1. Introduction
Reinforced concrete has been a go-to for infrastructure and housing projects in the last century and is paramount for our developed society. Most of our infrastructure has been built in the past 50 years with a service life of 50–100 years [
1], creating a demand for their monitoring. Concrete on its own is capable of withstanding large compressing forces. However, it requires embedded steel beams to minimize cracking under tensile forces [
2].
The properties of concrete are established early on during the hydration of cement and depend on the water-to-cement ratio (
w/c), the type of cement used, the added aggregates or pozzolans and the curing methods employed [
3,
4]. Cement curing has five different stages: Mixing, dormancy, hardening, cooling and densification [
3]. In mixing, the dissolution of cement grains occurs in a brief exothermic reaction, during which the formation of ettringite restricts the further dissolution of cement grains. Thus, cement advances to the next phase of hydration—dormancy. This lasts between two to four hours, whilst water begins to be saturated with calcium and hydroxide ions. Eventually, this triggers the formation of calcium–silicate–hydrate (C-S-H) and calcium hydroxide (CH) in an exothermic reaction, causing the cement to become stiffer—hardening. These hydration products, C-S-H and CH, begin to limit the dissolution of cement, which lowers its temperature—cooling. Over time undissolved cement continues to hydrate, leading to its densification.
Porosity is heavily dependent on the
w/c. The same volume of cement powder generates a larger volume of cement paste the more water is used during mixing. However, it also results in a more porous material [
5]. Hence, a higher
w/c equates to a more porous paste, better capillary continuity and better overall cement permeability. For 0.40, 0.50, 0.60 and 0.70
w/c the expected porosity is 11%, 22%, 30% and 37%, respectively [
5]. The interlink between pores is not static, e.g., while the capillaries from a 0.45
w/c paste are expected to become discontinuous after seven days, it will take six months for the same to happen for a 0.60
w/c paste [
3].
Over time, cement’s porosity as well as the formation of small (30–50 μm) to large (>150 μm) cracks lead the way for the decaying of reinforced concrete structures (RCS) [
6]. Carbonation [
7] and chloride ion ingress [
8] destroy the passivation of the embedded steel beams while freeze-thaw [
9] and alkali-silica reaction [
10] negatively affect the cement paste.
Monitoring RCS is fundamental to prevent catastrophic failures and optimize their expensive repair. Optical fiber sensors were applied for this purpose because they are light, small, resistant and impervious to electromagnetic interference. They were used to measure temperature, strain and relative humidity using fiber Bragg gratings and/or long period fiber gratings [
11,
12,
13,
14]. pH measurements, indicative of carbonation, also proved fruitful [
15], making use of multimode fibers with pH sensitive polymers in their tip. Non-reversible optical fiber sensors were, also, produced for the monitoring of chloride ion ingress [
16,
17].
The availability of water is a key factor in the life cycle of cement, being the driving force of curing [
3], self-healing [
18] and a requirement concerning many of its decay mechanisms [
19]. In the present work, a single fiber reflectance spectrometer [
20] is proposed for the monitoring of water in cement curing and, once hardened, in the pores. Thus, we present a solution that allows the monitoring of cement’s full life cycle, which could prove valuable for the monitoring of RCS given that cement is one of its major constituents. We found single fiber reflectance spectroscopy to be successful in achieving the capillary coefficient of cement paste, a parameter through which the durability of cement can be estimated. These values were compared to the sorptivity and the porosity of the samples achieved through gravimetric measurements of water uptake and using scanning electron microscope, respectively, as seen in the following sections.
1.1. Single Fiber Reflectance Spectroscopy
In single fiber reflectance spectroscopy, light from a broad-band light source travels through the first branch of a bundle of two multimode fibers into a larger, sensing, multimode fiber. At the distal end of the sensing fiber, light is reflected back into the bundle, being measured by a spectrometer at the end of the second multimode fiber,
Figure 1a.
The reflection of light on the fiber tip is dependent on the refractive index (RI) of the fiber core (n
c = 1.4584 at 589.29 nm) and the RI of the external medium (n
p), Equation (1). For cement, n
p depends on how the pores are filled; if they are filled with water n
p is 1.3325; if they have no water at all, n
p will be 1.0. Generally, the RI will be in between these two values with some pores being filled, some being partially filled and the others empty [
21]. Due to the durability of cement, we consider that throughout a single measurement of water uptake, there will not be enough change concerning the cement to introduce noise into the monitoring of the capillary coefficient, whether that be through changes in the refractive index of its constituents or micro/macro-mechanical changes in the cement matrix.
This type of sensor is typically used to study changes in the spectrum of reflected light after its interaction with a sample, e.g., human skin [
22]. Here it is employed for the monitoring of water during cement curing, and, once hardened, in the cement paste. The porosity of cement paste influences the sensor’s sensitivity, with changes in porosity and pore connectivity equating changes in the sensor’s response.
1.2. Capillary Coefficient and Sorptivity
The capillary coefficient is a parameter that defines the rate of water uptake of a porous material and has been used as a measure of concrete durability [
23,
24]. To achieve this value a water absorption test is conducted where the bottom face of a concrete sample is under water and the upper face is in open air. The sides of the sample should be impermeable, thus allowing water to travel in a single direction, vertically. The driving force of capillary absorption is surface tension on fine pores (10 nm–10 μm), which matches the gravity forces of water. The one-dimensional movement of water is described by the Lucas–Washburn equation [
25]:
where h is the height reached by water, k is the capillary coefficient and t is the time. If one measures the volume of water that is being absorbed by the sample per unit of cross section, the water absorption is described by a similar formula, Equation (3) [
25]:
where I is the volume of absorbed water per unit of cross section, S is the sorptivity and t is the time.
Figure 1b displays how the samples containing a sensing multimode fiber were set for the measuring of sorptivity. Measuring k requires robust technologies, such as: Neutron radiography, nuclear magnetic resonance, gamma ray or X-ray computed tomography. This makes measuring S more attractive, since it is achieved through gravimetric measurements, even though the relationship between k and concrete’s durability is easier to attain [
26]. Both k and S have the same dimensions
[
], but they are not the same thing, with sorptivity containing information of concrete’s porosity (φ), Equation (4) [
26]. This equation opens the possibility to cross-reference capillary coefficient values with sorptivity values provided the
w/c ratio or the porosity of cement are known. These measurements can also be employed to cement pastes, as seen below.
In these tests it should be assumed that concrete is fully matured, meaning that only a small amount of water will be lost to chemical interactions with the cement paste [
23]. If this is not the case, other solutions that do not interact with cement could be used: Water saturated with Ca(OH)
2 [
24].
1.3. Scanning Electron Microscope
In the Scanning Electron Microscope (SEM) a beam of electrons undergoes a series of inelastic and elastic collisions which generate a signal that is detected and transformed into an image [
27]. In inelastic collisions, incident electrons knock out electrons of atoms in the sample, with the latter having lower energy. The signal from these low energy electrons constitutes the secondary electrons (SE) where only those from the near surface can escape, making it a high-resolution method for the measurement of the topography of the sample. In SE, the edges from a rough surface are brighter since they have more area from which electrons can escape.
Electrons that experience elastic collisions, backscattered electrons (BSE), retain their energy, thus they can escape from greater depths of the sample. The brightness from these images is related to the atomic number of the atoms in the sample. A higher atomic number leads to more collisions, hence a brighter spot. In a polished piece of cement, anhydrous cement appears brightest, followed by calcium hydroxide, calcium silicate hydrate and ettringite. Porosity lowers the atomic size within a phase, making it darker, with voids being black [
28].
3. Results
A single fiber reflectance spectrometer was used to monitor both the cure and wet/dry cycles of a cement paste sample of 0.5
w/c, sample B. The data acquisition lasted for fifteen days of continuous monitoring (see
Figure 6a) with another wet cycle being done a week later (see
Figure 6b), resulting in a total of eighteen days of observation. The curing of samples A, D and E with, respectively, 0.45, 0.55 and 0.60
w/c were monitored. Samples C and F with
w/c of 0.55 and 0.60 were submerged in water once to estimate the capillary coefficient from the water ingress.
From all the data acquired, the worst signal-to-noise ratio was 18, measured in the “wet” cycle of the samples C and F with 0.55 and 0.60
w/c,
Table 2. The low SNR of samples C and F can be explained by the non-optimization of the integration time for these measurements. The small integration time employed led to a small amount of signal reaching the spectrometer, riddling the data with noise.
3.1. Cure
According to
Figure 6c, concerning the curing of sample B, in the first 3 h there was a slight decrease in reflected light followed by a step increase from 3 to 6 h, point 1 of the figure. The step increase is also found in samples A, D and E in
Figure 7a and happens at the same time as the samples become visibly stiffer (
Figure 7d), indicating that the cement is transitioning from dormancy to its hardening phase. This is corroborated by SEM images acquired through SE from cement extracted during the curing of sample D,
Figure 7b–d. The SEM images of
Figure 7b,c have particles of cement with little to no formations of C-S-H at the surface, in stark contrast with
Figure 7d where the particle’s surface is more uneven. This time frame agrees with the two to four hours the dormancy phase is expected to last [
3].
The depletion of water in the fiber vicinity is temporarily reversed between 6 and 16 h in sample B,
Figure 6c. This could be due to water bleeding, a common feature during cement hydration, where large aggregates could accumulate water underneath them [
5]. This did not happen for samples A and E, whose intensity kept increasing, indicating further depletion of water. The excess water ended up being used by 41 h and water was added externally to aid the curing of cement with it remaining saturated for the remainder of the curing. In this saturated state, the normalized intensity is between 44 and 59%. At the end of the seven days (168 h), sample B was removed from the mold and left to dry, leading to a fast increase in reflected light intensity,
Figure 6a.
3.2. Wet/Dry Cycles
Once sample B was dry, it underwent wet/dry cycles to access the sensor’s response. It is clear in
Figure 6a,b that the wet cycles led to a reduction in the reflected light on the fiber tip, while the dry cycles led to an increase. The signal for saturated cement paste went from 44% at the end of the curing, to 56% in the first wet cycle and 68% in the second. For the dry cycle, the planes were at 98%, 92% and 100%. Two separate zones of reflected light intensity, one for mostly dry cement paste and another for wet cement paste were found, divided by the dashed redline of
Figure 6a.
Plotting the wet cycles as the height of water on the fiber tip, deduced from Equation (5), over the square root of time (
Figure 8a) and applying the corrections of
Figure 4d to the slope values, the capillary coefficient of the sample B was estimated,
Figure 8b. There is a decrease of the capillary coefficient between the first and the other two measurements, decreasing from 1.373 ± 0.01 mm/√h to 0.668 ± 0.002 mm/√h (average of the last two measurements).
The same procedure was done for the samples of cement paste C and F (
Figure 9a,b); as expected, an increase in capillary coefficient with an increase in
w/c was found, with values ranging from 1.771 ± 0.05 mm/√h to 6.360 ± 0.27 mm/√h for 0.55 and 0.60
w/c respectively,
Figure 9c.
3.3. Samples’ Sorptivity and Porosity
Gravimetric water absorption tests (
Figure 1b) were conducted to estimate the sorptivity value of samples B, C and F, with the obtained data in
Figure 10a. An increase in sorptivity was found the higher the
w/c with samples B (0.5
w/c), C (0.55
w/c) and F (0.60
w/c) having, respectively, sorptivity values of 0.131 ± 0.004 mm/√h, 0.505 ± 0.080 mm/√h and 2.290 ± 0.110 mm/√h.
Using the corrected values of the capillary coefficient and these values of sorptivity, Equation (4) is used to achieve the porosity of the samples used: 19.4 ± 0.6 % (sample B), 28.5 ± 4.8% (sample C) and 35.9 ± 9.8 % (sample F). These porosity values are close to the expected ones [
5], meaning that both the capillary coefficients from the single fiber reflectance spectrometer and the sorptivity values are in agreement.
BSE images from SEM were used to confirm the porosity achieved previously. These images will not yield the true porosity of the samples, but they can be used to compare the porosity between samples [
27].
Figure 10b has BSE images that went through a Gaussian filter on the left and their porosity, pixels with brightness below 30 in 255, on the right. It is possible to see from this image alone that there is an increase in porosity with an increasing
w/c. The histograms of the scale of grays for the images taken, five for each sample, can be seen in
Figure 10c along with the chosen threshold (30/255).
Figure 10d compares the porosity achieved through the relationship of Equation (4) and the one measured through SEM. Both curves are extremely similar, having between them a Pearson product–moment correlation coefficient (ρ) of 0.99998.
4. Discussion
Monitoring the availability and the mobility of water in concrete is key in estimating the decaying rate of cement paste; thus, this has been one of the objectives of many previous studies [
19]. In this work the use of single fiber reflectance spectroscopy achieved valuable information for both the curing of the cement as well as for hardened cement paste. It is important to note that in single fiber reflectance spectroscopy water ought to be transparent to the chosen wavelength of the light source. Thus, theoretically, the measured light intensity should be only sensitive to changes in the refractive index at the fiber tip. This way, light that goes out of the fiber and bounces back into it from the cement paste is the same regardless of the portion of fiber tip in contact with water. Water is highly transparent to visible light, which broadens the pool of available light sources. A wavelength of 370 nm was chosen due to convenience and, despite the absorption at this wavelength being higher—1.37 × 10
−3 cm
−1—than the optimum value of 2.5 × 10
−4 cm
−1, at 475 nm [
31], the loss of signal at the vicinity of the fiber tip due to water absorption remained negligible: Considering an extreme case where there is gap of 0.5 cm between the fiber tip and the cement paste, the loss of signal due to water absorption would require an SNR of 730 to be measured. Even in this case, that value is greater than any other SNR achieved in this study,
Table 2.
This sensor was sensitive to the hardening of different samples of cement paste (
Figure 7a–d), a key mark of the cement’s hydration. At point 3 of
Figure 6c, an excessive amount of water was added, which left the sample saturated. Since the addition of water during the cement’s curing is one of the methods used to improve cement paste’s cohesion [
3], the monitoring of this procedure is an important feature of this sensor. This could enable the user to fine tune the amount of water and the timing of its addition.
The sensor can monitor the absorption of water in cement paste as seen in
Figure 6a,b, but its information on the amount of water in cement paste shows strong variability for sample B: Saturated cement paste had its signal change from 44% to 68%, while dry cement paste was between 92% and 100%. This is to be expected since over the lifetime of cement paste there are changes in the pore size and connectivity that may lead to the trapping of water and/or air in the cement paste that is in the vicinity of the fiber tip. This is especially important to consider during these measurements since we used recently made cement paste. There is, still, cement to be hydrated and for 0.50
w/c cement paste the breakage of pore connectivity is expected within the first 28 days [
3]. This variability is, also, to be expected in fully matured paste, since the cement paste that surrounds large aggregates (interfacial transition zones), in this case a multimode optical fiber, is different from the bulk cement paste: It is more brittle and with larger pores [
5]. Still, it is reasonable to assume that for values of reflected light above 80%, in
Figure 6a, the cement paste is mostly dry and below this value the cement paste is mostly wet.
Transforming the reflected light intensity to height of absorbed water through Equation (5) an estimation of the capillary coefficient was achieved from the slopes of the plot in
Figure 8a, as seen in
Figure 8b. These values were then corrected using the calibration slope of
Figure 4d. The decrease of the capillary coefficient from the first measurement to the last two, from 1.373 ± 0.010 mm/√h to 0.668 ± 0.002 mm/√h, strengthens the idea that there is a reduction in the pore size and connectivity. This is likely due to loss of pore connectivity as well as the further hydration of anhydrous cement. Submerging samples C and F yielded a capillary coefficient of 1.771 ± 0.010 mm/√h and 6.360 ± 0.269 mm/√h, which are expected values since the capillary coefficient is expected to increase with increasing
w/c.
The sorptivity values achieved, 0.131 ± 0.004 mm/√h, 0.505 ± 0.080 mm/√h and 2.290 ± 0.110 mm/√h, through gravimetric measurements of samples B, C and F (
Figure 10a) corroborate the capillary coefficients reached with the single fiber reflectance spectrometer, resulting, through Equation (4), in porosity values of 19.4 ± 0.6%, 28.5 ± 4.7% and 35.9 ± 9.7%, which are near the expected values [
5], and they also increase with increasing
w/c. Moreover, measuring the porosity of these samples through SEM, we found that both curves of porosity are identical with ρ = 0.99998. Thus, the capillary coefficient values from single fiber reflectance spectroscopy can be used to extract valuable information concerning the concrete’s decay.
For future work, the application of hydrogels for improvements in cement curing due to their water retaining properties can intrinsically be studied from this device. Moreover, the hydrogel’s usage to promote self-sealing and self-healing could also be monitored in hardened cement [
5,
17]. This sensor also has the potential to monitor the alkali–silica reaction through its gel since it has an RI of around 1.5 [
28].
5. Conclusions
A single fiber reflectance spectrometer was successfully used to monitor the amount of water available in the vicinity of a fiber tip embedded in cement paste. It could sense the water exhaust at the hardening stage of cement hydration in samples with different w/c, as well as the addition of extra water to aid curing the cement paste. This information is invaluable for the tweaking of cement paste’s long-term properties.
It continually monitored a sample of 0.50 w/c for 15 days, from the beginning of curing until the end of the wet/dry cycles. The latter contain information on the amount of water absorbed by the sample, as well as the rate of water uptake—the capillary coefficient. The capillary coefficient is also a measure of cement paste durability and the values obtained by the single fiber reflectance spectrometer agree with gravimetric measurements of sorptivity and SEM measurements of porosity for samples of 0.50, 0.55 and 0.60 w/c.