Next Article in Journal
PTHrP Modulates the Proliferation and Osteogenic Differentiation of Craniofacial Fibrous Dysplasia-Derived BMSCs
Next Article in Special Issue
Polyurethanes Modified by Ionic Liquids and Their Applications
Previous Article in Journal
Influence of Simulated Microgravity on Mammary Epithelial Cells Grown as 2D and 3D Cultures
Previous Article in Special Issue
Ionic Liquid-Supported Photocatalysts: A Reusable Environmentally Friendly Oxidation Reaction System That Uses Air and Light
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis of Ammonium-Based ILs with Different Lengths of Aliphatic Chains and Organic Halogen-Free Anions as Corrosion Inhibitors of API X52 Steel

by
Emiliano Cornejo Robles
1,
Octavio Olivares-Xometl
2,
Natalya V. Likhanova
3,
Paulina Arellanes-Lozada
2,
Irina V. Lijanova
1,* and
Víctor Díaz-Jiménez
2
1
CIITEC, Instituto Politécnico Nacional, Cerrada Cecati S/N, Colonia Santa Catarina de Azcapotzalco, Ciudad de Mexico 02250, Mexico
2
Facultad de Ingeniería Química, Benemérita Universidad Autónoma de Puebla, Av. San Claudio y 18 Sur, Ciudad Universitaria, Col. San Manuel, Puebla 72570, Mexico
3
Programa de Investigación y Posgrado, Instituto Mexicano del Petróleo, Eje Central Norte Lázaro Cárdenas No. 152, Col. San Bartolo Atepehuacan, G. A. Madero, Ciudad de Mexico 07730, Mexico
*
Author to whom correspondence should be addressed.
Int. J. Mol. Sci. 2023, 24(8), 7613; https://doi.org/10.3390/ijms24087613
Submission received: 21 March 2023 / Revised: 10 April 2023 / Accepted: 18 April 2023 / Published: 20 April 2023
(This article belongs to the Special Issue Advances in Ionic Liquids and Their Various Applications)

Abstract

:
In the present work, synthesis and characterization of 15 ionic liquids (ILs) derived from quaternary ammonium and carboxylates were carried out in order to proceed to their evaluation as corrosion inhibitors (CIs) of API X52 steel in 0.5 M HCl. Potentiodynamic tests confirmed the inhibition efficiency (IE) as a function of the chemical configuration of the anion and cation. It was observed that the presence of two carboxylic groups in long linear aliphatic chains reduced the IE, whereas in shorter chains it was increased. Tafel-polarization results revealed the ILs as mixed-type CIs and that the IE was directly proportional to the CI concentration. The compounds with the best IE were 2-amine-benzoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AA]), 3-carboxybut-3-enoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AI]), and dodecanoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AD]) within the 56–84% interval. Furthermore, it was found that the ILs obeyed the Langmuir adsorption isotherm model and inhibited the corrosion of steel through a physicochemical process. Finally, the surface analysis by scanning electron microscopy (SEM) confirmed less steel damage in the presence of CI due to the inhibitor–metal interaction.

Graphical Abstract

1. Introduction

Not only due to its physicochemical properties but also to economic factors and easy access, carbon steel is widely used in different sectors of the oil-and-gas industry. Despite displaying good mechanical resistance in the case of different shear-stress sources, this material is susceptible to suffering corrosion damage when exposed to corrosive media. API X52 is a type of carbon steel that is employed in the production of pipelines for transporting oil and gas [1]. At the industrial level, there are different aggressive media for API X52 steel, which have been classified as sweet, sour, and acid, where organic and inorganic substances, salts, and gases, among other compounds, can be found [2,3,4]. In this context, acid media are employed to increase the amount of extracted oil; this technique is known as stimulation through acidification, where acid solutions ranging from 5 to 28 wt.% of HCl are injected in order to modify the permeability of the reservoir rock, thus easing the oil flow [5]. Notwithstanding, the use of such a technique provokes a significant problem of internal corrosion in oil pipelines due to the presence of HCl [6]. In acid media, the medium aggressiveness depends on variables such as pH, temperature, flow regime, steel composition, pressure, etc. [7,8]. For this reason, steel corrosion is a complex process that is hard to control and understand [9,10].
Because of the importance of extending the useful life of steel, different methods against corrosion have been developed [11]. In this context, the synthesis and application of organic-type corrosion inhibitors (CIs) in different corrosive media is very common due to their easy use and low cost [12,13,14]. Notwithstanding, their employment is reduced to polar electrolytes because of their limited solubility, high volatility, non-biodegradability, and environment-hazardous features [15]. These disadvantages and present environmental regulations have promoted the implementation of new Cis known as ionic liquids (Ils), which have earned a well-deserved place due to their versatile structures, where heteroatoms such as nitrogen and oxygen define electronic densities and, at the same time, either aliphatic chains or aromatic rings provide hydrophobic features. Within the large number of possible combinations, halide-free Ils are specially promising as environmentally friendly Cis due to their green properties [16]. Among the different Ils, imidazolium-based compounds have been employed to mitigate the corrosion effects on metallic surfaces in different processes related to oil, desalination, and acid-cleaning applications [17,18]. In most cases, halogen-containing anions form part of ILs, and only a few works have reported on the use of halogen-free ILs, like the one by Chen et al., where compounds with ammonium-dibutyl-dithiophosphate anions displayed anti-corrosion performance [19,20]. Recently, ammonium-based ILs have reached the vanguard position thanks to their excellent inhibition properties, chemical stability, biodegradability, and low-cost production [21,22,23,24]. In general, tertiary amines are used to synthesize ammonium-based ILs, where the length of cationic aliphatic chains plays a major role in the inhibition process, without discarding the influence of the anionic part. Heteroatoms and π electrons of dimeric quaternary ammonium salts have been identified as favorable factors for efficient corrosion protection in strong acid media [25]. For instance, Likhanova et al. showed that the molecular orientation to metallic surfaces through high-density zones, represented either by organic (adipate) or inorganic (ethyl-sulfate) anionic structures of ammonium-based ILs, enhanced the anticorrosion effect (70–80%) [26]. In this context, another research work compared the aliphatic chains [22,27] of anionic parts formed by different dicarboxylic acids and found Gibbs-adsorption energy values equal to 37.2, 37.2, and 35.1 kJ mol−1, which were attributed to mixed adsorption (physicochemical) [21]. As for triethyl-methyl-ammonium ILs with different anions (either with long aliphatic chains or aromatic rings), they displayed anticorrosion activity in acid medium (H2SO4) above 70% [28]. At this point, it is worth emphasizing that ammonium-based ILs with organic anions are in the trend of green-chemistry conceptuality to diminish the corrosion effect [29]. Zhu et al. synthesized tetrabutyl-ammonium ILs with 14 different amino-acid anions and evaluated their corrosion resistance, finding that the ILs exhibited remarkable friction reduction and anti-wear features [30]. In this context, Aslam et al. reported that amino-acid-ester-salt/saccharine-based ILs worked as powerful green Cis of mild steel in acidic media [31]. From the different types of Ils that have been employed as Cis, most contain heteroatoms (phosphorus, nitrogen, oxygen, and nitrogen), functional groups (–C=N–, –NH2, –OH, –OCH3, –SH, etc.), and alkyl chains with different lengths. As a whole, this IL chemical configuration will define the hydrophilic and nucleophilic parts and establish the interface energy barrier due to either physical or chemical adsorption [32]. Based on the aforementioned, the search for new CIs for the industry is fundamental in order to extend the useful life of steel alloys employed in the transport and refining of oil. As part of these efforts, the present work deals with the synthesis, characterization, and evaluation of a series of 15 new ammonium-derived ILs as CIs of API X52 steel in 0.5 M HCl. The evaluated ILs are different from conventional ones because they present carboxylates and not halides in their anionic structure. The present study emphasized the importance of the chemical configuration of the cation and anion in the ILs, which consisted of different alkyl-chain lengths and functional groups such as amine, ammonium, benzoate, and carboxyl. A corrosion-inhibition mechanism supported by techniques such as polarization resistance (Rp), potentiodynamic polarization (PDP), electrochemical impedance spectroscopy (EIS), scanning electron microscopy/energy dispersive spectroscopy (SEM/EDS), and DFT theoretical calculations (B3LYP/6-311G) was proposed.

2. Results and Discussion

2.1. Characterization of ILs

Table 1 shows the ILs that were synthesized to be evaluated as CIs.
Prior to the evaluation as CIs, the ILs were characterized by the proton (1H) and carbon (13C) nuclear magnetic resonance (NMR) technique by employing a piece of JEOL Eclipse-300 equipment, which uses trimethylsilane (TMS) as a standard for the chemical displacements (ppm) and deuterated chloroform as solvent at ambient temperature. The synthesis of the ILs was confirmed by the FT-IR technique by means of a Nicolet Nexus 470 FT-IR spectrophotometer in attenuated-total-reflection (ATR) mode. The signals obtained for the studied compounds were the following:
Methyl-carbonate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][MC]; C21H45NO3; pasty brown dough; 98.7% yield): IR (KBr, cm−1): 3427, 2920, 2851, 2797, 2663, 1665, 1472, 961, 721. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 3H, CH3), 1.25 (m, 26H, CH2), 1.80 (d, 2H, CH2), 2.67 (s, 2H, CH2), 3.22 (s, 3H, CH3-O), 4.49 (s, 9H, CH3-N). 13C NMR (CDCl3) δH (ppm): 14.04 (CH3), 22.61 (CH2), 23.13 (CH2), 26.75 (CH2), 29.63 (CH2), 31.85 (CH2), 53.33 (O-CH3), 58.10 (CH3-N), 66.83 (CH2-N), 162.59 (C=O).
Butyrate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AB]; C23H49NO2; brown powder; 51.5% yield): IR (KBr, cm−1): 3401, 2929, 1560, 1486, 1417, 966, 717. 1H NMR (CDCl3) δH (ppm): 0.89 (m, 6H, CH3), 1.25 (m, 26H, CH2), 1.55 (m, 2H, CH2), 1.68 (s, 2H, CH2), 2.12 (t, 2H, CH2), 3.24 (s, 9H, CH3-N), 3.33 (t, 2H, CH2-N). 13C NMR (CDCl3) δH (ppm): 14.42 (CH2), 19.91 (CH2), 22.82 (CH2), 23.27 (CH2), 29.85 (CH2), 32.06 (CH2), 40.04 (CH2), 53.30 (CH3-N), 66.79 (CH2-N), 179.28 (C=O).
3-Carboxybut-3-enoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AI]; C24H47NO4 brown powder; 51.1% yield): IR (KBr, cm−1): 3248, 2918, 1702, 1435, 1216, 915. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 3H, CH3), 1.26 (m, 26H, CH2), 1.83 (d, 2H, CH2), 2.85 (s, 2H, CH2), 3.02 (s, 2H, CH2), 3.31 (m, 9H, CH3-N), 5.33 (s, 2H, H2C=C). 13C NMR (CDCl3) δH (ppm): 14.09 (CH3), 22.66 (CH2), 29.34 (CH2), 31.90 (CH2), 43.05 (CH2), 53.37 (CH3-N), 66.92 (CH2-N), 128.35 (C=C), 134.91 (C=C), 168.48 (COOH), 173.18 (COO).
3-Carboxy-2,2-dimethylpropanoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][2,2-DSA]; C25H51NO4; brown powder; 54.3% yield): IR (KBr, cm−1): 3100, 2920, 2848, 2675, 1699, 1432, 1311, 1220, 1141, 933, 627. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 3H, CH3), 1.25 (m, 26H, CH2), 1.34 (m, 6H, CH3), 1.81 (d, 2H, CH2) 2.59 (s, 2H, CH2-N), 2.85 (s, 2H, CH2), 3.25 (s, 9H, CH3-N). 13C NMR (CDCl3) δH (ppm): 14.11 (CH3), 22.68 (CH2), 24.25 (CH2), 26.59 (CH3), 29.07 (CH2), 29.50 (CH2), 31.91 (CH2), 40.16 (CH2), 44.23 (CH2), 53.35 (CH3-N), 66.88 (CH2-N), 174.72 (COOH), 181.19 (COO).
2-Amine-benzoate of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AA]; C26H48N2O2; brown powder; 52.7% yield): IR (KBr, cm−1): 3473, 3375, 3196, 2920, 1671, 1484, 1418, 1303, 1243, 917, 751. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 3H, CH3), 1.25 (m, 26H, CH2), 1.82 (d, 2H, CH2), 3.0 (m, 2H, CH2), 3.3 (s, 9H, CH3-N), 6.64 (t, 1H, Ar), 6.69 (d, 1H, Ar), 6.81 (s, 1H, Ar), 7.28 (t, 2H, Ar-NH2), 7.90 (d,1H, Ar). 13C NMR (CDCl3) δH (ppm): 14.12 (CH3), 22.68 (CH2), 24.24 (CH2), 26.60 (CH2), 29.71 (CH2), 31.92 (CH2), 53.46 (CH3-N), 67.04 (CH2-N), 110.07 (C-Ar), 116.35 (C-Ar), 116.83 (C-Ar), 132.03 (C-Ar), 134.78 (C-Ar), 150.92 (C-Ar), 172.61 (C=O).
Hexanoate of N,N,N-trimethy-lhexadecan-1-ammonium ([THDA+][AH]; C25H53NO2 brown powder; 51.7% yield): IR (KBr, cm−1): 3405, 2933, 2850, 1718, 1461, 1267, 962, 721. 1H NMR (CDCl3) δH (ppm): 0.87 (m, 6H, CH3), 1.25 (m, 30H, CH2), 1.55 (m, 2H, CH2), 1.68 (m, 2H, CH2), 2.12 (t, 2H, CH2), 3.23 (s, 9H, CH3-N), 3.32 (t, 2H, CH2-N). 13C NMR (CDCl3) δH (ppm): 13.82 (CH3), 22.58 (CH2), 23.11 (CH2), 26.26 (CH2), 29.67 (CH2), 31.95 (CH2), 32.03 (CH2), 37.94 (CH2), 53.13 (CH3-N), 66.64 (CH2-N), 179.70 (C=O).
Pentanoate 5-carboxy of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][AAD]; C25H51NO4; brown powder; 38% yield): IR (KBr, cm−1): 3425, 2919, 1691, 1467, 1282, 966, 719. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 3H, CH3), 1.25 (m, 26H, CH2), 1.29 (m, 2H, CH2), 1.35 (m, 2H, CH2), 1.74 (m, 2H, CH2), 2.66 (s, 2, CH2), 2.85 (s, 2H, CH2), 3.02 (m, 2H, CH2-N), 3.37 (s, 9H, CH3-N). 13C NMR (CDCl3) δH (ppm): 14.07 (CH3), 22.64 (CH2), 23.14 (CH2), 24.21 (CH2), 29.08 (CH2), 29.67(CH2), 31,88(CH2), 32.85(CH2), 42.82 (CH3-N), 67.07 (CH2-N), 175.98 (C=O).
Dodecanoate of N,N,N-trimethy-lhexadecan-1-ammonium ([THDA+][AD]; brown powder; C31H65NO2; 45.8% yield): IR (KBr, cm−1): 3487, 2851, 1697, 1432, 1217, 910, 729. 1H NMR (CDCl3) δH (ppm): 0.88 (t, 6H, CH3), 1.25 (m, 44H, CH2), 1.61 (m, 2H, CH2), 2.32 (t, 2H, CH2), 2.87 (s, 2H, CH2), 3.37 (s, 9H, CH3-N). 13C NMR (CDCl3) δH (ppm): 14.04 (CH3), 22.63 (CH2), 23.13 (CH2), 24.80 (CH2), 27.93 (CH2), 29.57 (CH2), 31.86 (CH2), 34.17 (CH2), 42.97 (CH3-N), 66.94 (CH2-N), 178.23 (C=O).
Undecanoate 11-carboxy of N,N,N-trimethyl-hexadecan-1-ammonium ([THDA+][A2D];C31H63NO4; brown powder; 42.7% yield): IR (KBr, cm−1): 3442, 2915, 2852, 1697, 1434, 1282, 927, 723. 1H NMR (CDCl3) δH (ppm): 0.86 (t, 3H, CH3), 1.23 (m, 40H, CH2), 1.55 (m, 4H, CH2), 2.21 (t, 4H, CH2), 3.24 (s, 9H, CH3-N), 3.36 (t, 2H, CH2-N). 13C NMR (CDCl3) δH (ppm): 14.09 (CH3), 22.62 (CH2), 25.63 (CH2), 29.28 (CH2), 31.85 (CH2), 36.03 (CH2), 53.10 (CH3-N), 66.68 (CH2-N), 178.27 (COOH, COO).
3-Carboxybut-3-enoate of N,N,N-trihexyl-N-methyl-ammonium ([TXMA+][AI]; C24H47NO4; brown viscous liquid; 96.1% yield): IR (KBr, cm−1): 3423, 3100, 2958, 2861, 1710, 1566, 1466, 1251, 942, 727, 556. 1H NMR (CDCl3) δH (ppm): 0.87 (t, 9H, CH3), 1.30 (m, 18H, CH2), 1.66 (m, 6H, CH2), 3.10 (s, 3H, CH3-N), 3.26 (m, 6H, CH2-N), 3.29 (s, 2H, CH2), 5.34 (s, 1H, C=CH2), 5.92 (s, 1H, C=CH2). 13C NMR (CDCl3) δH (ppm): 13.77 (CH3), 22.29 (CH2), 25.88 (CH2), 31.08 (CH2), 42.93 (CH2), 48.95 (CH3-N), 61.69 (CH2-N), 123.5 (H2C=C), 139.17 (C=CH2), 172.54 (COOH), 174.32 (COO).
3-Carboxy-2,2-dimethylpropanoate of N,N,N-trihexyl-N-methyl-ammonium ([TXMA+][2,2-DSA]; C25H51NO4; brown viscous liquid; 96% yield): IR (KBr, cm−1): 3432, 2964, 2861, 1713, 1592, 1474, 1304, 1207, 977, 706. 1H NMR (CDCl3) δH (ppm): 0.87 (t, 9H, CH3), 1.20 (t, 6H, CH3), 1.30 (m, 18H, CH2), 1.66 (m, 6H, CH2), 2.47 (s, 2H, CH2), 3.12 (s, 3H, CH3-N), 3.30 (t, 6H, CH2-N), 3.64 (m, 1H, COOH). 13C NMR (CDCl3) δH (ppm): 13.76 (CH3), 22.29 (CH2), 25.89 (CH2), 26.65 (CH3), 31.08 (CH2), 40.91 (CH2), 48.47 (CH3-N), 61.65 (CH2-N), 176.26 (COOH), 181.93 (COO).
2-Amine-benzoate of N,N,N-trihexyl-N-methyl-ammonium ([TXMA+][AA]; C26H48N2O2; brown viscous liquid; 95.7% yield): IR (KBr, cm−1): 3408, 2952, 2864, 1610, 1527, 1471, 1374, 1260, 1157, 753. 1H NMR (CDCl3) δH (ppm): 0.87 (t, 9H, CH3), 1.24 (m, 18H, CH2), 1.51 (m, 6H, CH2), 3.09 (s, 3H, CH3-N), 3.10 (t, 6H, CH2-N), 6.55 (m, 2H, Ar), 7.05 (t, 1H, Ar), 7.33 (s, 2H, Ar-NH2), 7.92 (d, 1H, Ar). 13C NMR (CDCl3) δH (ppm): 13.79 (CH3), 18.34 (CH2), 22.32 (CH2), 25.82 (CH2), 31.15 (CH2), 48.61 (CH3-N), 61.33 (CH2-N), 115.69 (C-Ar), 115.99 (C-Ar), 130.58 (C-Ar), 132.14 (C-Ar), 149.37 (Ar-NH2), 173.12 (COO).
3-Carboxybut-3-enoate of N,N,N-tripentyl-N-methyl-ammonium ([TPMA+][AI]; C21H41NO4; brown viscous liquid; 81% yield): IR (KBr, cm−1): 3432, 2955, 2870, 1919, 1704, 1574, 1466, 1248, 942, 733, 562. 1H NMR (CDCl3) δH (ppm): 0.89 (t, 9H, CH3), 1.34 (m, 12H, CH2), 1.66 (m, 6H, CH2), 3.09 (m, 3H, CH3-N), 3.26 (m, 6H, CH2-N), 3.28 (s, 2H, CH2), 5.35 (s, 1H, C=CH2), 5.92 (s, 1H, C=CH2). 13C NMR (CDCl3) δH (ppm): 13.70 (CH3), 21.89 (CH2), 28.24 (CH2), 42.82 (CH2), 48.46 (CH3-N), 61.68 (CH2-N), 123.44 (C=CH2), 139.03 (C=CH2), 172.54 (COOH), 174.36 (COO).
3-Carboxy-2,2-dimethylpropanoate of N,N,N-tripentyl-N-methyl-ammonium ([TPMA+][2,2-DSA]; C22H45NO4; brown viscous liquid; 85.6% yield): IR (KBr, cm−1): 3432, 3091, 2955, 2867, 1710, 1577, 1251, 942, 736, 544. 1H NMR (CDCl3) δH (ppm): 0.89 (t, 9H, CH3), 1.20 (s, 6H, CH3), 1.34 (m, 12H, CH2), 1.66 (m, 6H, CH2), 3.11 (s, 3H, CH3-N), 3.29 (t, 6H, CH2-N), 3.64 (m, 2H, CH2). 13C NMR (CDCl3) δH (ppm): 13.69 (CH3), 21.90 (CH2), 26.61 (CH3), 28.25 (CH2), 40.91 (CH2), 47.05 (CH2), 48.46 (CH3-N), 61.63 (CH2-N), 176.32 (COOH), 181.95 (COO).
2-Amine-benzoate of N,N,N-tripentyl-N-methyl-ammonium ([TPMA+][AA]; C23H42N2O2; brown viscous liquid; 98% yield): IR (KBr, cm−1): 3405, 3064, 2952, 2873, 1919, 1616, 1533, 1371, 1262, 859, 753, 659. 1H NMR (CDCl3) δH (ppm): 0.85 (t, 9H, CH3), 1.18 (m, 6H, CH2), 1.26 (m, 6H, CH2), 1.48 (m, 6H, CH2), 2.98 (s, 3H, CH3-N), 3.08 (m, 6H, CH2-N), 6.54 (m, 2H, Ar), 7.02 (m, 1H, Ar), 7.33 (s, 2, NH2), 7.92 (m, 1H, Ar). 13C NMR (CDCl3) δH (ppm): 13.71 (CH3), 18.44 (CH2), 21.86 (CH2), 28.16 (CH2), 48.49 (CH3-N), 61.28 (CH2-N), 115.55 (C-Ar), 115.93 (C-Ar), 120.66 (C-Ar), 130.56 (C-Ar), 132.15 (C-Ar), 149.45 (Ar-NH2), 172.82 (COO).

2.2. Rp- and Tafel-Polarization Analysis

Figure 1 shows the polarization-resistance (Rp) and corrosion-current-density (icorr) behavior of API X52 steel employing the ILs as CIs at 100 ppm in 0.5 M HCl by the Rp- and Tafel-polarization techniques, respectively. It can be observed that the presence of all the ILs in the corrosive medium increased the polarization resistance and decreased the corrosion-current density in the metal–electrolyte interface. The charge-transfer processes in the presence of ILs were affected by the formation of a protecting film that reduced the steel-mass loss, which is in good agreement with what has been reported on the evaluation of other ILs as CIs [13].
The group of ILs featuring the cation N,N,N-tripentyl-N-methyl-ammonium [TPMA+] reached the lowest Rp values of 522, 424, and 287 Ω cm2 for [AI, 2,2-DSA and AA], respectively, and accordingly, higher corrosion-current density than the rest of the compounds, thus evidencing less protection of the steel surface. These ILs possess pending groups in their chemical structure that are capable of forming coordinate bonds with the metal surface [33]; despite this fact, there was no synergistic effect between their ions favoring affinity toward the steel surface, which could be related mainly to the short aliphatic chain that promoted a higher degree of inhibitor-covered surface, which displaced water molecules. This fact reveals that the cation and anion chemical structures play a major role during the adsorption mechanism of CIs on the steel active sites in the corrosive medium.
By comparing the group of ILs with cation [TPMA+] with respect to the cation [TXMA+], the importance of the molecular size of the IL cation becomes evident, for the difference between both cations is of one carbon atom in their three aliphatic chains, with five and six carbon atoms, respectively. However, this slight cation difference allowed for the following Rp (Ω cm2) relationships: 684 [TXMA+][AI] > 522 [TPMA+][AI], 646 [TXMA+][2,2-DSA] > 424 [TPMA+][2,2-DSA], and 794 [TXMA+][AA] > 287 [TPMA+][AA]. These results indicate that the increase in aliphatic-chain length favors the CI molecule orientation and adsorption on the steel active sites, giving higher Rp and lower current-density values, which implies a slowing down of the corrosion rate and a reduction in the resistive processes in the metal–solution interface. The interaction between [TPMA+] and [TXMA+] and the API X52 steel surface was limited by the molecular orientation of the hydrophilic part toward the steel surface. Some research works have confirmed that the length of the aliphatic chains in the inhibitor structure is an important factor for its IE [21,34].
Furthermore, in the ILs with cation [THDA+], it was observed that the number of carboxyl groups in the anions positively promoted the CI behavior of these compounds as follows: For anions with very long aliphatic chains, higher Rp values were obtained when there was just one carboxylic group, [AD] > [A2D]. However, this was not the case for anions with short aliphatic chains, where the presence of two carboxylic groups improved the Rp response, [AI] > [AB] and [AAD] > [AH]. The compound [THDA+][AD] revealed the importance of the aliphatic chain (12 carbon atoms), whereas the IL [THDA+][AI] confirmed that in short chains, the presence of two carboxyl groups, improves the performance of the ILs as CIs. According to the structures of the studied ILs, the Rp and icorr behavior is related to the distribution of the electron density in the molecule structure, mainly in the anions.
Figure 2 shows the Rp and Tafel curves of API X52 steel in 0.5 M HCl at 100 ppm of some ILs; similar curves were obtained for the rest of the studied compounds. Regarding the ILs with cation [THDA+], they feature a significant difference with respect to the other ILs, for they had just a single 16-C-aliphatic chain; this change led to a decrease in the Rp slopes and the current density of the Tafel curves with respect to the cations [TXMA+] and [TPMA+], which led to a more efficient blocking of the active sites due to their adsorption on the steel surface, which promoted better properties as CIs [35]. From this group, the ILs with anions [AI] and [AA] presented outstanding results with the lower-current-density Tafel curves. However, the IL with the anion [AA] could be adsorbed more easily on the steel surface due to the presence of heteroatoms such as nitrogen and oxygen (amine and carboxyl groups) and molecule double bonds, which could contribute with higher electron density, and with it, to a higher capacity to interact with the metal surface, thus forming more stable bonds [36]. The CI properties of these ILs with cation [THDA+] depend mainly on the anion chemical structure.
Table 2 presents the electrochemical parameters calculated by linear regression of Rp and linear extrapolation of the Tafel polarization curves of API X52 steel in 0.5 M HCl at 100 ppm of ILs: Rp, corrosion potential (Ecorr), anodic and cathodic Tafel slopes (βa and βc), and icorr. The inhibition efficiency by Rp (IERp) and Tafel curves (IETafel) of the ILs are also reported in Table 2, which were calculated with Equations (1) and (2), respectively:
I E R p = R p C I R p 0 R p C I × 100
I E T a f e l = i c o r r 0 i c o r r C I i c o r r 0 × 100
where the superindexes 0 and CI represent the absence and presence of inhibitor, respectively.
In Table 2, it can be observed that in the presence of ILs the icorr value was lower than that of the blank. Due to the presence of inhibitor, the redox reactions in the metal–corrosive-medium interface were affected by the blocking of the active sites by IL molecules on the steel surface. The displacement of the steel Ecorr in the presence of ILs with respect to the blank was of −8 mV toward the cathodic zone and of +15 mV toward the anodic zone. The Ecorr displacement range with inhibitor indicates that the inhibition process occurred through either a mass-transfer phenomenon in the metal–solution interface or geometrical blocking. In both cases, the active sites are occupied by IL molecules and the rate of the redox reactions is affected by the inhibition process [4,37]. This fact confirms the adsorption of the ILs on the surface of the API X52 steel in both active zones. For this reason, these new ILs can be classified as mixed-type CIs at the evaluated concentration.
Table 2 shows that from the ILs with cation [THDA+], the compounds that displayed the lowest efficiencies were those featuring the anions [MC], [AB], and [AH], which were below 54 ± 3%; the three anions had a short aliphatic-chain length and a single carboxyl group. As for the [THDA+] compounds with anions [2,2-DSA], [AAD], and [A2D], the efficiencies were equal to 72, 72, and 68%, respectively; in comparison with the cation [TXMA+] and anion [AA], whose efficiency was equal to 68%, the IEs were very similar, confirming that both ions affected the corrosion-inhibition properties of the ILs. The highest IE values of 79, 84, and 78% for [THDA+] with [AI], [AA], and [AD], respectively, are related to the chemical structure of the cation and anion. These ion combinations in the ILs allowed their adsorption on surface-active sites and the formation of a physical barrier with nucleophilic and hydrophilic properties capable of repelling medium aggressive ions (O−2, OH, and Cl, among others) that promote the redox reactions of API X52 steel in 0.5 M HCl [38].
Table 3 shows the electrochemical parameters of the ILs with cation [THDA+] and anions [AI], [AA], and [AD] at different concentrations. It can be observed that the icorr values diminished with the increasing concentration of the three evaluated ILs; this phenomenon is associated with higher availability of the CI molecules in the aqueous medium, affinity and orientation toward the metallic surface, and their interaction with corrosion-complex products. These phenomena control the steel redox reactions [39]. Furthermore, the βa and βc values at different CI concentrations do not present a well-defined trend, and some authors have related this behavior to mixed-type CIs [40]. Likewise, the Ecorr displacements of the ILs with respect to the blank toward more negative values confirm the behavior of the compounds as mixed-type CIs with cathodic preference [41].
Figure 3 shows the inhibition-efficiency (IE) behavior as a function of the concentration of the ILs with cation [THDA+] and anions [AI], [AA], and AD] as CIs of API X52 steel in 0.5 M HCl. It can be observed that the IE was directly proportional to the concentration; however, it is clear that at concentrations above 100 ppm, the IE fell slightly. Similar behavior patterns have been reported for ILs featuring carboxylic groups [33].
Even when the carboxylic groups have a rich electronic density and affinity for the metallic surface, an increase in the CI concentration (greater than 100 ppm) does not imply the growth of the EI, since the kinetics of the physicochemical phenomena between the IL chemical structure and steel surface is limited by the active sites of the metallic surface and CI geometric arrangement on this surface.
For the ILs with cation [THDA+] and anions [AI], [AA], and [AD], the IE is a function of the length of the cation (hexadecyl) aliphatic chain and anion pending groups, which provide the nucleophilic and hydrophilic parts [42]. Although the [THDA+][AD] compound has a longer linear chain, its IE was lower than those of [THDA+][AI and AA], evidencing the importance of the anion chemical configuration during the steel corrosion-inhibition process. Finally, it can be concluded that two carboxyl groups in short-chain anions (2 amino-benzoate) and a very long alkyl chain improved the inhibition properties of the ILs with cation [THDA+].

2.3. Electrochemical Impedance Spectroscopy (EIS)

Figure 4a shows the Nyquist diagram obtained from the EIS tests for API X52 steel in 0.5 M HCl with and without [THDA+][AA] at different concentrations. The presence of a semicircle can be observed, which suggests that the corrosion mechanism was controlled by charge transfer [43]. Likewise, all the systems presented capacitive loops with similar shapes, indicating that the addition of different inhibitor concentrations does not modify the adsorption mechanism [44]. Furthermore, an in increase in the semicircle size with the inhibitor concentration was evidenced, suggesting higher protection as a consequence of the growing resistance to charge transfer due to the formation of a film on the steel surface in acid medium [41,45].
With respect to the Bode diagram from the impedance module, it can be observed that at low frequencies, the impedance grew with the CI concentration, which indicates better protection against corrosion [46], whereas the phase angle increased in the presence of [THDA+][AA] due to its adsorption on the steel surface, producing a surface covering in the metal–medium interface [37,47]. The presence of a single time constant, observed in the Bode diagram within a frequency interval ranging from 102 to 103 Hz, shows that the charge-transfer resistance is the phenomenon that prevails in the corrosion process in the presence of inhibitor [48].
Due to the fact that the Nyquist diagrams exhibited depressed semicircles, which are related to the roughness and heterogeneity of the metal surface, the experimental data were fitted by means of an equivalent electrical circuit with one constant phase element (Figure 5) [49]. The equivalent electrical circuit, known as a Randles circuit, presents one resistance to the solution (Rs), one resistance to the charge transfer (Rct), and one constant phase element related to the electrical double layer (CPEdl) [48,49].
The results obtained from fitting the spectra to the circuit are reported in Table 4. It can be observed that the Rs values displayed a slightly significant variation from 2 to 17 Ω cm2, which suggests that the ohmic fall of the experimental tests was minimal [37]. The n values indicate the homogeneity of the surface, where values close to 1 refer to a completely homogeneous surface [48,50]. In this study, n values from 0.86 a 0.9 were obtained, which suggests non-ideal capacitive behavior that is associated with the heterogeneity (irregularity) of the steel surface [7].
As observed in Table 4, Rct was directly proportional to the concentration, which reveals a diminution of the corrosion rate at high concentrations [51]. The highest Rct value was 1319 Ω cm2 at 100 ppm of [THDA+][AA] with respect to that of the blank, which was 134 Ω cm2, indicating the formation of a protecting film on the steel surface due to the adsorption of IL capable of protecting the metal from the corrosive medium [52].
The inhibition efficiency by the EIS (IEEIS) technique was calculated by means of Equation (3) [53]:
I E E I S = R c t R c t 0 R c t × 100
where Rct and R0ct correspond to the charge-transfer resistance with and without CI, respectively. Table 4 shows a maximal inhibition percentage of 89.9% at 100 ppm of [THDA+][AA].

2.4. Adsorption Isotherm

Different studies on the evaluation of CIs for the protection of alloys in corrosive media have reported that the CI molecules are adsorbed on the steel surface by means of a physical or chemical phenomenon [35]. In order to understand which kind of adsorption mechanism is involved, adsorption isotherm models are employed, where the CI surface-coverage degree (θ) is a function of the affinity that the IL molecules have with the steel surface through physical- and chemical-adsorption processes [13,54]. The θ values at different concentrations of the ILs [THDA+][AI, AA, and AD] were calculated (θ = IE/100) from the data of the Rp and Tafel techniques and fitted with the Frumkin, Temkin, and Langmuir adsorption isotherm models [35,55]. The best fit was obtained with the Langmuir isotherm, expressed by Equation (4):
C θ = 1 K a d s + C
where C is the IL concentration and Kads is the adsorption equilibrium constant. The Kads values were obtained by plotting C/θ vs. C, as shown in Figure 6, producing a good fit of the experimental data with a correlation coefficient (R2) close to unity. The obtained Kads values were 131.8, 179.9, and 34.6 M−1 for the ILs [THDA+][AD, AA, and AI], respectively. These values confirm the spontaneous adsorption of the IL molecules on the metallic surface [56].
Kads is associated with the standard Gibbs free energy of adsorption (ΔG0ads), expressed in Equation (5), which is a thermodynamic parameter that is frequently employed to elicit the interaction type between a CI and metallic surface [57]:
Δ G a d s 0 = R T ln ( 55.5 × K a d s )
where R is the universal gas constant and T is the absolute temperature (298.15 K). The ΔG0ads values obtained for the ILs [THDA+][AD, AI, and AA] were −29.2, −26.5, and −29.9 kJ mol−1, respectively. The negative ΔG0ads values are related to spontaneous-adsorption processes between the IL molecules and metallic surface [1]. It has been widely reported that ΔG0ads values between −40 kJ mol−1 and −20 kJ mol−1 imply a physicochemical-adsorption process. The anion in these ILs features a carboxylic group with rich electron density, and for this reason, they can work as active centers that make possible the adsorption on a steel surface [58]. In addition, their π electrons and free electrons of the oxygen atoms can form stable chemical bonds [27]. Notwithstanding, the additional combination of pending groups such as -NH2 and aromatic rings, like in the case of the IL [THDA+][AA], can contribute to electron-density synergy and to the formation of π-type coordination bonds with the metallic surface [12]. Furthermore, thanks to a suitable orientation and position of the carboxyl group, a physical-adsorption process can occur through Van der Waals electrostatic-attraction forces [27,58].

2.5. Surface-Morphology Analysis

To confirm the protection of API X52 steel in 0.5 M HCl by the ILs evaluated as CIs, SEM-EDS surface analyses were carried out. The micrograph in Figure 7a corresponds to the steel surface in the absence of IL, where uniform corrosion damage and irregular topography can be observed; the O and Cl EDS signals were also higher than those in Figure 7b,c, which reveals the steel oxidation through medium aggressive ions (O−2, OH and Cl) that provoke the formation of corrosion products such as oxyhydroxides, iron oxides, and iron chlorides. Figure 7b,c correspond to steel protected with 100 ppm of the ILs [THDA+][AA and AD], respectively. In both micrographs, a regular topography with a slight presence of corrosion products can be observed. The protection of the metallic surface is evident due to the blocking of the active sites and displacement of water molecules by the adsorption of IL molecules on the steel surface, thus reducing the corrosion rate.

2.6. Computer-Simulation Analysis

The quantum chemical calculations of the ILs with the best IE helped better understand the adsorption mechanism through analysis of the reactive sites in each optimized structure, the energy of the molecular orbitals, and other quantum parameters. The inhibiting behavior of the ILs was studied by employing MEP charge distribution and the energy values of the highest occupied molecular orbital (EHOMO) and the lowest unoccupied molecular orbital (ELUMO).
Table 5 shows the optimized structures and molecular-electrostatic-potential (MEP) map of the selected ILs. The structures of the IL anions presented characteristic double bonds (-COO and -COOH) with resonance, as obtained in other theoretical studies of similar structures based on different carboxylic acids, benzene rings, and/or combinations [59,60]. In the case of [AA], it displayed a “flat” benzene ring due to the presence of two functional groups, [-COO and -NH2] [59]. For [AI], the carboxylic groups yielded similar conformations to those described for some acids comparable to those employed during the synthesis [61]. As for the anion [AD], the alkyl chain presented the linear-conformation characteristic of C > 10 chains [62,63]. In the case of cations, the alkyl chains showed the common conformation of ammonium groups that has been reported in other studies [63,64,65]. Regarding the interactions, the -COO bonds in the anions oriented themselves preferably toward the front of the cation methyl groups, as has been found for other anionic species interacting with alkylammonium structures [64,66,67].
As can be observed in Table 5, MEP analysis of the isosurface allowed the regions of the molecule that were reactive sites for electrophilic and nucleophilic attacks to be identified through a color scale [63,68]: The red regions are associated with the most electronegative atoms and resonant rings, which are the molecule sites that are more susceptible to electrophilic attacks, i.e., that cede e to the steel surface to form coordinate bonds with the empty Fe d-orbital. The blue zones are related to sites that are vulnerable before nucleophilic attacks, i.e., that accept e- from other species located in the cation [N+], -NH2 of [AA] and their adjacent carbon atoms. Finally, the green regions are characteristic of groups that are involved in neither nucleophilic nor electrophilic attacks because their configuration is saturated and are located mainly in surrounding H atoms, cation alkyl chains, and particularly in [AD].
The data obtained from the MEP can be complemented by the analysis of molecular orbitals. Since HOMO is the external occupied orbital, it participates as an electron donor due to the presence of elements such as oxygen, which has a free electron pair and is, in general, located at the anion, which was the case of the three ILs analyzed in this work (Table 6). On the other hand, LUMO is the empty internal orbital that works as electron acceptor and is, in most cases, found in ammonium groups and the first adjacent carbon atoms [63]; however, in the particular case of [AA], it was located in the same group because it presented negative and positive heteroatoms, which is in contrast with the evaluated ILs with carboxylic and amine groups.
Table 7 shows the quantum parameters obtained for the IL optimized structures. As for the molecule donor–acceptor activity, it was estimated by means of the energy difference between HOMO and LUMO, which is referred to as the energy gap (ΔGL-H):
Δ G L H = E LUMO E HOMO
According to the literature, low ΔGL-H values suggest higher donor–acceptor activity. Based on the values shown in Table 7, ΔGL-H displayed the following trend based on the anion: [AA] < [AI] < [AD]. Such behavior is related to the number of heteroatoms and the anion complexity. The previous results obtained with respect to the ΔGL-H values are directly associated with the IE, for a low ΔGL-H value implies higher adsorption capacity of a molecule on a steel surface [63].
On the other hand, the highest values of the dipole moment (μ) displayed by the three ILs, in contrast with that of water (1.85 D), are associated with a higher tendency to replace water molecules adsorbed on a steel surface by means of dipole–dipole interactions [63,69].

2.7. Inhibition Mechanism

An inhibition mechanism occurring between the ILs and the metallic surface was proposed to explain the protection action (Figure 8). It should be noted that steel-oxidation products, salts, and molecular hydrogen were formed at the anodic and cathodic centers during the normal corrosion process. The situation changed with the presence of ILs. Probably, the anodic centers of the steel surface interacted with the functional groups of the anionic part of the ILs, where specifically, the carboxylic groups formed either weak bonds or were exchanged with hydroxyl, chlorine, or oxygen ions present in the aqueous solution. At the same time, the cationic part succeeded in forming a precipitation complex with steel-oxidation products, helping diminish the active centers and mitigate the corrosion process. The characteristics of the IL ions that improve their properties for inhibiting metal corrosion are the following: (i) very long aliphatic chains in both anions and cations, (ii) the presence of two carboxyl groups in the anion, and (iii) heteroatoms such as nitrogen and oxygen present in the amine and carboxyl functional groups and double molecular bonds that increase the electron density in the ions, thus forming more stable bonds. Based on the points mentioned above, the synergistic effect exerted by ammonium cations with long aliphatic chains and carboxyl groups in the anionic part of the obtained ILs produced good inhibition results.

3. Materials and Methods

3.1. Synthesis of ILs

For the synthesis of the ILs, analytic-grade reagents with purity above 98% (Sigma-Aldrich, CDMX, Mexico) were used. The ILs were divided into 3 main groups based on the base tertiary amine: dimethyl hexadecyl amine, trihexyl-amine, and tripentyl-amine. The synthesis took place in two stages: (a) A trialkylammonium-methylcarbonate-derived IL was produced by the reaction between a tertiary amine and dimethyl carbonate with a 1:2 molar ratio using methanol as the reaction medium in a Parr ® 4848 reactor at 160 °C for 6 h, and (b) the exchange of the methylcarbonate anion for any of the following carboxylic acids was carried out: 2,2-dimethylsuccinic acid (2,2-DSA), anthranilic acid (AA), hexanoic acid (AH), butyric acid (AB), itaconic acid (AI), dodecanoic acid (AD), dodecanedioic acid (A2D), or adipic acid (AAD). For this purpose, equimolar quantities of the methylcarbonate IL and corresponding acid were stirred using 40 mL of methanol as reaction medium at 40 °C for 30 min. Finally, methanol was removed under vacuum. The synthesis procedure was followed as in previous works [70].

3.2. Materials and Test Solutions

Analytic-grade hydrochloric acid and deionized water were employed to prepare the corrosive medium (0.5 M HCl). Initially, all the ILs were evaluated at a concentration of 100 ppm. Afterward, the compounds with the best IE were further evaluated at 25, 50, 75, and 200 ppm. The selected metallic material was API X52 steel. Prior to each electrochemical test, the metal surface was abraded with SiC emery paper No. 600-1200, followed by a cleaning and drying treatment [71]. In addition, the metal samples used in the SEM surface analyses were polished with 0.05 μm alumina to obtain a mirror-finish surface. The morphology of the surface with and without CI was analyzed using a JEOL-JSM-6300 microscope.

3.3. Electrochemical Techniques

A conventional glass cell was used in the electrochemical tests. This cell consisted of three electrodes: (a) a working electrode (API X52 steel) with a working area of 0.289 cm2, (b) a reference electrode (Ag/AgCl) placed within a Luggin capillary to reduce the ohmic drop, and (c) a counter electrode (high purity platinum, 99.9%). The performed electrochemical tests were Rp and Tafel, both from the open circuit potential (EOCP) obtained after 15 min. For Rp [72], the potential interval ranged from −25 mV to +25 mV vs. EOCP, and for Tafel [73], the interval ranged from −250 mV to +250 mV vs. EOCP, with both tests at a scanning rate of 0.166 mV/s. All the potentiodynamic tests were carried out in triplicate at 298 K (25 °C) in an aerated solution in a potentiostat/galvanostat model PGSTAT302N and employing the software NOVA 2.1.4. EIS tests were carried out at steady state at room temperature with a frequency range of 100 kHz to 10 mHz using a 5 mV sinusoidal signal once the EOCP was stabilized [74].

3.4. DFT Calculations

The inhibitory behavior of ILs was supported by quantum calculations. The three ILs with the best inhibitory behavior were structurally optimized by checking the optimal position without symmetry restriction and in the singlet state (M = 1). The computational calculations were developed under the density-functional theory (DFT) using the Gaussian 09W [75] software based on the B3LYP/6-311G level of the theory. Gauss view v6.0 was used for visualization and generation of input files. When obtaining the optimal structure, the molecular orbitals (MOs) and the dipole moment (μ) of each IL were analyzed.

4. Conclusions

The electrochemical results confirmed the importance of the chemical structure of the ILs and their role as mixed-type CIs. The obtained ∆Gads values suggested a physicochemical-adsorption process on the steel active sites, which diminished the damage of the steel surface.
The cation chemical configuration played a major role in the properties of the ILs evaluated as CIs, obtaining the following cation-based IE order relationship: [THDA+] > [TXMA+] > [TPMA+]. It became evident that the length of the aliphatic chain was a relevant factor in the inhibition of the corrosion of API X52 steel in 0.5 M HCl.
The carboxyl group and the size of the anions were also important variables for good IE: two carboxyl groups in a short linear structure and just a single carboxyl group in longer linear structures improved the inhibiting properties of the ILs as CIs.
The best IE results were displayed by the ILs [THDA+][AA > AI > AD] because the anions, in addition to a carboxyl group, featured two amino-benzoate groups, which represented an additional carboxyl group and a very long linear alkyl chain. These features favored the interaction with the steel surface by forming chemical-type coordinate bonds.

Author Contributions

Conceptualization, I.V.L.; methodology, N.V.L.; software, V.D.-J.; validation, I.V.L., O.O.-X. and N.V.L.; formal analysis, N.V.L.; investigation, E.C.R.; resources, O.O.-X.; data curation, E.C.R., V.D.-J.; P.A.-L.; writing—original draft preparation, E.C.R., I.V.L. and P.A.-L.; writing—review and editing, I.V.L., N.V.L. and O.O.-X.; visualization, N.V.L.; supervision, P.A.-L.; project administration, O.O.-X.; funding acquisition, P.A.-L. and I.V.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

Emiliano Cornejo Robles would like to thank CONACYT for the scholarship granted to pursue postgraduate studies. The authors are grateful to SIP-IPN (Proyecto 20231570) for their financial support and scholarships.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Heydari, M.; Javidi, M. Corrosion inhibition and adsorption behaviour of an amido-imidazoline derivative on API 5L X52 steel in CO2-saturated solution and synergistic effect of iodide ions. Corros. Sci. 2012, 61, 148–155. [Google Scholar] [CrossRef]
  2. Chauhan, D.S.; Quraishi, M.A.; Sorour, A.A.; Verma, C. A review on corrosion inhibitors for high-pressure supercritical CO2 environment: Challenges and opportunities. J. Pet. Sci. Eng. 2022, 215, 110695. [Google Scholar] [CrossRef]
  3. Karimi-Abadeh, H.; Javidi, M. Assessment and influence of temperature, NaCl and H2S on CO2 corrosion behavior of different microstructures of API 5L X52 carbon steel in aqueous environments. J. Nat. Gas Sci. Eng. 2019, 67, 93–107. [Google Scholar] [CrossRef]
  4. Arellanes-Lozada, P.; Díaz-Jiménez, V.; Hernández-Cocoletzi, H.; Nava, N.; Olivares-Xometl, O.; Likhanova, N.V. Corrosion inhibition properties of iodide ionic liquids for API 5L X52 steel in acid medium. Corros. Sci. 2020, 175, 108888. [Google Scholar] [CrossRef]
  5. Finšgar, M.; Jackson, J.; Dehghani, A.; Bahlakeh, G.; Ramezanzadeh, B.; Ramezanzadeh, M. Application of corrosion inhibitors for steels in acidic media for the oil and gas industry: A review. Corros. Sci. 2014, 86, 17–41. [Google Scholar] [CrossRef]
  6. Singh, A.; Ansari, K.R.; Quraishi, M.A.; Banerjee, P. Corrosion inhibition and adsorption of imidazolium based ionic liquid over P110 steel surface in 15% HCl under static and dynamic conditions: Experimental, surface and theoretical analysis. J. Mol. Liq. 2021, 323, 114608. [Google Scholar] [CrossRef]
  7. Abdallah, Y.M.; Shalabi, K.; Bayoumy, N.M. Eco-Friendly synthesis, biological activity and evaluation of some new pyridopyrimidinone derivatives as corrosion inhibitors for API 5L X52 carbon steel in 5% sulfamic acid medium. J. Mol. Struct. 2018, 1171, 658–671. [Google Scholar] [CrossRef]
  8. Shuai, Y.; Shuai, J.; Zhang, X. Experimental and numerical investigation of the strain response of a dented API 5L X52 pipeline subjected to continuously increasing internal pressure. J. Nat. Gas Sci. Eng. 2018, 56, 81–92. [Google Scholar] [CrossRef]
  9. Manrique, E.J.; Mogollon, J.L.; Linares, J.A.; Farrera, M. Basic nitrogen compounds in crude oils: Effect on mineral dissolution during acid stimulation processes. In Proceedings of the SPE International Symposium on Oilfield Chemistry, Houston, TX, USA, 18–21 February 1997; pp. 137–148. [Google Scholar]
  10. Afshari, F.; Ghomi, E.R.; Dinari, M.; Ramakrishna, S. Recent Advances on the Corrosion Inhibition Behavior of Schiff base Compounds on Mild Steel in Acidic Media. ChemistrySelect 2023, 8, e202203231. [Google Scholar] [CrossRef]
  11. Dwivedi, D.; Lepková, K.; Becker, T. Carbon steel corrosion: A review of key surface properties and characterization methods. RSC Adv. 2017, 7, 4580–4610. [Google Scholar] [CrossRef]
  12. Verma, C.; Haque, J.; Ebenso, E.E.; Quraishi, M.A. Melamine derivatives as effective corrosion inhibitors for mild steel in acidic solution: Chemical, electrochemical, surface and DFT studies. Results Phys. 2018, 9, 100–112. [Google Scholar] [CrossRef]
  13. Kobzar, Y.L.; Fatyeyeva, K. Ionic liquids as green and sustainable steel corrosion inhibitors: Recent developments. Chem. Eng. J. 2021, 425, 131480. [Google Scholar] [CrossRef]
  14. Cherrad, S.; Alrashdi, A.A.; Lee, H.-S.; El aoufir, Y.; Lgaz, H.; Satrani, B.; Ghanmi, M.; Aouane, E.M.; Chaouch, A. Cupressus arizonica fruit essential oil: A novel green inhibitor for acid corrosion of carbon steel. Arabian J. Chem. 2022, 15, 103849. [Google Scholar] [CrossRef]
  15. Al-Kaisy, G.M.J.; Mutalib, M.I.A.; Rao, T.V.V.L.N.; Senatore, A. Tribological performance of low viscosity halogen-free ammonium based protic ionic liquids with carboxylate anions as neat lubricants. Tribol. Int. 2021, 160, 107058. [Google Scholar] [CrossRef]
  16. Deyab, M.A. Understanding the anti-corrosion mechanism and performance of ionic liquids in desalination, petroleum, pickling, de-scaling, and acid cleaning applications. J. Mol. Liq. 2020, 309, 113107. [Google Scholar] [CrossRef]
  17. Gurjar, S.; Sharma, S.K.; Sharma, A.; Ratnani, S. Performance of imidazolium based ionic liquids as corrosion inhibitors in acidic medium: A review. Appl. Surf. Sci. Adv. 2021, 6, 100170. [Google Scholar] [CrossRef]
  18. Tecuapa-Flores, D.; Guadalupe Hernández, J.; Reyes Domínguez, I.; Turcio-Ortega, D.A.; Cruz-Borbolla, J.; Thangarasu, P. Understanding of benzimidazole based ionic liquid as an efficient corrosion inhibitor for carbon steel: Experimental and theoretical studies. J. Mol. Liq. 2022, 358, 119204. [Google Scholar] [CrossRef]
  19. Chen, G.; Li, F.; Zhang, C.; Guo, X.; Yang, Z.; Yu, Q.; Yu, B.; Cai, M.; Tian, D. Effect of two halogen-free ionic liquids with different anions on the tribological properties of TC4. J. Mol. Liq. 2021, 343, 117627. [Google Scholar] [CrossRef]
  20. Zhang, C.; Li, F.; Yang, Z.; Wang, X.; Chen, G.; Lu, Z.; Jia, L.; Yu, Q.; Cai, M. Comparing tribology properties of halogen-free ionic liquid, halogen-containing ionic liquid, and PAO 10 lubricants for steel–Al2024 friction contact at room temperature and high temperature. J. Mol. Liq. 2021, 323, 115041. [Google Scholar] [CrossRef]
  21. Olivares-Xometl, O.; Lijanova, I.V.; Likhanova, N.V.; Arellanes-Lozada, P.; Hernández-Cocoletzi, H.; Arriola-Morales, J. Theoretical and experimental study of the anion carboxylate in quaternary-ammonium-derived ionic liquids for inhibiting the corrosion of API X60 steel in 1 M H2SO4. J. Mol. Liq. 2020, 318, 114075. [Google Scholar] [CrossRef]
  22. Kannan, P.; Varghese, A.; Palanisamy, K.; Abousalem, A.S. Probing the effect of newly synthesized phenyltrimethylammonium tetrachloroaluminate ionic liquid as an inhibitor for carbon steel corrosion. Appl. Surf. Sci. Adv. 2021, 6, 100150. [Google Scholar] [CrossRef]
  23. Montalban, M.G.; Hidalgo, J.M.; Collado-Gonzalez, M.; Diaz Banos, F.G.; Villora, G. Assessing chemical toxicity of ionic liquids on Vibrio fischeri: Correlation with structure and composition. Chemosphere 2016, 155, 405–414. [Google Scholar] [CrossRef]
  24. Pham, T.P.; Cho, C.W.; Yun, Y.S. Structural effects of ionic liquids on microalgal growth inhibition and microbial degradation. Environ. Sci. Pollut. Res. Int. 2016, 23, 4294–4300. [Google Scholar] [CrossRef]
  25. Kaczerewska, O.; Leiva-Garcia, R.; Akid, R.; Brycki, B.; Kowalczyk, I.; Pospieszny, T. Heteroatoms and π electrons as favorable factors for efficient corrosion protection. Mater. Corros. 2019, 70, 1099–1110. [Google Scholar] [CrossRef]
  26. Likhanova, N.V.; Arellanes-Lozada, P.; Olivares-Xometl, O.; Lijanova, I.V.; Arriola-Morales, J.; Mendoza-Hérnandez, J.C.; Corro, G. Ionic Liquids with Carboxylic-Acid-Derived Anions Evaluated as Corrosion Inhibitors under Dynamic Conditions. Int. J. Electrochem. Sci. 2019, 14, 2655–2671. [Google Scholar] [CrossRef]
  27. Vinutha, M.R.; Venkatesha, T.V. Review on Mechanistic Action of Inhibitors on Steel Corrosion in Acidic Media. Port. Electrochim. Acta 2016, 34, 157–184. [Google Scholar] [CrossRef]
  28. Likhanova, N.V.; Arellanes-Lozada, P.; Olivares-Xometl, O.; Hernández-Cocoletzi, H.; Lijanova, I.V.; Arriola-Morales, J.; Castellanos-Aguila, J.E. Effect of organic anions on ionic liquids as corrosion inhibitors of steel in sulfuric acid solution. J. Mol. Liq. 2019, 279, 267–278. [Google Scholar] [CrossRef]
  29. Cabeza, O. Chapter 1—Properties and Green Aspects of Ionic Liquids. In Ionic Liquids in Separation Technology; Pérez De Los Ríos, A., Hernández Fernández, F.J., Eds.; Elsevier: Amsterdam, The Netherlands, 2014; pp. 1–93. [Google Scholar]
  30. Zhu, L.; Dong, J.; Zeng, Q.; Chao, M.; Gong, K.; Li, W.; Wang, X. A comprehensive study of amino acids based ionic liquids as green lubricants for various contacts. Tribol. Int. 2021, 162, 107137. [Google Scholar] [CrossRef]
  31. Aslam, R.; Mobin, M.; Huda; Obot, I.M.; Alamri, A.H. Ionic liquids derived from α-amino acid ester salts as potent green corrosion inhibitors for mild steel in 1M HCl. J. Mol. Liq. 2020, 318, 113982. [Google Scholar] [CrossRef]
  32. Berdimurodov, E.; Kholikov, A.; Akbarov, K.; Guo, L.; Kaya, S.; Katin, K.P.; Kumar-Verma, D.; Rbaa, M.; Dagdag, O.; Haldhar, R. Novel bromide–cucurbit[7]uril supramolecular ionic liquid as a green corrosion inhibitor for the oil and gas industry. J. Electroanal. Chem. 2021, 901, 115794. [Google Scholar] [CrossRef]
  33. Quraishi, M.A.; Chauhan, D.S.; Ansari, F.A. Development of environmentally benign corrosion inhibitors for organic acid environments for oil-gas industry. J. Mol. Liq. 2021, 329, 115514. [Google Scholar] [CrossRef]
  34. Verma, C.; Alrefaee, S.H.; Quraishi, M.A.; Ebenso, E.E.; Hussain, C.M. Recent developments in sustainable corrosion inhibition using ionic liquids: A review. J. Mol. Liq. 2021, 321, 114484. [Google Scholar] [CrossRef]
  35. Olivares-Xometl, O.; Likhanova, N.V.; Domínguez-Aguilar, M.A.; Arce, E.; Dorantes, H.; Arellanes-Lozada, P. Synthesis and corrosion inhibition of α-amino acids alkylamides for mild steel in acidic environment. Mater. Chem. Phys. 2008, 110, 344–351. [Google Scholar] [CrossRef]
  36. Verma, C.; Quraishi, M.A.; Ebenso, E.E. Microwave and ultrasound irradiations for the synthesis of environmentally sustainable corrosion inhibitors: An overview. Sustainable Chem. Pharm. 2018, 10, 134–147. [Google Scholar] [CrossRef]
  37. Zehra, S.; Mobin, M.; Aslam, R.; Lgaz, H.; Chung, I.-M. Assessment of biodegradable glycine and glutamic acid based ionic liquids as mild steel corrosion inhibitors in acid solution: An experimental and theoretical approach. J. Mol. Struct. 2021, 1240, 130505. [Google Scholar] [CrossRef]
  38. Ganjoo, R.; Sharma, S.; Thakur, A.; Assad, H.; Kumar-Sharma, P.; Dagdag, O.; Berisha, A.; Seydou, M.; Ebenso, E.E.; Kumar, A. Experimental and theoretical study of Sodium Cocoyl Glycinate as corrosion inhibitor for mild steel in hydrochloric acid medium. J. Mol. Liq. 2022, 364, 119988. [Google Scholar] [CrossRef]
  39. Liao, L.L.; Mo, S.; Luo, H.Q.; Feng, Y.J.; Yin, H.Y.; Li, N.B. Relationship between inhibition performance of melamine derivatives and molecular structure for mild steel in acid solution. Corros. Sci. 2017, 124, 167–177. [Google Scholar] [CrossRef]
  40. Scendo, M.; Uznanska, J. The Effect of Ionic Liquids on the Corrosion Inhibition of Copper in Acidic Chloride Solutions. Int. J. Corros. 2011, 2011, 718626. [Google Scholar] [CrossRef]
  41. Subasree, N.; Selvi, J.A. Imidazolium based ionic liquid derivatives; synthesis and evaluation of inhibitory effect on mild steel corrosion in hydrochloric acid solution. Heliyon 2020, 6, e03498. [Google Scholar] [CrossRef]
  42. Ansari, F.A.; Quraishi, M.A. Inhibitive Performance of Gemini Surfactants as Corrosion Inhibitors for Mild Steel in Formic Acid. Port. Electrochim. Acta 2010, 28, 321–335. [Google Scholar]
  43. Hajjaji, F.E.L.; Salim, R.; Ech-chihbi, E.; Titi, A.; Messali, M.; Kaya, S.; Ibrahimi, B.E.; Taleb, M. New imidazolium ionic liquids as ecofriendly corrosion inhibitors for mild steel in hydrochloric acid (1 M): Experimental and theoretical approach. J. Taiwan Inst. Chem. Eng. 2021, 123, 346–362. [Google Scholar] [CrossRef]
  44. Khamaysa, O.M.A.; Selatnia, I.; Lgaz, H.; Sid, A.; Lee, H.-S.; Zeghache, H.; Benahmed, M.; Ali, I.H.; Mosset, P. Hydrazone-Based green corrosion inhibitors for API grade carbon steel in HCl: Insights from electrochemical, XPS, and computational studies. Colloids Surf. A 2021, 626, 127047. [Google Scholar] [CrossRef]
  45. Corrales-Luna, M.; Le-Manh, T.; Romero-Romo, M.; Palomar-Pardavé, M.; Arce-Estrada, E.-M. 1-Ethyl 3-methylimidazolium thiocyanate ionic liquid as corrosion inhibitor of API 5L X52 steel in H2SO4 and HCl media. Corros. Sci. 2019, 153, 85–99. [Google Scholar] [CrossRef]
  46. Aslam, R.; Mobin, M.; Huda; Shoeb, M.; Murmu, M.; Banerjee, P. Proline nitrate ionic liquid as high temperature acid corrosion inhibitor for mild steel: Experimental and molecular-level insights. J. Ind. Eng. Chem. 2021, 100, 333–350. [Google Scholar] [CrossRef]
  47. Abd-El-Lateef, H.M.; Shalabi, K.; Abdelhamid, A.A. One-Pot synthesis of novel triphenyl hexyl imidazole derivatives catalyzed by ionic liquid for acid corrosion inhibition of C1018 steel: Experimental and computational perspectives. J. Mol. Liq. 2021, 334, 116081. [Google Scholar] [CrossRef]
  48. Kamali-Ardakani, E.; Kowsari, E.; Ehsani, A. Imidazolium-Derived polymeric ionic liquid as a green inhibitor for corrosion inhibition of mild steel in 1.0 M HCl: Experimental and computational study. Colloids Surf. A 2020, 586, 124195. [Google Scholar] [CrossRef]
  49. Kannan, P.; Varghese, A.; Palanisamy, K.; Abousalem, A.S. Evaluating prolonged corrosion inhibition performance of benzyltributylammonium tetrachloroaluminate ionic liquid using electrochemical analysis and Monte Carlo simulation. J. Mol. Liq. 2020, 297, 111855. [Google Scholar] [CrossRef]
  50. Elabbasy, H.M.; Gadow, H.S. Study the effect of expired tenoxicam on the inhibition of carbon steel corrosion in a solution of hydrochloric acid. J. Mol. Liq. 2021, 321, 114918. [Google Scholar] [CrossRef]
  51. Farag, Z.R.; Moustapha, M.E.; Anouar, E.-H.; Abd-El-Hafeez, G.M. The inhibition tendencies of novel hydrazide derivatives on the corrosion behavior of mild steel in hydrochloric acid solution. J. Mater. Res. Technol. 2022, 16, 1422–1434. [Google Scholar] [CrossRef]
  52. Ontiveros-Rosales, M.; Espinoza-Vázquez, A.; Rodríguez Gómez, F.J.; Valdez-Rodríguez, S.; Miralrio, A.; Acosta-Garcia, B.A.; Castro, M. Imidazolate of 1-butyl-3-ethyl imidazole as corrosion inhibitor on API 5L X52 steel in NaCl saturated with CO2. J. Mol. Liq. 2022, 363, 119826. [Google Scholar] [CrossRef]
  53. Deyab, M.A.; Zaky, M.T.; Nessim, M.I. Inhibition of acid corrosion of carbon steel using four imidazolium tetrafluoroborates ionic liquids. J. Mol. Liq. 2017, 229, 396–404. [Google Scholar] [CrossRef]
  54. Migahed, M.A.; El-Rabiei, M.M.; Nady, H.; Elgendy, A.; Zaki, E.G.; Abdou, M.I.; Noamy, E.S. Novel Ionic Liquid Compound Act as Sweet Corrosion Inhibitors for X-65 Carbon Tubing Steel: Experimental and Theoretical Studies. J. Bio- Tribo-Corros. 2017, 3, 31. [Google Scholar] [CrossRef]
  55. Ayawei, N.; Ebelegi, A.N.; Wankasi, D. Modelling and Interpretation of Adsorption Isotherms. J. Chem. 2017, 2017, 3039817. [Google Scholar] [CrossRef]
  56. Dehghani, A.; Bahlakeh, G.; Ramezanzadeh, B.; Ramezanzadeh, M. Potential role of a novel green eco-friendly inhibitor in corrosion inhibition of mild steel in HCl solution: Detailed macro/micro-scale experimental and computational explorations. Constr. Build. Mater. 2020, 245, 118464. [Google Scholar] [CrossRef]
  57. El-Azzouzi, M.; Aouniti, A.; El-Massaoudi, M.; Radi, S.; Hammouti, B.; Quraishi, M.A.; Bendaif, H.; El-Ouadi, Y. Inhibition effect of 1,1´-(pyridine-2,6-dihylbis(methylene))bis(5- methyl-1-H-pyrazole-3-carboxylic acid) on the corrosion of mild steel in 1 M HCl. Part A: Experimental study. Int. J. Corros. Scale Inhib. 2017, 6, 463–475. [Google Scholar]
  58. Cao, S.; Liu, D.; Ding, H.; Wang, J.; Lu, H.; Gui, J. Task-Specific ionic liquids as corrosion inhibitors on carbon steel in 0.5 M HCl solution: An experimental and theoretical study. Corros. Sci. 2019, 153, 301–313. [Google Scholar] [CrossRef]
  59. Mathammal, R.; Jayamani, N.; Geetha, N. Molecular Structure, NMR, HOMO, LUMO, and Vibrational Analysis of O-Anisic Acid and Anisic Acid Based on DFT Calculations. J. Spectrosc. 2013, 2013, 171735. [Google Scholar] [CrossRef]
  60. Kaya, S.; Tüzün, B.; Kaya, C.; Obot, I.B. Determination of corrosion inhibition effects of amino acids: Quantum chemical and molecular dynamic simulation study. J. Taiwan Inst. Chem. Eng. 2016, 58, 528–535. [Google Scholar] [CrossRef]
  61. Rees, R.J.; Lane, G.H.; Hollenkamp, A.F.; Best, A.S. Predicting properties of new ionic liquids: Density functional theory and experimental studies of tetra-alkylammonium salts of (thio)carboxylate anions, RCO2, RCOS and RCS2. Phys. Chem. Chem. Phys. 2011, 13, 10729–10740. [Google Scholar] [CrossRef]
  62. Díaz-Jiménez, V.; Arellanes-Lozada, P.; Likhanova, N.V.; Olivares-Xometl, O.; Chigo-Anota, E.; Lijanova, I.V.; Gómez-Sánchez, G.; Verpoort, F. Investigation of Sulfonium-Iodide-Based Ionic Liquids to Inhibit Corrosion of API 5L X52 Steel in Different Flow Regimes in Acid Medium. ACS Omega 2022, 7, 42975–42993. [Google Scholar] [CrossRef]
  63. Haque, J.; Srivastava, V.; Verma, C.; Lgaz, H.; Salghi, R.; Quraishi, M.A. N-Methyl-N,N,N-trioctylammonium chloride as a novel and green corrosion inhibitor for mild steel in an acid chloride medium: Electrochemical, DFT and MD studies. New J. Chem. 2017, 41, 13647–13662. [Google Scholar] [CrossRef]
  64. Verma, C.; Obot, I.B.; Bahadur, I.; Sherif, E.-S.M.; Ebenso, E.E. Choline based ionic liquids as sustainable corrosion inhibitors on mild steel surface in acidic medium: Gravimetric, electrochemical, surface morphology, DFT and Monte Carlo simulation studies. Appl. Surf. Sci. 2018, 457, 134–149. [Google Scholar] [CrossRef]
  65. Arellanes-Lozada, P.; Hernández-Cocoletzi, H.; Lijanova, I.V.; Olivares-Cuapa, J.C.; Olivares-Cuapa, J.M.; Calvillo-Muñoz, E.Y.; Likhanova, N.V. Effect of sulfonate anions on the performance of triethylmethylammonium-derived ionic liquids as corrosion inhibitors. J. Adhes. Sci. Technol. 2023, 1–25. [Google Scholar] [CrossRef]
  66. Lourenço, T.C.; Barros, L.M.S.; Anchieta, C.G.; Nepel, T.C.M.; Júlio, J.P.O.; Dias, L.G.; Filho, R.M.; Doubek, G.; Da Silva, J.L.F. Tuning aprotic solvent properties with long alkyl chain ionic liquid for lithium-based electrolytes. J. Mater. Chem. A 2022, 10, 11684–11701. [Google Scholar] [CrossRef]
  67. Assenine, M.A.; Haddad, B.; Paolone, A.; Brandán, S.A.; Villemin, D.; Boumediene, M.; Rahmouni, M.; Bresson, S. Experimental and DFT studies on structure, spectroscopic and thermal properties of N-Methyl-N,N,N-trioctylammonium chloride ionic liquid. J. Mol. Struct. 2021, 1230, 129625. [Google Scholar] [CrossRef]
  68. Znini, M.; Ansari, A.; Costa, J.; Senhaji, O.; Paolini, J.; Majidi, L. Experimental, Quantum Chemical and Molecular Dynamic Simulations Studies on the Corrosion Inhibition of C38 Steel in 1M HCl by Anethum graveolens Essential Oil. Anal. Bioanal. Electrochem. 2019, 11, 1426–1451. [Google Scholar]
  69. Jadaa, R.J.; Abd, A.N.; Khadom, A.A. Polyacrylamide as a corrosion inhibitor for mild steel in 2 M phosphoric acid: Experimental and theoretical studies. Chem. Pap. 2021, 75, 5375–5386. [Google Scholar] [CrossRef]
  70. Gómora-Herrera, D.; Lijanova, I.V.; Olivares-Xometl, O.; Toscano, A.; Likhanova, N.V. Synthesis of the symmetrical methylene diesters from carboxylic ionic liquids. Can. J. Chem. 2017, 95, 744–750. [Google Scholar] [CrossRef]
  71. Preparing, Cleaning, and Evaluating Corrosion Test Specimens. ASTMG1-03-(2011); ASTM International: West Conshohocken, PA, USA, 2011.
  72. Conducting Potentiodynamic Polarization Resistance Measurements. ASTMG59-97-(2002); ASTMG59-97-(2002). ASTM International: West Conshohocken, PA, USA, 2002.
  73. Conventions Applicable to Electrochemical Measurements in Corrosion Testing. ASTMG3-89-(1999); ASTM International: West Conshohocken, PA, USA, 1999.
  74. Verification of Algorithm and Equipment for Electrochemical Impedance Measurements. ASTMG106-89-(1999); ASTM International: West Conshohocken, PA, USA, 1999.
  75. Frisch, M.J.; Nakatsuji, H.; Ehara, M.; Toyota, K.; Fukuda, R.; Hasegawa, J.; Ishida, M.; Nakajima, T.; Honda, Y.; Kitao, O.; et al. Gaussian 09, Revision D.01; Gaussian, Inc.: Wallingford, CT, USA, 2013. [Google Scholar]
Figure 1. Rp and icorr values of API X52 steel in 0.5 M HCl and ILs at 100 ppm by the Rp- and Tafel-polarization techniques, respectively.
Figure 1. Rp and icorr values of API X52 steel in 0.5 M HCl and ILs at 100 ppm by the Rp- and Tafel-polarization techniques, respectively.
Ijms 24 07613 g001
Figure 2. Rp and Tafel polarization of API X52 steel in 0.5 M HCl at 100 ppm of ILs with cations [TPMA+], [TXMA+], and [THDA+] and anions: (a,b) [AI], (c,d) [2,2-DSA], and (e,f) [AA].
Figure 2. Rp and Tafel polarization of API X52 steel in 0.5 M HCl at 100 ppm of ILs with cations [TPMA+], [TXMA+], and [THDA+] and anions: (a,b) [AI], (c,d) [2,2-DSA], and (e,f) [AA].
Ijms 24 07613 g002aIjms 24 07613 g002b
Figure 3. Corrosion IE behavior for API X52 steel in 0.5 M HCl at different concentrations of ILs with cation [THDA+].
Figure 3. Corrosion IE behavior for API X52 steel in 0.5 M HCl at different concentrations of ILs with cation [THDA+].
Ijms 24 07613 g003
Figure 4. Impedance spectra of API X52 steel in 0.5 M HCl in the absence and presence of [THDA+][AA] at different concentrations: (a) Nyquist and (b) Bode diagrams.
Figure 4. Impedance spectra of API X52 steel in 0.5 M HCl in the absence and presence of [THDA+][AA] at different concentrations: (a) Nyquist and (b) Bode diagrams.
Ijms 24 07613 g004
Figure 5. Equivalent electrical circuit of the API X52 steel system in corrosive medium in the presence of [THDA+][AA].
Figure 5. Equivalent electrical circuit of the API X52 steel system in corrosive medium in the presence of [THDA+][AA].
Ijms 24 07613 g005
Figure 6. Langmuir adsorption isotherm for API X52 steel in 0.5 M HCl with ILs.
Figure 6. Langmuir adsorption isotherm for API X52 steel in 0.5 M HCl with ILs.
Ijms 24 07613 g006
Figure 7. SEM-EDS micrographs of the API X52 steel surface after 2 h of immersion in 0.5 M HCl: (a) without IL and in the presence of (b) [THDA+][AA] and (c) [THDA+][AD].
Figure 7. SEM-EDS micrographs of the API X52 steel surface after 2 h of immersion in 0.5 M HCl: (a) without IL and in the presence of (b) [THDA+][AA] and (c) [THDA+][AD].
Ijms 24 07613 g007
Figure 8. Inhibition mechanism carried out by the ILs evaluated as CIs of API X52 steel in 0.5 M HCl.
Figure 8. Inhibition mechanism carried out by the ILs evaluated as CIs of API X52 steel in 0.5 M HCl.
Ijms 24 07613 g008
Table 1. Structures of the synthesized ILs.
Table 1. Structures of the synthesized ILs.
AbbreviationNameChemical StructureYield (%)
[THDA+][MC]Methyl-carbonate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00198.7
[THDA+][AB]Butyrate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00251.5
[THDA+][AI]3-Carboxybut-3-enoate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00351.1
[THDA+][2,2-DSA]3-Carboxy-2,2-dimethylpropanoate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00454.3
[THDA+][AA]2-Amine-benzoate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00552.7
[THDA+][AH]Hexanoate of N,N,N-trimethy-l-hexadecan-1-ammoniumIjms 24 07613 i00651.7
[THDA+][AAD]Pentanoate 5-carboxy of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00738.0
[THDA+][AD]Dodecanoate of N,N,N-trimethy-l-hexadecan-1-ammoniumIjms 24 07613 i00845.8
[THDA+][A2D]11-Carboxyundecanoate of N,N,N-trimethyl-hexadecan-1-ammoniumIjms 24 07613 i00942.7
[TXMA+][AI]3-Carboxybut-3-enoate of N,N,N-trihexyl-N-methyl-ammoniumIjms 24 07613 i01096.1
[TXMA+][2,2-DSA]3-Carboxy-2,2-dimethylpropanoate of N,N,N-trihexyl-N-methyl-ammoniumIjms 24 07613 i01196.0
[TXMA+][AA]2-Amine-benzoate of N,N,N-trihexyl-N-methyl-ammoniumIjms 24 07613 i01295.7
[TPMA+][AI]3-Carboxybut-3-enoate of N,N,N-tripentyl-N-methyl-ammoniumIjms 24 07613 i01381.0
[TPMA+][2,2-DSA]3-Carboxy-2,2-dimethylpropanoate of N,N,N-tripentyl-N-methyl-ammoniumIjms 24 07613 i01485.6
[TPMA+][AA]2-Amine-benzoate of N,N,N-tripentyl-N-methyl-ammoniumIjms 24 07613 i01598.0
Table 2. Electrochemical parameters for API X52 steel in 0.5 M HCl at 100 ppm of ILs.
Table 2. Electrochemical parameters for API X52 steel in 0.5 M HCl at 100 ppm of ILs.
ILRp
(Ω cm2)
IERp
(%)
Ecorr
(mV)
βa
(mV dec−1)
βc
(mV dec−1)
icorr
(μA cm−2)
IETafel
(%)
Blank243 ± 9 −478 ± 189 ± 1113 ± 282 ± 0.7-
[THDA+][MC]619 ± 3360.5 ± 4.0−463 ± 7106 ± 16159 ± 1340 ± 0.151.2 ± 0.4
[THDA+][AB]442 ± 045.1 ± 0−478 ± 9112 ± 9144 ± 1939 ± 0.452.4 ± 0.6
[THDA+][AI]1263 ± 2680.9 ± 0.5−482 ± 299 ± 6214 ± 817 ± 0.879.2 ± 1
[THDA+][2,2-DSA]1013 ± 2775.9 ± 1.9−473 ± 298 ± 5227 ± 323 ± 0.471.9 ± 0.5
[THDA+][AA]1397 ± 3681.6 ± 2.3−485 ± 281 ± 3105 ± 813 ± 0.684.1 ± 0.7
[THDA+][AH]630 ± 3161.4 ± 1.9−476 ± 8106 ± 15137 ± 435 ± 0.457.3 ± 0.6
[THDA+][AAD]962 ± 3274.7 ± 1.8−486 ± 3100 ± 1223 ± 1223 ± 0.671.9 ± 0.8
[THDA+][AD]1203 ± 3779.8 ± 1.9−481 ± 081 ± 5231 ± 1518 ± 0.278 ± 0.3
[THDA+][A2D]841 ± 2971.0 ± 1.8−474 ± 093 ± 2224 ± 327 ± 0.167.1 ± 0.3
[TXMA+][AI]684 ± 3963.9 ± 6.8−480 ± 284 ± 8110 ± 2132 ± 0.560.9 ± 0.7
[TXMA+][2,2-DSA]646 ± 3362.1 ± 4.0−479 ± 488 ± 8125 ± 734 ± 0.358.5 ± 0.5
[TXMA+][AA]794 ± 669.4 ± 0.2−480 ± 383 ± 3117 ± 1026 ± 0.368.2 ± 0.5
[TPMA+][AI]522 ± 2953.1 ± 3.3−476 ± 675 ± 6126 ± 235 ± 0.157.3 ± 0.4
[TPMA+][2,2-DSA]424 ± 1538.6 ± 2.5−477 ± 089 ± 16125 ± 1852 ± 0.836.5 ± 1.1
[TPMA+][AA]287 ± 0.715.3 ± 0.2−477 ± 586 ± 12134 ± 1965 ± 1.420.7 ± 1.8
Table 3. Electrochemical data for [THDA+] and the anions [AI], [AA], and [AD] at different concentrations.
Table 3. Electrochemical data for [THDA+] and the anions [AI], [AA], and [AD] at different concentrations.
ILConcentration
(ppm)
Ecorr
(mV)
βa
(mV dec−1)
βc
(mV dec−1)
icorr
(μA/cm−2)
IE
(%)
Blank0−478 ± 189 ± 1113 ± 282 ± 0.7-
[THDA+][AI]25−495 ± 1130 ± 23253 ± 629 ± 0.364.6 ± 0.5
50−499 ± 1116 ± 3240 ± 927 ± 0.167.1 ± 0.3
75−492 ± 1102 ± 1223 ± 324 ± 0.270.7 ± 0.3
100−482 ± 299 ± 6214 ± 817 ± 0.879.2 ± 1
200−466 ± 778 ± 3193 ± 618 ± 0.178.0 ± 0.2
[THDA+][AA]25−491 ± 183 ± 198 ± 117 ± 0.279.3 ± 0.3
50−483 ± 580 ± 9115 ± 814 ± 0.182.9 ± 0.2
75−483 ± 178 ± 2111 ± 513 ± 0.384.1 ± 0.4
100−484 ± 281 ± 3105 ± 813 ± 0.684.1 ± 0.7
200−466 ± 778 ± 3112 ± 618 ± 078 ± 0.2
[THDA+][AD]25−487 ± 193 ± 3178 ± 1822 ± 0.173.1 ± 0.3
50−489 ± 1103 ± 3187 ± 1421 ± 074.4 ± 0.2
75−482 ± 089 ± 1207 ± 1919 ± 0.176.8 ± 0.2
100−481 ± 081 ± 5231 ± 1518 ± 0.278 ± 0.3
200−468 ± 576 ± 6198 ± 818 ± 0.678 ± 0.8
Table 4. EIS parameters for the corrosion of API X52 steel in 0.5 M HCl in the absence and presence of [THDA+][AA].
Table 4. EIS parameters for the corrosion of API X52 steel in 0.5 M HCl in the absence and presence of [THDA+][AA].
ConcentrationRs
(Ω cm2)
Y
(μΩ−1 sncm−2)
nRct
(Ω cm2)
IEEIS
17 ± 0.253 ± 2.20.90134 ± 3.4
253 ± 031 ± 5.10.88889 ± 7.785.0 ± 1.0
503 ± 0.135 ± 2.70.861290 ± 15.389.7 ± 0.9
752 ± 0.132 ± 1.30.871149 ± 37.688.4 ± 1.2
1003 ± 0.135 ± 11.90.861319 ± 88.689.9 ± 1.8
Table 5. Optimized structures and molecular-electrostatic-potential (MEP) mapping of the ILs obtained at B3LYP/6-311G level in aqueous medium.
Table 5. Optimized structures and molecular-electrostatic-potential (MEP) mapping of the ILs obtained at B3LYP/6-311G level in aqueous medium.
ILOptimized StructureMEP
[THDA+][AA]Ijms 24 07613 i016Ijms 24 07613 i017
[THDA+][AI]Ijms 24 07613 i018Ijms 24 07613 i019
[THDA+][AD]Ijms 24 07613 i020Ijms 24 07613 i021
Table 6. Molecular orbitals of the ILs obtained at the B3LYP/6-311G level in aqueous medium.
Table 6. Molecular orbitals of the ILs obtained at the B3LYP/6-311G level in aqueous medium.
ILHOMOLUMO
[THDA+][AA]Ijms 24 07613 i022Ijms 24 07613 i023
[THDA+][AI]Ijms 24 07613 i024Ijms 24 07613 i025
[THDA+][AD]Ijms 24 07613 i026Ijms 24 07613 i027
Table 7. IL quantum parameters at the B3LYP/6-311G level in aqueous medium.
Table 7. IL quantum parameters at the B3LYP/6-311G level in aqueous medium.
ILEHOMO
(eV)
ELUMO
(eV)
ΔGL-H
(eV)
μ
(D)
[THDA+][AA]−8.67−5.373.3115.39
[THDA+][AI]−9.96−5.514.4514.33
[THDA+][AD]−10.10−3.636.4614.37
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Cornejo Robles, E.; Olivares-Xometl, O.; Likhanova, N.V.; Arellanes-Lozada, P.; Lijanova, I.V.; Díaz-Jiménez, V. Synthesis of Ammonium-Based ILs with Different Lengths of Aliphatic Chains and Organic Halogen-Free Anions as Corrosion Inhibitors of API X52 Steel. Int. J. Mol. Sci. 2023, 24, 7613. https://doi.org/10.3390/ijms24087613

AMA Style

Cornejo Robles E, Olivares-Xometl O, Likhanova NV, Arellanes-Lozada P, Lijanova IV, Díaz-Jiménez V. Synthesis of Ammonium-Based ILs with Different Lengths of Aliphatic Chains and Organic Halogen-Free Anions as Corrosion Inhibitors of API X52 Steel. International Journal of Molecular Sciences. 2023; 24(8):7613. https://doi.org/10.3390/ijms24087613

Chicago/Turabian Style

Cornejo Robles, Emiliano, Octavio Olivares-Xometl, Natalya V. Likhanova, Paulina Arellanes-Lozada, Irina V. Lijanova, and Víctor Díaz-Jiménez. 2023. "Synthesis of Ammonium-Based ILs with Different Lengths of Aliphatic Chains and Organic Halogen-Free Anions as Corrosion Inhibitors of API X52 Steel" International Journal of Molecular Sciences 24, no. 8: 7613. https://doi.org/10.3390/ijms24087613

APA Style

Cornejo Robles, E., Olivares-Xometl, O., Likhanova, N. V., Arellanes-Lozada, P., Lijanova, I. V., & Díaz-Jiménez, V. (2023). Synthesis of Ammonium-Based ILs with Different Lengths of Aliphatic Chains and Organic Halogen-Free Anions as Corrosion Inhibitors of API X52 Steel. International Journal of Molecular Sciences, 24(8), 7613. https://doi.org/10.3390/ijms24087613

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop