Next Article in Journal
Quantum Phenomena Emerging Near a Ferroelectric Critical Point in a Donor–Acceptor Organic Charge-Transfer Complex
Next Article in Special Issue
Li2HgMS4 (M = Si, Ge, Sn): New Quaternary Diamond-Like Semiconductors for Infrared Laser Frequency Conversion
Previous Article in Journal
Structure and Optical Properties of K0.67Rb1.33Al2B2O7 Crystal
Previous Article in Special Issue
Site Identity and Importance in Cosubstituted Bixbyite In2O3
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Epoxy-Based Composites Embedded with High Performance BZT-0.5BCT Piezoelectric Nanoparticles Powders for Damping Vibration Absorber Application

1
School of Materials Science and Engineering, Southeast University, Nanjing 211189, China
2
National Institute for Materials Science, Tsukuba 305-0047, Japan
*
Authors to whom correspondence should be addressed.
Crystals 2017, 7(4), 105; https://doi.org/10.3390/cryst7040105
Submission received: 24 February 2017 / Revised: 6 April 2017 / Accepted: 6 April 2017 / Published: 9 April 2017
(This article belongs to the Special Issue Crystal Structure of Electroceramics)

Abstract

:
Lead-free, high piezoelectric performance, Ba(Zr0.2Ti0.8)O3-0.5(Ba0.7Ca0.3)TiO3 (BZT-0.5BCT) sub-micron powders with perovskite structure were fabricated using the sol-gel process. A 0–3 type composite was obtained by choosing epoxy resin as matrix and BZT-0.5BCT, acetylene black as functional phases. Particular attention was paid to the damping behavior of composite with different content of BZT-0.5BCT powders, the influence of frequency and loading force on the damping properties were also analyzed. A mathematical model was developed to characterize the damping properties of the composites. It found that the piezoelectric effects and interfacial friction play a key role in damping behavior of composites, and a large dissipated loss factor of tanδ was found at the BZT-0.5BCT content of 20 vol %.

1. Introduction

Unwanted vibrations may result in the fatigue and failure of structures from concrete steel buildings to precision instruments; therefore, vibration reduction and noise control is a serious engineering challenge. Much effort has been expended in attempting to minimize mechanical vibrations [1,2,3,4]. One of the approaches is to use damping materials to limit the vibration [5,6]. Viscoelastic material damping is recognized to make a contribution to energy loss due to hysteresis caused by internal sliding of the molecule chain. Thus, it is expected that the polymer possesses a broad, high damping peak applied to damping applications [7]. However, this is difficult or impossible for a single polymer because the height and width of the loss peak cannot be independently adjusted. Composites with piezoelectric materials contained showed excellent damping properties with wide temperature range and have attracted ever-greater attention [8,9].
Piezoelectric materials such as lead zirconate titanate (PZT), lead magnesio niobate (PMN), barium titanate (BT), zinc oxide (ZnO), poly(vinylidene fluoride) (PVDF), etc., have been intensively investigated for great ability of converting mechanical energy into electricity [10,11,12,13,14]. The electric energy can be dissipated through an external resistance in piezo-damping composites [15]. Hori et al. exploited a damper material which is composed of PZT powders, conductive carbon (CB) powders and epoxy (EP) resin, and studied their damping properties and the effects of CB content on the loss factor [16]. Tang et al. prepared a series of BaTiO3 filled polyurethane (PU)/unsaturated polyester resin (UP) interpenetrating polymer networks (IPNs) and explored the relationship between dielectric properties and damping properties of the mixtures [17]. Malakooti et al. fabricated vertically aligned ZnO nanowires on nanofillers and produced hybrid carbon fiber composites. The results showed that the morphology-controlled interphase between reinforcement and matrix not only exhibited remarkable damping enhancement but also stiffness improvement [18]. Recently, a lead-free Ba(Zr0.2Ti0.8)O3-x(Ba0.7Ca0.3)TiO3 (BZT-xBCT) piezoelectric system with optimal composition of x = 0.5 was reported to show outstanding room temperature piezoelectricity with the piezoelectric coefficient d33 = 560–620 pC/N which is comparable to PZT [19]. Zhou, et al. developed a scalable method to synthesize perovskite type 0.5Ba(Zr0.2Ti0.8)O3–0.5(Ba0.7Ca0.3)TiO3 (BZT–BCT) NWs with high piezoelectric coupling coefficient (90 pm/V) and the energy harvesting performance of the BZT–BCT NWs were demonstrated by fabricating a flexible nanocomposite exhibiting a high power density (2.25 µW/cm)[20]. Wu et al. synthesized a new kind of lead-free 0.5Ba(Zr0.2Ti0.8)O3–0.5(Ba0.7Ca0.3)TiO3 (BZT–BCT) NWs with high piezoelectric coefficients through the electrospinning method and subsequent calcining process which could harvest weak mechanical movement energy and generated an output voltage of 3.25 V and output current of 55 nA [21]. Therefore, there is much promise in such a high-performance lead-free piezoelectric material used in polymer-based damping materials through forming the composites containing piezoelectric phase and polymer matrix.
In this paper, we added BZT-0.5BCT powders and acetylene black powders into epoxy resin, and fabricated a series of piezo-damping composites through solution blending. In line with the corresponding ceramic counterpart, BZT-0.5BCT shows the highest value of Pr (22.15 mC/cm2) and fairly low Ec (68.06 kV/cm) [22]. The effects of different contents of BZT-0.5BCT, frequency and loading force on damping properties were investigated. A mathematical model was established to understand the piezoelectric damping mechanism in the composites.

2. Results and Discussions

Figure 1 shows the XRD patterns of the three BZT-0.5BCT/acetylene black/epoxy composites. It can be observed that without addition of piezoelectric phase, Epoxy E51 shown amorphous phase, with addition of 20 vol %, 40 vol % and 60 vol % piezoelectric material. All samples show the polycrystalline perovskite phase.
The particle distribution of the BZT-0.5BCT powder incorporated in the 0–3 epoxy-based piezoelectric composites was measured with sub-micron particle size analysis. According to the cumulative curve given in Figure 2a, the average grain size was around 500 nm. Figure 2b–d present the typical SEM image of the cross-section of the composite with 20 vol %, 40 vol % and 60 vol % powders contained, respectively. It can be clearly observed that with the increase of piezoelectric phase, most oval BZT-0.5BCT particles and conductive acetylene black were uniformly dispersed in the matrix of Epoxy resin. A small amount of reunion, the grain size of piezoelectric phase was consistent with that in Figure 2a. However, when the volume fraction reached up to 60%, the nanoparticles tended to agglomerate due to too high content of the piezoelectric phase.
DMA tests generally characterize the damping properties of materials such as the storage modulus (E′) as measurement of dynamic stiffness, loss modulus (E″) as a measurement for energy dissipation and the tangent of phase angle between the stress and strain vectors linking these two moduli (tan δ). Damping loss factor reflects an ability of converting the mechanical energy into heat energy when the material is subjected to external cyclic loading. Figure 3 shows the effect of different BZT-0.5BCT content on the loss factor of the composites when the preload fixed at 0.5 N and frequency 10 Hz. In the vicinity of the glass transition temperature (Tg) of the composites, the peaks shifted with variation of composing component.
Detailed damping properties are shown in Table 1. It indicated when different volume fraction BZT-0.5BCT (20%, 40% and 60%) was added to epoxy resin, the maximum loss factor and the effective temperature region initially increase and then decrease as the increase of the piezoelectric phase within our limited test range. The damping property of the composites resulted from comprehensive function of interfacial friction dissipation, retarded motion of polymer macromolecular and the piezoelectric effect. Because of the piezoelectric effect of BZT-0.5BCT powder, mechanical energy changes into electrical energy when the composites were subjected to external vibration. During the glass transition region, the composite chain movement happened under the impact load, and the piezoelectric effect of the piezoelectric phase consumed a strong response to the load which resulted in the maximum hysteresis damping and maximum lost energy. When BZT-0.5BCT powders content ranges from 20 to 40 vol %, the interaction between the piezoelectric phase and epoxy matrix became stronger and limitation for piezoelectric powder to the polymeric segmental relaxation would enhanced. Meanwhile, Tg grew from 71.8 °C to 87.5 °C as a result and widened the effective temperature range. However, when the volume fraction of the nanoparticles is 60%, a large number of two-phase interfaces formed and the epoxy resin molecules in the vicinity of the interface layer was blocked from moving, which led to the piezoelectric effect not being able to be fully utilized and a reduction of the dissipated energy. Only when the volume fraction of BZT-0.5BCT was 0.2 can the combined effects contribute to the most powerful enhancement of damping properties. The maximum loss factor was 0.846 when the effective temperature range was maximum.
Figure 4 and Table 2 show the damping properties of composite with 40 vol % BZT-0.5BCT powders under multi-frequency (1, 2, 4, 10 and 20 Hz). The maximum loss factor, glass transition temperature and the effective temperature range were all improved when the frequency gets higher and there was a trend of stability. The higher frequency speeded up the molecular chain movement and enhanced the piezoelectric activity of the BZT-0.5BCT powders, thus causing the improvement in the damping properties and the right shift of the peaks in the tan δ curves.
Figure 5 and Table 3 show the effects of loading force of composite with 20 vol % addition of BZT-0.5BCT powders with the loading force ranging from 0.5 N to 4 N. The maximum damping factor increased when the loading force was raised. Meanwhile, Tg increased at first then remained more or less the same. The effective temperature range of the composite showed almost no change, and reached a peak at the loading force of 4 N.
The composites behavior shown with different loading force is not like that of a conventional viscoelastic body [23]. When samples were with the preload force, the bond length and bond-angle of epoxy polymer’s molecular chain would change as a tensioning process, which would cause an obstacle to the deformation of the composites. The deformable parts in the matrix become smaller while the preload force increases. On the other hand, when the preload force raises, the piezoelectric effect and the interface friction would enhance, causing an increase in the maximum loss factor. Tg and effective temperature region mostly depended on the chain segment movement of epoxy so the peaks in tanδ curves shift slightly to the right side. We can speculate that the piezoelectric effect and interfacial friction mainly contribute to composites’ damping properties when the piezoelectric ceramic volume fraction exceeds 0.2. The damping capacity was enhanced by piezo-damping as the piezoelectric effect enlarged in the piezoelectric ceramic when the loading force increased. However, the changing range was lower.
To understand the damping mechanism in the piezoelectric/polymer composites, we can analyze the components and electric circuit in the piezoelectric composite. The damping function of the piezoelectric composite mainly originates from three parts: the viscoelastic damping of the epoxy resin, the interface friction damping between the matrix and the fillers, and piezoelectric damping of BZT-0.5BCT powders. As for the piezoelectric damping, the ceramic powders first generate electric energy upon deformation and then dissipate them as thermal energy through the conductive matrix. For the piezoelectric/polymer composites, we can assume that each piezoelectric particle was in contact with the matrix as shown in Figure 6, and could be equivalent to a RLC circuit in a parallel connection. Figure 7 shows a mathematical model of the BZT-0.5BCT/acetylene black/epoxy composite with 0–3 connectivity that is the equivalent circuit between them. Then an adjustable resistance was used to simulate the conductivity of the polymer matrix and we supposed there were n piezoelectric particles.
When a force is applied to the composite, in a single circuit unit an alternating voltage Vn produced by piezoelectric powder is generated and the electric energy is dissipated by the resistance R. The impedance (Z) in the circuit cell is
Z n = R + 1 j ω L n + 1 j ω C n + R n
the consumption energy (Wn) by R is expressed as
W n = V n 2 · R [ R + R n R n 2 + ( ω L 1 ω C ) 2 ] 2 + [ ω L 1 ω C R n 2 + ( ω L 1 ω C ) 2 ] 2
When it works at a resonance frequency,
L = 1 ω C
Wn takes a maximum value in Equation (2), that is
W n = V n 2 · R ( R + 1 R n ) 2
For the piezoelectric effect of piezoelectric materials, the mechanical energy transferred into electrical energy. Then it conversed into heat consumption through the conductive pathways and the load in composite materials. This indicated that the piezoelectric damping of composite was in closer association with the content of BZT-0.5BCT powders, frequency and the force, as the piezoelectric phase content directly affects the value of n and the loading force has an influence on the voltage (Vn).

3. Materials and Methods

BZT-0.5BCT nanopowders were prepared by a sol-gel process. The starting reagents were analytical graded barium acetate [Ba(CH3COO)2], calcium acetate monohydrate [Ca(CH3COO)2·H2O], tetrabutyl titanate [Ti(OC4H9)4], zirconium oxynitrate [ZrO(NO3)·2H2O], complexing agent of glacial acetic acid and solvent of 2-methoxyethanol. After obtaining sol solution, the dry gel was ground and followed post heat-treatment, then piezoelectric sub-micron powders were obtained.
The epoxy resin matrix (E-51) used in this research was provided by Wuxi Xinmeng Co. Ltd. (Wuxi, China) and acetylene black powders were provided by Taiyuan Yingze battery sales department (Taiyuan, China). To improve the surface lipophilic, BZT-0.5BCT powders were firstly treated by silane coupling agents and absolute alcohol. Conductive acetylene black was added into epoxy resin and mixed, then the pretreated piezoelectric powders and curing agents were added and stirred thoroughly under vacuum. The homogeneous viscous mixture was poured into a mold and solidified at 80 °C for 2 h. The BZT-0.5BCT/acetylene black/epoxy composite was obtained when cuing finished. The composite was cut, and poled. The three different composites fabricated contain 2 wt % acetylene black and 20, 40 and 60 vol % piezoelectric powders, respectively. Five 20 mm × 3 mm × 2 mm samples were fabricated for dynamic mechanical analysis.
The phase and morphology observations of composites were examined by X-ray diffractometer (XRD, Bruker D8 Discover) with Cu-Kα (1.5406 Å), tube voltage (40 kV), tube current (100 mA), scanning speed (0.15 degrees/s) and Field emission scanning electron microscope (FESEM, FEI Sirion-200). The damping properties of materials represented by the value of loss factor (tanδ) were carried out using Dynamic Mechanical Analyzer (DMA, TA-Q800). The measurements were made at different frequency and loading force in the temperature range of 0~120 °C at a heating rate of 2 °C/min with multi-frequency-strain mode.

4. Conclusions

In this work, 0–3 BZT-0.5BCT/ acetylene black/epoxy composites with different volume fraction ratio were prepared via sol-gel process and pouring method. The microstructure and morphology of composites were studied and the damping properties of the composite with different volume fraction, frequency and loading force were mainly related. The addition of piezoelectric phase intrinsically broadens its effective temperature region from 27.52 °C to 29.56 °C with only 20 vol % BZT-0.5BCT powders added and spurred the glass transition shift to a high temperature section. The composite damping ratio is a sum of the polymer damping and piezo-damping. The piezo effect and interfacial friction play a major role in damping capacity of the piezoelectric-damping composites when the piezo-ceramic volume fraction exceeds 0.2. The maximum loss factor rose as the content of BZT-0.5BCT powders, frequency and loading force reached a threshold level. The composites show less sensitivity to stress due to the fact that the BZT-0.5BCT powders can retain their piezoelectric properties in comparison to polymer damping materials. Also, an equivalent circuit was established to understand the mechanism of the piezoelectric damping properties.

Acknowledgments

This work is financially sponsored by Natural Science Foundation of China (Grants No. 51002029). Part of this work was supported by the GRENE (Green Network of Excellence) project by Ministry of Education, Culture, Sports, Science and Technology-Japan.

Author Contributions

Zengmei Wang and HuanHuan Wang conceived and designed the experiments; Huanhuan Wang performed the experiments; Wenyan Zhao and Hideo Kimura analyzed the data; Wenyan Zhao revised the paper.

Conflicts of Interest

The founding sponsors had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, and in the decision to publish the results.

References

  1. Amick, H.; Gendreau, M. Construction vibrations and their impact on vibration-sensitive facilities. ASCE Constr. Congr. 2000. [Google Scholar] [CrossRef]
  2. Yu, X.; Fu, Y. Dynamic analysis of damage behavior of vibration compaction on concrete bridges. In Proceedings of the Seventh International Conference on Traffic and Transportation Studies, Kunming, China, 3–5 August 2010. [Google Scholar]
  3. Alavinasab, A.; Padewski, E.; Holley, M.; Jha, R.; Ahmadi, G. Damage Identification Based on Vibration Response of Prestressed Concrete Pipes. In Proceedings of the ASCE Pipelines Conference: Climbing New Peaks to Infrastructure Reliability—Renew, Rehab, and Reinvest, Keystone, CO, USA, 28 August–1 September 2010. [Google Scholar]
  4. Fan, W.; Qiao, P. Vibration-based damage identification methods: A review and comparative study. Struct. Health Monit. 2011, 10, 83–111. [Google Scholar] [CrossRef]
  5. Kwak, G.H.; Inoue, K.; Tominaga, Y.; Asai, S.; Sumita, M. Characterization of the vibrational damping loss factor and viscoelastic properties of ethylene–propylene rubbers reinforced with micro-scale fillers. J. Appl. Polym. Sci. 2001, 82, 3058–3066. [Google Scholar] [CrossRef]
  6. Saravanan, C.; Ganesan, N.; Ramamurti, V. Vibration and damping analysis of multilayered fluid filled cylindrical shells with constrained viscoelastic damping using modal strain energy method. Comput. Struct. 2000, 75, 395–417. [Google Scholar] [CrossRef]
  7. Skandani, A.A.; Masghouni, N.; Case, S.W.; Leo, D.J.; Al-Haik, M. Enhanced vibration damping of carbon fibers-ZnO nanorods hybrid composites. Appl. Phys. Lett. 2012, 101, 73–111. [Google Scholar]
  8. Guo, X.J.; Zhang, J.S.; Xu, D.Y.; Xie, X.C.; Sha, F.; Huang, S.F. Effects of PMN Volume Fraction on the Damping Properties of 1–3 Piezoelectric Damping Composites. Appl. Mech. Mater. 2014, 624, 8–12. [Google Scholar] [CrossRef]
  9. Suhr, J.; Koratkar, N.A.; Ye, D.; Lu, T.M. Damping properties of epoxy films with nanoscale fillers. J. Intell. Mater. Syst. Struct. 2006, 17, 255–260. [Google Scholar] [CrossRef]
  10. Anton, S.R.; Sodano, H.A. A review of power harvesting using piezoelectric materials (2003–2006). Smart Mater. Struct. 2007, 16, R1. [Google Scholar] [CrossRef]
  11. Ren, B.; Or, S.W.; Zhang, Y.; Zhang, Q.; Li, X.; Jiao, J.; Wang, W.; Liu, D.; Zhao, X.; Luo, H. Piezoelectric energy harvesting using shear mode 0.71Pb(Mg1/3Nb2/3)O3–0.29PbTiO3 single crystal cantilever. Appl. Phys. Lett. 2010, 96, 083–502. [Google Scholar] [CrossRef]
  12. Deng, Z.; Dai, Y.; Chen, W.; Pei, X.; Liao, J. Synthesis and characterization of bowl-like single-crystalline BaTiO3 nanoparticles. Nanoscale Res. Lett. 2010, 7, 1217–1221. [Google Scholar] [CrossRef] [PubMed]
  13. Wang, X.D.; Song, J.H.; Liu, J.; Wang, Z.L. Direct-current nanogenerator driven by ultrasonic waves. Science 2007, 5821, 102–105. [Google Scholar] [CrossRef] [PubMed]
  14. Klimiec, E.; Zaraska, W.; Zaraska, K.; Gasiorski, K.P.; Sadowski, T.; Pajda, M. Piezoelectric polymer films as power converters for human powered electronics. Microelectron Reliab. 2008, 48, 897–901. [Google Scholar] [CrossRef]
  15. Marra, S.P.; Ramesh, K.T.; Douglas, A.S. The mechanical properties of lead-titanate/polymer 0–3 composites. Compos. Sci. Technol. 1999, 59, 2163–2173. [Google Scholar] [CrossRef]
  16. Hori, M.; Aoki, T.; Ohira, Y.; Yano, S. New type of mechanical damping composites composed of piezoelectric ceramics, carbon black and epoxy resin. Compos. Part A 2001, 32, 287–290. [Google Scholar] [CrossRef]
  17. Tang, D.; Zhang, J.; Zhou, D.; Zhao, L. Influence of BaTiO3 on damping and dielectric properties of filled polyurethane/unsaturated polyester resin interpenetrating polymer networks. J. Mater. Sci. 2005, 40, 3339–3345. [Google Scholar] [CrossRef]
  18. Malakooti, M.H.; Hwang, H.S.; Sodano, H.A. Morphology-Controlled ZnO Nanowire Arrays for Tailored Hybrid Composites with High Damping. ACS Appl. Mat. Interfaces 2014, 7, 332–339. [Google Scholar] [CrossRef] [PubMed]
  19. Cai, Z.L.; Wang, Z.M.; Wang, H.H.; Cheng, Z.X.; Li, B.W.; Guo, X.L.; Kimura, H.; Kasahara, A. An Investigation of the Nanomechanical Properties of 0.5Ba(Ti0.8Zr0.2)O3–0.5(Ba0.7Ca0.3)TiO3 Thin Films. J. Am. Ceram. Soc. 2015, 98, 114–118. [Google Scholar] [CrossRef]
  20. Zhou, Z.; Bowland, C.C.; Malakooti, M.H.; Tang, H.X.; Sodano, H.A. Lead-free 0.5Ba(Zr0.2Ti0.8)O3– 0.5(Ba0.7Ca0.3)TiO3 nanowires for energy harvesting. RSC Nanoscale 2016, 8, 5098–5105. [Google Scholar] [CrossRef] [PubMed]
  21. Wu, W.W.; Cheng, L.; Bai, S.; Dou, W.; Xu, Q.; Wei, Z.Y.; Qin, Y. Electrospinning lead-free 0.5Ba(Zr0.2Ti0.8)O3–0.5(Ba0.7Ca0.3)TiO3 nanowires and their application in energy harvesting. J. Mater. Chem. A 2013, 1, 7332–7338. [Google Scholar] [CrossRef]
  22. Wang, Z.M.; Zhao, K.; Guo, X.L.; Sun, W.; Jiang, H.L.; Han, X.Q.; Tao, X.T.; Cheng, Z.X.; Zhao, H.Y.; Kimura, H.; et al. Crystallization, phase evolution and ferroelectric properties of sol–gel-synthesized Ba(Ti0.8Zr0.2)O3–x(Ba0.7Ca0.3)TiO3 thin films. J. Mater. Chem. C 2013, 1, 522–530. [Google Scholar] [CrossRef]
  23. Guo, D.; Mao, W.; Qin, Y.; Huang, Z.; Wang, C.; Shen, Q.; Zhang, L. Damping properties of epoxy-based composite embedded with sol-gel derived Pb(Zr0.53Ti0.47)O3 thin film annealed at different temperatures. J. Mater. Sci. Mater. Electron. 2012, 23, 940–944. [Google Scholar] [CrossRef]
Figure 1. X-ray diffractometer (XRD) patterns of composites with different content of piezoelectric phase.
Figure 1. X-ray diffractometer (XRD) patterns of composites with different content of piezoelectric phase.
Crystals 07 00105 g001
Figure 2. Typical particle size distribution histogram of Ba(Zr0.2Ti0.8)O3-0.5(Ba0.7Ca0.3)TiO3 (BZT-0.5BCT) powders (a); Typical SEM image of composite with 20 vol % (b), 40 vol % (c) and 60 vol % (d) BZT-0.5BCT powders contained.
Figure 2. Typical particle size distribution histogram of Ba(Zr0.2Ti0.8)O3-0.5(Ba0.7Ca0.3)TiO3 (BZT-0.5BCT) powders (a); Typical SEM image of composite with 20 vol % (b), 40 vol % (c) and 60 vol % (d) BZT-0.5BCT powders contained.
Crystals 07 00105 g002
Figure 3. Loss factor-temperature curves of composite with different BZT-0.5BCT content.
Figure 3. Loss factor-temperature curves of composite with different BZT-0.5BCT content.
Crystals 07 00105 g003
Figure 4. Loss factor-temperature curves of composites at multi-frequency.
Figure 4. Loss factor-temperature curves of composites at multi-frequency.
Crystals 07 00105 g004
Figure 5. Loss factor-temperature curves of composites with different loading force.
Figure 5. Loss factor-temperature curves of composites with different loading force.
Crystals 07 00105 g005
Figure 6. Schematic representation of composite.
Figure 6. Schematic representation of composite.
Crystals 07 00105 g006
Figure 7. Equivalent circuit of composite.
Figure 7. Equivalent circuit of composite.
Crystals 07 00105 g007
Table 1. Damping Properties of Composites with Different BZT-0.5BCT Powders Content.
Table 1. Damping Properties of Composites with Different BZT-0.5BCT Powders Content.
Volume Fraction (vol %)Maximum Loss Factor (tan δmax)Glass Transition Temperature Tg (°C)Temperature Range (tan δ > 0.3) (°C)
01.13571.862.6~90.1(27.5)
200.84684.971.7~101.3(29.6)
400.85787.574.8~103.9(29.1)
600.82686.775.1~100.7(25.6)
Table 2. Damping Properties of Composite at Different Frequency.
Table 2. Damping Properties of Composite at Different Frequency.
Frequency (Hz)Maximum Loss Factor (tan δmax)Glass Transition Temperature Tg (°C)temperature Range (tan δ > 0.3) (°C)
10.80376.666.3~88.5(22.2)
20.83580.368.8~94.2(25.4)
40.84884.071.9~97.7(25.8)
100.85887.474.8~103.8(29.0)
200.86988.274.1~105.7(31.6)
Table 3. Damping Properties of Composite at Different Loading Force.
Table 3. Damping Properties of Composite at Different Loading Force.
Loading Force (N)Maximum Loss Factor (tan δ)Glass Transition Temperature Tg (°C)Temperature Range (tan δ > 0.3) (°C)
0.50.84784.971.7~101.3 (29.6)
10.86386.472.4~101.6 (29.2)
1.50.87187.374.1~102.9 (28.8)
20.87488.675.1~103.7 (28.6)
2.50.87688.575.0~103.7 (28.7)
30.87988.575.0~103.7 (28.7)
3.50.87585.071.3~100.6 (29.3)
40.88487.374.3~101.9 (27.6)

Share and Cite

MDPI and ACS Style

Wang, Z.; Wang, H.; Zhao, W.; Kimura, H. Epoxy-Based Composites Embedded with High Performance BZT-0.5BCT Piezoelectric Nanoparticles Powders for Damping Vibration Absorber Application. Crystals 2017, 7, 105. https://doi.org/10.3390/cryst7040105

AMA Style

Wang Z, Wang H, Zhao W, Kimura H. Epoxy-Based Composites Embedded with High Performance BZT-0.5BCT Piezoelectric Nanoparticles Powders for Damping Vibration Absorber Application. Crystals. 2017; 7(4):105. https://doi.org/10.3390/cryst7040105

Chicago/Turabian Style

Wang, Zengmei, Huanhuan Wang, Wenyan Zhao, and Hideo Kimura. 2017. "Epoxy-Based Composites Embedded with High Performance BZT-0.5BCT Piezoelectric Nanoparticles Powders for Damping Vibration Absorber Application" Crystals 7, no. 4: 105. https://doi.org/10.3390/cryst7040105

APA Style

Wang, Z., Wang, H., Zhao, W., & Kimura, H. (2017). Epoxy-Based Composites Embedded with High Performance BZT-0.5BCT Piezoelectric Nanoparticles Powders for Damping Vibration Absorber Application. Crystals, 7(4), 105. https://doi.org/10.3390/cryst7040105

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop