Next Article in Journal
Equivalent Circuit of a Stacked Piezoelectric Cymbal Vibrator
Next Article in Special Issue
3D Light-Direction Sensor Based on Segmented Concentric Nanorings Combined with Deep Learning
Previous Article in Journal
Development of a Compact NDIR CO2 Gas Sensor for a Portable Gas Analyzer
Previous Article in Special Issue
Preparation of High-Performance Transparent Al2O3 Dielectric Films via Self-Exothermic Reaction Based on Solution Method and Applications
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Capacitance–Voltage Fluctuation of SixNy-Based Metal–Insulator–Metal Capacitor Due to Silane Surface Treatment

School of Integrative Engineering, Chung-Ang University, 84, Heukseok-ro, Dongjak-gu, Seoul 06974, Republic of Korea
*
Author to whom correspondence should be addressed.
Micromachines 2024, 15(10), 1204; https://doi.org/10.3390/mi15101204
Submission received: 5 September 2024 / Revised: 25 September 2024 / Accepted: 27 September 2024 / Published: 28 September 2024
(This article belongs to the Special Issue Thin Film Microelectronic Devices and Circuits)

Abstract

:
In this study, we analyze metal–insulator–metal (MIM) capacitors with different thicknesses of SixNy film (650 Å, 500 Å, and 400 Å) and varying levels of film quality to improve their capacitance density. SixNy thicknesses of 650 Å, 500 Å, and 400 Å are used with four different conditions, designated as MIM (N content 1.49), NEWMIM (N content 28.1), DAMANIT (N content 1.43), and NIT (N content 0.30). We divide the C–V characteristics into two categories: voltage coefficient of capacitance (VCC) and temperature coefficient of capacitance (TCC). There was an overall increase in the VCC as the thickness of the SixNy film decreased, with some variation depending on the condition. However, the TCC did not vary significantly with thickness, only with condition. At the same thickness, the NIT condition yielded the highest capacitance density, while the MIM condition showed the lowest capacitance density. This difference was due to the actual thickness of the film and the variation in its k-value depending on the condition. The most influential factor for capacitance uniformity was the thickness uniformity of the SixNy film.

1. Introduction

A metal–insulator–metal (MIM) capacitor is an analog integrated circuit (IC) configuration device with the advantages of low electrode resistance and parasitic capacitance [1,2,3,4]. MIM capacitors have high charge mobility and burst power characteristics that make them excellent energy-storage devices and potential auxiliary power sources.
IM capacitors have been applied to ICs such as high-power microprocessor units and dynamic random-access memory. However, with the development of wireless communication, their application to radio frequency (RF) devices has been actively studied [5,6,7]. As current RF devices require high operating frequencies, MIM devices also require high capacitance per unit area [8,9,10,11].
According to this demand, the design of the structure, thin-film deposition method, selection of the bottom and top electrode materials, insulator material, thickness of the electrode and insulator, dielectric constant of the insulator, and crystal structure of the insulator must be considered in depth to produce a high-performance MIM capacitor with a high capacitance [12,13,14,15]. In the evaluation of MIM capacitors, it is important to conduct a comprehensive analysis considering factors such as capacitance density (CD), leakage current density, charge storage density, and dielectric breakdown strength [16,17,18,19].
The choice of insulator material is a crucial factor in capacitors, and the CD relies heavily on the dielectric constant and thickness of the insulator. According to Equation (1), the CD increases when the dielectric constant is higher, which is a natural property of the insulator, and when the thickness is lower [1,20]:
C = k ε 0 A d C A = k ε 0 d
where C denotes the capacitance (F), k is the dielectric constant, ε0 is the permittivity of the vacuum (8.854 × 10−12/m), and d is the thickness of the insulator (m).
Because of the abovementioned reasons, it is generally necessary to introduce a high-k material to increase the dielectric constant [21,22], which entails considerable investment and time because it requires equipment, facilities, and source replacement. In addition, according to Natori et al., the relative permittivity of the material (k) decreases as the insulator thickness of the capacitor decreases, and k tends to decrease significantly for high-k materials [13,23]. Therefore, the introduction of high-k materials is subject to many limitations. However, if the thickness of the currently used medium-k dielectric material, SixNy (k = 7), can be reduced by considering the leakage aspect, the capacitance value can be increased without using a high-k material [24,25,26]. Yu et al. explained the performance of HfO2-based MIM capacitors deposited by the atomic layer deposition (ALD) method with respect to the thickness of the dielectric [27]. As the thickness of the HfO2 insulator layer decreased, the CD and voltage coefficient of capacitance (VCC) increased [28,29,30,31]. In practice, GaAs-based MIM capacitors have been used in the past. In fact, for GaAs-based MIM capacitors, SixNy is the most commonly applied material owing to its excellent electrical properties, compliant dielectric constant, high dielectric breakdown voltage, and low leakage current [28,32,33]. Moreover, the electrical properties can be improved by optimizing the deposition condition of SixNy, which has the greatest effect on the electrical properties of MIM capacitors. Yota et al. confirmed that the stress, CD, breakdown voltage, and performance of MIM capacitors exhibited significant differences in each insulator layer, with a single layer or multiple layers of silicon nitride formed depending on the deposition conditions [34]. Therefore, the electrical properties of MIM capacitors can be improved by optimizing the deposition condition of SixNy.
In this study, to develop an optimal condition for the deposition conditions of SixNy that improves the insulator properties of MIM capacitors and secures feasibility, we fabricated MIM capacitors with different thicknesses of SixNy and deposition conditions on M4 wiring and then evaluated the capacitance–voltage (C–V) characteristics, focusing on the evaluation of cap density uniformity, the dielectric temperature coefficient of capacitance (TCC), and the VCC.

2. Materials and Methods

Patterned 200 mm Si (100) wafers were used to measure the integration process steps. Several different cap dielectrics were investigated and deposited by PE-ALD. An Applied Materials MIRRA tool(Applied Materials, Gloucester, MA, USA) was used for the blanket. In this study, the density of MIM capacitors was considered to be 8 fF/m2, and the capacitors were fully integrated using the 0.15 m Al interconnect processes. The first single MIM capacitor was formed using metal 3 and metal 4 to minimize the effect of the parasitic coupling of the silicon substrates. In addition, the second single MIM capacitor was formed using metal 5 and metal 6. It is crucial for MIM capacitors to have a symmetric structure by having identical boundary conditions on both sides of the dielectric [8,35,36].
The bottom electrode of the MIM capacitor was prepared using Ti (100 Å)/Al–Cu (4500 Å)/Ti (50 Å)/TiN (600 Å) wiring, and the top electrode was prepared using TiN (1500 Å). The insulator was SixNy. The capacitor fabrication process was as follows: bottom electrode deposition → bottom electrode scrub → insulator deposition → top metal deposition → MIM PH → MIM → TOP METAL etching → ((CH3)4NOH:H2O) cleaning 1 → MIM asher → ((CH3)4NOH:H2O) cleaning 2 → insulator etching → ACT 935 (wet PR strip solution including amine) →UVAS. MIM ET was performed using the endpoint detection method.
The top electrode layer was connected to the upper metal layer through a dense matrix of vias. All wafers mentioned in this paper were passivated using PE-ALD nitride and were annealed below 450 °C. To improve the voltage linearity, Interface plasma treatment was administered before and after the PE-ALD dielectrics. Further details of the interface plasma treatment and thickness ratio in each stack layer are listed in Table 1. The blanket film characteristics of PE-ALD dielectrics were evaluated by using an ellipsometer at 673 nm to measure the thickness, refractive index, and uniformity of the PE-ALD dielectrics. A Hg probe was used to measure the dielectric constant, and the deposition rate was calculated according to the thickness slope as a function of the cycle times [4].
The C–V characteristics were measured manually using an LCR meter (HP4284A, Agilent, Santa Clara, CA, USA) under the conditions given in Table 2. The VRDB was performed based on the JESD35-A standard. The thickness analysis of SixNy per condition was performed using transmission electron microscopy (CM200FEGTEM)/scanning transmission electron microscopy (STEMoperated at 300 keV with an energy-dispersive X-ray spectroscopy (EDS) SUTW-SiLi X-ray detector and a Gatan 666 parallel electron energy loss spectroscopy (PEELS) spectrometer (Philips, Eindhoven, Netherlands), and a focused ion beam (FIB). The via resistance and via chain yields were measured in dual-damascene structures. A wafer-level bias thermal stress (BTS) test was performed under different conditions to verify the effectiveness of the barrier layers. Failures were analyzed by scanning electron microscopy (SEM) and X-ray spectroscopy (EDX).(SIGMA, Carl Zeiss, Jena, Germany)

3. Results and Discussion

To understand the wafer-wide trend in CD, PCM measurements were performed with the split conditions given in Table 1; the corresponding results for a 25 × 25 cap size are presented in Figure 1.
The CD varied depending on the split condition but was uniform within the wafer. For all conditions, the CD increased with decreasing thickness, and at the same thickness, it varied slightly between conditions. By examining the range of CD in relation to thickness, the following values were observed for thicknesses of 650, 500, and 400 Å, respectively: 0.983–1.1, 1.24–1.4, and 1.57–1.79 fF/μm2. The difference in capacitance densities between conditions at the same thickness can be considered to be the difference between the actual thickness of the SixNy film and the target thickness and the difference in the k-value of the deposited film by condition. To confirm this, 500 Å thick SixNy films deposited under the different conditions were analyzed by TEM; the corresponding results are shown in Figure 2.
Figure 2a–d depict the cross-sectional TEM images of SixNy films deposited under MIM, NEWMIM, DAMANIT, and NIT conditions, respectively, and Figure 2e shows a barplot of the thickness of SixNy films obtained from the TEM images. The NIT condition showed the lowest thickness, while the NEWMIM condition showed the highest thickness. For accurate analysis, the k-value was calculated after matching the TEM analysis die and the PCM measurement die; the corresponding results are presented in Table 3.
In this experiment, we compared the capacitance densities of four materials with the same thickness (500 Å) and found that NIT afforded the highest CD, followed by NEWMIM, DAMANIT, and MIM. However, we noticed that the deposited thickness did not follow this trend. This indicates that thickness alone is not the only factor that affects the CD. The difference in the k-value according to the condition also appears to play a significant role in determining the CD. In general, the k-value is influenced by two primary factors, namely, the macroscopic electric field and the dipole moment per unit volume, as given by Equation (2) [2]:
K = 1 + 4 π P E
where P is the dipole moment per unit volume and E is the macroscopic electric field.
Because the p-value is dependent on the electronic polarizability, it is affected by the bond conformation and bond strength [21]. The SixNy films had different dipole moments due to the different values of Si-H/N-H (Table 4) depending on the deposition condition; therefore, the k-value was different for each condition.
To check the variation in CD according to capacitor size, the capacitor density by thickness and condition was measured for 10 × 10, 15 × 15, 20 × 20, 25 × 25, 30 × 30, and 50 × 50 μm2 samples; it is plotted in Figure 3. In this case, the CD according to size was taken as the average value within the wafer.
It can be observed that the CD decreases as the size of the capacitor increases, regardless of the thickness and condition of SixNy. After a certain point, the CD remains constant. This phenomenon can be attributed to the effect of fringe capacitance due to the perimeter/area ratio and the variation in fringe impedance CD (FICD) with respect to size. The difference between capacitor sizes of 10 × 10 and 20 × 20 μm2 is more pronounced in the case of FICD variation, as it has a greater impact on smaller sizes [37].
In terms of device fabrication, the uniformity of the CD is closely related to the process capability index (Cp, Cpk), with SixNy thickness uniformity being the most important factor.
As depicted in Figure 4, although there are a few points that deviate from the linear trend, a proportional relationship exists between SixNy thickness nonuniformity and CD nonuniformity, with a slope of 1.04.
Improving the uniformity of SixNy thickness can result in an improvement in CD uniformity, which, in turn, can increase the values of Cp and Cpk on the device manufacturing side to 1.33 or above.
To measure the VCC, an index indicating the degree of change in capacitance with respect to voltage variations, measurements were taken at the top, center, and bottom of the wafers according to the thickness of SixNy and the conditions. The VCC is denoted by Vcc1 (ppm/dV) and Vcc2 (ppm/dV2), as expressed by Equation (3) [38]:
C V C 0 C 0 = V c c 2 V 2 + V c c 1 V + C
where C(V) is the capacitance under variable voltage, C(0) is the capacitance at 0 V, Vcc1 and Vcc2 are the VCCs, and C is a constant value.
The VCC graph was plotted by performing a polynomial fit with the voltage on the X-axis and the normalized ΔC on the y-axis, as described in Equation (3). As an example, the VCC graph for the SixNy film processed with the NEWMIM condition at a thickness of 500 Å is depicted in Figure 5.
The VCC graph results for the SixNy films, which vary in thickness (650 Å, 500 Å, and 400 Å) and condition (MIM, NEWMIM, DAMANIT, and NIT), are summarized in Figure 6. Figure 6a displays the Vcc1 values according to thickness, while Figure 6b illustrates the Vcc2 values as a function of thickness. Both the Vcc1 and Vcc2 values showed an increasing trend as the thickness decreased, with the initial level and degree of increase varying according to the condition.
In the case of Vcc1, all conditions showed values below 60 ppm/dV at 650 Ǻ, but they values increased as the thickness decreased, and only the MIM and NEWMIM conditions showed values over 60 ppm/V. Vcc2 tended to increase as the thickness decreased; however, all other conditions except NIT could satisfy the value of 100 ppm/dV2 or less when implementing a 2-fF/μm2 MIM capacitor.
To investigate the TCC characteristics of the MIM capacitors, the capacitance was measured at the center of the wafers with varying thicknesses and conditions of the SixNy films while incrementally raising the temperature to 25 °C, 50 °C, 75 °C, 100 °C, and 125 °C. The TCC was calculated using Equation (4) [39]:
C T C 25 C 25 = T c c T + C
where C(T) is the capacitance under variable temperature, C(25) is the capacitance at 25 °C, TCC is the TCC, and C is a constant value.
The TCC serves as an indicator of the degree of change in capacitance in response to temperature variations. Unlike the VCC, the TCC exhibits a linear relationship with temperature. Therefore, when the temperature is plotted on the X-axis and the normalized ΔC on the Y-axis, the slope value corresponds to the TCC value.
As an illustration, a TCC graph for SixNy films fabricated with the NEWMIM condition at thicknesses of 650, 500, and 400 Å is presented in Figure 7. Additionally, the results for the other conditions are presented to depict the variation in the TCC values according to thickness in Figure 8. Except for the NIT condition, the remaining conditions exhibited values below 50 ppm/dT, even as the thickness decreased. Moreover, the TCC values varied according to the condition at identical thicknesses.
As revealed by Table 4, the differences in SixNy conditions are attributed to the N-H/Si-H ratio. To depict the changes in the TCC due to film quality, the N-H/Si-H vs. TCC values are plotted in Figure 9. The results indicate that as the N-H/Si-H ratio increased, the TCC values exhibited an exponential decay trend, confirming that the TCC values are influenced by the quality of the SixNy film.

4. Conclusions

An evaluation of the C–V characteristics was conducted for MIM capacitors based on the insulator (SixNy) deposition thickness and deposition conditions. The CD values were in the ranges of 0.983–1.1, 1.24–1.4, and 1.57–1.79 fF/µm2 for 650, 500, and 400 Å, respectively. Further, the CD increased as the thickness decreased, with variations across different conditions.
At the same thickness, the NIT condition exhibited the highest CD, while the MIM condition showed the lowest. This discrepancy is attributed to the effect of the actual thickness and the difference in the k-value of the SixNy film according to the condition. Additionally, the CD was observed to decrease with increasing capacitor size, possibly due to the influence of fringe capacitance, which increased in proportion to the perimeter/area ratio.
The thickness uniformity of SixNy was found to be the most significant factor affecting capacitance uniformity. Improvements in thickness uniformity can enhance Cp and Cpk on the device side. Across all conditions, a general increase was observed in the VCC as the thickness decreased, although there were some variations between conditions. However, the TCC showed no significant difference with thickness, indicating that the variations were mainly due to the conditions.
In summary, from the perspective of C–V analysis, all conditions, except NIT, demonstrated superior characteristics. Implementing thin SixNy film depositions with stable uniformity using conditions other than NIT could potentially provide MIM capacitors with CD values of less than 100 ppm/dV2, aiming for the achievement of 2 fF/µm2.

Author Contributions

Conceptualization, T.-M.C., E.-S.J. and S.-G.P.; methodology, S.-G.P.; validation, J.-U.Y. and H.-R.L.; writing—original draft preparation, T.-M.C.; supervision, S.-G.P.; project administration, S.-G.P. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Technology Innovation Program (or Industrial Strategic Technology Development Program—Public–private joint investment semiconductor R&D program (K-CHIPS) to foster high-quality human resources) (“RS-2023-00237003”, High selectivity etching technology using cryoetch) funded by the Ministry of Trade, Industry and Energy (MOTIE, Republic of Korea) (1415187674).

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Acknowledgments

This research was supported by the Chung-Ang University Graduate Research Scholarship in 2023.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Xiong, L.; Hu, J.; Yang, Z.; Li, X.; Zhang, H.; Zhang, G. Dielectric Properties Investigation of Metal–Insulator–Metal (MIM) Capacitors. Molecules 2022, 27, 3951. [Google Scholar] [CrossRef] [PubMed]
  2. Karthik, R.; Manjusha, K.A. Metal Insulator Metal Capacitors-State of the Art. J. Comput. Theor. Nanosci. 2018, 15, 2346–2349. [Google Scholar] [CrossRef]
  3. Ding, S.-J.; Hu, H.; Zhu, C.; Kim, S.J.; Yu, X.; Li, M.-F.; Cho, B.J.; Chan, D.S.H.; Yu, M.B.; Rustagi, S.C.; et al. RF, DC, and reliability characteristics of ALD HfO2-Al2O3 laminate MIM capacitors for Si RF IC applications. IEEE Trans. Electron Devices 2004, 51, 886–894. [Google Scholar] [CrossRef]
  4. Choi, E.; Kim, A.; Kwon, S.H.; Pyo, S.G. Effect of Interface Treatment on the Voltage Linearity in 8 fF/μm2 High-k Dielectric and Combination Stacks on Metal Insulator Metal (MIM) Capacitor. Sci. Adv. Mater. 2018, 10, 467–470. [Google Scholar] [CrossRef]
  5. Hoa, P.T. High-K Dielectrics in Metal Insulator Metal (MIM) Capacitors for RF Applications. Ph.D. Thesis, National University of Singapore, Singapore, 2011. [Google Scholar]
  6. Pavunny, S.P.; Misra, P.; Scott, J.F.; Katiyar, R.S. Advanced high-k dielectric amorphous LaGdO3 based high density metal-insulator-metal capacitors with sub-nanometer capacitance equivalent thickness. Appl. Phys. Lett. 2013, 102, 252905. [Google Scholar] [CrossRef]
  7. Ding, S.-J.; Hu, H.; Lim, H.; Kim, S.; Yu, X.; Zhu, C.; Li, M.; Cho, B.J.; Chan, D.S.; Rustagi, S.C. High-performance MIM capacitor using ALD high-k HfO2-Al2O3 laminate dielectrics. IEEE Electron Device Lett. 2003, 24, 730–732. [Google Scholar] [CrossRef]
  8. Sul, W.S.; Pyo, S.G. RF Characteristic Analysis Model Extraction on the Stacked Metal–Insulator–Metal Capacitors for Radio Frequency Applications. IEEE Trans. Electron Devices 2014, 61, 3011–3013. [Google Scholar] [CrossRef]
  9. Mu, J.; Chou, X.; Ma, Z.; He, J.; Xiong, J. High-Performance MIM Capacitors for a Secondary Power Supply Application. Micromachines 2018, 9, 69. [Google Scholar] [CrossRef]
  10. Li, W.; Lu, X.; Yang, R.; Liang, F.; Chen, W.; Xie, Z.; Zheng, J.; Zhu, J.; Huang, Y.; Yue, W.; et al. Highly sensitive and reproducible SERS substrates with binary colloidal crystals (bCCs) based on MIM structures. Appl. Surf. Sci. 2022, 597, 153654. [Google Scholar] [CrossRef]
  11. Jeon, S.; Sung, S.-K.; Jang, E.-H.; Jeong, J.; Surabhi, S.; Choi, J.-H.; Jeong, J.-R. Multilayer metal-oxide-metal nanopatterns via nanoimprint and strip-off for multispectral resonance. Appl. Surf. Sci. 2018, 428, 280–288. [Google Scholar] [CrossRef]
  12. Smitha, P.S.; Babu, V.S.; Shiny, G. Critical parameters of high performance metal-insulator-metal nanocapacitors: A review. Mater. Res. Express 2019, 6, 122003. [Google Scholar] [CrossRef]
  13. Sejas-García, S.C.; Torres-Torres, R.; Valderrama-B, R.; Molina, J. Complex Permittivity Determination of Thin-Films through RF-Measurements of a MIM Capacitor. IEEE Microw. Wirel. Compon. Lett. 2014, 24, 805–807. [Google Scholar] [CrossRef]
  14. Nam, M.; Kim, A.; Kang, K.; Choi, E.; Kwon, S.H.; Lee, S.J.; Pyo, S.G. Characterization of atomic layer deposited Al2O3/HfO2 and Ta2O5/Al2O3 combination stacks. Sci. Adv. Mater. 2016, 8, 1958–1962. [Google Scholar] [CrossRef]
  15. Jin Chung, J.; Hyuk Kim, T.; Ahsan Saeed, M.; Won Shim, J. Laminated indium-oxide/molybdenum-oxide nanocomposites for high-work-function electrodes in organic photovoltaics and capacitor devices. Appl. Surf. Sci. 2023, 610, 155526. [Google Scholar] [CrossRef]
  16. Guo, Y.; Wang, S.; Du, X.; Liang, S.; Huang, S.; Peng, S.; Xie, Y.; Ma, M.; Xiong, L. Construction of ultrahigh capacity density carbon nanotube based MIM capacitor. Energy Storage Mater. 2023, 63, 103064. [Google Scholar] [CrossRef]
  17. Ruhl, G.; Lehnert, W.; Lukosius, M.; Wenger, C.; Baristiran Kaynak, C.; Blomberg, T.; Haukka, S.; Baumann, P.K.; Besling, W.; Roest, A.; et al. Dielectric Material Options for Integrated Capacitors. ECS J. Solid State Sci. Technol. 2014, 3, N120–N125. [Google Scholar] [CrossRef]
  18. Zheng, G.; He, Y.L.; Zhu, B.; Wu, X.; Zhang, D.W.; Ding, S.J. Improvement of Voltage Linearity and Leakage Current of MIM Capacitors With Atomic Layer Deposited Ti-Doped ZrO2 Insulators. IEEE Trans. Electron Devices 2023, 70, 3064–3070. [Google Scholar] [CrossRef]
  19. Park, Y.S.; Cho, S.-J.; Boo, J.-H.; Hong, B. Surface and electrical properties of organic–inorganic hybrid structure as gate insulator to organic thin film transistor. Appl. Surf. Sci. 2009, 256, 1023–1027. [Google Scholar] [CrossRef]
  20. Wu, Y.-H.; Kao, C.-K.; Chen, B.-Y.; Lin, Y.-S.; Li, M.-Y.; Wu, H.-C. High density metal-insulator-metal capacitor based on ZrO2/Al2O3/ZrO2 laminate dielectric. Appl. Phys. Lett. 2008, 93, 033511. [Google Scholar] [CrossRef]
  21. Xu, T.; Tekes, C.; Degertekin, F.L. CMUTs with high-K atomic layer deposition dielectric material insulation layer. IEEE Trans. Ultrason. Ferroelectr. Freq. Control. 2014, 61, 2121–2131. [Google Scholar] [CrossRef]
  22. Sudheendran, K.; Pamu, D.; Ghanashyam Krishna, M.; James Raju, K.C. Determination of dielectric constant and loss of high-K thin films in the microwave frequencies. Measurement 2010, 43, 556–562. [Google Scholar] [CrossRef]
  23. Holden, K.E.K.; Hall, G.D.R.; Cook, M.; Kendrick, C.; Pabst, K.; Greenwood, B.; Daugherty, R.; Gambino, J.P.; Allman, D.D.J. Dielectric Relaxation, Aging and Recovery in High-K MIM Capacitors. In Proceedings of the 2021 IEEE International Reliability Physics Symposium (IRPS), Monterey, CA, USA, 21–25 March 2021; pp. 1–10. [Google Scholar]
  24. Zhao, C.; Zhao, C.Z.; Werner, M.; Taylor, S.; Chalker, P. Dielectric relaxation of high-k oxides. Nanoscale Res. Lett. 2013, 8, 456. [Google Scholar] [CrossRef]
  25. Ohshima, I.; Cheng, W.; Ono, Y.; Higuchi, M.; Hirayama, M.; Teramoto, A.; Sugawa, S.; Ohmi, T. Reliability of silicon nitride gate dielectrics grown at 400 °C formed by microwave-excited high-density plasma. Appl. Surf. Sci. 2003, 216, 246–251. [Google Scholar] [CrossRef]
  26. Ma, T.P. Gate dielectric properties of silicon nitride films formed by jet vapor deposition. Appl. Surf. Sci. 1997, 117–118, 259–267. [Google Scholar] [CrossRef]
  27. Yu, H.Y.; Li, M.F.; Kwong, D.L. ALD (HfO2)x(Al2O3)1−x high-k gate dielectrics for advanced MOS devices application. Thin Solid Films 2004, 462–463, 110–113. [Google Scholar] [CrossRef]
  28. Lue, H.T.; Lai, S.C.; Hsu, T.H.; Du, P.Y.; Wang, S.Y.; Hsieh, K.Y.; Liu, R.; Lu, C.Y. Understanding barrier engineered charge-trapping NAND flash devices with and without high-K dielectric. In Proceedings of the 2009 IEEE International Reliability Physics Symposium, Montreal, QC, Canada, 26–30 April 2009; pp. 874–882. [Google Scholar]
  29. Cockbain, A.G.; Harrop, P.J. The temperature coefficient of capacitance. J. Phys. D Appl. Phys. 1968, 1, 1109. [Google Scholar] [CrossRef]
  30. Khaldi, O.; Jomni, F.; Gonon, P.; Mannequin, C.; Yangui, B. Investigation of electrical properties of HfO2 metal–insulator–metal (MIM) devices. Appl. Phys. A 2014, 116, 1647–1653. [Google Scholar] [CrossRef]
  31. Lee, A.J.; Kim, B.S.; Hwang, J.H.; Kim, Y.; Oh, H.; Park, Y.; Jeon, W. Controlling the crystallinity of HfO2 thin film using the surface energy-driven phase stabilization and template effect. Appl. Surf. Sci. 2022, 590, 153082. [Google Scholar] [CrossRef]
  32. Li, H.; Yun, H.; Liang, W.; Dong, A.; Miao, M.; Sundaram, K.B. Characterization of Dielectric Breakdown and Lifetime Analysis for Silicon Nitride Metal-Insulator-Metal Capacitors under Electrostatic Discharge Stresses. In Proceedings of the 2018 IEEE International Symposium on the Physical and Failure Analysis of Integrated Circuits (IPFA), Singapore, 16–19 July 2018; pp. 1–5. [Google Scholar]
  33. Kim, K.H.; Kim, K.S.; Ji, Y.J.; Kang, J.E.; Yeom, G.Y. Silicon nitride deposited by laser assisted plasma enhanced chemical vapor deposition for next generation organic electronic devices. Appl. Surf. Sci. 2021, 541, 148313. [Google Scholar] [CrossRef]
  34. Yota, J. Effects of Deposition Method of PECVD Silicon Nitride as MIM Capacitor Dielectric for GaAs HBT Technology. ECS Trans. 2011, 35, 229. [Google Scholar] [CrossRef]
  35. Iversen, C.-R. A high density MIM capacitor in a standard CMOS process. JSTS J. Semicond. Technol. Sci. 2001, 1, 189–192. [Google Scholar]
  36. Bertaud, T.; Bermond, C.; Blonkowski, S.; Vallee, C.; Lacrevaz, T.; Farcy, A.; Gros-Jean, M.; Flechet, B. Electrical Characterization of Advanced MIM Capacitors With ZrO2 Insulator for High-Density Packaging and RF Applications. IEEE Trans. Compon. Packag. Manuf. Technol. 2012, 2, 502–509. [Google Scholar] [CrossRef]
  37. Sharp, K.A.; Honig, B. Electrostatic Interactions in Macromolecules: Theory and Applications. Annu. Rev. Biophys. 1990, 19, 301–332. [Google Scholar] [CrossRef]
  38. Kittel, C. Introduction to Solid State Physics; Wiley: Hoboken, NJ, USA, 2004. [Google Scholar]
  39. Kim, S.J.; Cho, B.J.; Li, M.-F.; Ding, S.-J.; Zhu, C.; Yu, M.B.; Narayanan, B.; Chin, A.; Kwong, D.-L. Improvement of voltage linearity in high-/spl kappa/ MIM capacitors using HfO2-SiO2 stacked dielectric. IEEE Electron Device Lett. 2004, 25, 538–540. [Google Scholar] [CrossRef]
Figure 1. Accumulation curves for CD obtained from different thicknesses and conditions of SixNy films for MIM capacitors.
Figure 1. Accumulation curves for CD obtained from different thicknesses and conditions of SixNy films for MIM capacitors.
Micromachines 15 01204 g001
Figure 2. Cross-sectional TEM images of SixNy films with (a) MIM, (b) NEWMIM, (c) DAMANIT, and (d) NIT. The thicknesses of the SixNy films are presented in the (e) rod graph.
Figure 2. Cross-sectional TEM images of SixNy films with (a) MIM, (b) NEWMIM, (c) DAMANIT, and (d) NIT. The thicknesses of the SixNy films are presented in the (e) rod graph.
Micromachines 15 01204 g002
Figure 3. Effect of capacitor size on MIM CD with different SixNy thicknesses and conditions.
Figure 3. Effect of capacitor size on MIM CD with different SixNy thicknesses and conditions.
Micromachines 15 01204 g003
Figure 4. Relationship between nonuniformity of CD and SixNy thickness.
Figure 4. Relationship between nonuniformity of CD and SixNy thickness.
Micromachines 15 01204 g004
Figure 5. Normalized ΔC vs. voltage at the top, center, and bottom positions. The condition and thickness of the SixNy film are NEWMIM and 500 Ǻ, respectively.
Figure 5. Normalized ΔC vs. voltage at the top, center, and bottom positions. The condition and thickness of the SixNy film are NEWMIM and 500 Ǻ, respectively.
Micromachines 15 01204 g005
Figure 6. Graphs of (a) VCC1 and (b) VCC2 vs. thickness with SixNy conditions.
Figure 6. Graphs of (a) VCC1 and (b) VCC2 vs. thickness with SixNy conditions.
Micromachines 15 01204 g006
Figure 7. The TCC graph for SixNy films fabricated with the NEWMIM condition at thicknesses of 650, 500, and 400 Å.
Figure 7. The TCC graph for SixNy films fabricated with the NEWMIM condition at thicknesses of 650, 500, and 400 Å.
Micromachines 15 01204 g007
Figure 8. Graph of TCC1 vs. thickness with different SixNy conditions.
Figure 8. Graph of TCC1 vs. thickness with different SixNy conditions.
Micromachines 15 01204 g008
Figure 9. Graph of TCC vs. thickness with varying N:H/Si-H ratio.
Figure 9. Graph of TCC vs. thickness with varying N:H/Si-H ratio.
Micromachines 15 01204 g009
Table 1. (a) SixNy film properties and (b) corresponding process conditions.
Table 1. (a) SixNy film properties and (b) corresponding process conditions.
(a)MIMNEW MIM 650DAMA NITNIT
Dep. rate~149 Å/s~29 Å/s~59 Å/s88 Å/s
Within W/F unit (1σ)1.14%1.90%2.34%2.77%
W/F to W/F unit (1σ)1.58%2.21%1.05%2.30%
Stress−2.23 × 109−1.75 × 1010−2.34 × 109
H content (N-H: Si-H)12.7%: 8.5%22.5%: 0.8%10.5%: 7.3%4.4%: 14.8%
N content (N-H/Si-H)1.4928.11.430.30
(b)MIM 650NEW MIM 650DAMA NITNIT 650
Step end controlBy timeBy timeBy timeBy time
Maximum step time4.4 s22.8 s11.0 s
Endpoint selectionNo endpointNo endpointNo endpointNo endpoint
PressureServo 4.25 TorrServo 4.25 TorrServo 4.2 TorrServo 4.5 Torr
RF power690 W690 W420 W425 W
Susc. temperature400 °C400 °C400 °C400 °C
Susceptor spacing620 mils620 mils550 mils475 mils
N23800 sccm3800 sccm2500 sccm4000 sccm
NH3130 sccm50 sccm38 sccm60 sccm
SiH4260 sccm100 sccm110 sccm170 sccm
Table 2. C–V characterization measurement conditions.
Table 2. C–V characterization measurement conditions.
ParameterSetting
Display modeCp (parallel capacitor), D (dissipation factor)
Sweep voltage (V)−5~5
Step (V)0.5
Oscillation0.025
Frequency (kHz)100
Capacitor size (μm2)10 × 10, 15 × 15, 20 × 20, 25 × 25, 30 × 30, 50 × 50
Measurement pointsThree points (top, center, and bottom)
Temperature (°C)25, 50, 75, 100, 125
Table 3. The k-values of the MIM capacitor with SixNy conditions of MIM, NEWMIM, DAMANIT, and NIT.
Table 3. The k-values of the MIM capacitor with SixNy conditions of MIM, NEWMIM, DAMANIT, and NIT.
Deposition ConditionMIMNEWMIMDAMANITNIT
CD (fF/μm2)1.32561.32031.31031.3606
Thickness (TEM, Å)453473457422
k-value (ε0·ε)6.00 × 10−176.25 × 10−175.99 × 10−175.74 × 10−17
Table 4. Properties of SixNy films according to different conditions.
Table 4. Properties of SixNy films according to different conditions.
MIM 650 DEPNEW MIM 650 DEPDAMA NIT 650 DEPNIT 650 DEP
Deposition rate (Å/s)~149~29~5988
Within W/F unit (1σ, %)1.141.902.342.77
W/F to W/F unit (1σ, %)1.582.211.052.30
Stress−2.23 × 109−1.75 × 1010−2.34 × 109-
H content (N-H:Si-H)12.7%:8.5%22.5%:0.8%10.5%:7.3%4.4%:14.8%
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Choi, T.-M.; Jung, E.-S.; Yoo, J.-U.; Lee, H.-R.; Pyo, S.-G. Capacitance–Voltage Fluctuation of SixNy-Based Metal–Insulator–Metal Capacitor Due to Silane Surface Treatment. Micromachines 2024, 15, 1204. https://doi.org/10.3390/mi15101204

AMA Style

Choi T-M, Jung E-S, Yoo J-U, Lee H-R, Pyo S-G. Capacitance–Voltage Fluctuation of SixNy-Based Metal–Insulator–Metal Capacitor Due to Silane Surface Treatment. Micromachines. 2024; 15(10):1204. https://doi.org/10.3390/mi15101204

Chicago/Turabian Style

Choi, Tae-Min, Eun-Su Jung, Jin-Uk Yoo, Hwa-Rim Lee, and Sung-Gyu Pyo. 2024. "Capacitance–Voltage Fluctuation of SixNy-Based Metal–Insulator–Metal Capacitor Due to Silane Surface Treatment" Micromachines 15, no. 10: 1204. https://doi.org/10.3390/mi15101204

APA Style

Choi, T. -M., Jung, E. -S., Yoo, J. -U., Lee, H. -R., & Pyo, S. -G. (2024). Capacitance–Voltage Fluctuation of SixNy-Based Metal–Insulator–Metal Capacitor Due to Silane Surface Treatment. Micromachines, 15(10), 1204. https://doi.org/10.3390/mi15101204

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop