Next Article in Journal
Effect of Differentiated Injection Ratio, Gas Flow Rate, and Slag Thickness on Mixing Time and Open Eye Area in Gas-Stirred Ladle Assisted by Physical Modeling
Next Article in Special Issue
Mixing Phenomenon and Flow Field in Ladle of RH Process
Previous Article in Journal
On the Free-Surface Roughness in Incremental Forming of a Sheet Metal: A Study from the Perspective of ISF Strain, Surface Morphology, Post-Forming Properties, and Process Conditions
Previous Article in Special Issue
Comparison of Transverse Uniform and Non-Uniform Secondary Cooling Strategies on Heat Transfer and Solidification Structure of Continuous-Casting Billet
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Reoxidation of Al-Killed Steel by Cr2O3 from Tundish Cover Flux

1
Engineering Research Institute, University of Science and Technology Beijing, Beijing 100083, China
2
School of Metallurgical and Ecological Engineering, University of Science and Technology Beijing, Beijing 100083, China
*
Authors to whom correspondence should be addressed.
Metals 2019, 9(5), 554; https://doi.org/10.3390/met9050554
Submission received: 2 April 2019 / Revised: 1 May 2019 / Accepted: 4 May 2019 / Published: 12 May 2019
(This article belongs to the Special Issue Refining and Casting of Steel)

Abstract

:
Reoxidation has long been a problem when casting ultra-low oxygen liquid steel. An experimental study of the reoxidation phenomenon caused by Cr2O3-bearing cover flux of Al-killed steel is presented here. MgO-CaO-SiO2-Al2O3-Cr2O3 tundish cover flux with various Cr2O3 contents were used to study the effects of Cr2O3 on total oxygen content (T[O]) and alumina and silicone loss of Al-killed steel at 1923 K (1650 °C). It was found that Cr2O3 can be reduced by Al to cause reoxidation, and the reaction occurs mainly within 2 to 3 min after the addition of the tundish cover flux with 5% and 10% Cr2O3 concentration. T[O] and Al loss increase with higher Cr2O3 concentration flux. Two controlled experiments were also made to investigate the oxygen transported to the steel by the decomposition of Cr2O3. It was calculated that when Al is present in steel, more than 90% of the reoxidation of Cr2O3 is caused by Al, and the rest is caused by decomposition.

1. Introduction

The total oxygen content (T[O]) of high-grade steel has been required to be as low as possible in recent years [1,2]. For example, line pipe steel requires sulfur, phosphorus, and T[O] all to be less than 30 ppm, and bearing steel requires T[O] to be less than 10 ppm [3]. This low oxygen liquid steel is very hard to cast due to reoxidation during the process. The tundish used in continuous casting is the last vessel in contact with molten steel during steel production, with this final step being the most important in protecting the steel from oxygen and maintaining cleanliness [4,5]. However, due to the extremely low oxygen content in liquid steel, it can be easily reoxidized by the oxygen from the refractory, the slag, and the air environment [6,7]. The reoxidation phenomenon has been a problem for tundishes and is the obstacle to producing clean steel [8,9,10].
The role of tundish cover flux is to protect the molten steel from the air. However, in recent years, reoxidation of steel by the cover flux has been observed and widely investigated. Researchers have found that the reoxidation capacity of the slag was related to the oxygen potential in the slag, such as the FeO, SiO2, and MnO content in the slag phase [11,12,13]. The high oxygen potential slag easily reacts with deoxidizing agents such as the Al and Ti contained in liquid steel. Some researchers [14] studied the effect of refining slag components on the reoxidation of molten steel through the double-membrane theory and found that reducing the CaO/Al2O3 ratio and FeO content in the slag can reduce the reoxidation of steel by refined slag.
Recently, Cr2O3 has been found in tundish cover flux [15]. Cr is usually used as an alloying element for stainless steel, working as a protecting element that generates Cr2O3 on the metal surface to prevent further oxidation [16]. Due to the steel-slag equilibrium reaction, some Cr2O3 shows up in the refining slag of stainless steel [17,18]. The reduction of Cr2O3 during the refining process will increase T[O] and thus will do harm to steel cleanliness [19]. It has been reported that the amount of Cr2O3 forming in slag could be reduced by lowering the basicity of the slag or by adding Al2O3, the reason for this being the increase in the liquid phase fraction of the slag [19].
When using cover flux containing Cr2O3, Cr2O3 may work as a medium carrying oxygen from the air that reoxidizes the liquid steel instead of protecting it. Cover flux is a semi-molten slag that, when compared to other totally melted refining slags, makes the reduction of Cr2O3 in the flux special and worth studying. Reoxidation is related to the Si and Al content in steel and the slag composition. Therefore, in the present work, reoxidation of steel, with and without Al, by Cr2O3 in the tundish cover flux was investigated using experimental methods. The effects of the Cr2O3 content of flux on the T[O] and the loss of Al and Si in steel was investigated, and the different results of reoxidation by reduction and decomposition were compared and discussed.

2. Experimental Procedures

A tube resistance furnace (Baotou Yunjie Furnace Ltd., Baotou, China) was used in the experiments to melt the steel and the tundish cover flux. The schematic diagram of the tube resistance furnace is shown in Figure 1. Four hundred grams of pure industrial iron (the composition is shown in Table 1) was put into a magnesia crucible (inner diameter: 42 mm, outside diameter: 51 mm, height: 101 mm, Boshan Refratory Material Ltd., Zibo, China) and then melted in an argon gas atmosphere at 1873 K (1600 °C). Al was added to the molten steel at a concentration of 0.2 mass% to make Al-killed steel. Then, after adjusting the molten steel temperature to 1923 K (1650 °C) and holding for 30 min, 20 g tundish cover flux of different Cr2O3 concentrations were added wrapped with iron foil. The crucible was held at 1923 K (1650 °C) for another 30 min to ensure a uniform covering of the molten steel by slag. The composition of the cover flux is presented in Table 2.
During the experiments, steel samples were taken as follows: (a) before adding the tundish cover flux, and (b) 5, 10, and 15 min after adding the tundish cover flux. Tundish cover flux samples were collected after the experiments.
Oxygen content was determined using the infrared method. The calculated aluminum, silicon, and chromium contents of the steel were determined using ICP-AES (NCS plasma 2000, NCS Testing Technology Co., Ltd., Beijing, China). FeO content in the tundish cover flux was analyzed using XRF (ZSX Primus II, Rigaku Corporation, Tokyo, Japan).

3. Results and Discussion

3.1. Reoxidation of Al-Killed Steel by Cr2O3

The changes in Al and T[O] content in Experiments 1, 2, and 3 are shown in Figure 2 and Figure 3. It can be seen that the Al content in the steel dropped sharply and the O content rose sharply when flux with Cr2O3 was added. This indicated that Cr2O3 in the tundish cover flux can be reduced by Al in the molten steel and lead to the reoxidation. The changes in Al and O contents mainly occurred in the first 5 min after the addition of the tundish cover flux. The reduction of Cr2O3 by Al occurred immediately after the addition of the tundish cover flux, and it was very quick. The increase in Cr2O3 from 5% to 10% showed no obvious difference on the Al and O contents. This indicates that for the slag-steel system used in this study, as the content of Cr2O3 increased, the transport of O from slag to steel showed no increase, and that the 5% Cr2O3 flux had already reached the limitation. After 5 min, T[O] began to drop sharply, suggesting that the reduction reaction was very fast and reached the equilibrium quickly. Thus, after the first 5 min of the reaction, Al2O3 inclusions floated up and were removed, resulting in the drop in T[O] [11]. However, compared with no Cr2O3 flux, the T[O] at 15 min was much higher in the other two experiments, indicating the reoxidation of steel by the Cr2O3 flux.
In order to determine the speed of the reduction reaction, another experiment with more frequent sampling was designed. The sampling time was 1, 2, 3, 4, and 5 min after the tundish cover flux was added, as shown in Figure 4. It can be seen that the reaction of Al reducing Cr2O3 occurred mainly within 2 min after adding the cover flux for the 5% Cr2O3 flux and within 3 min for the 10% flux. Moreover, the reaction rates were almost the same in the first minute after adding the flux, and the Cr content rose to 0.08% in the first minute for both. Between the first and second minute, the rate remained at 0.08%/min for the 5% Cr2O3 flux, while the 10% flux reached the highest rate of 0.16%/min. Then at 3 min, the reduction of Cr2O3 stopped for the 5% Cr2O3 flux, while the reduction of the 10% flux lasted another minute at a rate of 0.08%/min. The reduction reaction in this study happened at a very high rate and required little time. The increase of the equilibrium of Cr in steel was caused by the change in Cr2O3 content of the flux. The highest reaction rate occurred with the higher Cr2O3 concentration flux, and this may be explained by the doubling of the concentration of Cr2O3 in the slag being the driving force behind the transport of Cr2O3 from the slag to the interface [19].
The changes in Si and Cr in Experiments 1, 2, and 3 are shown in Figure 5 and Figure 6. It can be seen from Figure 5 that before the addition of flux with Cr2O3, the Si content in the steel increased first and then decreased, and after the flux was added, the Si content in the steel was significantly reduced. Furthermore, when adding flux with 10% Cr2O3, the Si content in the steel first decreased and then increased. It is known that Al in steel preferentially reacts with Cr2O3 in the cover flux. This means Cr2O3 is superior to SiO2 when reacting with Al in steel. Thus, it is assumed that Reaction (1) will be weakened by Reaction (2) [20,21] because of the limited oxygen supplement [17,18]. The dashed line in Figure 6 represents the ideal value of Cr content that can be reduced in the flux according to a mass balance calculation. It was found that almost all of the Cr2O3 in the cover flux was reduced, which made Cr close to the ideal value. When increasing the Cr2O3 content from 5% to 10%, there was even less Si due to the oxidation of the Si in the steel. This indicates that if not enough oxygen is provided by the flux, the reoxidation of molten steel by Cr2O3 will first involve Al, while the reaction will involve both Al and Si when sufficient oxygen is supplied by the flux.
4 [ A l ] + 3 ( S i O 2 ) 3 [ S i ] + 2 ( A l 2 O 3 )
[ A l ] + ( C r 2 O 3 ) [ C r ] + ( A l 2 O 3 )

3.2. Reoxidation of Non-Al Steel by Cr2O3

Compared to Experiments 2 and 3, no Al was added to the molten steel in Experiments 4 and 5. The changes in the Cr and Si contents in Experiments 4 and 5 are shown in Figure 7 and Figure 8, respectively. It can be seen from these figures that even if Al is not added to the steel, the Cr content in the steel will still rise dominantly. In Experiment 4, the Si content of the steel first increased and then decreased, which indicates that Cr2O3 and SiO2 in the tundish cover flux can transport oxygen to the steel by decomposition [22]. By comparing the magnitude of the rise, it can be seen that the decomposition of Cr2O3 dominates, and that the Si content in the steel begins to decrease due to the increase in the oxygen potential of the steel caused by the continued decomposition of Cr2O3, which causes the Si in the steel to be oxidized. The Si content in Experiment 5 first decreased and then remained unchanged. This was due to the Cr2O3 content in the tundish cover flux being higher, causing the decomposition of Cr2O3 to be very intense from the beginning. Therefore, the oxidation rate of the Si in the steel was greater than the decomposition rate of SiO2 in the tundish cover flux, which led to a decrease in the Si content of the steel. The subsequent decomposition of the Cr2O3 further reduced the Si content in the steel until it reached a very low value, after which the Cr in the steel began to be oxidized (as shown in Figure 8). Combining the change in Al content of the Experiment 3 steel and the stoichiometry of Reaction (2), it can be calculated that when Al is present in steel, the contribution of Al reduction to the increase in Cr content of steel is more than 90%, and that of Cr2O3 decomposition is less than 10%. Figure 9 and Figure 10 compare the T[O] changes with time between Experiments 2 and 4 and Experiments 3 and 5, respectively. It can be seen from Figure 9 and Figure 10 that the oxygen content in Experiments 4 and 5 was significantly greater than that in Experiments 2 and 3. The main reason for this was that Al was not added, and thus the deoxidation element was mainly Si in Experiments 4 and 5.

4. Conclusions

In this work, the unwanted reoxidation of steel by Cr2O3-bearing tundish cover flux was investigated through high temperature experiments. It was found that Cr2O3 can be reduced by Al to cause the reoxidation of steel. Moreover, as the Cr2O3 concentration increased, the reoxidation of the steel became more and more serious, and the Al loss also increased. It was also found that the reduction of Cr2O3 by Al mainly occurred within 2 to 3 min after the addition of the tundish cover flux with Cr2O3 concentrations of 5% and 10%. During the reduction of Cr2O3 by Al, the reaction rate reached a maximum value 2 min after the addition of the tundish cover flux with 10% Cr2O3, which may be related to kinetic conditions, and requires further investigation. Moreover, the reoxidation of molten steel by Cr2O3 caused the oxygen potential of the molten steel to rise, thereby suppressing the reoxidation of SiO2. It was concluded from two controlled experiments that Cr2O3 can also transport oxygen to the steel through decomposition. Furthermore, it was calculated that when Al is present in steel, more than 90% the reoxidation of Cr2O3 is caused by Al, and the rest is caused by decomposition.

Author Contributions

S.Y. and F.W. conceived and designed the experiments and interpreted the data; D.L. and W.L. wrote the paper; F.W. and J.L. analyzed the data and collected the literature; D.L. and F.W. performed the experiments.

Funding

This research was funded by National Natural Science Foundation of China, grant number 51734003 and 51674023.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Yoon, B.H.; Heo, K.H.; Kim, J.S.; Sohn, H.S. Improvement of steel cleanliness by controlling slag composition. Ironmak. Steelmak. 2002, 29, 214–217. [Google Scholar] [CrossRef]
  2. Deng, Z.; Zhu, M. A new double calcium treatment method for clean steel refining. Steel Res. Int. 2013, 84, 519–525. [Google Scholar] [CrossRef]
  3. Zhang, L.; Zhi, J.; Mei, F.; Zhu, L.; Jiang, X.; Shen, J.; Thomas, B.G. Basic oxygen furnace based steelmaking processes and cleanliness control at Baosteel. Ironmak. Steelmak. 2006, 33, 129–139. [Google Scholar] [CrossRef] [Green Version]
  4. Yan, P.; Van Ende, M.A.; Zinngrebe, E.; Laan, S.; Blanpain, B.; Guo, M. Interaction between steel and distinct gunning materials in the tundish. ISIJ Int. 2014, 54, 2551–2558. [Google Scholar] [CrossRef]
  5. Mantovani, M.C.; Moraes, L.R.; Silva, R.L.; Cabral, E.F.; Possente, E.A.; Barbosa, C.A.; Ramos, B.P. Interaction between molten steel and different kinds of MgO based tundish linings. Ironmak. Steelmak. 2013, 40, 319–325. [Google Scholar] [CrossRef]
  6. SchÜRmann, E.; Braun, U.; Pluschkell, W. Investigations on the equilibria between Al-Ca-O containing iron melts and CaO-Al2O3-FeOn slags. Steel Res. 1998, 69, 355–361. [Google Scholar] [CrossRef]
  7. Katsuhiro, S.; Yoshimasa, M. Reoxidation behavior of molten steel in tundish. ISIJ Int. 2000, 40, 40–47. [Google Scholar]
  8. Wang, C.; Verma, N.; Kwon, Y.; Tiekink, W.; Kikuchi, N.; Sridhar, S. A study on the transient inclusion evolution during reoxidation of a Fe–Al–Ti–O melt. ISIJ Int. 2011, 51, 375–381. [Google Scholar] [CrossRef]
  9. Yan, P.; Arnout, S.; Ende, M.A.V.; Zinngrebe, E.; Jones, T.; Blanpain, B.; Guo, M.X. Steel Reoxidation by Gunning Mass and Tundish Slag. Metall. Mater. Trans. B 2015, 46, 1242–1251. [Google Scholar] [CrossRef]
  10. Yang, G.; Wang, X.; Huang, F.; Wang, W.; Yin, Y.; Tang, C. Influence of reoxidation in tundish on inclusion for Ca-treated Al-killed steel. Steel Res. Int. 2014, 85, 784–792. [Google Scholar] [CrossRef]
  11. Kim, S.H.; Song, B. Thermodynamic aspects of steel reoxidation behavior by the ladle slag system of CaO-MgO-SiO2-Al2O3-FetO-MnO-P2O5. Metall. Mater. Trans. B 1999, 30, 435–442. [Google Scholar] [CrossRef]
  12. Brooks, G.A.; Rhamdhani, M.A.; Coley, K.S.; Subagyo; Pan, Y. Transient kinetics of slag metal reactions. Metall. Mater. Trans. B 2009, 40, 353–362. [Google Scholar] [CrossRef]
  13. Jiang, F.; Liu, Y.; Xie, Y.; Cheng, G. Reoxidation of Al-Killed Steel by Ca(OH)2 in the High Basicity Slag. Steel Res. Int. 2012, 83, 892–895. [Google Scholar] [CrossRef]
  14. Qin, Y.; Wang, X.; Li, L.; Huang, F. Effect of oxidizing slag on cleanliness of IF steel during ladle holding process. Steel Res. Int. 2015, 86, 1037–1045. [Google Scholar] [CrossRef]
  15. Ludlow, V.; Harris, B.; Riaz, S.; Normanton, A. Continuous casting mould powder and casting process interaction: Why powders do not always work as expected. Ironmak. Steelmak. 2005, 32, 120–126. [Google Scholar] [CrossRef]
  16. Sabioni, A.C.S.; Huntz, A.M.; Silva, F.D.; Jomard, F. Diffusion of iron in Cr2O3: Polycrystals and thin films. Mater. Sci. Eng. A 2005, 392, 254–261. [Google Scholar] [CrossRef]
  17. Pretorius, E.B.; Nunnington, R.C. Stainless steel slag fundamentals: From furnace to tundish. Ironmak. Steelmak. 2002, 29, 133–139. [Google Scholar] [CrossRef]
  18. Albertsson, G.; Teng, L.; Björkman, B.; Seetharaman, S.; Engström, F. Effect of low oxygen partial pressure on the chromium partition in CaO–MgO–SiO2–Cr2O3–Al2O3 synthetic slag at elevated temperatures. Steel Res. Int. 2013, 84, 670–679. [Google Scholar] [CrossRef]
  19. Jo, S.K.; Kim, S.H. Thermodynamic assessment of CaO-SiO2-Al2O3-MgO-Cr2O3-MnO-FetO slags for refining chromium-containing steels. Steel Res. Int. 2000, 71, 281–287. [Google Scholar] [CrossRef]
  20. Nakasuga, T.; Nakashima, K.; Mori, K. Recovery rate of chromium from stainless slag by iron melts. ISIJ Int. 2004, 44, 665–672. [Google Scholar] [CrossRef]
  21. Jiang, F.; Cheng, G.; Xie, Y.; Qian, G.; Rui, Q.; Song, Y. Reoxidation of Al-killed molten steel by Fe2O3 and Cr2O3 in the magnesia-chromite refractory. Steel Res. Int. 2013, 84, 1098–1103. [Google Scholar] [CrossRef]
  22. Park, D.C.; Jung, I.H.; Rhee, P.C.; Lee, H.G. Reoxidation of Al-Ti containing steels by CaO-Al2O3-MgO-SiO2 slag. ISIJ Int. 2004, 44, 1669–1678. [Google Scholar] [CrossRef]
Figure 1. Schematic diagram of experimental apparatus.
Figure 1. Schematic diagram of experimental apparatus.
Metals 09 00554 g001
Figure 2. Variations in Al concentrations of steel with time with different concentrations of Cr2O3 cover flux added.
Figure 2. Variations in Al concentrations of steel with time with different concentrations of Cr2O3 cover flux added.
Metals 09 00554 g002
Figure 3. Variations in total oxygen content (T[O]) of steel with different concentrations of Cr2O3 cover flux added.
Figure 3. Variations in total oxygen content (T[O]) of steel with different concentrations of Cr2O3 cover flux added.
Metals 09 00554 g003
Figure 4. Variations in Cr concentrations of steel with time for Experiments 2 and 3.
Figure 4. Variations in Cr concentrations of steel with time for Experiments 2 and 3.
Metals 09 00554 g004
Figure 5. Variations in Si concentrations of steel with time for Experiments 1, 2, and 3.
Figure 5. Variations in Si concentrations of steel with time for Experiments 1, 2, and 3.
Metals 09 00554 g005
Figure 6. Variations in Cr concentrations of steel with time for Experiments 2 and 3.
Figure 6. Variations in Cr concentrations of steel with time for Experiments 2 and 3.
Metals 09 00554 g006
Figure 7. Variations in Cr and Si concentrations of steel with time for Experiment 4: (a) Cr, (b) Si.
Figure 7. Variations in Cr and Si concentrations of steel with time for Experiment 4: (a) Cr, (b) Si.
Metals 09 00554 g007
Figure 8. Variations in Cr and Si concentrations of steel with time for Experiment 5: (a) [Cr], (b) [Si].
Figure 8. Variations in Cr and Si concentrations of steel with time for Experiment 5: (a) [Cr], (b) [Si].
Metals 09 00554 g008
Figure 9. Variations in T[O] of steel with time for Experiments 2 and 4.
Figure 9. Variations in T[O] of steel with time for Experiments 2 and 4.
Metals 09 00554 g009
Figure 10. Variation in T[O] of steel with time for Experiments 3 and 5.
Figure 10. Variation in T[O] of steel with time for Experiments 3 and 5.
Metals 09 00554 g010
Table 1. Chemical composition of YT01 (wt. %).
Table 1. Chemical composition of YT01 (wt. %).
CSiMnPSAlNiTiNCaFe
0.00160.00330.010.00530.00170.0030.00380.0010.002-99.95
Table 2. Compositions of slags (wt. %).
Table 2. Compositions of slags (wt. %).
ExperimentCaOAl2O3MgOSiO2Cr2O3
1503010100
2482710105
34624101010
4482710105
54624101010

Share and Cite

MDPI and ACS Style

Wang, F.; Liu, D.; Liu, W.; Yang, S.; Li, J. Reoxidation of Al-Killed Steel by Cr2O3 from Tundish Cover Flux. Metals 2019, 9, 554. https://doi.org/10.3390/met9050554

AMA Style

Wang F, Liu D, Liu W, Yang S, Li J. Reoxidation of Al-Killed Steel by Cr2O3 from Tundish Cover Flux. Metals. 2019; 9(5):554. https://doi.org/10.3390/met9050554

Chicago/Turabian Style

Wang, Feng, Daoxu Liu, Wei Liu, Shufeng Yang, and Jingshe Li. 2019. "Reoxidation of Al-Killed Steel by Cr2O3 from Tundish Cover Flux" Metals 9, no. 5: 554. https://doi.org/10.3390/met9050554

APA Style

Wang, F., Liu, D., Liu, W., Yang, S., & Li, J. (2019). Reoxidation of Al-Killed Steel by Cr2O3 from Tundish Cover Flux. Metals, 9(5), 554. https://doi.org/10.3390/met9050554

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop