Article

Microwave and Ultrasound Augmented Leaching of Complicated Zinc Oxide Ores in Ammonia and Ammonium Citrate Solutions

1
State Key Laboratory of Complex Nonferrous Metal Resources Clean Utilization, Kunming University of Science and Technology, Kunming 650093, China
2
Faculty of Metallurgical and Energy Engineering, Kunming University of Science and Technology, Kunming 650093, China
3
Chemical Engineering Program, The Petroleum Institute, P.O. Box 2533, Abu Dhabi 999041, UAE
*
Author to whom correspondence should be addressed.
Metals 2017, 7(6), 216; https://doi.org/10.3390/met7060216
Submission received: 9 May 2017 / Revised: 6 June 2017 / Accepted: 6 June 2017 / Published: 12 June 2017

Abstract

:
Recovery of zinc from low grade zinc oxide ore is attempted with ammonia and ammonium citrate solutions augmented by microwave roasting and ultrasound radiation. The influence of the ammonia-ammonium ratio, roasting temperature, ultrasound power, and leaching time were assessed on the recovery of zinc. A maximum zinc recovery of 88.57% could be achieved at a roasting temperature of 673 K, leaching temperature of 298 K, stirring speed of 300 rpm, total ammonia concentration of 5 mol/L with an ammonium citrate concentration of 1.2 mol/L, liquid to solid ratio of 5:1, the ultrasound power was 600 W and the leaching time was 120 min. The enhancement in recovery with increases in the roasting temperature up to 673 K was attributed to the conversion of ZnCO3 to ZnO. The phases of mineral samples and the reaction residues were characterized by X-ray diffraction (XRD).

1. Introduction

With the availability of zinc sulfide ores dwindling, the need to identify alternative ores is imperative [1,2]. Zinc oxide ores are recently being considered as an appropriate alternative. However, the zinc oxide ore grade is too low to enrich, demanding some special methods to extract the zinc economically [3,4].
The zinc oxide ore could be dissociated using acidic leaching processes, however the presence of contaminants such as Ca, Fe, Mg, etc., along with zinc, render the further processing as very complex [5,6,7]. The recent efforts in literature indicate utilization of an alkali such as ammonia for leaching metals like cobalt, nickel and copper due to the formation of stable metal amine complexes, leading to higher solubility in most cases. Other harmful impurities, such as Fe, Pb, Ca, and Mg precipitate as hydroxides due to their poor complexability with ammonia [8]. However, reports on the process of optimization of the ammonia leaching process for the separation of zinc ores are not available, necessitating such an effort in the field of hydrometallurgy.
The microwave heating is a method of pre-treatment of raw ore commonly utilized in hydrometallurgy [9]. Microwave-assisted leaching in metallurgy and extraction of minerals has been a subject of interest in the last few decades, but most of the microwave-assisted extraction works were related by leaching with mineral acids [10]. In the last few years, ultrasonic processes emerged as a preferred alternative for enhancing the leaching efficiency of the metal ores [11]. The merit of the ultrasonic cavitation effect, contributing to an improved rate of leaching is well documented [12,13,14]. Nevertheless, its application in the hydrometallurgical industry is in its infancy, in particular with respect to ammonia media.
This work attempts to develop a new hydrometallurgical technology to enrich low grade zinc ore in a medium of ammonia and ammonium citrate solutions, utilizing ultrasound and microwave heating [15]. In this connection, the optimal process conditions were identified covering the process parameters of ammonia-ammonium ratio, roasting temperature, ultrasound power, and leaching duration.

2. Materials and Methods

2.1. Materials

The complicated zinc ore received from Yunnan province of China, was crushed and ground to a powder of size less than 75 μm, and its chemical composition is recorded in Table 1. The X-ray diffraction (XRD, Rigaku, Japan) pattern of the zinc residue shows the mineralogical content of the sample before and after roasting at various temperatures is shown in Figure 1. It can be seen that XRD analysis shows the smithsonite (ZnCO3), hemimorphite (Zn4Si2O7(OH)2·H2O), and gangue, such as calcite (CaCO3) and quartz (SiO2). All the chemical reagents used in this study were of analytical grade.

2.2. Sample Preparation

The samples were placed in a crucible (Cheng Chen Industrial Co., Ltd., Shanghai, China), evenly spread as a thin layer and exposed to temperatures of 573, 623, 673, 723, and 773 K, roasted in the atmosphere for a duration of 30 min in a microwave oven (Maike Wei Microwave Innovation Technology Co., Ltd, Qingdao, China). The duration of 30 min refers to the time the samples were retained in the furnace after reaching the set temperature. The roasted samples were leached adopting the details provided in the section below.

2.3. Leaching Experiments

The microwave roasted sample of 24 g was taken along with 120 mL of ammonia of a 5 mol/L concentration along with ammonium citrate of a 1.2 mol/L concentration into a reaction vessel (Shu bo Industrial Co., Ltd., Sichuan, China) at a default ultrasound power (200–1000 W), default temperature (298 K) for a default duration of (10–180 min), at a stirring speed of 300 rpm and at a liquid to solid ratio of 5:1. Upon completion of the experiment, the lixivium and leached residue were separated, and the concentration of zinc in the leached solutions was measured. The % leaching of zinc was calculated in different periods of the experiment. Moreover, the Zn recovery was estimated by using the equation:
η Zn = C Zn × V m × W Zn × 100 %
where, CZn, V, m, and WZn represent the Zn concentration of lixivium (g/L), the volume of lixivium (L), the mass of the zinc oxide ore (g), and the proportion of zinc in the ore (%), respectively. The CZn was determined by the ICP (ICP-OES, LEEMAN prodigy 7, Hudson, NH, USA).
The effect of ultrasound power on the % leaching of zinc is assessed by varying the ultrasound power from 200 to 1000 W.

2.4. Reaction Mechanism

The citrate and ammonium can be coordinated with zinc to leach the zinc in the mineral to increase the % leaching of the zinc. The coordination of zinc ions with ammonium is detailed in the reactions below (1) to (4):
Zn2+(aq) + NH3·H2O(aq) = [Zn(NH3)]2+(aq) + H2O
Zn2+(aq) + 2NH3·H2O(aq) = [Zn(NH3)2]2+(aq) + 2H2O
Zn2+(aq) + 3NH3·H2O(aq) = [Zn(NH3)3]2+(aq) + 3H2O
Zn2+(aq) + 4NH3·H2O(aq) = [Zn(NH3)4]2+(aq) + 4H2O
In the process of ammonia leaching, zinc oxide and zinc carbonate dissolve due to the formation of Zn (П)-ammonia complex ion. Thermodynamic calculation [16] shows that in liquid ammonia, all of the ZnCO3 cannot be converted into the solution, but ZnO can do it easily. Under the condition of the microwave, roasting the ZnCO3 gets converted to ZnO facilitating leaching with ammonia.
ZnCO 3 + 4 NH 3 · H 2 O ( aq ) = Zn ( NH 3 ) 4 2 + + CO 3 2 ( aq ) + 4 H 2 O
ZnO + 4 NH 3 + H 2 O = Zn ( NH 3 ) 4 2 + + 2 OH ( aq )
ZnCO 3 = ZnO + CO 2

3. Results and Discussion

3.1. Effect of Microwave Roasting on % Leaching of Zinc

Figure 2 shows the zinc leaching for the unroasted zinc ore increases with the increase of ammonia concentration, with maximum % leaching being 59.5%. Under the same conditions the % leaching with the microwave roasted ore increased from 64.5% to 75.2% (Figure 3). A comparison of the XRD pattern of the raw ore and the residue after leaching are shown in Figure 4. It is conspicuous, that the presence of ZnCO3 is the reason for the low leaching %. Similarly a comparison of the XRD pattern for the raw ore with the microwave roasted leached residue is shown in Figure 5. The XRD pattern confirms the transformation of ZnCO3 to ZnO after microwave roasting, which contributes to the increased % leaching of Zn.

3.2. Effect of Microwave Roasting Temperature

The effect of the roasting temperature on the % leaching of zinc is shown in Figure 6. The % leaching was found to increase with an increase in the microwave roasting temperature until 673 K, with a marginal decrease beyond 673 K. The highest % leaching is as high as 71.77%. Under the same conditions, the unroasted ore yielded only 51.5%. In Figure 1, the ZnCO3 phase in the mineral disappears and the ZnO phase appears in 673 K, which improves the highest yield at 673 K. At temperatures higher than 673 K, the decrease in zinc yield could be attributed to the formation of zinc ferrite, which has poor capacity to be assimilated by ammonia. Therefore, when the calcination temperature of the mineral exceeds 673 K, the % leaching of the calcined ore decreased. Zhang et al. [17] also have reported that zinc oxide ore calcined at 673 K, and alkali leaching resulted in the highest recovery, while at temperatures higher than 673 K, the tendency of the calcined ore to form zinc ferrite, contributed to a lower Zn recovery.

3.3. Effects of Ultrasound Power

Figure 7 shows the effect of the ultrasonic power on the % Zn recovery covering an ultrasonic power range of 200 to 1000 W. The figure shows the maximum recovery is observed at an ultrasonic power of 600 W, while beyond that it was found to decrease. The increase in the % Zn recovery with an increase in the ultrasonic power can be attributed to the increase in the cavitation effect, the mechanical stirring effect, which increased the degree of turbulence in the solid-liquid interface that contributed to a higher recovery. In addition, the micro-jet generated by the cavitation of the ultrasonic wave will promote the diffusion of the leachant to the surface of the mineral, liberating the zinc ions. At ultrasonic powers in excess of 600 W, a marginal decrease in the Zn recovery could be attributed to the ultrasonic power contributing to the volatilization of ammonia and the decomposition of ammonium chloride in the leaching system. The reduction of ammonium ions in the leaching solution inevitably contributed to a reduction in the Zn recovery. This phenomenon is also reported by Li et al. [18].
For the zinc ore microwave roasted at 673 K, and leaching conditions at a temperature of 298 K, a solid to liquid ratio of 1:5, stirring speed of 300 rpm, reaction time of 60 min, ammonia concentration of 5 mol/L and with an ammonium citrate concentration of 1.2 mol/L, the maximum % Zn recovery obtained was 80.2%.

3.4. Effect of Leaching Time with Ultrasound

The influence of the leaching duration on the Zn recovery is presented in Figure 8. With increases to the leaching duration, an increase in the Zn recovery was observed, the maximum Zn leaching was 88.57% for a duration of 120 min.

3.5. Characterization Analysis

The leached zinc oxide ores with the maximum Zn recovery were dried at 373 K and ground for Chemical composition detection, and the major elements were listed in Table 2. It can be seen that the leached zinc oxide ore mainly consisted of Zn, Pb, Fe, Si, Ca, and S elements. It is generally known that the most Pb, Fe, Si, and Ca containing compounds can’t be dissolved in the ammonia and ammonium citrate solutions. With the reduction of zinc in the ores, the contents of the elements such as Pb, Fe, Si, and Ca significantly increase. For example, the ratio of lead and zinc in the ore before roasting was 1 to 4.18, and that in the leaching residue was as high as 1 to 0.52. During roasting, the oxidation of S element can occur, so the content of S in the leached ores decreases.

4. Conclusions

The zinc recovery from complicated zinc ores could be accomplished successfully with the maximum recovery being 88.57% under the experimental conditions, of a roasting temperature of 673 K, leaching temperature of 298 K, stirring speed of 300 rpm, total ammonia concentration of 5 mol/L with an ammonium citrate concentration of 1.2 mol/L, liquid to solid ratio of 5:1, ultrasound power of 600 W and a leaching time of 120 min.

Acknowledgments

This work was supported by National Natural Science Foundation of China (51604135).

Author Contributions

Haoyu Li, Shiwei Li, Libo Zhang, Jinhui Peng conceived and designed the experiments; Haoyu Li, performed the experiments and analyzed the data; Libo Zhang, Jinhui Peng contributed reagents/materials/analysis tools; Shaohua Yin, Chandrasekar Srinivasakannan modified the paper before submission; all the authors analyzed the data and wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chen, A.; Zhao, Z.W.; Jia, X.; Long, S.; Huo, G.S.; Chen, X.Y. Alkaline leaching Zn and its concomitant metals from refractory hemimorphite zinc oxide ore. Hydrometallurgy 2009, 97, 228–232. [Google Scholar] [CrossRef]
  2. Ferdous, R.; Khan, F.; Veitch, B.; Amyotte, P.R. Methodology for computer-aided fault tree analysis. Process Saf. Environ. Prot. 2007, 85, 70–80. [Google Scholar] [CrossRef]
  3. Yang, T.; Rao, S.; Zhang, D.; Wen, J.; Liu, W.; Chen, L. Leaching of low grade zinc oxide ores in nitrilotriacetic acid solutions. Hydrometallurgy 2016, 161, 107–111. [Google Scholar] [CrossRef]
  4. Moradi, S.; Monhemius, A.J. Mixed sulfide-oxide lead and zinc ores: Problems and solutions. Miner. Eng. 2011, 24, 1062–1076. [Google Scholar] [CrossRef]
  5. Anjum, F.; Shahid, M.; Akcil, A. Biohydrometallurgy techniques of low grade ores: A review on black shale. Hydrometallurgy 2012, 117–118, 1–12. [Google Scholar] [CrossRef]
  6. Huisman, J.L.; Schouten, G.; Schultz, C. Biologically produced sulphide for purification of process streams, effluent treatment and recovery of metals in the metal and mining industry. Hydrometallurgy 2006, 83, 106–113. [Google Scholar] [CrossRef]
  7. Crundwell, F.K. The mechanism of dissolution of minerals in acidic and alkaline solutions: Part III. Application to oxide, hydroxide and sulphide minerals. Hydrometallurgy 2014, 149, 265–275. [Google Scholar] [CrossRef]
  8. Ding, Z.; Yin, Z.; Hu, H.; Chen, Q. Dissolution kinetics of zinc silicate (hemimorphite) in ammoniacal solution. Hydrometallurgy 2010, 104, 201–206. [Google Scholar] [CrossRef]
  9. Lovás, M.; Murová, I.; Mockovciaková, A.; Rowson, N.; Jakabský, Š. Intensification of magnetic separation and leaching of Cu-ores by microwave radiation. Sep. Purif. Technol. 2003, 31, 291–299. [Google Scholar] [CrossRef]
  10. Pinto, I.S.S.; Soares, H.M.V.M. Microwave-assisted selective leaching of nickel from spent hydrodesulphurization catalyst: A comparative study between sulfuric and organic acids. Hydrometallurgy 2013, 140, 20–27. [Google Scholar] [CrossRef]
  11. Wang, X.; Srinivasakannan, C.; Duan, X.H.; Peng, J.H.; Yang, D.J.; Ju, S.H. Leaching kinetics of zinc residues augmented with ultrasound. Sep. Purif. Technol. 2013, 115, 66–72. [Google Scholar]
  12. Choi, J.K.; Jayaprakash, A.; Chahine, G.L. Scaling of cavitation erosion progression with cavitation intensity and cavitation source. Wear 2012, 278, 53–61. [Google Scholar] [CrossRef]
  13. Lei, Y.; Chang, H.; Guo, X.; Li, T.; Xiao, L. Ultrasonic cavitation erosion of 316L steel weld joint in liquid Pb–Bi eutectic alloy at 550 °C. Ultrason. Sonochem. 2017, 39, 77–86. [Google Scholar] [CrossRef]
  14. Lebon, G.S.B.; Tzanakis, I.; Djambazov, G.; Pericleous, K.; Eskin, D.G. Numerical modelling of ultrasonic waves in a bubbly Newtonian liquid using a high-order acoustic cavitation model. Ultrason. Sonochem. 2017, 37, 660–668. [Google Scholar] [CrossRef] [PubMed]
  15. Fischmann, A.J.; Dixon, D.G. Awaruite (Ni3Fe) as a nickel resource-leaching with ammoniacal–ammonium solution containing citrate and thiosulfate. Hydrometallurgy 2009, 99, 214–224. [Google Scholar] [CrossRef]
  16. Zhang, Y. The High Temperature Aqueous Solution Thermodynamics Data Calculation Handbook; Metallurgical Industry Press: Beijing, China, 1983. [Google Scholar]
  17. Zhang, Y.; Deng, J.; Chen, J.; Yu, R.; Xing, X. Leaching of zinc from calcined smithsonite using sodium hydroxide. Hydrometallurgy 2013, 131–132, 89–92. [Google Scholar] [CrossRef]
  18. Li, J.G.; Zhao, R.S.; Liu, H.C. Recovery of metal values from spent lithium-ion batteries. Acta Scientiarum Nat. Univ. Sunyatseni 2007, 46, 256–257. [Google Scholar]
Figure 1. X-ray diffraction (XRD) patterns of complicated zinc ore before and after roasting at various temperatures with microwave power.
Figure 1. X-ray diffraction (XRD) patterns of complicated zinc ore before and after roasting at various temperatures with microwave power.
Metals 07 00216 g001
Figure 2. Effects of different ammonium citrate concentrations (from 0.3 to 1.5 mol/L) on leaching efficiency of zinc from the unroasted ores.
Figure 2. Effects of different ammonium citrate concentrations (from 0.3 to 1.5 mol/L) on leaching efficiency of zinc from the unroasted ores.
Metals 07 00216 g002
Figure 3. Effect of 5 mol/L ammonia with different ammonium citrate concentrations (from 0.3 to 1.5 mol/L) on the zinc recovery of the roasted ores at 673 K.
Figure 3. Effect of 5 mol/L ammonia with different ammonium citrate concentrations (from 0.3 to 1.5 mol/L) on the zinc recovery of the roasted ores at 673 K.
Metals 07 00216 g003
Figure 4. XRD patterns of the complicated zinc ores before raw ore and the residue after the raw ore leached at the same condition.
Figure 4. XRD patterns of the complicated zinc ores before raw ore and the residue after the raw ore leached at the same condition.
Metals 07 00216 g004
Figure 5. XRD patterns of the complicated zinc ores before and after roasting at 673 K.
Figure 5. XRD patterns of the complicated zinc ores before and after roasting at 673 K.
Metals 07 00216 g005
Figure 6. Zinc leaching recovery after roasting at different calcination temperatures.
Figure 6. Zinc leaching recovery after roasting at different calcination temperatures.
Metals 07 00216 g006
Figure 7. Effects of ultrasonic power on zinc recovery.
Figure 7. Effects of ultrasonic power on zinc recovery.
Metals 07 00216 g007
Figure 8. Effects of leaching time on the Zn recovery.
Figure 8. Effects of leaching time on the Zn recovery.
Metals 07 00216 g008
Table 1. Chemical composition of the zinc oxide ores (wt %).
Table 1. Chemical composition of the zinc oxide ores (wt %).
ZnPbFeSiCaS
15.33.6813.2413.674.860.89
Table 2. Chemical composition of leached zinc oxide ores (wt %).
Table 2. Chemical composition of leached zinc oxide ores (wt %).
ZnPbFeSiCaS
2.735.2318.2220.17.310.31

Share and Cite

MDPI and ACS Style

Zhang, L.; Li, H.; Peng, J.; Srinivasakannan, C.; Li, S.; Yin, S. Microwave and Ultrasound Augmented Leaching of Complicated Zinc Oxide Ores in Ammonia and Ammonium Citrate Solutions. Metals 2017, 7, 216. https://doi.org/10.3390/met7060216

AMA Style

Zhang L, Li H, Peng J, Srinivasakannan C, Li S, Yin S. Microwave and Ultrasound Augmented Leaching of Complicated Zinc Oxide Ores in Ammonia and Ammonium Citrate Solutions. Metals. 2017; 7(6):216. https://doi.org/10.3390/met7060216

Chicago/Turabian Style

Zhang, Libo, Haoyu Li, Jinhui Peng, Chandrasekar Srinivasakannan, Shiwei Li, and Shaohua Yin. 2017. "Microwave and Ultrasound Augmented Leaching of Complicated Zinc Oxide Ores in Ammonia and Ammonium Citrate Solutions" Metals 7, no. 6: 216. https://doi.org/10.3390/met7060216

APA Style

Zhang, L., Li, H., Peng, J., Srinivasakannan, C., Li, S., & Yin, S. (2017). Microwave and Ultrasound Augmented Leaching of Complicated Zinc Oxide Ores in Ammonia and Ammonium Citrate Solutions. Metals, 7(6), 216. https://doi.org/10.3390/met7060216

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop