1. Introduction
To achieve global greenhouse gas reduction targets, it is necessary to force a rapid transition from fossil fuels to a renewable-energy-based energy supply. However, when increasing the rate of utilization of renewable energies from wind and solar, their weather and seasonal dependencies do represent a technical challenge [
1,
2]. Their temporal variations in electricity production and consumption therefore raise the need for effective, affordable, and safe storage systems.
One emission-free opportunity to store surpluses of renewable electricity is to transform it into green hydrogen. To this aim, surplus renewable electrical energy can be utilized to split water into hydrogen and oxygen by an electrolyser. Green hydrogen can thus be stored and reused as soon as the energy demand increases. In a fuel cell or a hydrogen combustion engine connected to a generator, it can be converted back into electricity and heat. Hydrogen, as a cross-sector energy carrier, can also be used to decarbonize the transport and chemical sectors [
3,
4].
The storage of hydrogen at reasonable energy densities provides economic and technical challenges, because of its low density. Indeed, at atmospheric pressure conditions, hydrogen has a low energy density of 0.0033 kWh l
. The current state-of-the-art methodologies to increase its volumetric energy density are to compress or liquefy hydrogen. At compressions of 350 and 700 bar, a volumetric energy density of 0.792 and 1.32 kWh l
can be reached, respectively. The second form of hydrogen storage technology is in the form of liquefied hydrogen. To liquify hydrogen, it has to be cooled down to about −253
C, which represents the boiling point of hydrogen (−252.9
C or 20.3 K). The simplest liquefaction process is the so-called Linde cycle, in which pure hydrogen is compressed and cooled down, e.g., by liquid nitrogen. The compressed, cold, and non-condensed gas is forced to pass through an adiabatic throttling valve. The result is a saturated liquid–vapour mixture, which is typically formed at a temperature of −253
C. “The liquid hydrogen is collected as the desired product, and the vapor is routed through a heat exchanger to cool the compressed gas on its way to the throttling valve” [
5]. The obtained liquefied hydrogen is then stored in vacuum-insulated cryogenic tanks. In the case of liquid H
2, the volumetric storage density amounts to about 2.3 kWh l
[
4,
5,
6,
7,
8].
In addition to the above-mentioned physical storage technologies, hydrogen can also be chemically stored. Currently, a way to store hydrogen chemically in liquid form is to use liquid organic hydrogen carriers (LOHC). In the exothermic charging phase (hydrogenation), unsaturated organic compounds are hydrated at an elevated temperature and pressure. The endothermic dehydrogenation of the saturated, hydrogen-rich compounds (discharging) also requires an elevated temperature and a slightly increased pressure. Due to the low boiling point of LOHC materials, in most cases, the hydrogen has to be purified after dehydrogenation. In addition, typically, a catalyst is used in both charging and discharging. The process conditions and the storage density strongly depend on the used organic carrier material. In the case of N-ethylcarbazole [
9,
10], the hydrogenation typically takes places at a temperature between 130–160
C and a pressure of about 70 bar. To release the hydrogen, a temperature of 200–230
C and a slight overpressure is usually needed. With this N-ethylcarbazole, a storage density up to 5.8 wt.-% can be achieved [
11,
12].
Hydrogen can also be bonded onto solid materials. Due to their capability to strongly bind hydrogen, metals are often used as carrier materials (metal hydrides). In the exothermic charging phase, the adsorption of hydrogen into the metal lattice takes place. Due to the exothermic reaction, the temperature increases during charging. This shifts the reaction equilibrium towards higher pressures and leads to a decreased storage capacity unless the storage tank is cooled. The stored hydrogen can be released from the metal hydride during the desporption phase (endothermic discharging). The process temperature and pressure depend on the properties of the used metal/metal hydride, especially the absorption/desporption properties [
4,
13]. Metal hydrides such as magnesium hydride (MgH
2) can reach a high storage density of about 6 wt.-% (theoretically 7.6 wt.-%). A temperature of about 300
C and a pressure of 30 bar must be applied for charging, whereas the discharging temperature is about 350
C [
14].
A promising approach for hydrogen storage is represented by the thermochemical reduction and oxidation (redox) of metal oxides (M
O
)/metals (M). In such a hydrogen storage process, hydrogen is not chemically stored within the metal bulk. Instead, hydrogen reduces the metal oxide to metal and is oxidized to steam (H
2O). Due to its high availability, low cost, and thermodynamic behavior, iron is considered to be the most suitable oxide carrier material [
15]. The basis of the iron redox storage process was developed in the early 20th test century with the so-called “steam-iron” process, which was developed to produce hydrogen with a high purity and established on an industrial scale [
16,
17]. In the redox storage process, iron oxide/iron is repeatedly reduced and oxidized at atmospheric pressure conditions in a hydrogen and a steam gas stream, respectively. During the charging, iron oxide (magnetite, Fe
O
) is first reduced to wuestite (simplified as FeO). In the next step, it is further reduced to elemental iron (Fe). During this process, oxygen (O
) is removed from the iron oxide and reacts with hydrogen (H
2) to create steam (H
2O). The discharging represents the reverse process in a steam atmosphere, where iron is oxidized back to iron oxide (see Equations (
1) and (
2)). To obtain a higher reaction speed, the redox reaction takes place in a temperature range between 600 and 800
C. Due to the process temperature and an oxygen partial pressure (
) of less than 10
bar, hematite (Fe
O
) cannot be formed, i.e., Fe
3O
4 cannot be oxidized to Fe
2O
3 by water vapor [
18,
19,
20,
21,
22]. The absence of elementary hydrogen in the charged system represents a major safety advantage in comparison with the state-of-the-art technologies. In addition, redox storage systems can achieve a high volumetric energy density of about 2.8 kWh l
[
23].
However, the repeated redox reactions usually result in aging effects, such as the compaction of the porous storage material. As a consequence, the reactive surface area decreases, and the gas diffusion of the reacting gas slows down. This implies a reduction in the energy storage capacity and an increase in the reaction time, which is considered as a decrement in cycle stability. To improve the cycle stability, support materials can be added [
15,
24].
Several researchers in the field of chemical looping (CL) processes [
25,
26,
27], solid oxide fuel cells (SOFC), and oxide ceramic batteries (ROB) [
15,
28,
29] have shown that this aging can be reduced by the addition of supporting materials, e.g., silica, alumina, or calcium oxide. An improvement of both reaction kinetics and cycle stability during the redox storage process by adding different support materials was also proven in our previous work [
30]. Therein, the pure iron oxide sample already required nine times more time for the second reduction compared to the first reduction. Furthermore, only 35
of the initial redox potential could be achieved in the third oxidation cycle. In contrast, the sample with 10 wt.-% support material lost only 5% of its redox potential after nine redox cycles. In addition, two different sintering temperatures, namely 950 and 1100
C, were selected to investigate the influence of sintering temperature on the reaction kinetics of storage samples. The results showed that the reaction kinetics of samples with the higher sintering temperature of 1100
C was strongly reduced. Already in the first oxidation cycle, this sample was nine times slower than the sample sintered at 950
C. Furthermore, the redox reaction kinetics was measured at two constant temperatures (800 and 700
C). Compared to the results obtained at 700
C, the sample tested at 800
C exhibited faster aging, with the reaction time being more strongly increased with the number of redox cycles. For example, a factor of nine between the reaction time needed at 700
C and 800
C for the eighth oxidation was observed [
30].
This work represents a continuation of our previous publication [
30] and describes the manufacturing process of the redox pellets in a lab-scale pelletizing disk. First, we analyzed the influence of the disk inclination angle and the rotational speed on the pellet shape. The core of the experimental work is dedicated, however, to the investigation of the influence of the amount of added water during the pelletizing process on both cycle stability and structure of the pellets. Based on the results obtained in [
30], we used a temperature of 950
C for sintering the samples and an amount of 10 wt.-% support material. In [
30], a temperature of 800
C resulted in rapid aging during cycling. Thus, the effects of various parameters on cycle stability and reaction kinetics can be seen in less than nine cycles. Therefore, a cycle temperature of 800
C was chosen in this work. To investigate the structure of the samples before and after several redox cycles, micro-computed tomography scans have been conducted. In addition, the total open porosity of the samples has been investigated.
2. Material and Methods
As described before, the storage composites were manufactured with 90 wt.-% iron oxide (Fe
2O
3) and 10 wt.-% support material (cement). This ratio of 9:1 was chosen in order to maintain a high amount of the reactive storage material (iron oxide). In our previous publication [
30], we already presented the difference between having 0 wt.-% (pure iron oxide) and 10 wt.-% support material on the redox cycle stability.
2.1. Manufacturing Process
The manufacturing of the iron oxide pellets follows a three-stage process. In the first stage, iron oxide and the support material are dried at 105
C for 24 h and mixed in a double cone laboratory mixer (J. Engelsmann AG, Ludwigshafen, Germany) for 60 min at a rotation speed of 50 min
(100% power of the mixer). After this stage, the pelletizing disk (illustrated in
Figure 1) is applied to produce the so-called green pellets. Due to the rotation of the pelletizing disk and the alternating dosing of the powder mixture and water, agglomerated green pellets are formed. The internal structure of the pellets is affected by the way the pellets form, e.g., their coalescence, breakage, and abrasion transfer, which directly influences both the mechanical strength and the porosity of the pellets [
31,
32,
33].
The inclination angle
is the angle between the surface of the pelletizing disk and the horizontal. The literature recommends keeping this angle between about 40 and 60
[
31,
32,
34,
35].
In a dedicated investigation campaign on the influence of on the shape of the manufactured pellets, different angles were tested within the range between 30 and 65. It turned out that, with lower than 35, the pellets tended to have an oval shape. With between 50 and 60, almost spherical pellets could be formed. Further increasing above 60 led to increased material loss due to more ejection of the material from the pelletizing disk during rotation. Accordingly, was set to 52 during the manufacturing of all produced and tested samples in this work.
The optimum rotation speed
n of the pelletizing disk was defined by [
34,
35] as in the range between 0.6 to 0.75 of the critical speed
n. The latter can be obtained by setting equal the centrifugal and weight forces acting on the material during the rotation of the pelletizing disk. Solving the resulting equation for the rotational speed yields Equation (
3), in which
g represents the gravitational acceleration in m s
,
represents the inclination angle in
, and
D represents the diameter of the pelletizing disk in m.
The laboratory pelletizing disk has a diameter of 0.4 m. Considering the previously set inclination angle of 52, the optimum rotation speed n is estimated to be in the range between 35.6 and 44.5 min. During our preliminary pelletizing runs, the rotation speed was set between about 35 and 40 min. Within this range, no influence on the stability or on the shape of pellets could be identified.
As mentioned before, water dosing takes place alternately with the dosing powder mixture during the pelletizing process. In order to determine the amount of water that exists in the green pellets, the difference between the mass of the pellets immediately after being pelletized (wet green pellets) and after drying was measured. Thereby, the mass of the wet green pellets represents the 100% reference mass. The lowest amount of water by which pellets could still be formed was 18 wt.-%, while an amount of more than 33 wt.-% led to less stable and deformed wet pellets. Accordingly, pellets with a water amount between 18 and 33 wt.-% were produced and investigated.
The last manufacturing step is the sintering of the dried samples to increase their mechanical strength. The sintering temperature was selected to be higher than the maximum process temperature during the redox reactions in order to minimize the possibility of having the samples being sintered during the redox reactions. According to the results of our previous investigations [
30], the sintering temperature was set to 950
C.
In
Table 1, the abbreviations of the produced and investigated samples are listed, along with the water content (wc) and the sample mass after sintering, which represent the initial mass of the pellets before the first reduction reaction (
m).
2.2. Experimental Setup
Figure 2 illustrates the experimental setup for cycling the produced storage pellets and investigating their kinetic performance during the repeated redox reactions. The core component of the setup was the simultaneous thermal analyzer (STA 449 Jupiter F3, Netzsch, Selb, Germany). The supply of hydrogen and nitrogen, as a carrier gas, could be regulated in the range of 0 to 250 mL min
± 0.5% through a mass flow control (MFC) device for each gas. Moreover, a steam generator (aSTEAM DV2, aDROP) was applied to produce the required steam during the oxidation reaction. The amount of steam could be set within a range from 0 to 25 g h
with an accuracy of 1%. The accuracy of the weight measurement by the STA device amounted to ±0.1
g, while the temperature was adjustable within a tolerance limit of ±0.3
C. All devices were connected to a computer for process control as well as data monitoring and recording.
The redox reactions were conducted with the use of a thermogravimetric (TG) analyzer device in an atmosphere of 50% nitrogen and 50% hydrogen (reduction) or 50% steam (oxidation). In order to achieve fast aging in the investigated samples (in less than nine redox cycles), the TG measurements were carried out at 800
C [
30].
To analyze the measured reaction kinetics, the conversion rate for the reduction (
(
t)) and oxidation (
(
t)) was determined by Equations (
4) and (
5). Thereby, the time-dependent mass change of the sample (
m(
t)) was divided by the maximum mass change after a complete conversion (
m−
m). The maximum mass (
m) represents the mass of the sample in the fully oxidized state (Fe
3O
4), considering the amount of the supporting material, while the minimum mass (
m) is the wight of the pellet in its completely reduced state (Fe). Under the tested process conditions (800
C,
< 10
bar), hematite is not stable. This implies a difference between initial sample mass and measured maximum mass of about 3% [
29,
30]. A fixed data point at
= 0.8 and
= 0.8 was chosen to compare the kinetic behavior of the tested storage samples.
Furthermore, the structure of the cycled storage samples was investigated in a micro-computed tomography facility (CT; Phoenix V|tome|x s240/180 from Waygate Technologies Digital Solutions Baker Hughes, Houston, TX, USA). The voxel size for the analysis was about 8 m, and the number of images was 3000. The scanning parameters for the CT scans were as follows: 140–160 kV voltage, 50–60 A current, and 0.1 mm Cu filter. Reconstructed volumes were processed using the manufacturer’s software phoenix datos|x 2 reconstruction 2.4.0. The software VG Studio Max 2022.2 from Volume Graphics was used to determine the parameters of the 3D images, including their surface area and volume.
To measure the open porosity of the samples (
), the volume of void space (
V) was determined and divided by the total volume (
V; see Equation (
6)). To this aim, the density (
) of each sample was measured by a He-pycnometer (Pynomatic ATC, Thermo Fisher Scientific) with an accuracy of 0.01%. For the density measurements, the maximum standard deviation was about 0.3%. The total volume of the sample was estimated by the data from the
CT scans.
3. Results and Discussion
As mentioned before, the storage samples were manufactured by varying the amount of added water between wc = 18 and 33 wt.-%. After sintering these samples, their reaction kinetics upon carrying out several redox cycles were measured by the TG analyzer. Moreover, the macroscopic structure of the samples was investigated using CT scans, and their open porosity was measured. The obtained results are presented and discussed in the following subsections.
3.1. Thermogravimetric Analysis
Table 2 summarizes the kinetic results, which are discussed in the following paragraphs, and presents the required time for the investigated samples to reach a conversion rate of
and
= 0.8 during reduction and oxidation.
Figure 3 presents the time-dependent conversion rate (
(
t)) for the reduction and oxidation (
Figure 3a,b) reactions during the second redox cycle.
During the reduction, sample P9, with the highest water content (wc = 33 wt.-%), achieved the highest kinetic performance, as the conversion rate of = 0.8 was reached after 14 min, while samples P4 (wc = 25 wt.-%) and P7 (wc = 27 wt.-%) needed almost two more minutes to reach the same conversion rate. The samples with the lowest water contents, P1 (wc = 18 wt.-%) and P3 (wc = 21 wt.-%), required as much as 18 min to achieve a conversion level of 80%.
A similar trend was observed during the oxidation. It can be first concluded that the oxidation reactions are notably faster compared to the reduction reactions. Indeed, sample P9 reached the 80% level after about 8 min, while samples P4 and P7 achieved the same conversion rate about 1 min later. Finally, the samples with the lowest water content (P1, P3) needed two minutes more to make it to = 0.8.
The results of the second redox cycle indicate that a higher water content during the pelletizing process leads to faster reaction kinetics. To determine the influence of the water content on the cycle stability, the conversion rate over several cycles was investigated. In the following discussions, the investigated samples were split into three categories depending on their water content, namely wc
≤ 20 wt.-% (
Figure 4a,b), wc
= 26–27 wt.-% (
Figure 4c,d), and wc
= 33 wt.-% (
Figure 4e,f).
Figure 4a,b illustrates the time-dependent conversion rates of samples P1 and P2, which had the lowest water content of equal to or less than 20 wt.-% (wc
). It is clear that the reduction reaction kinetics strongly decreases with the number of cycles (cf.
= 0.8:
t = 18 min,
t ≈ 21 min, and
t ≈ 25 min). A similar behavior can be observed during the oxidation reactions (cf.
= 0.8:
t ≈ 10 min,
t ≈ 14 min, and
t ≈ 18 min). It is also observable that samples P1 and P2 cannot reach the complete oxidation conversion of
= 1 in 60 min. In addition, the reaction kinetics of both samples P1 and P2 during the sixth redox cycle is clearly slower than those of the samples with higher water contents during the ninth redox cycle (cf.
= 0.8:
t ≈ 15 min, and
t ≈ 13 min). Thus, no further cycles have been measured for P1 and P2.
In
Figure 4c,d, the time-dependent conversion rates for the reduction and oxidation reactions of the samples P5, P6, and P7 (wc
) during the second, fifth, and ninth cycles are illustrated. For those samples, the conversion rates during the second and the fifth reduction cycles are approximately the same (
= 0.8:
t ≈
t = 16 min). In case of sample P5,
= 0.8 can be reached about 1 min faster during the second cycle. Between the fifth and the ninth cycle, the time needed for
to reach 0.8 increases by 7 min. Additionally, for the samples P5, P6, and P7, the kinetics of the oxidation reactions were notably faster compared to the reduction reactions. Strictly speaking, the required time for the oxidation to reach
= 0.8 during the second, fifth, and ninth oxidation cycles is about 8 min, 10 min and 15 min, respectively.
In comparison to samples with the water contents wc
and wc
, the conversion rates of samples P8, P9, and P10 (wc
in
Figure 4e,f) exhibit a smaller decrease over the nine redox cycles, which is attributed to less aging effects. During the second redox cycle, the average reaction time to reach a conversion level of 80% is about 15 min for reduction and 8 min for oxidation, respectively. The time required to achieve an 80% conversion rate during the fifth redox cycle of the reaction is about 1 min longer for the reduction and 2 min longer for the oxidation reactions. Sample P10 is, on average, 3 min slower than P8 and P9 (cf.
= 0.8:
t ≈ 22 min). Additionally, sample P10 cannot reach the complete conversion to
= 1 in 60 min. However, during the ninth oxidation, sample P10 shows a comparable reaction behavior to P8 and P9 (
= 0.8:
t ≈ 14 min,
t ≈ 14 min, and
t ≈ 12 min).
The discussed results so far indicate that the samples with a higher water content (wc
33 wt.-%) have a higher cycle stability. To illustrate this conclusion more clearly, the conversion rates of sample P3 (wc = 21 wt.-%), P6 (wc = 27 wt.-%), P2 (wc = 20 wt.-%), and P9 (wc = 33 wt.-%) are compared in
Figure 5.
In the following, the relative increase in reaction time during the redox cycles (illustrated in
Figure 5) is discussed. Concerning sample P2, the time needed to reach
= 0.8 increases from the second to the sixth cycle by 40% during the reduction reaction and 90% during the oxidation reaction. In contrast, sample P3 showed a higher cycle stability, with
t ≈ 20 min and
t ≈ 13 min necessary to reach
= 0.8 during the reduction and oxidation reactions, respectively. This is equivalent to a decrement of 10% in the reduction and 30% in the oxidation kinetics between the second and the sixth cycle. Between the second and the ninth cycle, the aging effect becomes more obvious as the decrement in the reduction kinetics amounts to 50% (
t ≈ 27 min), while the oxidation kinetics are reduced by 80% (
t ≈ 17 min). In comparison, sample P6, with the medium water content of 27 wt.-%, reaches
= 0.8 in about 23 min during the 9th reduction and 16 min during the 9th oxidation. Compared with the second redox cycle, a decrement in the kinetic performance of 50% for the reduction and 90% for the oxidation reaction can be determined.
Indeed, sample P9, with the highest water content (33 wt.-%), showed the highest reduction and oxidation kinetics and cycle stability (cf. t ≈ 14 min, t ≈ 18 min; t ≈ 8 min, t ≈ 14 min). This implies an increase in the reaction time of 20% and 60% regarding the second and ninth reduction and oxidation cycles, respectively.
The rather large difference in the performance of sample P3 with 21 wt.-% compared to sample P2 with 20 wt.-% of water content indicates that the water content might have a dominant effect on the reaction kinetics and the cycle stability as the key performance indicators (KPIs). However, other factors, such as the sample structure, may also influence both KPIs. Accordingly, further investigations regarding the influence of the micro structure of the investigated samples on the reaction kinetics and cycle stability were carried out. The results of theses investigations are documented and discussed in the following section.
3.2. Structural Investigations
In the flowing
CT scans, the areas with no storage material (only air) are marked in black. Gray areas represent the material of the storage samples. The brightness of the parts is an indicator of their density [
36]. For iron oxide samples, a higher brightness can be attributed to areas with a more dense structure or material with a higher density, e.g., iron compared to iron oxide particles. Due to the fully oxidized state of the investigated samples, it is assumed that areas with higher brightness are areas with a more dense structure. Through
CT scans, the internal macroscopic structure of the samples can be obtained without the necessity of destroying them, which makes it possible to study the sample structure before and after cycling.
In
Figure 6, the
CT images of the samples with the lowest water contents (≤21 wt.-%), namely P1 and P2 after the sixth redox cycle, as well as P3 after the ninth cycle, are presented. In particular, the internal structure of sample P1 (wc = 18 wt.-%;
Figure 6a) exhibits separated spherical areas with material accumulations (≈ 0.1–1.8 mm) and cavities in between. On the other hand, the outermost shell appears as a continuous dense layer. Sample P2 shows also an agglomerated internal structure (
Figure 6b). In contrast to sample P1, a higher amount of smaller agglomerates with a diameter of about 0.3 mm can be recognized. Accumulations up to about 1.3 mm can also be observed. Compared to sample P1 and P2, sample P3 shows less and smaller material accumulations ≤ 0.3 mm, which appear around a porous core (see
Figure 6c). However, a dense exterior shell also forms after the ninth redox cycle.
The obtained results indicate that the agglomerated structure and the formation of an outward dense layer lead to the presented slowdown of the reaction kinetics. This is caused by the correlated less effective gas transport of H
2 or H
2O towards the sample structure during the reduction and oxidation reactions, respectively. These results are in line with our previously published results [
30] as well as [
15,
37].
To verify the suggestion of a structure with a higher density, the open porosity
of the investigated samples was determined according to Equation (
6). This measuring campaign resulted in an open porosity of about 23% (P1: wc = 18 wt.-%), 25% (P2: wc = 20 wt.-%) and 31% (P3: wc = 21 wt.-%). Compared to the open porosity of the other samples, the named three samples acquire the lowest porosities (cf.
Table 3). Furthermore, sample P3 after the ninth redox cycle does record a higher porosity than samples P1 and P2 after six cycles. This is consistent with the observed higher kinetics and cycle stability of sample P3. The results of the
CT scans in combination with the determined porosity indicate that the cavities inside the internal structure of samples P1 and P2 are mostly closed and barely contribute to the enhancement of the reaction kinetics [
38].
Figure 7 illustrates the
CT images of the samples P5 and P7 after nine redox cycles. The structure also shows internal cracks and the formation of an external shell with a higher density compared to the interior. However, the storage material of the samples is nearly homogeneously distributed without agglomerations, such as in sample P1.
The average porosity is about 35% (cf.
Table 3). This suggests that increasing the added water amount during the pelletizing process from about 20 to 27 wt.-% does have a positive effect on the sample’s structure.
The
CT images of samples P8, P9, and P10 with the highest water contents of 33 wt.-% (see
Figure 8) display a homogeneous distribution of storage material and pores. Furthermore, the formation of cracks can be seen, which extend from the outside shell towards the internal structure. Compared to the other investigated samples in
Table 3, samples P8, P9, and P10 reach the highest porosity, with an average of about 44%. The visualized internal structure of the samples along with the higher total porosities indicate an increased specific reaction surface, which positively affect the reaction kinetics upon improving the gas transport rates.
In addition to the
CT scans after six or nine cycles, the structures of the samples P2, P5, and P8 were investigated right after the sintering phase and before the start of the redox cycling tests. The obtained results are depicted in (
Figure 9).
In
Figure 9a, the formation of a dense outer shell and the agglomerated internal structure of sample P2 is already visible. This indicates that these pellets were formed primarily by the coalescence of compressed agglomerates. A reason for this could be the small amount of added water, since agglomerates with a low moisture content are comparatively more brittle, leading to more frequent breakage and abrasion [
32,
34].
With further cycling, the cavities in the internal structure expand (cf.
Figure 6b and
Figure 9a), which is assumed to take place because of the increasing sintering effects of iron/iron oxide during the repeated redox cycles.
Figure 9b demonstrates that an increased water content has a positive effect on the distribution of storage material and small pores during the pelletizing process.
Figure 9c illustrates the initial structure of sample P8 with the highest added water amount of 33 wt.-%. Compared to sample P2 and P5, sample P8 shows a much higher porosity, most specifically in the outermost layers. The results indicate that a higher open porosity can be generated by adding a larger amount of water during the pelletizing process.
Indeed, all investigated samples have shown visible aging effects. Compared to the CT images before the redox cycling, a more compact structure is formed after few redox cycles, especially in the outermost layers. The sintering effect due to the execution of the redox cycles at 800 C can also be determined when comparing the sample volume of the initial (V) and the re-oxidized (V) samples. In fact, the volume of sample P2 is reduced from V = 630 mm down to V = 387 mm, while the sample P5 contracts from V = 1064 mm to V = 452 mm. Considering the sample P8, it is reduced from V = 1180 mm to V = 571 mm after nine redox cycles.
Moreover, it is noticeable that the cracks within the sample structure are mostly in the shape of a shell, which can be attributed to the step-wise agglomeration of the storage material in layers during the applied pelletizing process.
The obtained results indicate that increasing the amount of added water during the pelletizing process results in a more homogeneous distribution and a higher open porosity of the produced pellet samples. This promotes faster reaction kinetics and an increased gas permeability [
30,
39,
40].
The correlated higher reaction kinetics and cycle stability of the samples with higher water contents pave the way to more dedicated developments, in which the number of redox cycles over which the samples should remain stable must be increased to guarantee a promising practical application as a hydrogen storage material. In addition, the change in the microscopic structure and chemical phase composition due to the repeated reduction and oxidation of iron storage masses will be investigated in more detail. Furthermore, the mechanical stability of the samples in bulk will be tested as a prerequisite for studying the reaction kinetics of the storage sample in a lab-scaled iron redox reactor. The results of these development steps will be the subject of our subsequent publications.
4. Conclusions
In this work, the influence of the amount of water added during the pelletizing process on the redox cycle stability and on the reaction kinetics of iron oxide pellets was studied. To this aim, the water content was varied between wc = 18 to 33 wt.-%. After sintering at 950 C, the reaction kinetics of the repeated reduction and oxidation at 800 C was investigated. Furthermore, the micro-structure and the open porosity of the produced pellet samples were determined.
The obtained results indicate a direct correlation between the added water amount, the structure of the pellets, and their reaction kinetics. Pellets with a higher water content tend to have faster kinetics and a higher cycle stability. Considering the sixth redox cycle, sample P1 with the lowest water content of 18 wt.-% needed about 26 min and 19 min to reach a conversion rate of = 0.8 during the reduction and oxidation, respectively. In contrast, sample P10 with the highest water content of 33 wt.-% could achieve a similar conversion rate after only 18 min (reduction) and 13 min (oxidation) in the ninth cycle.
Micro-computed tomography scans before and after the redox cycling showed that samples with lower water contents are subjected to a more agglomerated internal structure with a dense outermost shell. In addition, sample P1 (wc = 18 wt.-%) showed the lowest open porosity of ≈ 23%, compared to samples P8 and P10 (wc = 33 wt.-%) with the highest open porosities of ≈ 46% and ≈ 45%, respectively. Furthermore, increasing the added water content resulted in a more homogeneously distributed pore structure. A homogeneous distributed pore structure and a higher porosity are associated with higher reaction kinetics and better cycle stability due to an increased specific reaction surface and gas permeability. Indeed, more development work is needed to approve the cycle stability over more redox cycles and to investigate the mechanical stability of the iron oxide pellets.