Next Article in Journal
Interfering with mRNA Methylation by the 2′O-Methyltransferase (NSP16) from SARS-CoV-2 to Tackle the COVID-19 Disease
Next Article in Special Issue
Rice Crust-Like ZnO/Ti3C2Tx MXene Hybrid Structures for Improved Photocatalytic Activity
Previous Article in Journal
Alkaline-Based Catalysts for Glycerol Polymerization Reaction: A Review
Previous Article in Special Issue
Examination of Photocatalyzed Chlorophenols for Sequential Photocatalytic-Biological Treatment Optimization
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Dynamics of Photogenerated Charge Carriers in TiO2/MoO3, TiO2/WO3 and TiO2/V2O5 Photocatalysts with Mosaic Structure

by
Alexander I. Kokorin
1,2,
Tatyana V. Sviridova
3,
Elizaveta A. Konstantinova
4,5,6,*,
Dmitry V. Sviridov
3 and
Detlef W. Bahnemann
7,8
1
N.N. Semenov Federal Research Center for Chemical Physics RAS, 119991 Moscow, Russia
2
Department of Technology, Plekhanov Russian University of Economics, 119991 Moscow, Russia
3
Chemical Department, Belarusian State University, 220030 Minsk, Belarus
4
Physics Department, Lomonosov Moscow State University, 119991 Moscow, Russia
5
National Research Center “Kurchatov Institute”, 123182 Moscow, Russia
6
Faculty of Nano-, Bio-, Information and Cognitive Technologies, Moscow Institute of Physics and Technology, 141700 Dolgoprudny, Russia
7
Laboratory “Photoactive Nanocomposite Materials”, Saint-Petersburg State University, 198504 Saint-Petersburg, Russia
8
Institut für Technische Chemie, Leibniz Universität Hannover, D-30167 Hannover, Germany
*
Author to whom correspondence should be addressed.
Catalysts 2020, 10(9), 1022; https://doi.org/10.3390/catal10091022
Submission received: 9 August 2020 / Revised: 29 August 2020 / Accepted: 1 September 2020 / Published: 4 September 2020
(This article belongs to the Special Issue Photocatalytic Nanocomposite Materials)

Abstract

:
Titania is a widely used photocatalytic material possessing such advantages as low cost and high reactivity under the ultraviolet light illumination. However, the fast recombination of photoexcited charge carriers limits its application. Herein, we have synthesized original nanomaterials with mosaic structures that exhibited well-defined heterojunctions and new properties. Using SEM, XRD, EPR spectroscopy, photocatalytic measurements, and photoinduced pathphysiological activity of these photocatalysts, we studied the processes of charge carrier accumulation in TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 under in situ UV illumination with emphasis on the charge exchange between energy levels of these nanosized semiconductors. It is shown that the accumulation of photoinduced charges occurs in two forms (i) filled electron traps corresponding to Ti4+/Ti3+ levels and (ii) Mo5+ centers, both forms contributing to the photoinduced biocide activity of the samples. This work demonstrates that light exposure of heterostructure photocatalysts with mosaic surfaces produces different types of charge-trapping centers capable of interacting with molecular oxygen yielding peroxo species, which provide long-life light-induced ”self-cleaning” behavior. Such photoaccumulating materials open new opportunities in developing light-driven self-sterilization structures exhibiting a prolonged bactericidal effect up to 10 h after stopping light exposure.

1. Introduction

Numerous photocatalysts have been synthesized and tested during the last 30 years, e.g., [1,2,3,4,5,6,7,8,9] and references therein. The combination of titania as a highly active semiconductor catalyst [5] with redox-active oxides [10,11], hydroxides [12] and polyoxometallates [13] enables the accumulation of photoinduced charge carriers which can be then spent in bacteria killing processes under dark conditions as well as for the degradation of toxic organic chemicals. However, the photoaccumulating catalysts of this type demonstrate rather low charge storage capacity that constrain the prospects of their application for developing the photobiocide materials with prolonged antimicrobial activity. The real breakthrough in developing a charge storage photocatalyst was achieved recently when the metastable phase of MoO3, WO3, and V2O5 with open channel structures was used together with TiO2 yielding thin-film heterostructure photocatalysts capable of retaining microbiocide activity for a unprecedentedly long time (up to 10 h) after exposure [14,15,16,17,18].
The idea of a systematic study of metal ion doping in nanosized TiO2 particles has already been discussed in [19]. The photoreactivities and the transient charge carrier recombination dynamics in Fe3+, Mo5+, Ru3+, Os3+, Re5+, V4+, and the Rh3+ doped TiO2 crystalline matrix were measured and significantly influenced photoreactivity, charge carrier recombination rates, and interfacial electron-transfer rates [19]. The conduction band electron reduction in an electron acceptor (CCl4 dechlorination) and the valence band hole oxidation of an electron donor (CHCl3 degradation) were studied in detail. Doping with ions shown above at 0.1–0.5% increased the photoactivity for both redox reactions, while Co3+ and Al3+ doping decreased the photoactivity. It was revealed that transient absorption signals upon laser flash photolysis (λex = 355 nm) at λ = 600 nm were extended up to 50 ms for Fe3+-, V4+-, Mo5+-, and Ru3+-doped TiO2, and the undoped nano-TiO2 showed a complete “blue electron” signal decay within 200 μs. Co3+- and Al3+-doped TiO2 were characterized by rapid signal decays with a complete loss of absorption signals within 5 μs. Photoactivities increased with the concentration of trapped charge carriers and the authors concluded the complex function effecting of the dopant concentration, the energy level of dopants within the TiO2 lattice, their electronic states, the electron donor concentration and distribution, and the light intensity on the rate of the process and its mechanism [19].
The photoinduced redox transformations responsible for charge storage in these photocatalytic systems are based on the light-induced charge carrier separation using composites of two and three different metal oxides, which are accompanied by the generation of paramagnetic centers that makes the electron paramagnetic resonance (EPR) spectroscopy a powerful tool for the investigation of the mechanism of such processes, as well as the features of photoaccumulation effects. Experimental results quantitatively described changes in EPR spectra; dynamics of the processes occurred in N-, Ti3+-, Mo5+-, and V4+-doped TiO2 (anatase); and their most probable mechanisms were recently discussed in detail in [15,16,17,18].
Similar independent results based on the EPR method in the investigation of phenomena occurring in heterogeneous photocatalysis, the stabilization of the carriers, and their consequent surface reactivity was also recently published in [20]. The authors described the behavior of four photoactive oxides (ZrO2, ZrTiO4, TiO2, and ZnO) with different band gaps which exhibited electron and hole stabilization. The EPR technique revealed the following stabilized centers: Zr4+, Ti4+, and Zn2+ for trapped electrons and the hole trapping such as the formation of O centers [20]. The electron transfer reactivity at the surface of the photogenerated carriers was monitored using specific scavengers in the gas phase over the solid (molecular O2 and H2) for electron scavenging and hole scavenging, respectively. EPR was particularly useful for checking the features of novel photocatalytic materials [20].
In this paper, we used the SEM, XRD, EPR spectroscopy, photocatalytic measurements, and photoinduced pathphysiological activity of photocatalysts to elucidate the structure of energy levels involved in the storage of the reductive energy in TiO2/MoO3 (WO3, V2O5) heterostructure photocatalysts under in situ UV light illumination with emphasis on the charge exchange between these levels of different nanosized oxide semiconductors.

2. Results and Discussion

2.1. Characterization of the Samples

2.1.1. Microscopy

All materials used in the work were purchased from Sigma–Aldrich Chemical Co. and used as supplied. For preparation of solutions, the Milli-Q water was used. The thin-film photocatalysts were prepared using aqueous dispersions of TiO2, MoO3, WO3, and V2O5 contrastingly to hydrolytically, pyrolytically, or mechanochemically derived TiO2/MoO3 (V2O5, V2O5:MoO3) composite photocatalysts investigated in our previous works [14,15,16,17,18,21]. These photocatalysts consisting of the initially synthesized crystallites exhibited well-defined heterojunctions and demonstrated a mosaic structure. The detailed mechanism behind solvothermal synthesis based on the polycondensation of oxo-compounds is discussed elsewhere [14,21]. This synthetic procedure yields perfect crystallites of hexagonal MoO3, hexagonal WO3, and V2O5 xerogel (both crystalline polymorphs possess the lamellar structure) with the medium size of 200–500 nm.
The morphological investigations employing SEM provided evidence about mosaic structure (Figure 1).
The AFM (atomic force microscope) images for TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 heterostructure photocatalysts given in Figure 2 show that the size of building blocks forming the surface of composite film exhibited a considerable decrease when going from TiO2/MoO3 film to TiO2/WO3 film and then to TiO2/V2O5 (the mean roughness evaluated from AFM 10 × 10 μm plots decreased from 398 nm to 380 and 306 nm, correspondingly).
The observed decrease in the composite roughness can be attributed to the well-known fact of a mutual protective action of composite-forming oxide components against their crystallization that hampers rearrangements in the composite film during an annealing and a strong tendency to form aggregates inherent in V2O5 particles. Notwithstanding these variations in the surface roughness that should considerably affect the specific contact angle values, the heterogeneous binary surface of composite films remained hydrophilic (the water contact angle amounted to ~25° even for TiO2/V2O5 film with the smoothest surface) that should facilitate water adsorption from humid air and thus creates favorable conditions for photocatalyst operation.

2.1.2. XRD

According to XRD analysis, hexagonal MoO3 with an admixture of monoclinic MoO3·H2O, hexagonal WO3 with an admixture of orthorhombic WO3·0.33H2O, and lamellar V2O5 xerogel crystallites were formed (Figure 3).
According to XRD analysis, the resultant titania was anatase (Figure 4) with the medium size of crystallites of ca. 4 nm. The size of crystallites (regions of coherent scattering) was estimated from the broadening of diffraction reflections using the Scherer formula:
d X R D = k λ β cos θ
where dXRD is the average size of the coherent scattering region, β is the width of the corresponding diffraction peak at half maximum, λ is the wavelength of the radiation used, θ is the diffraction angle, and k = 0.9.
The mixtures of TiO2 sol and MoO3 (V2O5) suspensions (2:1 in the case of TiO2/MoO3 and TiO2/V2O5 photocatalysts) were deposited onto the glass substrate by pulverization. The resultant coating was then annealed at 400 °C. The XRD analysis evidenced that the annealing did not result in the recrystallization of the oxide phases forming the photocatalytic film. According to the AFM measurements thus obtained, thin-film photocatalytic coatings had a thickness of ca. 2.5 μm.

2.2. Photocatalytic and Pathphysiological Activity of TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 Heterostructure Photocatalysts

The kinetic curves shown in Figure 5a demonstrate degradation of probing dye at the surface of pre-exposed TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 heterostructure photocatalysts; for comparison, the curve for bare titania is given. The efficient storage of photoproduced negative charge observed for all binary photocatalysts resulting in the induced oxidation activity imparted to their surface. This oxidation activity retains for a long time after exposure due to the formation of hydrogen bronzes of variable composition [14,22] which exhibit one-electron oxidation with molecular oxygen yielding peroxo species [16].
The continuous generation of peroxo species during the course of discharging is also responsible for the long-term microbiocide effect as evident by Figure 5b. It is seen from Figure 5b that the survival ratio for heterostructure photocatalysts even exhibited some further decreases when standing in the dark after exposure due to the buildup of the surface concentration of peroxide and then began to decline. From this point of view, the photoaccumulating heterostructure catalysts differed radically from bare TiO2, which lost the light-induced pathophysiological activity almost immediately (within one minute) after UV illumination due to short lifetimes inherent in reactive oxygen species generated at the titania surface under illumination (the lifetime of hydroxyl radicals is below a second, while the lifetime of O2 does not exceed 50 s [23,24]). The survival ratio versus time dependencies given in Figure 5b permit a conclusion that pre-exposed TiO2/V2O5 photocatalyst demonstrated higher biocide activity as compared to TiO2/MoO3 and TiO2/WO3 photocatalysts.

2.3. EPR Measurements of Heterostructure Photocatalysts

At the next step of the work, we applied an EPR technique for investigating the nature, concentration of paramagnetic centers (PCs) existing in mixed photocatalysts initially, and their change after UV irradiation. Indeed, all PCs in these systems are kinds of structural “defects” because TiO2, MoO3, WO3, and V2O5 contain transition metal ions, in principle, in the ground diamagnetic states such as Ti4+, Mo6+, W6+, and V5+; hence, one electron that reduced Ti3+, Mo5+, W5+, and V4+ ions can be assumed as a specific spin probe.
Spectra shown in Figure 6 demonstrate the presence of several different PCs in the initial TiO2/MoO3 oxide, e.g., titanium (3+) ions located in the lattice (Ti3+lat) or on the surface (Ti3+surf), molybdenum Mo5+ PCs, and nitrogen atoms usually marked as N for stressing its paramagnetic nature. Spin Hamiltonian parameters, g-tensor and A-tensor characterizing Zeeman and hyperfine (hfi) interactions, determined from EasySpin modeling gave values represented in Table 1, which coincide in the error limits with those reported in [16,17,25,26] and references therein. Earlier, it was shown by double integration of EPR spectra that no more than 1–2% of the total content of nitrogen 14N atoms are paramagnetic in these systems [26,27], while the others remain diamagnetic. It was proved that the signal from N-radical definitely appeared after high temperature treatment of oxide–hydroxide precipitate, and its source was NH4+ residues adsorbed on the TiO2 particle surface or incorporated into the TiO2 matrix. Positions of EPR lines of other paramagnetic centers are shown in Figure 6 and agree with the literature very well. We should note that in our case, two types of Mo5+ centers were observed: (i) a signal Mo5+(1) and (ii) a broad single line Mo5+(2) with a line width ΔH ≈ 7.0 ± 0.6 mT, most likely caused by the presence of Mo5+ PCs in two various structural states or phases.
UV illumination of TiO2/MoO3 sample produced sufficient changes in the EPR spectrum (Figure 6). Since the intensity of the surface Ti3+surf lines and both Mo5+ PCs increased, that of the bulk Ti3+lat centers did not practically change, and of N atoms decreased ca. fourfold without any changes in the line positions. Evidently, these spectral transformations directly reflect the corresponding changes in PC concentration. Note that in this system, we could also observe the appearance of the O2 radicals (see Figure 6). Kinetic dependences of these changes under UV irradiation are reproduced graphically in Figure 7. For better comparison, we plotted all these curves in arbitrary units.
One can see that UV illumination increased the concentrations of paramagnetic metal ions and decreased that of N-radical during ca. 50–60 min of treatment, and afterwards they stayed constant reflecting stationary rates of the creation and decay of these PCs. All changes were impressive: from four- to fivefold (Figure 7). It is also obvious that the rate of photogeneration of all these metal PCs at first 60 min of irradiation was practically equal, and this allows the assumption that all observed reduction processes were correlated and not independent.
In the dark conditions after switching off illumination, created paramagnetic centers were re-oxidized by air dioxygen and by electron transfer reactions between reduced PCs according to their red-ox potentials. These processes were much slower (over 30–40 h, see Figure 8) due to complex character of the electron transfer in such nanosized heterojunction systems [14,15,16,17,18,25]. Note that (i) at the first 10 h in the dark, the decay was exponential, and later it became practically linear fitted; (ii) the rate of the decay processes varied on the metal nature: Ti3+surf concentration changed faster than that of V4+; (iii) concentration of N radicals increased linearly during all 40 h (Figure 8).
UV irradiation of TiO2/WO3 also produced noticeable changes (Figure 9): initial EPR signal recorded in dark conditions (g ≈ 1.63 and ΔH ≈ 23.0 mT) transformed to a new spectrum with parameters listed in Table 1, which correlate with g-values published in [28,29,30,31]. The observed three-axes anisotropy is usual for W5+ PCs. Unfortunately, we could not quantitatively characterize kinetics under illumination and in the dark afterwards due to very noisy EPR spectra recording (Figure 9).
Figure 10 represents changes in EPR spectra after 10 min of UV illumination of TiO2/V2O5 photocatalyst, which led to an approximately twofold increase in the spectrum intensity. The kinetics of V4+ signal grove and its decay in the dark conditions are shown in Figure 7 and Figure 8. We would stress that the EPR signal intensity of V4+ PCs in mixed oxides containing vanadium pentoxide as one of the components is so high that spectra of Ti3+ or Mo5+ paramagnetic species cannot be observed due to their much lower amplitude as well as the high oxidative properties of V5+ ions in V2O5.
It has been shown recently that the position of energy levels corresponding to the charge accepting states in the bandgap of TiO2, MoO3, and V2O5 (Mo6+/Mo5+, V5+/V4+, Ti4+/Ti3+) can be determined from EPR measurements under in situ illumination [16]. The energies of these levels measured against the valence band of corresponding semiconductors are collected in Table 2. It should be noted that Ti4+/Ti3+ states involved into the charge exchange correspond to the surface states, whereas the population of lattice Ti4+/Ti3+ states is not modulated under illumination [16].
Due to the low signal-to-noise ratio exhibited by TiO2/WO3 that did not allow the determination of reliable energy value of W6+/W5+ states from EPR spectra, this energy was estimated from the X-ray photoelectron spectra for tungsten oxide bronzes [32]. Using the photocurrent onset potential values, Eon, given in Table 3 as the rough estimation of the energy position of the bottom of the conduction band of highly doped TiO2, MoO3, WO3, and V2O5, one can obtain the detailed energy diagram of the energy storage photocatalysts under consideration (Figure 11).
The EPR measurements strongly show that in the case of TiO2/MoO3 photocatalyst, there were two mechanisms of accumulation of negative charge photoproduced in TiO2: (i) injection of electrons into MoO3 followed by redox transformations of oxide accompanied by the formation of Mo(V) centers readily detectable in EPR spectra; (ii) ”indirect” filling of Ti4+/Ti3+ surface states via electron transfer from Mo6+/Mo5+ states which lie at higher energies. The latter process in the case of bare TiO2 appeared to be completely hindered since the rate constant of electron trapping at these states was much lower as compared to the rate constant of surface recombination. In the TiO2/MoO3 heterostructure photocatalyst, Ti4+/Ti3+ states were in equilibrium with the Mo6+/Mo5+ states, and their filling was not compete with recombination. By contrast, it is seen from the energy diagram given in Figure 11 that both W6+/W5+ and V5+/V4+ states lay below Ti4+/Ti3+ states and thus did not contribute to their filling. As a result, in the case of TiO2/WO3 and TiO2/V2O5 photocatalysts, the redox transformations in WO3 and V2O5 appeared to be the only mechanism responsible for charge storage.
The charged Ti4+/Ti3+ states at the surface of titania nanoparticles can be readily oxidized with oxygen from the air yielding peroxo species, which resulted in a high initial rate of probing dye degradation at the pre-exposed photocatalyst (Figure 1). However, due to rapid consumption of the charges accumulated at Ti4+/Ti3+ states, their contribution to the long-term pathophysiological activity was marginal. As a result, the photoinduced biocide activity of TiO2/MoO3 photocatalyst (as evident by Figure 2) appeared to be less than the photoinduced biocide activity of TiO2/WO3 and TiO2/V2O5 photocatalysts accumulating photoinduced charges solely in the form of hydrogen bronzes (and, therefore, demonstrating a lower initial rate of probing dye degradation—Figure 1). The oxidation of the hydrogen bronzes occurred slowly being governed by the diffusion of redox centers from the bulk of nanocrystals of redox-active oxides to their surface that ensure continuous production of peroxide (and guarantees high antimicrobial activity level) during a long period of time. The energy diagram given in Figure 11 also shows that combining nanoparticles of different oxides in the photocayalyst film, it is possible to realize cascade effects that ensure efficient separation and accumulation of photoproduced charges.
The EPR measurements thus provide evidence that in the case of heterostructure photocatalysts with mosaic surfaces (i.e., comprising photogenerating and redox-active components), the exposure to the actinic light results in the generation of charge-trapping reaction centers of several types exhibiting different oxidation activity and long-term stability. As a result, these centers make different contributions in the induced pathophysiological behavior of energy storage photocatalysts.

3. Materials and Methods

The thin-film photocatalysts were prepared using aqueous dispersions of TiO2, MoO3, WO3, and V2O5 (Sigma-Aldrich, St. Louis, MO, USA). The aqueous sol of titania was prepared by adding 12.5% NH4OH dropwise to 2.5 M TiCl4 + 0.65 M HCl aqueous solution (Sigma-Aldrich, St. Louis, MO, USA) cooled to 0 °C under vigorous stirring until pH 5 was reached. The obtained precipitate after thorough washing with distilled water was dispersed by ultrasonic treatment. The size of the obtained TiO2 particles (anatase) was of ca. 4 nm. The aqueous suspensions of MoO3 and V2O5 were synthesized via the thermally-induced polycondensation of corresponding oxo-compounds in aqueous medium. The oxo-acids used as precursors were prepared by acidification of aqueous solutions of sodium molybdate and sodium vanadate on a resin. The two-step synthetic route yielding oxide particles of submicron size [21] was used. At the first step, 0.5 M solutions of molybdic, vanadic, and tungstic acids were heated at 100 °C for 4 min; the resultant solution was diluted 1:5 to stop further nucleation as well as to provide dispersion of grown oxide particles and then incubated for 4 h at 100 °C (the solution volume was maintained constant).
The X-ray diffraction analysis of the samples was performed with the use of a PANalytical Empyrean difractometer with Cu Kα radiation. The morphological investigations emploed SEM (LEO 1420, KARL ZEISS, Germany) and AFM microscope (NT-206, MICROTESTMACHINES, Gomel, Belaru).
As the UV light source in the photocatalytic measurements, the high-pressure mercury lamp Philips HPK 125 W was used. The intensity of the incident light was of ca. 10 mW/cm2.
The photoinduced oxidation activity of TiO2/MoO3 and TiO2/V2O5 systems was evaluated using the reaction of degradation of probing dye (Rhodamine 6G) deposited onto the photocatalyst surface which was preliminary exposed to UV light for 10 min. Rhodamine 6G was applied onto the photocatalyst surface at different times after exposure in an amount of ca. 2 × 10−8 mol/cm2, and a diffuse reflectance, R, at 530 nm that corresponded to the absorption of the dye in the adsorbed state was measured. The value proportional to the surface dye concentration (Γ) was calculated from the reflectance data using the Kubelka–Munk function [33]:
Γ ~ (1 − R)2/2R.
The photocurrent onset potentials for the TiO2, MoO3, WO3, and V2O5 thin films deposited onto ITO were obtained from photocurrent versus potential dependencies measured in 0.25 Na2SO4 + 0.1 CH3COONa electrolyte using the Autolab PGStat 204 potentiostat (Metrohm Autolab, Utrecht, The Netherlands). All potentials are given against saturated Ag/AgCl reference electrode.
The photoinduced pathphysiological activity of photoaccumulating catalyst was investigated using Escherichia coli ATCC 8739 bacteria. For this purpose, the samples of thin-film photocatalysts at glass substrates (4 × 4 cm) pasted with the agar at the bottom of Petri dish were exposed to UV light for 10 min and left in the dark for different times to evaluate the deactivation kinetics. Then, 5 mL of suspension of microorganisms in 0.5% LB agar medium was poured into the dish. Plates were then incubated for 48 h at 37 °C, and the number of arising colonies, N, was calculated. In the control experiments, the photocatalyst-free glass substrates were used. To evaluate the biocide activity of the pre-illuminated photocataylys, the survived ratio, S = (N/N0)∙100%, was used (N0 is the number of colony-forming units in the case of the nonexposed photocatalyst used as the control sample). The respective data were the average values obtained from the triplicate runs. The standard deviations of these replicate experiments were within 14%.
The EPR spectra were recorded with a EPR spectrometer (ELEXSYS-E500, X-band, the sensitivity up to 1010 spin/G, Bruker, Karlsruhe, Germany). For investigation of photogenerated paramagnetic centers (PCs), the samples were illuminated directly in the cavity of the spectrometer with the use of a 50 W high pressure mercury lamp. The concentration of PCs was evaluated using CuCl2·2H2O monocrystal with the known number of spins as the standard. The EPR spectra simulation permitting the determination of g-factor values of paramagnetic centers was carried out with the use of EasySpin MATLAB toolbox (Comprehensive Software Package for Spectral Simulation and Analysis in EPR, Stoll, S.; Schweiger, A., Physical Chemistry Laboratory, ETH Hönggerberg, Zürich, Switzerland, 2006) [34].

4. Conclusions

The obtained results provide evidence that the structure of energy levels involved in the separation of photoproduced charges in the case of TiO2/MoO3 photocatalyst creates favorable conditions for filling the energy states of TiO2 (the latter process is not observed for bare TiO2). As a result, the accumulation of photoinduced charges occurs in two forms: (i) filled electron traps corresponding to Ti4+/Ti3+ levels and (ii) Mo5+ centers produced as the result of electron trapping by MoO3, both forms contributing to the photoinduced biocide activity of the heterostructure photocatalyst. This effect of ”indirect” filling of Ti4+/Ti3+ surface states resulted from the cascade effect is not observed for TiO2/WO3 and TiO2/V2O5 heterostructures due to deeper lying W+6/W+5 and V5+/V4+ levels involved in the electron trapping. In the case of TiO2/WO3 and TiO2/V2O5 photocatalysts, the electron trapping is irreversible and occurs at the bulk W+6/W+5 and V5+/V4+ states. This permits the conclusion that the exposure of energy storage heterostructure photocatalysts with mosaic surfaces (i.e., comprising photogenerating and redox-active components) to actinic light can result in the generation of different types of charge-trapping centers capable of interacting with molecular oxygen yielding peroxo species; these centers differ as to their long-term stability and contribution to the induced pathophysiological behavior.

Author Contributions

Conceptualization, A.I.K. and D.W.B.; methodology, T.V.S.; validation, E.A.K., T.V.S., and A.I.K.; formal analysis, D.V.S.; investigation, T.V.S., E.A.K.; data curation, D.V.S.; writing—original draft preparation, A.I.K.; writing—review and editing, D.W.B., A.I.K.; visualization, D.V.S., E.A.K.; supervision, D.W.B. All authors have read and agreed to the published version of the manuscript.

Funding

A.I.K. and E.A.K. are thankful to the Russian Foundation of Basic Research for financial support (Grant No. 18-53-00020-Bel-a). T.V.S and D.V.S. acknowledge the support from the Belarusian Republican Foundation for Fundamental Research (Grant Kh19MS-017).

Acknowledgments

The EPR measurements were performed using the facilities of the Collective Use Center at the Moscow State University.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Ge, M.; Li, Q.; Cao, C.; Huang, J.; Li, S.; Zhang, S.; Chen, Z.; Zhang, K.; Al-Deyab, S.S.; Lai, Y.; et al. One-dimensional TiO2 nanotube photocatalysts for solar water splitting. Adv. Sci. 2017, 4, 1–31. [Google Scholar]
  2. Hoffmann, M.R.; Martin, S.T.; Choi, W.; Bahnemann, D.W. Environmental applications of semiconductor photocatalysis. Chem. Rev. 1995, 95, 69–96. [Google Scholar] [CrossRef]
  3. Hagfeldt, A.; Graetzel, M. Light-Induced redox reactions in nanocrystalline systems. Chem. Rev. 1995, 95, 49–68. [Google Scholar] [CrossRef]
  4. Ibhadon, A.O.; Fitzpatrick, P. Heterogeneous photocatalysis: Recent advances and applications. Catalysts 2013, 3, 189–218. [Google Scholar] [CrossRef] [Green Version]
  5. Bahnemann, D. Photocatalytic water treatment: Solar energy applications. Solar Energy 2004, 77, 445–459. [Google Scholar] [CrossRef]
  6. Chen, X.; Mao, S. Titanium dioxide nanomaterials: Synthesis, properties, modifications, and applications. Chem. Rev. 2007, 107, 2891–2959. [Google Scholar] [CrossRef]
  7. Zhang, H.; Chen, G.; Bahnemann, D. Photoelectrocatalytic materials for environmental applications. J. Mat. Chem. 2009, 19, 5089–5121. [Google Scholar] [CrossRef]
  8. Chen, W.F.; Koshy, P.; Huang, Y.; Adabifiroozjaei, E.; Yao, Y.; Sorrell, C.C. Effects of Precipitation, Liquid. Formation, and Intervalence Charge Transfer on the Properties and Photocatalytic Performance of Cobalt-. or Vanadium-Doped TiO2 Thin Films. Int. J. Hydrog. Energy 2016, 41, 19025–19056. [Google Scholar] [CrossRef]
  9. Schneider, J.; Matsuoka, M.; Takeuchi, M.; Zhang, J.; Horiuchi, Y.; Anpo, M.; Bahnemann, D.W. Understanding TiO2 photocatalysis: Mechanisms and materials. Chem. Rev. 2014, 114, 9919–9986. [Google Scholar] [CrossRef]
  10. Tatsuma, T.; Takeda, S.; Saitoh, S.; Ohko, Y.; Fujishima, A. Bactericidal effect of an energy storage TiO2–WO3 photocatalyst in dark. Electrochem. Comm. 2003, 5, 793–796. [Google Scholar] [CrossRef]
  11. Takahashi, Y.; Ngaotrakanwiwat, P.; Tatsuma, T. Energy storage TiO2-MoO3 photocatalysts. Electrochim. Acta 2004, 49, 2025–2029. [Google Scholar] [CrossRef]
  12. Yang, F.; Takahashi, Y.; Sakai, N.; Tatsuma, T. Visible light driven photocatalysts with oxidative energy storage abilities. J. Mat. Chem. 2011, 21, 2288–2293. [Google Scholar] [CrossRef]
  13. Ngaotrakanwiwat, P.; Saitoh, S.; Ohko, Y.; Tatsuma, T.; Fujishima, A. TiO2-phosphotungstic acid photocatalysis systems with an energy storage ability. J. Electrochem. Soc. 2003, 150, A1405–A1407. [Google Scholar] [CrossRef]
  14. Sviridova, T.V.; Sadovskaya, L.Y.; Shchukina, E.M.; Logvinovich, A.S.; Shchukin, D.G.; Sviridov, D.V. Nanoengineered Thin-Film TiO2/h-MoO3 Photocatalysts Capable to Accumulate Photoinduced Charge. J. Photochem. Photobiol. A 2016, 327, 44–50. [Google Scholar] [CrossRef] [Green Version]
  15. Sviridova, T.V.; Antonova, A.A.; Kokorin, A.I.; Degtyarev, E.N.; Sviridov, D.V. Thermally Induced Transformations in Nanostructured Molybdenum-Vanadium Oxides Synthesized by a Solvothermal Method. Russ. J. Phys. Chem. B 2015, 9, 36–42. [Google Scholar] [CrossRef]
  16. Konstantinova, E.A.; Kokorin, A.I.; Minnekhanov, A.A.; Sviridova, T.V.; Sviridov, D.V. EPR Study of Photoexcited Charge Carrier Behavior in TiO2/MoO3 and TiO2/MoO3:V2O5 Photocatalysts. Catal. Lett. 2019, 149, 2256–2267. [Google Scholar] [CrossRef]
  17. Sviridova, T.V.; Sadovskaya, L.Y.; Konstantinova, E.A.; Belyasova, N.A.; Kokorin, A.I.; Sviridov, D.V. Photoaccumulating TiO2–MoO3, TiO2–V2O5, and TiO2–WO3 Heterostructures for Self-Sterilizing Systems with the Prolonged Bactericidal Activity. Catal. Lett. 2019, 149, 1147–1153. [Google Scholar] [CrossRef]
  18. Kokorin, A.I.; Sviridova, T.V.; Kolbanev, I.V.; Sadovskaya, L.Y.; Degtyarev, E.N.; Vorobyeva, G.A.; Streletskii, A.N.; Sviridov, D.V. Structure and Photocatalytic Properties of TiO2/MoO3 and TiO2/V2O5 Nanocomposites Obtained by Mechanochemical Activation. Russ. J. Phys. Chem. B 2018, 12, 330–335. [Google Scholar] [CrossRef]
  19. Choi, W.; Termin, A.; Hoffmann, M.R. The Role of Metal Ion Dopants in Quantum-Sized TiO2: Correlation between Photoreactivity and Charge Carrier Recombination Dynamics. J. Phys. Chem. 1994, 98, 13669–13679. [Google Scholar] [CrossRef]
  20. Polliotto, V.; Livraghi, S.; Giamello, E. Electron magnetic resonance as a tool to monitor charge separation and reactivity in photocatalytic materials. Res. Chem. Intermed. 2018, 44, 3905–3921. [Google Scholar] [CrossRef]
  21. Sviridova, T.V.; Stepanova, L.I.; Sviridov, D.V. Molybdenum: Characteristics, Production and Applications in Nano- and Microcrystals of Molybdenum Trioxide and Metal-Matrix Composites on Their Basis; Ortiz, M., Herrera, T., Eds.; Nova Science Publishers: New York, NY, USA, 2012; p. 147. [Google Scholar]
  22. Sviridova, T.V.; Stepanova, L.I.; Sviridov, D.V. Electrochemical synthesis of Ni-MoO3 composite films: Redox-mediated mechanism of electrochemical growth of metal-matrix composite. J. Sol. St. Electrochem. 2012, 16, 3799–3803. [Google Scholar] [CrossRef]
  23. Ishibashi, K.; Fujishima, A.; Watanabe, T.; Hashimoto, K. Quantum yields of active oxidative species formed on TiO2 photocatalyst. J. Photochem. Photobiol. A 2000, 134, 139–142. [Google Scholar] [CrossRef]
  24. Ishibashi, K.; Fujishima, A.; Watanabe, T.; Hashimoto, K. Generation and deactivation processes of superoxide formed on TiO2 film illuminated byvery weak UV light in air or water. J. Phys. Chem. B 2000, 104, 4934–4938. [Google Scholar] [CrossRef]
  25. Konstantinova, E.A.; Minnekhanov, A.A.; Kokorin, A.I.; Sviridova, T.V.; Sviridov, D.V. Determination of the Energy Levels of Paramagnetic Centers in the Band Gap of Nanostructured Oxide Semiconductors Using EPR Spectroscopy. J. Phys. Chem. C 2018, 122, 10248–10254. [Google Scholar] [CrossRef]
  26. Konstantinova, E.A.; Kokorin, A.I.; Lips, K.; Sakthivel, S.; Kisch, H. EPR study of illumination effect on properties of paramagnetic centers in nitrogen–doped TiO2, active in visible light photocatalysis. Appl. Magn. Reson. 2009, 35, 421–427. [Google Scholar] [CrossRef]
  27. Sviridova, T.V.; Sadovskaya, L.Y.; Kokorin, A.I.; Konstantinova, E.A.; Agabekov, V.E.; Sviridov, D.V. Photoaccumulating Film Systems Based on TiO2/MoO3 and TiO2/MoO3:V2O5 Nanoheterostructures. Russ. J. Phys. Chem. B 2017, 11, 348–353. [Google Scholar] [CrossRef]
  28. Kokorin, A.I. Electron Spin Resonance of Nanostructured Oxide Semiconductors in Chemical Physics of Nanostructured Semiconductors; Kokorin, A.I., Bahnemann, D.W., Eds.; VSP-Brill Academic Publishers: Utrecht, The Netherlands; Boston, MA, USA, 2003; p. 203. [Google Scholar]
  29. Occhiuzzi, M.; Cordischi, D.; Gazzoli, D.; Valigi, M.; Heydorn, P.C. WOx/ZrO2 catalysts: Part 4. Redox properties as investigated by redox cycles, XPS and EPR. Appl. Catal. A 2004, 269, 169–177. [Google Scholar] [CrossRef]
  30. Folli, A.; Blohb, J.Z.; Macphee, D.E. Band structure and charge carrier dynamics in (W,N)-codoped TiO2 resolved by electrochemical impedance spectroscopy combined with UV–vis and EPR spectroscopies. J. Electroanalyt. Chem. 2016, 780, 367–372. [Google Scholar] [CrossRef] [Green Version]
  31. Gazzinelli, R.; Schirmer, O.F. Light induced W5+ ESR in WO3. J. Phys. C Sol. St. Phys. 1977, 10, L145–L149. [Google Scholar] [CrossRef]
  32. Hashimoto, S.; Matsuoka, H. Mechanism of electrochromism for amorphous WO3 thin films. J. Appl. Phys. 1991, 69, 933–937. [Google Scholar] [CrossRef]
  33. Wedland, W.; Hecht, H. Reflectance Spectroscopy; Interscience Publishers: New York, NY, USA, 1966. [Google Scholar]
  34. Stoll, S.; Schweiger, A. EasySpin, a Comprehensive Software Package for Spectral Simulation and Analysis in EPR. J. Magn. Reson. 2006, 178, 42–55. [Google Scholar] [CrossRef]
Figure 1. SEM images of submicron-sized crystallites of (a) h-MoO3, (b) h-WO3, and (c) V2O5 xerogel used for preparation of heterostructure photocatalysts.
Figure 1. SEM images of submicron-sized crystallites of (a) h-MoO3, (b) h-WO3, and (c) V2O5 xerogel used for preparation of heterostructure photocatalysts.
Catalysts 10 01022 g001
Figure 2. AFM surface plots for (a) TiO2-MoO3, (b) TiO2-WO3, and (c) TiO2-V2O5.
Figure 2. AFM surface plots for (a) TiO2-MoO3, (b) TiO2-WO3, and (c) TiO2-V2O5.
Catalysts 10 01022 g002
Figure 3. XRD patterns of (a) h-MoO3, (b) h-WO3, and (c) monoclinic V2O5 xerogel crystallites used for preparation of heterostructure photocatalysts. Hexagonal MoO3 and WO3 (marked at the pattern with asterisks) contain an admixture of monoclinic MoO3·H2O and orthorhombic WO3·0.33 H2O (marked with squares). θ is the diffraction angle.
Figure 3. XRD patterns of (a) h-MoO3, (b) h-WO3, and (c) monoclinic V2O5 xerogel crystallites used for preparation of heterostructure photocatalysts. Hexagonal MoO3 and WO3 (marked at the pattern with asterisks) contain an admixture of monoclinic MoO3·H2O and orthorhombic WO3·0.33 H2O (marked with squares). θ is the diffraction angle.
Catalysts 10 01022 g003
Figure 4. XRD pattern and TEM image of TiO2 nanophase used for preparation of heterostructure photocatalysts.
Figure 4. XRD pattern and TEM image of TiO2 nanophase used for preparation of heterostructure photocatalysts.
Catalysts 10 01022 g004
Figure 5. (a) Degradation kinetics of Rhodamine 6G at the glass substrate (○), TiO2 (●), TiO2/MoO3 (Δ), TiO2/WO3 (▲), and TiO2/V2O5 (∇) photocatalysts under dark conditions after the samples were exposed to UV light for 10 min at 298 K. Γ/Γ0 is a ratio between measured (Γ) and initial (Γ0) concentration of Rhodamine 6G. (b) The time dependence of the survival ratio for Escherichia coli bacteria at the surface of TiO2 (●), TiO2/MoO3 (Δ), TiO2/WO3 (▲), andTiO2/V2O5 (∇) samples exposed to UV light for 10 min and then put in the dark for different times.
Figure 5. (a) Degradation kinetics of Rhodamine 6G at the glass substrate (○), TiO2 (●), TiO2/MoO3 (Δ), TiO2/WO3 (▲), and TiO2/V2O5 (∇) photocatalysts under dark conditions after the samples were exposed to UV light for 10 min at 298 K. Γ/Γ0 is a ratio between measured (Γ) and initial (Γ0) concentration of Rhodamine 6G. (b) The time dependence of the survival ratio for Escherichia coli bacteria at the surface of TiO2 (●), TiO2/MoO3 (Δ), TiO2/WO3 (▲), andTiO2/V2O5 (∇) samples exposed to UV light for 10 min and then put in the dark for different times.
Catalysts 10 01022 g005
Figure 6. EPR spectra at 30 K of TiO2/MoO3 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Figure 6. EPR spectra at 30 K of TiO2/MoO3 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Catalysts 10 01022 g006
Figure 7. Dependences of EPR signal intensity as a function of UV illumination time for Ti3+surf (▲), N radical (star), Mo5+ (○), and V4+ (●) PCs.
Figure 7. Dependences of EPR signal intensity as a function of UV illumination time for Ti3+surf (▲), N radical (star), Mo5+ (○), and V4+ (●) PCs.
Catalysts 10 01022 g007
Figure 8. Dependences of EPR signal intensity as a function of time after switching off UV light for Ti3+surf (▲), N radical (star), Mo5+ (○), and V4+ (●) PCs.
Figure 8. Dependences of EPR signal intensity as a function of time after switching off UV light for Ti3+surf (▲), N radical (star), Mo5+ (○), and V4+ (●) PCs.
Catalysts 10 01022 g008
Figure 9. EPR spectra of TiO2/WO3 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Figure 9. EPR spectra of TiO2/WO3 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Catalysts 10 01022 g009
Figure 10. EPR spectra of TiO2/V2O5 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Figure 10. EPR spectra of TiO2/V2O5 photocatalyst before (a) and after 10 min (b) of UV light illumination.
Catalysts 10 01022 g010
Figure 11. Schematic energy diagram of TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 photocatalysts.
Figure 11. Schematic energy diagram of TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 photocatalysts.
Catalysts 10 01022 g011
Table 1. Spin-Hamiltonian parameters calculated from EPR spectra for paramagnetic centers (PCs).
Table 1. Spin-Hamiltonian parameters calculated from EPR spectra for paramagnetic centers (PCs).
Centergg||C, Spin/g
Ti3+lat1.9711.9672 × 1015
Ti3+surf1.9391.929(4–5) × 1017
Mo5+(1)1.918, 1.891 a1.819(7–9) × 1017
Mo5+(2)1.804 b--
W5+1.74, 1.6251.568<1015
V4+
A, mT
1.980
7.7
1.931
20.3
>(2–3) × 1019
N
<A>, mT
2.007, 2.0057 a
0.13, 0.36 c
gzz = 2.0043
Azz = 3.29
1.7 × 1016
O22.022, 2.011 dg3 = 1.999-
a,b singlet; c Axx, Ayy; d g1, g2.
Table 2. Energy position of levels involved in the charge storage in TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 photocatalysts (energy is measured against the valence band of semiconductor).
Table 2. Energy position of levels involved in the charge storage in TiO2/MoO3, TiO2/WO3, and TiO2/V2O5 photocatalysts (energy is measured against the valence band of semiconductor).
Charge Accepting StatesEnergy, eV
Ti4+/Ti3+ *2.9 *
Mo6+/Mo5+2.7 *
W6+/W5+2.4 **
V5+/V4+2.2 *
* The value was obtained from the EPR measurements [16]; ** the value was obtained from the X-ray photoelectron spectra [32].
Table 3. The band gap energies (Eg) and the photocurrent onset potentials (Eon) for oxides used for preparation of heterostructured photocatalysts.
Table 3. The band gap energies (Eg) and the photocurrent onset potentials (Eon) for oxides used for preparation of heterostructured photocatalysts.
OxideEg *, eVEon, V
TiO23.50–0.4
MoO33.01–0.2
WO32.75–0.1
V2O52.450.0
* Eg values were obtained from the optical absorption spectra.

Share and Cite

MDPI and ACS Style

Kokorin, A.I.; Sviridova, T.V.; Konstantinova, E.A.; Sviridov, D.V.; Bahnemann, D.W. Dynamics of Photogenerated Charge Carriers in TiO2/MoO3, TiO2/WO3 and TiO2/V2O5 Photocatalysts with Mosaic Structure. Catalysts 2020, 10, 1022. https://doi.org/10.3390/catal10091022

AMA Style

Kokorin AI, Sviridova TV, Konstantinova EA, Sviridov DV, Bahnemann DW. Dynamics of Photogenerated Charge Carriers in TiO2/MoO3, TiO2/WO3 and TiO2/V2O5 Photocatalysts with Mosaic Structure. Catalysts. 2020; 10(9):1022. https://doi.org/10.3390/catal10091022

Chicago/Turabian Style

Kokorin, Alexander I., Tatyana V. Sviridova, Elizaveta A. Konstantinova, Dmitry V. Sviridov, and Detlef W. Bahnemann. 2020. "Dynamics of Photogenerated Charge Carriers in TiO2/MoO3, TiO2/WO3 and TiO2/V2O5 Photocatalysts with Mosaic Structure" Catalysts 10, no. 9: 1022. https://doi.org/10.3390/catal10091022

APA Style

Kokorin, A. I., Sviridova, T. V., Konstantinova, E. A., Sviridov, D. V., & Bahnemann, D. W. (2020). Dynamics of Photogenerated Charge Carriers in TiO2/MoO3, TiO2/WO3 and TiO2/V2O5 Photocatalysts with Mosaic Structure. Catalysts, 10(9), 1022. https://doi.org/10.3390/catal10091022

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop