Next Article in Journal
Interaction of Wild Strains of Aspergilla with Aspergillus parasiticus ATCC15517 on Aflatoxins Production
Next Article in Special Issue
Supramolecular Layer-by-Layer Assembly of 3D Multicomponent Nanostructures via Multivalent Molecular Recognition
Previous Article in Journal
Fusarium Graminearum Growth Inhibition Due to Glucose Starvation Caused by Osthol
Previous Article in Special Issue
Noncovalently Modified Carbon Nanotubes with Carboxymethylated Chitosan: A Controllable Donor-Acceptor Nanohybrid
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis and Characterization of Polyacetylene with Side-chain Thiophene Functionality

Istanbul Technical University, Department of Chemistry, Maslak 34469, Istanbul, Turkey
*
Author to whom correspondence should be addressed.
Int. J. Mol. Sci. 2008, 9(3), 383-393; https://doi.org/10.3390/ijms9030383
Submission received: 30 November 2007 / Revised: 30 January 2008 / Accepted: 29 February 2008 / Published: 18 March 2008

Abstract

:
A new polyacetylene derivative with electroactive thiophene substituent, namely poly(2-methylbut-2-enyl thiophene-3-carboxylate) was synthesized and characterized. For this purpose, novel acetylene monomer was synthesized by the reaction of 3-thiophenecarboxylic acid with propargyl bromide and polymerized with a Rh catalyst to give the corresponding polymer. The chemical structure of the polymer was characterized to comprise the conjugated backbone and electroactive thiophene side group. UV spectral changes of the polymer with temperature were also studied. The polymer exhibited better thermal stability than the unsubstituted polyacetylenes.

Introduction

It is known that substituted acetylenes polymerize with transition metal catalysts [14]. Among various catalysts used, Rh based catalysts received particular interest as they efficiently polymerize mono-substituted acetylenes, especially phenylacetylene [412]. Rh catalysts are also capable of polymerizing monomers with polar substituents such as propiolic esters [1318] and propargyl amide [1922]. Moreover, polymerization is tolerant to protic solvents such as alcohols [5, 7], amines [8], and even water [10] and ionic liquids [9] and selectively give stereo-regular polymers with cistransoid isomer having helical main chain [46]. Providing that the helical sense of the π-conjugated polymers is controlled, the polymer backbone becomes optically active [2326]. The backbone chirality of the π-conjugated polymers can be detected directly by measuring their CD behavior, since the main-chain itself is a chromophore. Meanwhile, substituted polyacetylenes exhibit unique properties such as semi-conductivity, nonlinear optical properties, and high gas permeability due to the conjugated main chain and rigid molecular structure [1, 2729]. However, notoriously intractable and thermally unstable nature of polyacetylenes is deterrent for their potential use in technological applications. Attachment of aromatic pendants to the polyacetylene backbone is one way to overcome problems associated with intractability and thermal degradation [4, 3038]. For example, poly-(1-phenyl-1-alkyne)s are soluble in common solvents and do not decompose at elevated temperatures for a prolonged period of time [35] It is expected that incorporation of various substituents to acetylenes and their subsequent polymerization may lead to the conjugated polymers with new properties. Polymers containing thiophene units have been the subject of extensive research for more than 25 years. Polythiophenes are interesting for their not only electrical properties, but also electrophysical, magnetic, liquid crystalline and optical properties [39, 40]. However, polythiophenes suffer from the poor mechanical and physical properties. These properties can be improved by incorporating thiophene moieties into other insulating polymers and subsequent polymerization through these electroactive thiophene groups [4143]. Various controlled [4447] and conventional [48] polymerization methods to incorporate thiophene groups into polymers have recently been reported. It seemed therefore appropriate to synthesize acetylene with electroactive thiophene group. The corresponding polymers may form helical thiophene strands as well as a helical polyacetylene main chain possessing unique electronic and photonic functions. In this study, we report synthesis of acetylene with side-chain thiophene moiety and its polymerization with Rh catalyst in conjunction with co-catalyst. Structural, thermal and electrochemical characterizations of the monomer and corresponding polymer were performed by FT-IR, 1H-NMR, UV, TGA and CV measurements.

Results and Discussions

The synthetic strategy used to prepare propargyl thiophene, as monomer, based on heterogeneous esterification reaction between 3-thiophenecarboxylic acid and propargyl bromide in basic medium (Scheme 1).
The chemical structure of propargyl thiophene was confirmed by both FT-IR and 1H-NMR spectroscopy. As can be seen from Figure 1, 1H-NMR spectrum exhibits structural characteristics of both acetylene and thiophene units. The signal of terminal acetylene proton emerges as triplet at 2.50 ppm with 2.4 Hz J, and the two C3 protons of the propargyl part were noted as a doublet at 4.86 ppm with 2.5 Hz J. Additionally, C2, C4 and C5 protons of thiophene heterocycle appear at 8.16 ppm as doublet of doublet (dd) with 4J13: 3 Hz and 5J14: 1.3 Hz, at 7.30 ppm as dd, 3J34: 5.9 Hz and 4J13: 3 Hz, at 7.53 ppm as dd, 3J34: 5.2 Hz and 5J14: 1.3 Hz, respectively.
The FT-IR spectrum shown in Figure 2 (b) also establishes the structure of the monomer. Accordingly, diagnostic stretching vibrations of ester carbonyl, aromatic C-H and terminal acetylenic C-H and C ≡ C bands appear at 1716 cm−1, 3112 cm−1, 3292 cm−1 and 2128 cm−1, respectively. Moreover, sp2 C-O and sp C-O stretching vibrations observed at 1246 and 1095 cm−1 are additional support for the ester structure.
Propargyl thiophene is expected to undergo polymerization with Rh catalyst through the acetylenic group as depicted in Scheme 1. The Rh-catalyzed polymerization reaction in toluene proceeded smoothly at ambient temperature and gave the expected polyacetylene in moderate yields after precipitation. In this polymerization, (bicyclo[2,2,1]hepta-2,5-diene)chlororhodium(I) dimer, abbreviated as [(nbd)RhCl]2, was selected as the catalyst due to its widespread use in related polymerizations. The results of polymerizations under different experimental conditions are given in Table 1.
As can be seen, polymerization with all co-catalysts used resulted in polymers with relatively low yields and molecular weights. Limited chain growth is probably due to the inefficient ligation of co-catalysts and monomer together to the growing species [49, 50]. The chemical structure of the polyacetylene obtained was confirmed by both FT-IR and 1H-NMR spectroscopy. In the FT-IR spectrum (Figure 2), the disappearance of the acetylenic C-H and C ≡ C stretching vibrations at 3292 cm−1 at 2128 cm−1, respectively, was clearly noted. Also, carbonyl C=O stretching at 1716 cm−1 and sp2 C-O and sp C-O stretching vibrations at 1246, 1095 cm−1 are evidencing the retention of ester group after the polymerization.
Further analysis of the polymer by 1H-NMR as presented in Figure 3 indicated the characteristic peak for cisoid =C-H proton at 6.4 ppm. Additionally, the two protons, neighboring ester group and double bond emerge at 4.75 ppm with a slight shift compared to C3 protons of the precursor propargyl unit (see Figure 1). This shift clearly suggests the transformation of triple bond to double bond. The retention of aromatic peaks was also noted.
Electrochemical property of the polymer was investigated by cyclic voltammetry (CV). Reversible redox potentials and LUMO energy values based on the value of 4.8 eV for ferrocene (FC) with respect to zero vacuum level [51, 52] were determined and summarized in Table 2. As can be seen poly(acetylene-thiophene) displays two cathodic peaks and two anodic peaks. The reduction potentials are 0.71 V and 1.16 V and LUMO is 4.09 eV. These results clearly indicate the electroactivity of the polymer. It is worth to mention that no detectable redox peaks were observed with the polymers possessing non-conjugated backbone i.e., methacrylate and maleimide polymers with side chain thiophene unit [4243]. However, they become electroactive only in the presence of bare monomers such as thiophene and pyrrole. The enhanced activity in our case may be due to the conjugated backbone. In this connection, it should be pointed out that polyacetylenes with directly attached thiophene units were previously reported. However, no information on their electrochemical properties was given [53].
Figure 4 shows the UV spectral changes of the polymer solution in CHCl3 with temperature. As can be seen, the absorbance at lower wavelengths increases by increasing the temperature probably due to the transformation to a non-ordered structure. Thermal stability of the poly(acetylene-thiophene) (PAT-2) was investigated by thermal gravimetric analysis (TGA) under nitrogen exposure. The TGA profile of the polymer is shown in Figure 5 and the results are summarized in Table 3. It is well known that monosubstituted polyacetylenes are generally thermally unstable. Typically, poly(1-hexyne) starts to lose its weight at ∼ 150 °C. Interestingly, the temperature for 5% weight loss is 230 °C for PAT-2. In fact, this value is slightly lower than that of the another aromatic substitutued poly(phenyl acetylene) (T= ∼ 264 °C) [3538].
In conclusion, a new conjugated polymer, polyacetylene, with electroactive active thiophene groups was synthesized by using a Rh catalyst and characterized. The polymer structure, electrochemical and thermal properties were characterized by various instrumental methods. The new polymer is expected to undergo electropolymerization leading to crosslinked polymers having conjugated segments in both main- and side-chain with enhanced conductivities and helical tunnels in the structure. Further studies in this line are now in progress.

Experimental Section

Materials

3-Thiophenecarboxylic acid % 99 (Acros), propargyl bromide solution in toluene ∼ %80 (Fluka), te-trabutylammonium bromide (+ %99) (Acros), (bicyclo[2,2,1]hepta-2,5-diene)chlororhodium(I) dimer ([(nbd)RhCl]2)≥ %98 (Fluka), diisopropylamine ≥ % 99 (Merck), triethylamine ≥ % 99.5 (Aldrich), were purchased and used as received. Solvents used for polymerization were purified before usage by the standard drying and distillation procedures.

Characterization

The molecular weights of polymers were measured by GPC at 30 °C with an Agilent instrument (Model 1100) consisting of a pump, refractive index and UV detectors and four Waters Styragel columns (HR 5E, HR 4E, HR 3, and HR 2) eluent THF, flow rate of 0.3 mL/min and calibrated with polystyrene standards. Toluene was used as an internal standard. Data analyses were performed with PL caliber Software. 1H NMR spectra were recorded on a Bruker 250 Mhz spectrometer using CDCl3 as solvent and tetramethylsilane as the internal standard. FT-IR spectra were measured on Perkin-Elmer FT-IR Spectrum One spectrometer. Thermal gravimetric analysis (TGA) was performed on Perkin-Elmer Diamond TA/TGA with a heating rate of 10 °C min under nitrogen flow. Cylic voltammetry measurements were carried out using a Princeton Applied Research Model 2263. Cylic voltammetry in dichloromethane was performed using a 3-electrode cell (BASI model solid cell stand) with a polished 2mm sized Pt disc electrode as working electrode, a Pt wire counter electrode and an Ag/AgCl reference electrode, with a solution of polymer (6.6 g/l) and tetrabutylammonium perchlorate (TBAP,0.1, M) in CH2Cl2. All solutions were purged with nitrogen for at least 10 min before starting the measurements.UV-vis spectra were recorded on JASCO V-530 UV-vis spectro photometer.

Monomer synthesis

In a 250 mL flask, of 3-thiophenecarboxylic acid (2.0 g, 15 mmol) was dissolved in 100 mL of 0.1 N NaOH. The mixture was heated at 50 °C until a clear solution was formed. To this solution, tetrabu-tylammonium bromide (0.50 g, 1.55 mmol) was added as a phase transfer catalyst. Then, a solution of propargylbromide (2.0 g, 17 mmol) in 20 mL of toluene was added portion wise. The mixture was kept stirring at 60 °C for 24 h. At the end of this period, it was cooled to afford solid. Additonally, the remaining toluene layer was separated and washed repeatedly with %2 NaOH (200 mL, 0.1 N) and with water. Evaporating toluene afforded extra solid.

Polymerization

Polymerization was carried out under N2 atmosphere in a Schlenk tube equipped with a three-way stopcock. A typical polymerization procedure is as follows: A toluene solution (2.0 mL) of 1 (1 mmol) was added to a toluene solution (3.0 mL) of [(nbd)RhCl]2 (10−3 mmol) with co-catalyst diisopropylamine (10−2 mmol). Polymerization was carried out at 30 °C for 24 h.

Acknowledgments

The authors would like to thank Istanbul Technical University, Research Fund for financial support. One of the authors (B.Koz) would like to thank Tubitak (Turkish Scientific and Technologic Research Council) for the financial support by means of a postdoctoral fellowship.

References

  1. Masuda, T; Sanda, F. Polymerization of substituted acetylenes. Handbook of metathesis 2003, 3, Chapter 11. 375. [Google Scholar]
  2. Sedlacek, J; Vohlidal, J. Controlled and living polymerizations induced with rhodium catalysts. Collect Czech Chem Commun 2003, 68, 1745–1790. [Google Scholar]
  3. Choi, S-K; Gal, Y-S; Jin, S-H; Kim, HK. Poly(1,6-heptadiyne)-based materials by metathesis polymerization. Chem Rev 2000, 100, 1645–1682. [Google Scholar]
  4. Tabata, M; Sone, T; Sadahiro, Y. Precise synthesis of monosubstituted polyacetylenes using Rh complex catalysts. Control of solid structure and π-conjugation length. Macromol Chem Phys 1999, 200, 265–282. [Google Scholar]
  5. Furlani, A; Napoletano, C; Russo, MV; Camus, A; Marsich, N. The influence of the ligands on the catalytic activity of a series of RhI complexes in reactions with phenylacetylene: Synthesis of stereoregular poly(phenyl) acetylene. J Polym Sci, Part A: Polym Chem 1989, 27, 75–86. [Google Scholar]
  6. Furlani, A; Napoletano, C; Russo, MV; Feast, WJ. Stereoregular polyphenylacetylene. Polym Bull 1986, 16, 311–317. [Google Scholar]
  7. Tabata, M; Yang, W; Yokota, K. 1H-NMR and UV studies of Rh complexes as a stereoregular polymerization catalysts for phenylacetylenes: Effects of ligands and solvents on its catalyst activity. J Polym Sci, Part A: Polym Chem 1994, 32, 1113–1120. [Google Scholar]
  8. Tabata, M; Yang, W; Yokota, K. Polymerization of m-chlorophenylacetylene initiated by [Rh(norbornadiene)Cl]2-triethylamine catalyst containing long-lived propagation species. Polym. J. 1990, 22, 1105–1107. [Google Scholar]
  9. Mastrorilli, P; Nobile, CF; Gallo, V; Suranna, GP; Farinola, G. Rhodium(I) catalyzed polymerization of phenylacetylene in ionic liquids. J. Mol. Catal. A: Chem. 2002, 184, 73–78. [Google Scholar]
  10. Tang, BZ; Poon, WH; Leung, SM; Leung, WH; Peng, H. Synthesis of stereoregular poly(phenylacetylene)s by organorhodium complexes in aqueous Media. Macromolecules 1997, 30, 2209–2212. [Google Scholar]
  11. Kishimoto, Y; Itou, M; Miyatake, Y; Ikariya, T; Noyori, R. Polymerization of monosubstituted acetylenes with a zwitterionic rhodium(I) complex, Rh+(2,5-norbornadiene)[.eta.6-C6H5)B-(C6H5)3]. Macromolecules 1995, 28, 6662–6666. [Google Scholar]
  12. Aoki, T; Kokai, M; Shinohara, K; Oikawa, E. Chiral helical conformation of the polyphenylacetylene having optically-active bulky substituent. Chem. Lett. 1993, 22, 2009. [Google Scholar]
  13. Kozuka, M; Sone, T; Sadahiro, Y; Tabata, M; Enoto, T. Columnar. Assemblies of Aliphatic Poly(acetylene ester)s prepared with a [Rh(norbornadiene)Cl]2 Catalyst. 1H and 13C NMR, X-Ray Diffraction and AFM Studies. Macromol. Chem. Phys. 2002, 203, 66–70. [Google Scholar]
  14. Tabata, M; Inaba, Y; Yokota, K; Nozaki, Y. Stereoregular polymerization of alkyl propiolate catalyzed by Rh complex. J. Macromol. Sci., Pure Appl. Chem. 1994, A31, 465–475. [Google Scholar]
  15. Nakako, H; Nomura, R; Masuda, T. Helix inversion of poly(propiolic esters). Macromolecules 2001, 34, 1496–1502. [Google Scholar]
  16. Nakako, H; Mayahara, Y; Nomura, R; Tabata, M; Masuda, T. Effect of chiral substituents on the helical conformation of poly(propiolic esters). Macromolecules 2000, 33, 3978–3982. [Google Scholar]
  17. Nomura, R; Fukushima, Y; Nakako, H; Masuda, T. Conformational study of helical poly(propiolic esters) in solution. J. Am. Chem. Soc. 2000, 122, 8830–8836. [Google Scholar]
  18. Nakako, H; Nomura, R; Tabata, M; Masuda, T. Synthesis and structure in solution of poly[(-)-menthyl propiolate] as a new class of helical polyacetylene. Macromolecules 1999, 32, 2861–2864. [Google Scholar]
  19. Tabei, J; Nomura, R; Masuda, T. Synthesis and structure of poly(N-propargylbenzamides) bearing chiral ester groups. Macromolecules 2003, 36, 573–577. [Google Scholar]
  20. Nomura, R; Tabei, J; Masuda, T. Effect of side chain structure on the conformation of poly(N-propargylalkylamide). Macromolecules 2002, 35, 2955–2961. [Google Scholar]
  21. Tabei, J; Nomura, R; Masuda, T. Conformational study of poly(N-propargylamides) having bulky pendant groups. Macromolecules 2002, 35, 5405–5409. [Google Scholar]
  22. Nomura, R; Tabei, J; Masuda, T. Biomimetic stabilization of helical structure in a synthetic polymer by means of intramolecular hydrogen bonds. J. Am. Chem. Soc. 2001, 123, 8430–8431. [Google Scholar]
  23. Yashima, E; Matsushima, T; Okamoto, Y. Chirality assignment of amines and amino alcohols based on circular dichroism induced by helix formation of a stereoregular poly((4-carboxyphenyl)acetylene) through acid-base complexation. J. Am. Chem. Soc. 1997, 119, 6345–6359. [Google Scholar]
  24. Yashima, E; Oobo, M; Nonokawa, R. Helicity induction on a poly(phenylacetylene) derivative bearing aza-15-crown-5 ether pendants in organic solvents and water. Macromolecules 2003, 36, 6599–6606. [Google Scholar]
  25. Yashima, E; Zhang, H-Q; Goto, H. Chiral stimuli-responsive gels: Helicity induction in poly(phenylacetylene) gels bearing a carboxyl group with chiral amines. J. Am. Chem. Soc. 2003, 125, 2516–2523. [Google Scholar]
  26. Yashima, E; Maeda, K; Sato, T; Okamoto, Y; Morini, K. Mechanism of helix induction on a stereoregular poly((4-carboxyphenyl)acetylene) with chiral amines and memory of the macromolecular helicity assisted by interaction with achiral amines. J. Am. Chem. Soc. 2004, 126, 4329–4342. [Google Scholar]
  27. Masuda, T; Sanda, F; Shiotsuki, M. Polymerization of acetylenes. Comprehensive Organometallic Chemistry III 2006, 11. Chapter 18. [Google Scholar]
  28. Aoki, T; Kaneko, T; Teraguchi, M. Synthesis of functional π-conjugated polymers from aromatic acetylenes. Polymer 2006, 47, 4867–4892. [Google Scholar]
  29. Lam, JWY; Tang, BZ. Functional Polyacetylenes. Acc. Chem Res. 2005, 38, 745–754. [Google Scholar]
  30. Masuda, T; Higashimura, T. Polyacetylenes with substituents: Their synthesis and properties. Adv. Polym. Sci. 1987, 81, 121–165. [Google Scholar]
  31. Gibson, HW; Pochan, JM. Concise encyclopedia of polymer science and engineering; Kroschwitz, JI, Ed.; Wiley: New York, NY, 1990; pp. 7–9. [Google Scholar]
  32. Ginsburg, EJ; Gorman, CB; Grubbs, RH. Modern acetylene chemistry; Stang, PJ, Diederich, F, Eds.; VCH: New York, NY, 1995; Chapter 10; pp. 353–383. [Google Scholar]
  33. Reddinger, JL; Reynolds, JR. Molecular Engineering of p-Conjugated Polymers. Adv. Polym. Sci. 1999, 145, 57–122. [Google Scholar]
  34. Volidal, J; Sedlacek, J. Chromatography of polymers: Hyphenated and multidimensional techniques; ACS Symposium Series 731; Provder, T, Ed.; American Chemical Society: Washington, DC, 1999; Chapter 19; p. 263. [Google Scholar]
  35. Masuda, T; Tang, BZ; Higashimura, T. Thermal degradation of polyacetylenes carrying substituents. Macromolecules 1985, 18, 2369–2373. [Google Scholar]
  36. Masuda, T; Tang, BZ; Tanaka, T; Higashimura, T. Mechanical properties of substituted polyacetylenes. Macromolecules 1986, 19, 1459–1464. [Google Scholar]
  37. Seki, H; Tang, BZ; Tanaka, A; Masuda, T. Tensile and dynamic viscoelastic properties of various new substituted polyacetylenes. Polymer 1994, 35, 3456–3462. [Google Scholar]
  38. Karim, SM; Nomura, R; Masuda, T. Degradation behavior of stereoregular cis-transoidal poly(phenylacetylene)s. J. Polym. Sci., Part A: Polym Chem. 2001, 39, 3130–3136. [Google Scholar]
  39. Hong, XM; Collard, DM. Liquid crystalline regioregular semifluoroalkyl-substituted polythiophenes. Macromolecules 2000, 33, 6916–6917. [Google Scholar]
  40. Goto, H. Cholesteric liquid crystal inductive asymmetric polymerization: Synthesis of chiral polythiophene derivatives from achiral monomers in a cholesteric liquid crystal. Macromolecules 2007, 40, 1377–1385. [Google Scholar]
  41. Yagci, Y; Toppare, L. Electroactive macromonomers based on pyrrole and thiophene: A versatile route to conducting block and graft copolymers. Polym. Int. 2003, 52, 1573–1578. [Google Scholar]
  42. Yilmaz, F; Guner, Y; Toppare, L; Yagci, Y. Synthesis and characterization of alternating copolymers of thiophene containing N- phenyl maleimide and styrene via photo-induced radical polymerization and their use in electropolymerization. Polymer 2004, 45, 5765–5774. [Google Scholar]
  43. Cianga, L; Yagci, Y. Synthesis and characterization of poly(N-phenyl maleimide) polymers with pendant thiophene rings by photoinduced radical polymerization. Polym. Sci., Polym. Chem. Ed. 2002, 15, 995–1004. [Google Scholar]
  44. Yagci, Y; Toppare, L. Synthesis of conducting block and graf copolymers containing polyether segments. Macromol. Symp. 2000, 157, 29–38. [Google Scholar]
  45. Oztemiz, S; Toppare, L; Onen, A; Yagci, Y. Conducting multiphase block copolymers of pyrrole with polytetrahydrofuran and polyetrahydrofuran-b-polystyrene. J. Macromol. Sci. 2000, A37, 277–291. [Google Scholar]
  46. Alkan, S; Toppare, L; Hepuzer, Y; Yagci, Y. Block copolymers of thiophene-capped poly(methyl methacrylate) with pyrrole. J. Polym. Sci., Polym. Chem. Ed. 1999, 37, 4218–4225. [Google Scholar]
  47. Alkan, S; Toppare, L; Hepuzer, Y; Yagci, Y. Synthesis and characterization of conducting block copolymers of thiophene-ended polystyrene with pyrrole. Synt. Met. 2001, 119, 133–134. [Google Scholar]
  48. Cirpan, A; Alkan, S; Toppare, L; Hepuzer, Y; Yagci, Y. Conducting graft copolymers of poly(3-methyl thienyl methacrylate) with pyrrole and thiophene. J. Polym. Sci., Polym. Chem. Ed. 2002, 40, 4131–4140. [Google Scholar]
  49. Kanki, K; Misumi, Y; Masuda, T. Remarkable cocatalytic effect of organometallics and rate control by triphenylphosphine in the Rh-catalyzed polymerization of phenylacetylene. Macromolecules 1999, 32, 2384–2386. [Google Scholar]
  50. Nakazato, A; Saeed, I; Katsumata, T; Shiotsuki, M; Masuda, T; Zednik, J; Vohlidal, J. Polymerization of Substituted Acetylenes by Various Rhodium Catalysts: Comparison of Catalyst Activity and Effect of Additives. J. Polym. Sci. Part A Polym. Chem. 2005, 43, 4530–4536. [Google Scholar]
  51. Koepp, HM; Wendt, H; Strehlow, HZ. Der vergleich der spannungsreihen in verschiedenen solventien II. Elektrochem. 1960, 64, 483. [Google Scholar]
  52. Bredas, JL; Silbey, R; Bourdreaux, DS; Chance, RR. Chain-length dependence of electronic and electrochemical properties of conjugated systems: polyacetylene, polyphenylene, polythiophene, and polpyrrole. J. Am. Chem. Soc. 1983, 105, 6555–6559. [Google Scholar]
  53. Nakamura, M; Tabata, M; Sone, T; Mawatari, Y; Miyasaka, A. Photoinduced cis-to-trans isomerization of poly(2-ethynylthiophene) prepared with a [Rh(norbornadiene)Cl]2 catalyst.1H NMR, UV, and ESR studies. Macromolecules 2002, 35, 200–2004. [Google Scholar]
Figure 1. 1H NMR spectrum of propargyl-thiophene.
Figure 1. 1H NMR spectrum of propargyl-thiophene.
Ijms 09 00383 f1
Figure 2. FT-IR spectra of (a) PAT-2 and (b) propargyl-thiophene.
Figure 2. FT-IR spectra of (a) PAT-2 and (b) propargyl-thiophene.
Ijms 09 00383 f2
Figure 3. 1H NMR spectrum of polymer PAT-2.
Figure 3. 1H NMR spectrum of polymer PAT-2.
Ijms 09 00383 f3
Figure 4. UV-vis spectral changes of PAT-2 from 5 to 55 °C measured in CHCl3 [PAT-2]= 1.8 × 10−5.
Figure 4. UV-vis spectral changes of PAT-2 from 5 to 55 °C measured in CHCl3 [PAT-2]= 1.8 × 10−5.
Ijms 09 00383 f4
Figure 5. TGA thermogram of PAT-2 (a) recorded under nitrogen at a heating rate of 10 °C/min., (b) derivative of curve (a).
Figure 5. TGA thermogram of PAT-2 (a) recorded under nitrogen at a heating rate of 10 °C/min., (b) derivative of curve (a).
Ijms 09 00383 f5
Scheme 1. Synthesis and Polymerization of Propargyl-thiophene by Using Rh(nbd)Cl2].
Scheme 1. Synthesis and Polymerization of Propargyl-thiophene by Using Rh(nbd)Cl2].
Ijms 09 00383 f6
Table 1. Polymerizationa of acetylene-thiophene by Rh catalysts in conjunctiona with different co-catalysts.
Table 1. Polymerizationa of acetylene-thiophene by Rh catalysts in conjunctiona with different co-catalysts.
PolymerCo-catalystYield (%)MnbMw/Mnb
PAT-1Triethylamine1227901.46
PAT-2Diisopropylamine2044601.67
PAT-3Butylamine646901.33
a[M]o = 0.2 M, [Rh]= 2 mM, [Co-catalyst] =20mM, 30 °C, 24 h;
bDetermined by GPC according to polystyrene standards.
Table 2. Cylic voltammetrya data and LUMO energy values of poly(acetylene thiophene) in dichloromethane. E1/2/V vs. Fc is the reduction potential versus ferrocene electrode (E1/2/V vs. Fc= (E1/2/V vs. Ag/AgCl)-(EFc/V vs. Ag/AgCl)).
Table 2. Cylic voltammetrya data and LUMO energy values of poly(acetylene thiophene) in dichloromethane. E1/2/V vs. Fc is the reduction potential versus ferrocene electrode (E1/2/V vs. Fc= (E1/2/V vs. Ag/AgCl)-(EFc/V vs. Ag/AgCl)).
ElectrodeEpc/VEpa/VE1/2/V vs. (Ag/AgCl)EFc/V vs.(Ag/AgCl)E1/2/V vs. FcLUMO (eV)
Pt disc0.80−0.330.240.470.714.09
−0.61−0.770.690.471.163.64
aSupporting electrolyte is 0.1 M tetrabutylammonium perchlorate (TBAP). [PAT-2] = 6.6 g/l.
Table 3. Thermal properties of polyacetylenes.
Table 3. Thermal properties of polyacetylenes.
PolymerT5%a (°C)T10%b (°C)Tcd max (°C)Ycd at 500°C (%)Ref.
PAT-223024836329This work
Poly(phenylacetylene)∼264∼280--∼12[35]
aT5%: The temperature for which the weight loss is 5%;
bT10%: The temperature for which the weight loss is 10%;
cTd max: Maximum weight loss temperature;
dYc: Char yields

Share and Cite

MDPI and ACS Style

Koz, B.; Kiskan, B.; Yagci, Y. Synthesis and Characterization of Polyacetylene with Side-chain Thiophene Functionality. Int. J. Mol. Sci. 2008, 9, 383-393. https://doi.org/10.3390/ijms9030383

AMA Style

Koz B, Kiskan B, Yagci Y. Synthesis and Characterization of Polyacetylene with Side-chain Thiophene Functionality. International Journal of Molecular Sciences. 2008; 9(3):383-393. https://doi.org/10.3390/ijms9030383

Chicago/Turabian Style

Koz, Banu, Baris Kiskan, and Yusuf Yagci. 2008. "Synthesis and Characterization of Polyacetylene with Side-chain Thiophene Functionality" International Journal of Molecular Sciences 9, no. 3: 383-393. https://doi.org/10.3390/ijms9030383

APA Style

Koz, B., Kiskan, B., & Yagci, Y. (2008). Synthesis and Characterization of Polyacetylene with Side-chain Thiophene Functionality. International Journal of Molecular Sciences, 9(3), 383-393. https://doi.org/10.3390/ijms9030383

Article Metrics