O3 catalyst, Pd diffractions were not found since its loading was low (0.2%) and only Al2O3 peaks were visible (Figure 6b). Pd/MgO/Al2O3 (Figure 6c) showed characteristic diffraction peaks shifted to the direction in lower values of 2θ due to the substitution of Al3+ by Mg2+ [23]. Pd/CaO/Al2O3 (Figure 6d) showed no diffraction peaks of CaO, indicating the high dispersion of CaO in the corresponding catalyst. Peaks at 23.5°, 33.4°, 41.2°, 47.9°, 54.1°, 60.0°, 70.1° in the pattern of Pd/La2O3/Al2O3 (Figure 6e) were ascribed to the formation of LaAlO3 (JCPDS 31-22) at high temperatures [24]. The characteristic diffraction peaks of Pd/La2O3/CaO/Al2O3 (Figure 6f) were similar to those of Pd/La2O3/Al2O3 (Figure 6e), again without the peaks of CaO species.
Figure 6. XRD patterns of support and egg-shell catalysts reduced at 750 °C. (a) Al2O3; (b) Pd/Al2O3; (c) Pd/MgO/Al2O3; (d) Pd/CaO/Al2O3; (e) Pd/La2O3/Al2O3; (f) Pd/La2O3/CaO/Al2O3.
Figure 6. XRD patterns of support and egg-shell catalysts reduced at 750 °C. (a) Al2O3; (b) Pd/Al2O3; (c) Pd/MgO/Al2O3; (d) Pd/CaO/Al2O3; (e) Pd/La2O3/Al2O3; (f) Pd/La2O3/CaO/Al2O3.
Molecules 18 08289 g006
Figure 7 shows the XRD patterns of spent egg-shell catalysts. The diffraction peaks due to α-Al2O3 (JCPDS 10-0173) of the used Pd/Al2O3 catalyst appeared as shown in Figure 7a. Meanwhile, the diffraction peaks attributed to δ-Al2O3 became weaker, indicating the partial transformation from δ-Al2O3 into α-Al2O3 phase during POM. The addition of Mg slightly impeded the phase transformation of Al2O3, whereas the addition of CaO and/or La2O3 dramatically inhibited the phase transformation of Al2O3. The inhibition of phase transformation of Al2O3 by addition of La was probably due to the formation of LaAlO3 in Al2O3 surface. Chen and co-workers found that the deactivation of egg-shell Ni/MgO-Al2O3 catalyst in POM was due to the formation of NiO-MgO solution and/or NiAl2O4, phase transformation, and sintering [14].
Figure 7. XRD patterns of spent egg-shell catalysts collected after operation for 10 h. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Figure 7. XRD patterns of spent egg-shell catalysts collected after operation for 10 h. (a) Pd/Al2O3; (b) Pd/MgO/Al2O3; (c) Pd/CaO/Al2O3; (d) Pd/La2O3/Al2O3; (e) Pd/La2O3/CaO/Al2O3.
Molecules 18 08289 g007

3. Experimental

3.1. Catalyst Preparation

Preparation of PdO/Al2O3, PdO/MgO/Al2O3, and PdO/CaO/Al2O3 egg-shell samples: γ-Al2O3 Raschig rings purchased from Yixing YiPu Catalyst Company (Yixing, China) were pre-calcined at 1,000 °C for 2 h and then crushed to 1.0–1.3 mm particles. Al2O3 particles (5 g) were impregnated with an aqueous solution of Pd precursor by the previously described preparation method [19]. The obtained materials were calcined at 500 °C for 2 h to obtain PdO/Al2O3. The PdO/Al2O3 samples were impregnated with an aqueous solution of Mg(NO3)2 or Ca(NO3)2 at room temperature by an incipient impregnation method, and then calcined at 500 °C for 2 h to obtain PdO/MgO/Al2O3 and PdO/CaO/Al2O3, respectively. For the preparation of PdO/La2O3/Al2O3 and PdO/La2O3/CaO/Al2O3, pre-calcined Al2O3 particles (5 g) were impregnated with an aqueous solution of La(NO3)3 and then calcined to obtain La2O3/Al2O3 supports. The supports were impregnated with an aqueous solution of Pd precursor by the preparation method provided by [19] and then calcined at 500 °C for 2 h for the preparation of egg-shell PdO/La2O3/Al2O3 samples. The above PdO/La2O3/Al2O3 was impregnated with an aqueous solution of Ca(NO3)2, and then calcined at 500 °C for 2 h to obtain PdO/La2O3/CaO/Al2O3. The Pd loading contents were 0.2% (wt %) in all catalysts. The weight ratios of the additive La, Mg, and Ca to Al2O3 were 0.1, 0.05, and 0.05, respectively.

3.2. Catalyst Characterization

The powder X-ray diffraction (XRD) patterns were recorded on a Bruker Advance diffractometer (Bruker, Karlsruhe, Germany) with a Cu Kα monochromatic radiation operated at 40 kV and 40 mA, using a scanning range 2θ between 10° and 90°.
The BET surface areas of the support materials and catalysts were measured by N2 adsorption at −196 °C using a Micromeritics ASAP 2020 instrument (Micromeritics, Norcross, GA, USA). The samples were outgassed under N2 flow at 300 °C for 2 h before the measurements.
The amount of carbon deposited on the catalysts after reaction was determined on a Pyris Diamond TG instrument (PerkinElmer, Waltham, MA, USA) by heating the samples from room temperature to 1,000 °C (heating rate 10 °C/min) in a flowing air (25 mL/min).

3.3. Catalytic Test

The POM reaction was carried out in a continuous flow reactor apparatus equipped with a quartz tube reactor operated at atmospheric pressure. The flow rate of gases was controlled by mass flow controllers. The catalysts (0.5 g) were firstly reduced in a 60 mL/min H2 flow at 750 °C for 30 min, then a 60 mL/min Ar flow was introduced to flush the system. Afterwards, a mixture of CH4 (99.9%, 277.8 mL/min) and O2 (99.999%, 138.9 mL/min) with a molar ratio of 2:1 at weight hour space velocity (WHSV) of 5 × 104 mL·g1·h1 was introduced. The product gases were analyzed online by a gas chromatograph equipped with a TCD detector and TDX-01 packed column. Water was trapped before gases entered the gas chromatograph.

4. Conclusions

A series of Pd/Al2O3-based egg-shell catalysts were tested in the partial oxidation of methane. The addition of MgO, CaO, or La2O3 additives had no dramatic effect on the initial CH4 conversion. The addition of MgO additive had no effect on the catalyst stability, whereas the addition of CaO and/or La2O3 significantly improved the catalyst stability because they suppressed the formation of carbon deposit and phase transformation of the Al2O3 support. More experiments should be done in the future to understand why the addition of certain additives could suppress the deposition of carbon.

Acknowledgments

S.H. Zhou thanks the Ministry of Science and Technology of China (Grant No. 2012DFA40550) for its financial support. Z. Ma acknowledges the financial support by National Natural Science Foundation of China (Grant Nos. 21007011 and 21177028), the Ph.D. Programs Foundation of the Ministry of Education in China (Grant No. 20100071120012), and the Overseas Returnees Start-Up Research Fund of the Ministry of Education in China.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Bitsch-Larsen, A.; Horn, R.; Schmidt, L.D. Catalytic partial oxidation of methane on rhodium and platinum: Spatial profiles at elevated pressure. Appl. Catal. A 2008, 348, 165–172. [Google Scholar] [CrossRef]
  2. Nurunnabi, M.; Mukainakano, Y.; Kado, S.; Li, B.T.; Kunimori, K.; Suzuki, K.; Fujimoto, K.; Tomishige, K. Additive effect of noble metals on NiO-MgO solid solution in oxidative steam reforming of methane under atmospheric and pressurized conditions. Appl. Catal. A 2006, 299, 145–156. [Google Scholar] [CrossRef]
  3. Kikuchi, E.; Chen, Y. Syngas formation by partial oxidation of methane in palladium membrane reactor. Stud. Surf. Sci. Catal. 1998, 119, 441–446. [Google Scholar] [CrossRef]
  4. Qin, D.Y.; Lapszewicz, J.; Jiang, X.Z. Comparison of partial oxidation and steam-CO2 mixed reforming of CH4 to syngas on MgO-supported metals. J. Catal. 1996, 159, 140–149. [Google Scholar] [CrossRef]
  5. York, A.P.E.; Xiao, T.C.; Green, M.L.H. Brief overview of the partial oxidation of methane to synthesis gas. Top. Catal. 2003, 22, 345–358. [Google Scholar] [CrossRef]
  6. Enger, B.C.; Lødeng, R.; Holmen, A. A review of catalytic partial oxidation of methane to synthesis gas with emphasis on reaction mechanisms over transition metal catalysts. Appl. Catal. A 2008, 346, 1–27. [Google Scholar] [CrossRef]
  7. Tsang, S.C.; Claridge, J.B.; Green, M.L.H. Recent advances in the conversion of methane to synthesis gas. Catal. Today 1995, 23, 3–15. [Google Scholar] [CrossRef]
  8. Lanza, R.; Velascoa, J.A.; Järås, S.G. Recent Developments and Achievements inPartial Oxidation of Methane with andwithout Addition of Steam. In Catalysis; Spivey, J.J., Dooley, K.M., Eds.; The Royal Society of Chemistry: Cambridge, UK, 2011; Volumn 23, pp. 50–95. [Google Scholar]
  9. Yang, S.W.; Kondo, J.N.; Hayashi, K.; Hirano, M.; Domen, K.; Hosono, H. Partial oxidation of methane to syngas over promoted C12A7. Appl. Catal. A 2004, 277, 239–246. [Google Scholar] [CrossRef]
  10. Choque, V.; Homs, N.; Cicha-Szot, R.; de la Piscina, P.R. Study of ruthenium supported on Ta2O5-ZrO2 and Nb2O5-ZrO2 as catalysts for the partial oxidation of methane. Catal. Today 2009, 142, 308–313. [Google Scholar] [CrossRef]
  11. Choudhary, V.R.; Prabhakar, B.; Rajput, A.M.; Mamman, A.S. Oxidative conversion of methane to CO and H2 over Pt or Pd containing alkaline and rare earth oxide catalysts. Fuel 1998, 77, 1477–1481. [Google Scholar] [CrossRef]
  12. Bhattacharya, A.K.; Breach, J.A.; Chand, S.; Ghorai, D.K.; Hartridge, A.; Keary, J.; Mallick, K.K. Selective oxidation of methane to carbon monoxide on supported palladium catalyst. Appl. Catal. A 1992, 80, L1–L5. [Google Scholar]
  13. Ryu, J.H.; Lee, K.Y.; Kim, H.J.; Yang, J.I.; Jung, H. Promotion of palladium-based catalysts on metal monolith for partial oxidation of methane to syngas. Appl. Catal. B 2008, 80, 306–312. [Google Scholar] [CrossRef]
  14. Qiu, Y.J.; Chen, J.X.; Zhang, J.Y. Effect of calcination temperature on properties of eggshell Ni/MgO-Al2O3 catalyst for partial oxidation of methane to syngas. Catal. Lett. 2009, 127, 312–328. [Google Scholar] [CrossRef]
  15. Vella, L.D.; Montini, T.; Specchia, S.; Fornasiero, P. Fixed beds of Rh/Al2O3-based catalysts for syngas production in methane SCT-GPO reactors. Int. J. Hydrogen Energy 2011, 36, 7776–7784. [Google Scholar] [CrossRef]
  16. Specchia, S.; Vella, L.D.; de Rogatis, L.; Montini, T.; Specchia, V.; Fornasiero, P. Rh-based catalysts for syngas production via SCT-CPO reactors. Catal. Today 2010, 155, 101–107. [Google Scholar] [CrossRef]
  17. Qiu, Y.J.; Chen, J.X.; Zhang, J.Y. Influence of nickel distribution on properties of spherical catalysts for partial oxidation of methane to synthesis gas. Catal. Commun. 2007, 8, 508–512. [Google Scholar] [CrossRef]
  18. Qiu, Y.J.; Chen, J.X.; Zhang, J.Y. Effects of CeO2 and CaO composite promoters on the properties of eggshell Ni/MgO-Al2O3 catalysts for partial oxidation of methane to syngas. React. Kinet. Catal. Lett. 2008, 94, 351–357. [Google Scholar] [CrossRef]
  19. Liu, Z.N.; Zhou, S.H.; Hou, M.B.; Xie, Z.K.; Zhu, H.Y. First-stage selective hydrogenation catalyst for pyrolysis gasaline. Chinese Patent CN1443829A, 24 September 2003. [Google Scholar]
  20. Dissanayake, D.; Rosynek, M.P.; Kharas, K.C.C.; Lunsford, J.H. Partial oxidation of methane to carbon monoxide and hydrogen over a Ni/Al2O3 catalyst. J. Catal. 1991, 132, 117–127. [Google Scholar]
  21. Zhang, Z.L.; Verykios, X.E. Carbon dioxide reforming of methane to synthesis gas over supported Ni catalysts. Catal. Today 1994, 21, 589–595. [Google Scholar] [CrossRef]
  22. Zhang, Y.H.; Xiong, G.X.; Sheng, S.S.; Yang, W.S. Deactivation studies over NiO/γ-Al2O3 catalysts for partial oxidation of methane to syngas. Catal. Today 2000, 63, 517–522. [Google Scholar] [CrossRef]
  23. Jing, S.Y.; Lin, L.B.; Huang, N.K.; Zhang, J.; Lu, Y. Investigation on lattice constants of Mg-Al spinels. J. Mater. Sci Lett. 2000, 19, 225–227. [Google Scholar] [CrossRef]
  24. Shi, C.K.; Zhang, P. Effect of a second metal (Y, K, Ca, Mn or Cu) addition on the carbon dioxide reforming of methane over nanostructured palladium catalysts. Appl. Catal. B 2012, 115–116, 190–200. [Google Scholar] [CrossRef]
  • Sample Availability: Samples of the compounds are available from the authors.

Share and Cite

MDPI and ACS Style

Wang, J.; Yu, H.; Ma, Z.; Zhou, S. Enhanced Stability of CaO and/or La2O3 Promoted Pd/Al2O3 Egg-Shell Catalysts in Partial Oxidation of Methane to Syngas. Molecules 2013, 18, 8289-8297. https://doi.org/10.3390/molecules18078289

AMA Style

Wang J, Yu H, Ma Z, Zhou S. Enhanced Stability of CaO and/or La2O3 Promoted Pd/Al2O3 Egg-Shell Catalysts in Partial Oxidation of Methane to Syngas. Molecules. 2013; 18(7):8289-8297. https://doi.org/10.3390/molecules18078289

Chicago/Turabian Style

Wang, Jinlong, Hongbo Yu, Zhen Ma, and Shenghu Zhou. 2013. "Enhanced Stability of CaO and/or La2O3 Promoted Pd/Al2O3 Egg-Shell Catalysts in Partial Oxidation of Methane to Syngas" Molecules 18, no. 7: 8289-8297. https://doi.org/10.3390/molecules18078289

APA Style

Wang, J., Yu, H., Ma, Z., & Zhou, S. (2013). Enhanced Stability of CaO and/or La2O3 Promoted Pd/Al2O3 Egg-Shell Catalysts in Partial Oxidation of Methane to Syngas. Molecules, 18(7), 8289-8297. https://doi.org/10.3390/molecules18078289

Article Metrics

Back to TopTop