Next Article in Journal
Melt Blending Modification of Commercial Polystyrene with Its Half Critical Molecular Weight, High Ion Content Ionomer, Poly(styrene–ran–cinnamic Acid) Zn Salt, toward Heat Resistance Improvement
Next Article in Special Issue
Waterborne Intumescent Coatings Containing Industrial and Bio-Fillers for Fire Protection of Timber Materials
Previous Article in Journal
Improved Properties of Metallocene Polyethylene/Poly(ethylene terephthalate) Blends Processed by an Innovative Eccentric Rotor Extruder
Previous Article in Special Issue
Incorporation of Comonomer exo-5-(Diphenylphosphato)Isosorbide-2-endo-Acrylate to Generate Flame Retardant Poly(Styrene)
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Thermal and Calorimetric Evaluations of Some Chemically Modified Carbohydrate-Based Substrates with Phosphorus-Containing Groups

1
Institute for Sustainable Industries and Liveable Cities, Victoria University, P.O. Box 14428, Melbourne, VIC 8001, Australia
2
Institute for Frontier Materials, Deakin University, Melbourne, VIC 3125, Australia
3
Belfast School of Architecture and the Built Environment, Ulster University, Newtownabbey BT37 0QB, Northern Ireland, UK
*
Author to whom correspondence should be addressed.
Polymers 2020, 12(3), 588; https://doi.org/10.3390/polym12030588
Submission received: 2 December 2019 / Revised: 19 February 2020 / Accepted: 23 February 2020 / Published: 5 March 2020
(This article belongs to the Special Issue Flame Retardancy of Polymeric Materials)

Abstract

:
In the present article, we report on the chemical modifications of some carbohydrate-based substrates, such as potato starch, dextran, β-cyclodextrin, agar agar and tamarind, by reacting with diethylchlorophosphate (DECP), in dispersions in dichloromethane (DCM), in the presence of triethylamine (TEA) as the base. The modified substrates, after recovery and purification, were analyzed for their chemical constitutions, thermal stabilities and calorimetric properties using a variety of analytical techniques. These included: solid-state 31P NMR, inductively coupled plasma-optical emission spectroscopy (ICP-OES), thermogravimetric analysis (TGA) and pyrolysis combustion flow calorimetry (PCFC). The unmodified counterparts were also subjected to the same set of analyses with a view to serving as controls. Phosphorus analyses, primarily through ICP-OES on the recovered samples, showed different degrees of incorporation. Such observations were optionally verified through solid-state 31P NMR spectroscopy. The thermograms of the modified substrates were noticeably different from the unmodified counterparts, both in terms of the general profiles and the amounts of char residues produced. Such observations correlated well with the relevant parameters obtained through PCFC runs. Overall, the modified systems containing phosphorus were found to be less combustible than the parent substrates, and thus can be considered as promising matrices for environmentally benign fire-resistant coatings.

Graphical Abstract

1. Introduction

Much attention has been paid to the development of bio-degradable, carbohydrate-based materials, mainly owing to rising environmental concerns spurred by an overdependence on petro-chemically derived raw materials and polymers [1,2,3]. For example, the well-known carbohydrate starch is a natural polymer possessing a variety of advantageous properties including sustainability and bio-degradability, and its derivatives are generally non-toxic and relatively low-priced. However, in order to expand the domain of application of carbohydrate-based materials, they need to be modified, or blended, with appropriate materials with a view to enhancing their thermal stability and fire-retardant properties [2,3]. Therefore, several studies have been carried out to improve the flame-retardant efficacies of these materials, including surface modification, impregnation, and chemical modification to functionalize the hydroxyl groups of the base glucose units [4,5,6]. In this context, our long-term interest is to use phosphorus-modified systems, derived from carbohydrate-based agricultural products, as passive fire protection coatings on wood-based structural elements that are commonly used in the construction sector. The synthetic routes to phosphorylate the glucopyranose units of carbohydrate-based materials are well documented in the literature [7,8,9,10,11]. Keglevich et al. established that multiple phosphorylation reactions were possible with different propensities, and the amount of phosphorylation was found to occur predominantly in positions 6 and 3 [7,11]. These observations were supported by Blennow et al. in their comprehensive review, where steric factors were also duly considered [8]. The evidence, primarily based on the 31P spectrum, with regard to the exact position(s) and formation of multiple phosphorylated units was also reported [9]. In a related study, Muhammad et al. reported on the influence of pH on the degree and nature of phosphorylation of a starch substrate [10].
The usage of many halogenated compounds has been restricted due to the ecological, environmental and health issues that they often cause [2,3,12]. Hence, over the past few decades, there has been a shift in focus towards using halogen-free compounds and formulations. Besides, the flame-retardant efficiency of compounds with covalently bound phosphorus was found to be better than the usage of equally loaded halogenated compounds [5]. Consequently, phosphorus-based compounds are increasingly being used for imparting fire-retardant properties to several commercially important polymeric materials, both synthetic and natural. In addition, phosphorus-containing compounds, when used as additives, were proven to facilitate the thermal degradation of cellulose, and favored the formation of solid products instead of releasing volatile gases [1,13]. Furthermore, phosphorus-based compounds seem to work better for cellulosic materials since they contain a significant number of hydroxyl groups, some of which can be functionalized, thereby increasing their char-forming tendency and hence their fire-retardant properties [1,8,14,15].
With this mind, we have endeavored to chemically modify some common carbohydrate-based substrates, such as potato starch, dextran, β-cyclodextrin, agar agar and tamarind, where all the substrates not only widely differed in terms of their molecular weights but also in terms of their chemical structures. We chose to carry out a simple condensation reaction, in the presence of a base (TEA), with a view to covalently binding the phosphorus group of interest (i.e., phosphate functional group) for obvious reasons. These mainly include: low levels of loadings might suffice; once covalently bound, the fire-retardant moieties are less likely to leach out from the base substrates; and the favored spatial dispositions of pendent modifying groups make them more amenable for intra-chain condensation reactions and/or neighboring group participation in bringing about char formation reactions. The recovered polymers were subjected to a variety of characterization techniques, primarily to gain insights into their chemical natures, and thermal and combustion properties. Furthermore, we have attempted to correlate some of the relevant parameters obtained through thermogravimetric analysis (TGA) runs and pyrolysis combustion flow calorimetry (PCFC) measurements.

2. Materials and Methods

2.1. Materials

The carbohydrate-based materials selected for the current study included potato starch, dextran, β-cyclodextrin and agar agar, which were obtained from Aldrich Chemical Company, Melbourne, Victoria, Australia, whereas tamarind kernel powder was sourced locally (Figure 1). The reagents, solvents and other chemicals used for the preparative procedures, including diethylchlorophosphate (DECP), triethylamine (TEA), dichloromethane (DCM) and concentrated nitric acid (AR grade), were also purchased from Aldrich Chemical Company. All the substrates, reagents and solvents were used as received, unless specified. Generally, DECP, TEA and DCM were dried and stored over molecular sieves (4 Å) prior to use.

2.2. Methods

2.2.1. Synthetic Procedures

Chemical Modification of the Base Substrates

A typical procedure on a ca. 2–3 g scale was as follows: approximately 2.5 g of each material (potato starch, or dextran, or β-cyclodextrin, or agar agar, or tamarind), as the case may be, was taken in a 250 cm3 conical flask, and about 40 cm3 of dry dichloromethane and ca. 5 cm3 of TEA were added to the substrate and the flask was stoppered. To this mixture, 2.2 cm3 of dry diethylchlorophosphate was introduced, over a period of 30 min, and the contents were stirred at room temperature for about 24 h. After the required reaction period, the content of the conical flask was filtered under a vacuum, through a qualitative filter paper, in a Buckner funnel. The solid residue that was collected onto the filter paper was thoroughly washed with deionized water in order to ensure that all unreacted DECP was washed out (at least six times with 50 cm3 of deionized water). The product thus obtained was dried in a hot air oven (ca. 70 °C) for at least 72 h (see Table 1 for details).

2.2.2. Characterization Techniques

The primary aim of the characterization was to calculate the extent of incorporation of phosphorus-containing groups (primarily through inductively coupled plasma-optical emission spectroscopy (ICP-OES)), and also to gauge the thermal and calorimetric properties of the modified materials. For the latter purpose, thermogravimetric analysis (TGA) and pyrolysis combustion flow calorimetry (PCFC) were employed. The 31P solid-state NMR spectrum of the modified starch provided conclusive proof of phosphorus functionalization of the base matrix. The unmodified counterparts were also subjected to the same set of analyses for the purpose of comparison.

Spectroscopic Analyses (Solid-State NMR)

The solid-state NMR (31P with cross-polarization/magic angle spinning: CP-MAS mode) was obtained by employing a 500 MHz Bruker machine at ambient probe conditions, typically at 10 kHz rotor speed, and the signals were calibrated against phosphoric acid as the external calibrant. The raw data were then processed by using proprietary software from the manufacturer, Bruker Pty Ltd., Melbourne, Victoria, Australia (TopSpin 4.0.6).

Inductively Coupled Plasma-Optical Emission Spectroscopy (ICP-OES)

The samples were first accurately weighed (ca. 10–15 mg, in triplicate), and then were digested by boiling with 5 cm3 of analytical grade concentrated HNO3 in 50 cm3 beakers. Following the digestion of the unmodified samples and modified versions of dextran, β-cyclodextrin, potato starch, agar agar and tamarind (as the case may be), the resulting solutions were transferred quantitatively into 25 cm3 volumetric flasks and the volumes were adjusted to the marks with deionized water. In the case of an incomplete digestion, as inferred from the presence of solid residues, the contents were first filtered using a filter before making up to the required volumes. The prepared solutions were transferred to 15 cm3 tubes before being injected into an ICP-OES instrument, Shimadzu ICPE-9000 (Shimadzu Scientific Instruments, Melbourne, Victoria, Australia). Each of the samples was repeated three times, so as to attain a more accurate value of the phosphorus content in each sample. The quantitative assessments of the phosphorus contents in the samples (see in Table 2) were obtained through constructing a Beer–Lambert plot.

Thermogravimetric Analysis (TGA)

In the present study, TGA runs were performed on samples (ca. 5–10 mg) under an atmosphere of nitrogen, in the temperature range from 30 to 800 °C, at a heating rate of 60 °C/min, using a Mettler-Toledo instrument. The relatively higher heating rate (i.e., 60 °C/min) was specifically chosen for the TGA experiments with a view to match it with the corresponding heating rate that was employed in the PCFC runs (i.e., 1 °C/s) (Figures 3–7). The reproducibility of the thermogram’s rates was periodically checked by performing duplicate/triplicate runs.

Pyrolysis Combustion Flow Calorimetry (PCFC)

This is a small-scale experimental technique used for evaluating the general flammability behaviors of materials. PCFC works on the principle of oxygen consumption calorimetry. It is also known as micro-scale combustion calorimetry, in which a very small sample size (ca. 25–40 mg) provides a wide range of combustion/flammability-related data. This process is carried out in an inert gas stream of nitrogen, or in a mixture of oxygen and nitrogen, with high temperatures to facilitate oxidation of the volatile products of pyrolysis. The useful parameters that were obtained through PCFC include heat release rates, total heat released, mass of the residue left, effective heats of combustion and the heat release capacity [16]. In the present study, we employed an FAA Micro Calorimeter to obtain the plots of heat release rates (HRRs) versus the temperatures (Figures 8–12). The samples were pyrolyzed in an inert atmosphere (i.e., in nitrogen), and pyrolytic gases were sent to a combustor at 900 °C in the presence of oxygen in excess. The mass of the samples was adjusted based on their respective oxygen consumption values (ca. 7–13%).

3. Results and Discussion

The chemical incorporation of the phosphorus-containing groups (i.e., phosphate) was clearly evident from the solid-state NMR spectrum in the case of potato starch (see Figure 2). In the case of all the other substrates (i.e., β-cyclodextrin, dextran, agar agar and tamarind), such a modification reaction was primarily inferred from ICP-OES measurements. Table 1 summarizes the details of the preparative procedures including the recovered yields and the corresponding phosphorus loadings (as wt. % obtained through ICP-OES measurements). Phosphorus estimations of unmodified substrates were also carried as blank runs, which showed no detectable levels according to ICP-OES measurements. It should be noted here that the coupling reactions between the hydroxyls (OH) in the substrate and the diethylchlorophosphate (DECP) were attempted in the presence of a base (TEA). Here, the base was expected to act as an acid scavenger, aiding in the removal of the product of condensation (HCl) between the hydroxyl groups (presumably in positions 3 and 6 of the glucopyranose rings) and the reagent, DECP [7,8,9,10,11].
Figure 3, Figure 4, Figure 5, Figure 6 and Figure 7 show the thermograms of β-cyclodextrin, dextran, potato starch, agar agar and tamarind. It can be clearly seen that the general profiles, induction temperatures and the amounts of the char residue obtained at 800 °C differed markedly with the modified versions as compared with the unmodified material in all cases (see Table 3 for details).
It is quite evident that the incorporation of phosphorus-bearing moieties (i.e., phosphate groups) clearly changes the degradation pathways of all the substrates. These effects are reflected in the somewhat altered values for the induction temperature, and in the lower temperature ranges for the primary degradation steps coupled to a slower rate of degradation, and in finally producing higher char yields for the modified systems as compared to the unmodified matrices. It is also interesting to note that the temperature at 50 wt. % showed the minimum value in the case of phosphorus-modified samples except in the case of potato starch. In addition, the temperature corresponding to the peak heat release rates (pHRRs) showed the same trend in all cases. Overall, the thermal and calorimetric behaviors of the modified materials are indicative of their lower combustibility attributes in comparison with the unmodified counterparts. It should be noted here that the degree of alteration of the thermal degradation characteristics is in tune with the phosphorus loadings. This inference could be corroborated with the relevant values obtained from the PCFC curves (see Figure 8, Figure 9, Figure 10, Figure 11 and Figure 12 and Table 3).
Generally, phosphorus-modified samples very clearly exhibited earlier combustion exothermic peaks on thermograms, as compared to the corresponding unmodified materials, presumably owing to the thermal cracking of the modifying phosphate groups [17]. Concomitantly, acidic species derived from the phosphorus functionalities could trigger dehydration reactions of the glucose units in the substrates, thus promoting char production. The latter effect is reflected in the enhanced values of char residue yields, as recorded by the TGA and PCFC measurements (see Table 2 and Table 3). The enhancements in char yields often result in carbon-rich residues, thus resulting in decreases in the values of the relevant combustion parameters, such as pHRR, THR and HRC, obtained through the PCFC measurements, including the calculated values of the effective heats of combustion.
Apparent values of heats of combustion (hc) of solid fuels can be calculated from the THR values normalized to the mass fractions of the material that underwent combustion, where the required denominator can be obtained from the initial mass of the material and amount of char residue obtained [16].
h c = T H R 1 Y p
Here, THR is the specific heat release of the sample, i.e., the area under the corresponding HRR curve (kJ/g); Y p is the pyrolysis residue (g/g).
The values so obtained are given in Table 4. The relatively lower values for the apparent heats of combustion, which in turn seemed to depend on the extent of phosphorus loading, can be attributed to the changes in the amounts and/or nature of the pyrolysis gases generated by the first stage of the experiment.
We also noticed some degree of correlation of the results from TGA and PCFC in terms of the amounts of char residues obtained for all the substrates (see Figure 13), where the samples underwent degradation reaction(s) in nitrogen. The degradative processes in a TGA experiment can be thought of as the fuel production stage (hence the amount of combustible volatiles) in the case of solid fuels. Therefore, this should be considered as the first stage in a PCFC experiment, where the material is pyrolyzed in a nitrogen atmosphere. It can be seen here that there is a noticeable relationship between the flame retardancy effect of the phosphorus-containing groups and their loadings (Figure 14, Figure 15, Figure 16 and Figure 17). As mentioned earlier, phosphorus modification of the base substrates results in altered degradative pathways, thus changing the nature and composition of the pyrolysis gases. This is in agreement with literature precedents, especially in the case of some commercially important thermoplastics, where acceptable levels of fire retardation are observed with phosphorus loadings achieved through a reactive strategy between 2.0 and 5.0 wt. %, whereas any higher loadings often result in diminished returns [18,19,20].

4. Conclusions

In the present work, we have successfully modified five different types of polymeric and oligomeric carbohydrates (potato starch, dextran, β-cyclodextrin, agar agar and tamarind), by covalently binding phosphate groups through the reaction of diethylchlorophosphate (DECP) with the substrates in dispersions in dichloromethane (DCM), in the presence of trimethylamine (TEA). The chemical constitutions of the modified substrates were, optionally, inferred from solid-state NMR spectroscopy, and the extents of the phosphorus loadings were determined through inductively coupled plasma-optical emission spectroscopy (ICP-OES). The thermal and calorimetric properties of the modified materials were primarily assessed through thermogravimetric analysis (TGA) and pyrolysis combustion flow calorimetric (PCFC) measurements. The experimental parameters obtained for the modified versions were also compared with the corresponding empirical values for the unmodified counterparts.
Phosphorus incorporation, through covalent linkages to the hydroxyl groups of the carbohydrate substrates, has clearly influenced the thermal degradation characteristics and combustion attributes of the base materials. Generally, the modified materials produced larger amounts of char residues, thus resulting in lesser amounts of combustible volatiles. The latter aspect was clearly evident from the PCFC runs. These effects can be attributed to the presence of covalently bound phosphate groups in the modified systems. Furthermore, noticeable degrees of flame retardancy effect in the modifying groups were obtained through nominal phosphorus loading (ca. 2–4 wt. %) achieved through a reactive strategy. Thus, the present work opens up the tangible prospect of formulating fire-resistant water-borne coatings, incorporating modified carbohydrates, both natural and synthetic, as polymeric materials. Following on from this, the most promising systems can be scaled up with a view to exploring the commercial viability of such products.

Author Contributions

The corresponding author, A.T., carried out all the essential experiment work, collated the data, carried out the analyses and produced the original draft manuscript. P.J. and K.M., who are the supervisors for Ananya Thomas, in collaboration with S.T.-M. were responsible for conceptualizing the research idea. H.Z. was primarily responsible for recording and interpreting solid-state NMR and also took part in the correction of the manuscript. All authors have read and agreed to the published version of the manuscript

Funding

One of us, AT, is grateful to Victoria University, Melbourne, Australia, for the provision of a PhD studentship.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Costes, L.; Laoutid, F.; Brohez, S.; Dubois, P. Bio-based flame retardants: When nature meets fire protection. Mater. Sci. Eng. R Rep. 2017, 117, 1–25. [Google Scholar] [CrossRef]
  2. Wang, X.; Hu, Y.; Song, L.; Xuan, S.; Xing, W.; Bai, Z.; Lu, H. Flame retardancy and thermal degradation of intumescent flame retardant poly (lactic acid)/starch biocomposites. Ind. Eng. Chem. Res. 2010, 50, 713–720. [Google Scholar] [CrossRef]
  3. Demirgöz, D.; Elvira, C.; Mano, J.F.; Cunha, A.M.; Piskin, E.; Reis, R.L. Chemical modification of starch based biodegradable polymeric blends: Effects on water uptake, degradation behaviour and mechanical properties. Polym. Degrad. Stab. 2000, 70, 161–170. [Google Scholar] [CrossRef]
  4. Kishore, K.; Mohandas, K. Action of phosphorus compounds on fire-retardancy of cellulosic materials: A review. Fire Mater. 1982, 6, 54–58. [Google Scholar] [CrossRef]
  5. Liu, Y.L.; Hsiue, G.H.; Chiu, Y.S.; Jeng, R.J.; Ma, C. Synthesis and flame-retardant properties of phosphorus-containing polymers based on poly (4-hydroxystyrene). J. Appl. Polym. Sci. 1996, 59, 1619–1625. [Google Scholar] [CrossRef]
  6. Matko, S.; Toldy, A.; Keszei, S.; Anna, P.; Bertalan, G.; Marosi, G. Flame retardancy of biodegradable polymers and biocomposites. Polym. Degrad. Stab. 2005, 88, 138–145. [Google Scholar] [CrossRef]
  7. Keglevich, G.; Bagi, P.; Rapi, Z.; Bako, P.; Drahos, L.; Szolnoki, B.; Marosi, G. The Synthesis of Bio-Based Flame-Retarded Epoxy-Precursors. Macromol. Symp. 2015, 352, 46–50. [Google Scholar] [CrossRef]
  8. Blennow, A.; Nielsen, T.H.; Baunsgaard, L.; Mikkelsen, R.; Engelsen, S.B. Starch phosphorylation: A new front line in starch research. Trends Plant Sci. 2002, 7, 445–450. [Google Scholar] [CrossRef]
  9. Passauer, L.; Liebner, F.; Fischer, K. Starch phosphate hydrogels. Part I: Synthesis by mono-phosphorylation and cross-linking of starch. Starch Stärke 2009, 61, 621–627. [Google Scholar] [CrossRef]
  10. Muhammad, K.; Hussin, F.; Man, Y.C.; Ghazali, H.M.; Kennedy, J.F. Effect of pH on phosphorylation of sago starch. Carbohydr. Polym. 2000, 42, 85–90. [Google Scholar] [CrossRef]
  11. Blennow, A.; Engelsen, S.B.; Munck, L.; Moller, B.L. Starch molecular structure and phosphorylation investigated by a combined chromatographic and chemometric approach. Carbohydr. Polym. 2000, 41, 163–174. [Google Scholar] [CrossRef]
  12. Levchik, S.V.; Weil, E.D. A review of recent progress in phosphorus-based flame retardants. J. Fire Sci. 2006, 24, 345–364. [Google Scholar] [CrossRef]
  13. Green, J. Mechanisms for flame retardancy and smoke suppression-a review. J. Fire Sci. 1996, 14, 426–442. [Google Scholar] [CrossRef]
  14. Horrocks, A.R.; Kandola, B.K.; Davies, P.J.; Zhang, S.; Padbury, S. Developments in flame retardant textiles—A review. Polym. Degrad. Stab. 2005, 88, 3–12. [Google Scholar] [CrossRef]
  15. Horrocks, A.R. Developments in flame retardants for heat and fire resistant textiles—The role of char formation and intumescence. Polym. Degrad. Stab. 1996, 54, 143–154. [Google Scholar] [CrossRef]
  16. Lyon, R.E.; Walters, R.N. Pyrolysis combustion flow calorimetry. J. Anal. Appl. Pyrolysis 2004, 71, 27–46. [Google Scholar] [CrossRef]
  17. Joseph, P.; Tretsiakova-Mcnally, S. Reactive modifications of some chain-and step-growth polymers with phosphorus-containing compounds: Effects on flame retardance—A review. Polym. Adv. Technol. 2011, 22, 395–406. [Google Scholar] [CrossRef]
  18. Tretsiakova-McNally, S.; Joseph, P. Thermal and calorimetric evaluations of polyacrylonitrile containing covalently-bound phosphonate groups. Polymers 2018, 10, 131. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  19. Tretsiakova-McNally, S.; Joseph, P. Pyrolysis combustion flow calorimetry studies on some reactively modified polymers. Polymers 2015, 7, 453–467. [Google Scholar] [CrossRef] [Green Version]
  20. Joseph, P.; Tretsiakova-McNally, S. Combustion behaviours of chemically modified polyacrylonitrile polymers containing phosphorylamino groups. Polym. Degrad. Stab. 2012, 97, 2531–2535. [Google Scholar] [CrossRef]
Figure 1. Chemical structures of the substrates: (a) β-cyclodextrin, (b) potato starch, (c) dextran, (d) agar agar, (e) tamarind.
Figure 1. Chemical structures of the substrates: (a) β-cyclodextrin, (b) potato starch, (c) dextran, (d) agar agar, (e) tamarind.
Polymers 12 00588 g001
Figure 2. 31P-NMR spectrum of potato starch modified with phosphate groups (the abscissa denotes the chemical shift values, δ, in ppm, and the ordinate corresponds to the signal intensity in arbitrary units).
Figure 2. 31P-NMR spectrum of potato starch modified with phosphate groups (the abscissa denotes the chemical shift values, δ, in ppm, and the ordinate corresponds to the signal intensity in arbitrary units).
Polymers 12 00588 g002
Figure 3. Thermograms of modified and unmodified versions of β-cyclodextrin at 60 °C/min.
Figure 3. Thermograms of modified and unmodified versions of β-cyclodextrin at 60 °C/min.
Polymers 12 00588 g003
Figure 4. Thermograms of modified and unmodified versions of dextran at 60 °C/min.
Figure 4. Thermograms of modified and unmodified versions of dextran at 60 °C/min.
Polymers 12 00588 g004
Figure 5. Thermograms of modified and unmodified versions of potato starch at 60 °C/min.
Figure 5. Thermograms of modified and unmodified versions of potato starch at 60 °C/min.
Polymers 12 00588 g005
Figure 6. Thermograms of modified and unmodified versions of tamarind at 60 °C/min.
Figure 6. Thermograms of modified and unmodified versions of tamarind at 60 °C/min.
Polymers 12 00588 g006
Figure 7. Thermograms of modified and unmodified versions of agar agar at 60 °C/min.
Figure 7. Thermograms of modified and unmodified versions of agar agar at 60 °C/min.
Polymers 12 00588 g007
Figure 8. Plot of the heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of β-cyclodextrin.
Figure 8. Plot of the heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of β-cyclodextrin.
Polymers 12 00588 g008
Figure 9. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of dextran.
Figure 9. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of dextran.
Polymers 12 00588 g009
Figure 10. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of potato starch.
Figure 10. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of potato starch.
Polymers 12 00588 g010
Figure 11. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of agar.
Figure 11. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of agar.
Polymers 12 00588 g011
Figure 12. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of tamarind.
Figure 12. Plot of heat release rate (HRR) (W/g) versus temperature (°C) for modified and unmodified versions of tamarind.
Polymers 12 00588 g012
Figure 13. Correlation of char residues (wt. %) from TGA experiments and PCFC runs of the substrates.
Figure 13. Correlation of char residues (wt. %) from TGA experiments and PCFC runs of the substrates.
Polymers 12 00588 g013
Figure 14. Plot of total heat release (THR) versus phosphorus content (wt. %) of the substrates.
Figure 14. Plot of total heat release (THR) versus phosphorus content (wt. %) of the substrates.
Polymers 12 00588 g014
Figure 15. Plot of the heat release capacity versus phosphorus content (wt. %) of the substrates.
Figure 15. Plot of the heat release capacity versus phosphorus content (wt. %) of the substrates.
Polymers 12 00588 g015
Figure 16. Plot of peak heat release rates (pHRR) versus phosphorus content (wt. %) of the substrates.
Figure 16. Plot of peak heat release rates (pHRR) versus phosphorus content (wt. %) of the substrates.
Polymers 12 00588 g016
Figure 17. Plot of heats of combustion (hc) versus phosphorus content (wt. %).
Figure 17. Plot of heats of combustion (hc) versus phosphorus content (wt. %).
Polymers 12 00588 g017
Table 1. Details of the chemical modification reactions.
Table 1. Details of the chemical modification reactions.
Sl. No.SubstrateSample Weight (g)DECP (g)DCM (cm3)TEA (cm3)Recovered Yield (wt %)P (wt %)
1β-cyclodextrin2.52.6340549.901.7
2Dextran2.42.6340579.151.0
3Potato starch2.32.6340555.173.2
4Agar agar2.72.6340566.455.55
5Tamarind2.82.6340568.236.68
Table 2. Details from thermogravimetric analysis (TGA).
Table 2. Details from thermogravimetric analysis (TGA).
SampleP (wt %)Induction Temperature (°C)Temperature at 50 wt % (°C)Residue at 400 °C (wt %)Final Residue at 800 °C (wt %)
β-cyclodextrin0.094.035611.46.00
β-cyclodextrin1.796.033439.722.9
Dextran0.085.034015.29.80
Dextran1.093.027329.318.7
Potato Starch0.093.033518.311.9
Potato Starch3.212936645.625.4
Agar agar0.077.033336.714.8
Agar agar5.590.028036.923.7
Tamarind0.086.035738.521.3
Tamarind6.610533839.624.0
Table 3. Pyrolysis combustion flow calorimetry (PCFC) data for modified and unmodified versions of base substrates (average values of triplicate runs).
Table 3. Pyrolysis combustion flow calorimetry (PCFC) data for modified and unmodified versions of base substrates (average values of triplicate runs).
SampleP (wt %)Temp to pHRR (°C)pHRR (W/g)THR (kJ/g)Heat Release Capacity (J/g K)Char Yield (wt %)
β-cyclodextrin0.0342452.711.645911.11
β-cyclodextrin1.729066.024.2067.025.54
Dextran0.0319289.010.4288<1.0
Dextran1.0252199.97.5021723.52
Potato Starch0.0310362.810.436812.50
Potato Starch3.226057.183.9060.031.85
Agar agar0.0272256.012.32503.680
Agar agar5.5234219.48.3023423.40
Tamarind0.0326158.010.015525.12
Tamarind6.6291126.08.1012829.36
Table 4. Heats of combustion values.
Table 4. Heats of combustion values.
SampleP (wt %)Pyrolysis Residue (g/g)hc (kJ/g)
β-cyclodextrin0.00.1113.03
β-cyclodextrin1.70.255.600
Dextran0.0— *
Dextran1.00.276.980
Potato Starch0.00.2311.81
Potato Starch3.20.315.650
Agar agar0.00.03612.75
Agar agar5.50.2310.78
Tamarind0.00.2513.30
Tamarind6.60.2711.36
* Pyrolysis residue could not be measured accurately as the sample expanded considerably and spilled over the pan upon the degradation/combustion.

Share and Cite

MDPI and ACS Style

Thomas, A.; Joseph, P.; Moinuddin, K.; Zhu, H.; Tretsiakova-McNally, S. Thermal and Calorimetric Evaluations of Some Chemically Modified Carbohydrate-Based Substrates with Phosphorus-Containing Groups. Polymers 2020, 12, 588. https://doi.org/10.3390/polym12030588

AMA Style

Thomas A, Joseph P, Moinuddin K, Zhu H, Tretsiakova-McNally S. Thermal and Calorimetric Evaluations of Some Chemically Modified Carbohydrate-Based Substrates with Phosphorus-Containing Groups. Polymers. 2020; 12(3):588. https://doi.org/10.3390/polym12030588

Chicago/Turabian Style

Thomas, Ananya, Paul Joseph, Khalid Moinuddin, Haijin Zhu, and Svetlana Tretsiakova-McNally. 2020. "Thermal and Calorimetric Evaluations of Some Chemically Modified Carbohydrate-Based Substrates with Phosphorus-Containing Groups" Polymers 12, no. 3: 588. https://doi.org/10.3390/polym12030588

APA Style

Thomas, A., Joseph, P., Moinuddin, K., Zhu, H., & Tretsiakova-McNally, S. (2020). Thermal and Calorimetric Evaluations of Some Chemically Modified Carbohydrate-Based Substrates with Phosphorus-Containing Groups. Polymers, 12(3), 588. https://doi.org/10.3390/polym12030588

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics