Next Article in Journal
Glucanases and Chitinases in Mangifera indica: Identification, Classification, Phylogeny, and Expression Analysis of Defense Genes against Colletotrichum spp.
Next Article in Special Issue
A Novel Synthesis Method of Dumbbell-like (Gd1−xTbx)2O(CO3)2·H2O Phosphor for Latent Fingerprint
Previous Article in Journal
Fundamentals, Synthetic Strategies and Applications of Non-Covalently Imprinted Polymers
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

The Structure and Optical Properties of Luminescent Europium Terephthalate Antenna Metal–Organic Frameworks Doped by Yttrium, Gadolinium, and Lanthanum Ions

by
Oleg S. Butorlin
1,
Anna S. Petrova
1,
Yulia N. Toikka
1,
Ilya E. Kolesnikov
1,
Sergey N. Orlov
1,2,
Mikhail N. Ryazantsev
1,3,
Nikita A. Bogachev
1,
Mikhail Yu. Skripkin
1 and
Andrey S. Mereshchenko
1,*
1
Saint Petersburg State University, 7/9 Universitetskaya emb., Saint Petersburg 199034, Russia
2
Institute of Nuclear Industry, Peter the Great St. Petersburg Polytechnic University (SPbSU), 29, Polytechnicheskaya Street, Saint Petersburg 195251, Russia
3
Nanotechnology Research and Education Centre RAS, Saint Petersburg Academic University, ul. Khlopina 8/3, Saint Petersburg 194021, Russia
*
Author to whom correspondence should be addressed.
Molecules 2024, 29(15), 3558; https://doi.org/10.3390/molecules29153558
Submission received: 3 July 2024 / Revised: 23 July 2024 / Accepted: 26 July 2024 / Published: 28 July 2024
(This article belongs to the Special Issue Synthesis and Crystal Structure of Rare-Earth Metal Compounds)

Abstract

:
New heterometallic antenna terephthalate MOFs, namely, (EuxM1−x)2bdc3·4H2O (M = Y, La, Gd) (x = 0.001–1), were synthesized by a one-step method from aqueous solutions. The resulting compounds are isomorphic to each other; the crystalline phase corresponds to Ln2bdc3∙4H2O. Upon 300 nm excitation to the singlet excited state of terephthalate ions, all compounds exhibit a bright red emission corresponding to the of 5D07FJ (J = 0–4) f-f transitions of Eu3+ ions. The Eu(III) concentration dependence of the photophysical properties was carefully studied. We revealed that Gd-doping results in photoluminescence enhancement due to the heavy atom effect. To quantitatively compare the antenna effect among different compounds, we proposed the new approach, where the quantum yield of the 5D0 formation is used to characterize the efficiency of energy transfer from the ligand antenna to the Eu3+ emitter.

1. Introduction

Metal–organic frameworks (MOFs) represent a large class of crystalline materials defined as porous networks, consisting of metallic ions or clusters linked together by organic multidentate ligands. Due to their well-defined crystallinity, porosity, high stability, and wide diversity of structures and topologies, these materials have attracted considerable attention in the past two decades. Rare-earth element (REE) metal–organic frameworks (MOFs) are of particular interest due to their unique luminescence properties significantly determined by the type of lanthanide ion. Thus, REE-MOFs have been revealed as promising candidates for light-emitting materials, sensors, multimodal image contrast agents, catalysts, and analytes to reveal the hazardous substances in food and enviroment [1,2,3,4,5,6,7]. The f-f transitions are forbidden by selection rules, which results in inefficiency of direct excitation of lanthanide ions. This problem can be overcome by using the energy transfer from the excited ligand to the lanthanide ion, which is called the “antenna effect” [8,9]. The organic ligands, which are used as “antenna” compounds, have high UV absorption coefficients, easily coordinate with REE ions, and efficiently transfer energy to REE ions. The mechanism of the antenna effect can be explained as follows. Upon photon absorption, the ligand in the ground singlet state (S0) is promoted to the singlet excited state (S1, S2, etc.), followed by fast internal conversion to a lower excited energy level (S1). The excited singlet state can then either (i) return to the ground state (S1→S0) by internal conversion and fluorescence or (ii) undergo an intersystem crossing to the triplet state. Through internal conversion, the ligand reaches the lowest triplet level electronic state, T1, followed by the energy transfer to the REE ion [10]. In Eu-based antenna complexes, the quantum yield of luminescence from the europium ion depends on the relative energy level of the ligand triplet state and the atomic level of the Eu3+ ion. Energy transfer has been found to occur from the lowest energy triplet state of the ligand T1 to the 5DJ (J = 0–3) level of the Eu3+ ion followed by internal conversion to 5D0. The radiative transitions 5D07FJ (J = 0–4) to the term of ground state 7F of the Eu3+ ion correspond to the resulting photoluminescence of such antenna complexes. For the most efficient energy transfer, the difference in energy between the ligand triplet state and the 5DJ level of Eu3+ should be approximately 2500–4000 cm−1 [11]. However, it has also been proposed that energy transfer can occur from a singlet excited state as well [12,13]. For example, in a study by Shinji Miyazaki et al., the possibility of two energy transfer pathways was revealed from both the triplet and singlet levels for the Eu(hfa)3(DPPTO)2 complex (hfa—hexafluoroacetylacetonate, DPPTO—2-diphenylphosphoryltriphenylene) [14].
The simultaneous presence of both luminescent and nonluminescent REE ions, such as Sc3+, Y3+, La3+, Gd3+, Lu3+, can significantly affect the structural and photophysical properties of these compounds. The structural properties of heterometallic REE-MOFs have been investigated in several studies. It has been found that at low concentrations of the luminescent lanthanide ions, substitution occurs isomorphically, without changing the crystalline structure. However, it has been observed that in some compounds, the structure changes as concentration increases. For example, Jarley Nascimento et al. showed that compounds Gd1−xEux(1,4-bdc)3(dmf)2(H2O)n (bdc—benzenedecarboxylate, dmf—dimethylformamide; x = 0.01, 0.03, 0.05, 0.07, 0.09) are isostructural with [Eu2(1,4-bdc)3(dmf)2(H2O)] at the Eu3+ content between 1 and 7 at. % (at. %—the relative atom content of a certain lanthanide to all lanthanide atoms). However, at the Eu3+ concentration of 9 at. %, the compound was isostructural with [Eu2(1,4-bdc)3(dmf)2(H2O)2] [15]. In our previous research, we found that the compound (EuxLu1−x)2(1,4-bdc)3∙nH2O forms different crystal structures depending on the concentration of the Eu3+ ions. At the Eu3+ concentration range of 6–100 at. %, the samples were found to be isostructural with Ln2(1,4-bdc)3∙4H2O. However at the Eu3+ concentration of 0–2 at. %, the samples were isostructural with the Ln2bdc3. At the Eu3+ concentration between 3 and 5 at. %, both the Ln2bdc3∙4H2O and the Ln2(1,4-bdc)3 phases were observed in the samples [16]. The changes in the crystal structure can significantly affect the optical properties of compounds, such as the fine structure of emission spectra, quantum yields, and lifetime values.
Meanwhile, the optical properties of the heterometallic MOFs also depend on the concentration of the luminescent ion in the case of isomorphic substitution of the REE ion by the luminescent ion in the whole concertation range where the single crystalline phase is formed. However, very few works have studied such a concentration dependence. Thus, Utochnikova et al. studied the optical properties of heterometallic solid solutions of (TbxY1−x)2(1,4-bdc)3(H2O)4 and EuxGd1−x(dbm)3(phen) (dbm—dibenzoylmethanate, phen—o-phenantroline) MOFs. The steep quantum yield rise was observed at the low concentrations of Eu3+ or Tb3+ ions. Then, in the range of 20–100 at. % of Tb3+ for (TbxY1−x)2(1,4-bdc)3(H2O)4 and 10–100 at. % of Eu3+ for EuxGd1−x(dbm)3(phen), the quantum yield does not depend on the concentration of the luminescent ions. It has also been observed that lifetimes decrease with increasing concentration of the luminescent ion [17].
We note that the majority of studies focus on compounds with a single or a few concentrations of the luminescent lanthanide ion [17,18,19] or a narrow range of concentrations [15]. The properties of the synthesized compounds have been studied incompletely, and, therefore, at the moment, we have limited information about the mechanism of the dopant concentration effect on photophysical properties of heterometallic REE-MOFs.
In this article, the photophysical properties (photoluminescence decay time constants, radiative, nonradiative, and total decay rates, quantum efficiencies, and formation quantum yields of the 5D0 level; photoluminescence quantum yields, asymmetric ratios) of REE-MOFs of solid solutions of heterometallic (EuxM1−x)2(1,4-bdc)3∙4H2O MOFs (M = Y, La, Gd) were studied in detail in a wide concentration range of the Eu3+ ion (0.1–100 at. %).

2. Results

2.1. Structure and Morphology

The phase composition of (EuxM1−x)2(1,4-bdc)3·nH2O (M = Y, Gd, La) with a Eu3+ concentration from 0 to 100 at. % was studied using powder X-ray diffraction (PXRD). The experimental PXRD patterns at. %of the synthesized materials are presented in Figure 1a and Figure S1 (Supplementary Materials). The positions of the diffraction maxima in the PXRD patterns indicate that all the synthesized compounds correspond to the Ln2(1,4-bdc)3·4H2O crystalline phase (Ln = Ce − Yb) [20], and no additional peaks were observed. In the Ln2(1,4-bdc)3·4H2O structure (Figure 1b), the octacoordinated lanthanide ions are bound to the two water molecules and six different terephthalate ions through the oxygen atoms.
The refinement of the unit cell parameters and the calculation of the unit cell volumes were performed for the selected samples over the Eu3+ concentration range between 0 and 100 at. %. Unit cell parameters (Table S1, Supplementary Materials) were refined using UnitCell software [21]. This program can retrieve unit cell parameters from diffraction data using a least-squares method from the positions of the indexed diffraction maxima of the PXRD patterns (Pawley method [22]). The Eu3+ concentration effect on the unit cell volumes is shown in Figure 2. For the (EuxLa1−x)2(1,4-bdc)3·4H2O compounds, the increase in La3+ content leads to increased unit cell volumes due to a higher ionic radius of La3+ ions (1.160 Å, the coordination number is eight) than the ionic radius of Eu3+ ions (1.066 Å) [23].
The ionic radius of the Gd3+ ion (1.053 Å) is close to that of Eu3+. Therefore, the unit cell parameters do not change significantly in the (EuxGd1−x)2(1,4-bdc)3·4H2O series. The Y3+ ion (0.977 Å) is less than Eu3+; therefore, substitution of Eu3+ by the Y3+ ion results in a decrease in the unit cell volumes in the (EuxM1−x)2(1,4-bdc)3·4H2O series. In general, the dependence of unit cell volume obeys Vegard’s law [24], with a slight deviation from linearity that falls within the error limits.
Scanning electron microscopy (SEM) was used to reveal the particle morphology and the porosity of the selected synthesized materials, namely, (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, La, Gd). The resulting compounds had a distinct porous structure, as can be seen from the SEM images in Figure 3. On average, the particles are between 5 and 20 µm in size, and the pore diameter ranges from 20 to 150 nanometers. This observation confirms that the synthesized compounds are MOFs according to the definition of IUPAC [25]. Heterometallic europium terephthalates doped with yttrium and gadolinium formed spindle-shaped particles, while those with lanthanum formed flake-like particles.

2.2. IR Spectroscopy

To reveal the doping effect on the vibrational structure of the ligands, we measured the IR spectra of the selected samples of heterometallic (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and homometallic M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu) terephthalates (Figure 4). The broad band with the maximum at about the 3500 cm−1 region corresponds to the O-H stretching vibrations of the water molecules coordinated to the metal. The multiple narrow bands in the 1270–1470 and 1470–1800 cm−1 regions correspond to the symmetric and asymmetric stretching vibrations of the carboxylic -COO group of the terephthalate ion, respectively. The data obtained are consistent with the data in the literature obtained for REE terephthalates [26,27]. The spectral shape, including the fine structure of the absorption bands and the position of the absorption maxima, is almost identical for the studied compounds, which indicates the similar structure of these terephthalates. This conclusion is in agreement with PXRD data, demonstrating that all the synthesized compounds have the same crystalline phase, namely, Ln2(1,4-bdc)3·4H2O.

2.3. Thermogravimetric Analysis

Thermogravimetric analysis (TGA) was performed for selected heterometallic (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and homometallic M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu) terephthalates in the temperature range of 35–200 °C (Figure 5). Weight loss between 8.5 and 9.3% was observed at a temperature of 120–180 °C for all measured samples. As previously reported [28], weight loss in this temperature range may be associated with the dehydration of compounds, leading to the formation of anhydrous terephthalates with a general formula of M2(1,4-bdc)3. The weight loss of 8.5–9.3% corresponds to the elimination of 3.8–4.1 water molecules from the initial terephthalates, which is in agreement with the PXRD data, showing that all studied materials are formed in the Ln2(1,4-bdc)3∙4H2O crystalline phase.

2.4. Luminescent Properties

For all synthesized compounds, emission spectra were measured upon 300 nm excitation into the Sn singlet state of the terephthalate ion. Figure 6 shows the normalized emission spectra of selected samples with different Eu3+ content ((EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, La, Gd) (x = 0.001, 0.01, 0.1, 0.5, 1)). The emission spectra of all studied materials are given in Figure S2 (Supplementary Materials). All emission spectra contain the same narrow bands, which correspond to the 5D07FJ (J = 1, 2, 4) transitions of Eu3+: 5D07F1 (587.9 and 591.6 nm), 5D07F2 (614 nm), and 5D07F4 (696 nm).
5D07F3 transitions are also present in emission spectra, but they were not observed due to their weak intensity. The presence of Eu3+ f-f bands in the emission spectra upon excitation to the Sn singlet state of the terephthalate ion clearly reveals an antenna effect. Thus, the terephthalate ion absorbs UV radiation followed by efficient energy transfer to the luminescent lanthanide ion. Upon the excitation, the terephthalate ion is promoted into the Sn state, followed by the fast internal conversion to the S1 state. Due to the heavy atom effect caused by the lanthanide atom, the S1 state efficiently undergoes intersystem crossing to the T1 triplet electronic excited state. The T1 state of the terephthalate ion is close in energy to the 5D1 energy level of the Eu3+ ion [11,17]. Therefore, an efficient energy transfer occurs from the sensitizer to the luminescent lanthanide ion. The 5D1 level of Eu3+ then undergoes an internal conversion to the 5D0 state, followed by the emission to the 7FJ (J = 1, 2, 4) lower-lying energy levels.
The shape of the emission spectra for the Y-, Gd-, and La-doped compounds is identical to that of the pure europium terephthalate emission spectrum (Figure S3, Supplementary Materials), implying the same coordination environment of Eu3+ in the solid solutions studied. This observation agrees with the PXRD data, which show the presence of the same crystalline structure, (EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, Gd, La), among the studied series. However, the peak intensity of emission spectra depends on the concentrations of europium ions in the studied solid solutions due to different photoluminescence quantum yields, which will be discussed further.
The photoluminescence decay curves of the (EuxM1−x)2(1,4-bdc)3·4H2O phosphors monitored at 615 nm (5D07F2 transition) are presented in Figure 7ex. = 300 nm). The decay curves were fitted by a single exponential function:
I = I 0 · e t τ
where τ is the observed 5D0 lifetime (Table 1).
Figure 7 and Table 1 present the photoluminescence decay curves and lifetime data for the selected concentrations of Eu3+ ions in (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y) (x = 0.01, 0.1, and 1) among the whole concentration range. As can be seen from Table 1, all the samples have similar lifetimes. This allows us to assume that the 5D0 lifetime of the Eu3+ ion almost does not depend on the Eu3+ content in the 1–100 at. % concentration range of Eu3+.
The measured photoluminescence quantum yields (PLQYs) of the (EuxM1−x)2(1,4-bdc)3·4H2O are shown in Figure 8a. It should be noted that the 5D0 lifetimes do not depend significantly on the sample composition and are equal to about 0.45 ms. Meanwhile, the photoluminescence luminescence quantum yields increase with an increase in the Eu3+ concentration from 1 to 10 at. % due to the number of luminescence sites increasing. In particular, for the Eu–Y series, there is a rapid increase in the quantum yield up to 10%, after which the PLQY remains within small deviations of values from 10 at. % and reaches a plateau, up to Eu 100%. For the Eu–La series, there is also a rapid increase in the PLQY at low concentrations of Eu up to ~12% and a slight decrease in quantum yield to 10% in the range of Eu concentrations from 20 to 100 at. %. The Eu–Gd series is different from the Eu–Y and Eu–La ones: the PLQY has a maximum at the Eu3+ content of 10 at. %. The PLQY of (Eu0.1Gd0.9)2(1,4-bdc)3·4H2O is equal to 15%, which is 1.5 times greater than that of (Eu0.1Y0.9)2(1,4-bdc)3·4H2O and (Eu0.1La0.9)2(1,4-bdc)3·4H2O. Upon further Eu3+ content increase, the PLQY of (EuxGd1−x)2(1,4-bdc)3·4H2O decreases, whereas the PLQY of (EuxY1−x)2(1,4-bdc)3·4H2O and (EuxLa1−x)2(1,4-bdc)3·4H2O stays about the same (10%).
Luminescence decay is determined by both radiative and nonradiative processes. Radiative decay rate is determined by dipole transition strength and local-field correction. Nonradiative processes include multiphonon relaxation, quenching on impurities, and cooperative processes such as cross-relaxation and energy migration, the influence of which increases with increasing concentration of europium ions in the solid solution. Radiative and nonradiative decay rates of Eu3+-doped phosphors can be calculated from the emission spectrum using the 4f–4f intensity theory [29]. The magnetic dipole 5D07F1 transition probability A 0 1 = A M D 0 · n 0 3 =   49   s 1 . A M D 0 is the spontaneous emission probability of the magnetic dipole 5D07F1, 14.65 s−1, and n 0 is the refractive index, 1.5 [30]. Radiative decay rates A 0 - J (J = 2, 4) of the 5D07FJ emission transition can be obtained as follows:
A 0 J = A 0 1 · ν 0 1 · I 0 J ν 0 J · I 0 1
where ν0–J and I0–J are, respectively, the frequency and intensity of the corresponding transition 5D07FJ in the emission spectrum. The radiative decay rate is the sum of all the A 0 - J values A Rad = A 0 1 + A 0 2 + A 0 4 . The nonradiative decay rate can be determined using the observed lifetime and the obtained radiative decay rate: A total = A Rad + A Nonrad = 1 τ f ; the quantum efficiency of the 5D0 is
η D 0 , 5 = A Rad A total = n ( 5 D 0 7 F J ) em . n ( 5 D 0 )
Knowledge of both the PLQY (Figure 8a) and the quantum efficiency of 5D0 (Figure 8b) allows us to calculate the quantum yield of the 5D0 formation. The studied terephthalate solid solutions are antenna complexes, where 5D0 is populated as a result of the energy transfer from the initial excited terephthalate ion (Sn(bdc2−)→S1(bdc2−)→T1(bdc2−)→5D0(Eu3+)). Therefore, the PLQY can be calculated as the direct product of the quantum efficiency of the 5D0 ( η D 0 , 5 ) and quantum yield of the 5D0 formation ( Φ form . 5 D 0 ):
PLQY = η , 5 D 0 · Φ form . 5 D 0
Therefore, the quantum yield of the 5D0 formation (Figure 8c) was calculated as follows:
Φ form . 5 D 0 = PLQY η , 5 D 0
At Eu3+ concentrations up to 10 at. %, the quantum yield of the 5D0 formation increases as a result of the number of luminescence sites increasing. For the Eu–Y series, it remains unchanged up to 100 at. % of Eu3+, whereas for the Eu–La and Eu–Gd series, it reaches a maximum at 10 at. % of Eu3+ and then decays. The maximum values of quantum yield of the 5D0 formation decrease in a dopant row of Gd–La–Y. The QY of 5D0 formation is close to 100%, which indicates a very-high-efficiency energy transfer from the terephthalate antenna to the light-emitting Eu3+ ion. We propose that this observation can be explained by the heavy atom effect, which is more pronounced for the Gd3+ ion and less pronounced for the Y3+ ion.
The emission spectrum of the Eu3+ ion includes a very sensitive forced electric dipole transition 5D07F2. At the same time, the 5D07F1 magnetic dipole transition is not sensitive to environmental changes. Changes in the environment can be judged by the asymmetry ratio, which is determined by the ratio between the 5D07F2 and 5D07F1 transition intensities. The higher the asymmetry coefficient, the further away the luminescence center is located from the centrosymmetric geometry [31]. The effect of Eu3+ ion concentration on local symmetry in samples (EuxM1−x)2(1,4-bdc)3∙4H2O MOFs (M = Y, La, Gd) is shown in Figure 9. It is seen that an increase in the concentration of the Eu3+ ion leads to the growth of the asymmetry ratio due to distortion of the crystal structure near the luminescent atom. Starting from 10 at. % of Eu3+, the asymmetry ratio reaches a plateau and does not change within the margin of error. Thus, the data once again confirm the fact that three-charged REE ions replace each other isomorphically in crystalline substances.
The abovementioned results clearly show that the presence of a gadolinium ion leads to the luminescence enhancement in Eu–Gd terephthalates, whereas this effect is almost not pronounced in the Eu–La and Eu–Y series. Thus, (Eu0.1Gd0.9)2(1,4-bdc)3∙4H2O demonstrates the maximum PLQY among the Eu–Gd series, 15%. The PLQY value is 4–5% higher than that in the Eu–La and Eu–Y series at the same Eu3+ ion content (10 at. %). At the higher Eu3+ concentrations, the values of PLQY decrease smoothly for the Eu–Gd series, reaching 10% for Eu2(1,4-bdc)3∙4H2O. For the Eu–La and Eu–Y series, the PLQY stays about the same (9–11%) up to Eu3+ concentration of 100 at. %. Therefore, we do not observe Eu3+ concentration quenching. The Gd-doping effect is also observed for the calculated values of 5D0 formation quantum yield: for (Eu0.1Gd0.9)2(1,4-bdc)3∙4H2O, the QY of 5D0 formation values become close to 100%, which indicates a very-high-efficiency energy transfer from the terephthalate antenna to the light-emitting Eu3+ ion. The Gd3+ ion has an f7 configuration and, therefore, increases the probability (rate) of S1-T1 intersystem crossing in the terephthalate ion, which is associated with the heavy atom effect manifested by paramagnetic Gd3+ ions. To confirm the proposed mechanism, we measured the emission spectra of gadolinium and yttrium terephthalates upon 300 nm excitation into the 1ππ band of the terephthalate ion. The prominent increase in the phosphorescence band (510 nm) was observed for Gd2(1,4-bdc)3∙4H2O compared with Y2(1,4-bdc)3∙4H2O, which confirms the increase in the intersystem crossing quantum yield resulting from the increase in the S1-T1 nonradiative transition rate (Figure 10) as a result of the presence of the Gd3+ ion.

3. Materials and Methods

Europium (III) chloride hexahydrate, yttrium (III) chloride hexahydrate, gadolinium (III) chloride hexahydrate, and lanthanum (III) chloride hexahydrate were purchased from Chemcraft (Kaliningrad, Russia). Benzene-1,4-dicarboxylic (terephtalic, H2(1,4-bdc)) acid (>98%), sodium hydroxide (>99%), nickel(II) chloride hexahydrate (>99%), EDTA disodium salt (0.1 M aqueous solution), and murexide were purchased from Sigma-Aldrich Chemie GmbH (Taufkirchen, Germany) and used without additional purification.
The 0.2 M solutions of EuCl3, YCl3, GdCl3, and LaCl3 were prepared and standardized using back complexometric titration with EDTA and nickel chloride solution in the presence of an ammonia buffer (pH ≈ 9). A total of 0.6 mole of sodium hydroxide and 0.3 mole of terephthalic acid were dissolved in distilled water to obtain a 1 L solution of a 0.3 M solution of the disodium terephthalate (Na2(1,4-bdc)).
Heterometallic terephthalates with a general formula (EuxM1−x)2(1,4-bdc)3∙4H2O (M = Y, Gd, La) were obtained by mixing 0.2 M EuCl3, 0.2 M MCl3 (M = Y, La, Gd) with 2 mL of 0.3 M Na2bdc water solution. EuCl3 and MCl3 were taken in stoichiometric ratios. The total volume of 0.2 M EuCl3 and 0.2 M MCl3 solutions was equal to 1 mL. White precipitates of the resulting terephthalates were separated from the reaction mixture using centrifugation (4000× g) and washed using deionized water 3 times. The samples of compounds were then dried at 60 °C.
The Eu3+/M3+ (M = Y, Gd, La) ratios in the heterometallic terephthalates were confirmed using energy-dispersive X-ray spectroscopy (EDX) (EDX spectrometer EDX-800P, Shimadzu, Kyoto, Japan). The Eu/M (M = Y, Gd, La) ratios obtained from EDX were consistent with the expected ratios of Eu3+/M3+ (M = Y, Gd, La) taken for the synthesis for Eu3+ content within 1 at. % accuracy for the most of the samples. The EDX data are provided in the Supplementary Materials in Table S2. X-ray powder diffraction (PXRD) measurements were performed with a D2 Phaser (Bruker, Billerica, MA, USA) X-ray diffractometer using Cu Kα radiation (λ = 1.54056 Å). Thermogravimetry curves were obtained using a TG 209 F1 Libra thermo-microbalance (Netzsch, Selb, Germany). The measurement of FTIR spectra was carried out using the IRAffinity-1 spectrometer (Shimadzu, Kyoto, Japan). To carry out photoluminescence studies, the synthesized samples (20 mg) and potassium bromide (300 mg) were pressed into pellets (diameter 13 mm). The photoluminescence data were obtained with a Fluoromax-4 fluorescence spectrometer (Horiba Jobin Yvon, Kyoto, Japan). Lifetime measurements were performed with the same spectrometer using a pulsed Xe lamp (pulse duration: 3 µs). The absolute values of the photoluminescence quantum yields were recorded using a Fluorolog 3 Quanta-phi device (Horiba Jobin Yvon, Kyoto, Japan). All measurements were performed at 25 °C.

4. Conclusions

In this study, we explored the structure and the optical properties of brightly luminescent heterometallic terephthalate antenna MOFs, namely, (EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, La, Gd) (x = 0.001–1), which were obtained by precipitation from the aqueous solutions. The crystalline phase of all synthesized compounds corresponds to the Ln2(1,4-bdc)3·4H2O (Ln = Ce − Yb) [20]. Unit cell parameters of the obtained compounds were refined by Pawley method. The replacement of Eu3+ ions by the larger La3+ ions results in an increase in unit cell parameters in (EuxLa1−x)2(1,4-bdc)3·4H2O compounds, whereas the substitution of Eu3+ by smaller Y3+ ion results in a decrease in the unit cell volumes in the (EuxM1−x)2(1,4-bdc)3·4H2O series. Unit cell parameters almost do not change in the (EuxGd1−x)2(1,4-bdc)3·4H2O series due to close values of ionic radii of Eu3+ and Gd3+. The dependence of unit cell volume obeys Vegard’s law [24], which allows one to consider the studied systems as solid solutions. All compounds demonstrate a pronounced antenna effect. Upon 300 nm excitation into Sn singlet state of the terephthalate ion, obtained compounds demonstrate emission corresponding to the 5D07FJ (J = 1, 2, 4) transitions of Eu3+: 5D07F1 (587.9 and 591.6 nm), 5D07F2 (614 nm, maximal intensity), and 5D07F4 (696 nm). The shape of the emission spectra for the Y-, Gd-, and La-doped compounds is identical to that of pure europium terephthalate emission spectrum due to same local symmetry of Eu3+ in the studied solid solutions as a result of crystalline phase isomorphism. The 5D0 excited state lifetime does not depend on the sample composition and is equal to 0.45 ± 0.03 ms. Meanwhile, the peak intensity of emission spectra depends on the concentrations of europium ions in the studied solid solutions due to different photoluminescence quantum yields. Thus, the peak emission intensities and photoluminescence quantum yields increase with an increase in the Eu3+ concentration from 1 to 10 at. % due to the number of luminescence sites increasing. At larger Eu3+ concentrations, for the Eu–Y and Eu–La series, PLQY and the peak emission intensities remain the same (about 9–11%), whereas in the Eu–Gd series, they reach a maximum of 15% at the Eu3+ content of 10 at. % and then slightly decrease, reaching 10% in pure europium(III) terephthalate. The quantum efficiency of the 5D0 state was calculated using the relative intensities of 5D07FJ (J = 1, 2, 4) transitions and 5D0 excited state lifetimes. To quantitatively compare the antenna effect among different compounds, we propose to use the new approach. Based on the values of PLQYs and quantum efficiency of the 5D0 state, we calculated the quantum yields of the 5D0 formation, which reflect the efficiency of energy transfer from the ligand antenna to the Eu3+ emitter. The quantum yields of 5D0 formation are larger for Gd3+-doped terephthalates. In the MOFs possessing the highest reported compound values of the PLQY, namely, (Eu0.1Gd0.9)2(1,4-bdc)3∙4H2O, the value of quantum yield of 5D0 formation is close to 100%, which indicates a very high efficiency of the energy transfer from the terephthalate antenna to the light-emitting Eu3+ ion. The Gd3+ ion has the f7 configuration and, therefore, the increase in the probability (rate) of S1-T1 intersystem crossing in the terephthalate ion is associated with the heavy atom effect of paramagnetic Gd3+ ions, resulting in the increase in emission intensity, PLQY, and quantum yields of 5D0 formation.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/molecules29153558/s1, Figure S1: The powder X-ray diffraction (PXRD) patterns of the synthesized compounds series: (a) (EuxGd1−x)2(1,4-bdc)3·nH2O (x = 0.001–1) including the Gd2(1,4-bdc)3·nH2O, (b) (EuxLa1−x)2(1,4-bdc)3·nH2O (x = 0.001–1) including the La2(1,4-bdc)3·nH2O, (c) (EuxY1−x)2(1,4-bdc)3·nH2O (x = 0.001–1) including the Y2(1,4-bdc)3·nH2O. The positions and relative intensities of diffraction maxima of Eu2(1,4-bdc)3·4H2O taken from ref. [20] are shown as bars, Figure S2: The normalized emission spectra of (a) (EuxGd1−x)2(1,4-bdc)3·4H2O, (b) (EuxLa1−x)2(1,4-bdc)3·4H2O, and (c) (EuxY1−x)2(1,4-bdc)3·4H2O at a wide concentration range of Eu3+ (x = 0.001–1; given in legend) upon 300 nm excitation, Figure S3: The superimposed emission spectra of (a) (EuxGd1−x)2(1.4-bdc)3·4H2O, (b) (EuxLa1−x)2(1.4-bdc)3·4H2O, and (c) (EuxY1−x)2(1.4-bdc)3·4H2O at a wide concentration range of Eu3+ (x = 0.001–1; given in legend) upon 300 nm excitation, Table S1: Unit cell parameters of the (EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, La, Gd; x = 0.04–1). Table S2: Eu3+ atomic fractions (at. %) in the synthesized compounds, namely, (EuxM1−x)2(1,4-bdc)3∙4H2O. Measured data were obtained from EDX.

Author Contributions

Conceptualization, A.S.M., A.S.P. and O.S.B.; methodology, A.S.M., Y.N.T., A.S.P. and O.S.B.; validation, M.N.R. and I.E.K.; formal analysis, A.S.M., A.S.P. and O.S.B.; investigation, A.S.M., A.S.P., S.N.O., I.E.K. and O.S.B.; resources, A.S.M., M.Y.S. and N.A.B.; data curation, A.S.M., A.S.P. and O.S.B.; writing—original draft preparation, A.S.M., N.A.B., A.S.P. and O.S.B.; writing—review and editing, M.Y.S., Y.N.T., I.E.K., N.A.B., A.S.P., O.S.B. and A.S.M.; visualization, A.S.M., A.S.P. and O.S.B.; supervision, A.S.M.; project administration, A.S.M.; funding acquisition, A.S.M. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Russian Science Foundation under grant No. 22-73-10040 (https://rscf.ru/en/project/22-73-10040/, accessed on 2 July 2024).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in the study are included in the article (and Supplementary Material), further inquiries can be directed to the corresponding authors.

Acknowledgments

The measurements were performed in the Research Park of Saint Petersburg State University (Magnetic Resonance Research Centre, Chemical Analysis and Materials Research Centre, Cryogenic Department, Interdisciplinary Resource Centre for Nanotechnology, Centre for X-ray Diffraction Studies, Centre for Optical and Laser Materials Research, Thermogravimetric and Calorimetric Research Centre, and Centre for Innovative Technologies of Composite Nanomaterials). This article was published in commemoration of the 300th anniversary of Saint Petersburg State University’s founding.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Cui, Y.; Chen, B.; Qian, G. Lanthanide metal-organic frameworks for luminescent sensing and light-emitting applications. Coord. Chem. Rev. 2014, 273, 76–86. [Google Scholar] [CrossRef]
  2. Chen, B.; Wang, L.; Xiao, Y.; Fronczek, F.R.; Xue, M.; Cui, Y.; Qian, G. A luminescent metal–organic framework with lewis basic pyridyl sites for the sensing of metal ions. Angew. Chem. Int. Ed. 2009, 48, 500–503. [Google Scholar] [CrossRef] [PubMed]
  3. Harbuzaru, B.V.; Corma, A.; Rey, F.; Atienzar, P.; Jorda, J.L.; García, H.; Rocha, J. Metal–organic nanoporous structures with anisotropic photoluminescence and magnetic properties and their use as sensors. Angew. Chem. Int. Ed. 2008, 47, 1080–1083. [Google Scholar] [CrossRef] [PubMed]
  4. Pellé, F.; Aschehoug, P.; Surblé, S.; Millange, F.; Serre, C.; Férey, G. Interactions between Eu3+ ions in inorganic–organic hybrid materials. J. Solid State Chem. 2010, 183, 795–802. [Google Scholar] [CrossRef]
  5. Lee, J.; Farha, O.K.; Roberts, J.; Scheidt, K.A.; Nguyen, S.T.; Hupp, J.T. Metal-organic framework materials as catalysts. Chem. Soc. Rev. 2009, 38, 1450–1459. [Google Scholar] [CrossRef] [PubMed]
  6. Massi, M.; Ogden, M. Luminescent lanthanoid calixarene complexes and materials. Materials 2017, 10, 1369. [Google Scholar] [CrossRef] [PubMed]
  7. Alpha, B.; Ballardini, R.; Balzani, V.; Lehn, J.; Perathoner, S.; Sabbatini, N. Antenna effect in luminescent lanthanide cryptates: A photophysical study. Photochem. Photobiol. 1990, 52, 299–306. [Google Scholar] [CrossRef]
  8. Zhang, X.; Huang, T.; Gao, Y.; Cai, Y.; Liu, J.; Ramachandraiah, K.; Mao, J.; Ke, F. Functional modification engineering of metal–organic frameworks for the contaminants detection in food. Coord. Chem. Rev. 2024, 516, 215990. [Google Scholar] [CrossRef]
  9. Tan, G.; Wang, S.; Yu, J.; Chen, J.; Liao, D.; Liu, M.; Nezamzadeh-Ejhieh, A.; Pan, Y.; Liu, J. Detection mechanism and the outlook of metal-organic frameworks for the detection of hazardous substances in milk. Food Chem. 2024, 430, 136934. [Google Scholar] [CrossRef]
  10. Cao, W.; Tang, Y.; Cui, Y.; Qian, G. Energy transfer in metal–organic frameworks and its applications. Small Struct. 2020, 1, 2000019. [Google Scholar] [CrossRef]
  11. Latva, M.; Takalo, H.; Mukkala, V.-M.; Matachescu, C.; Rodriguez-Ubis, J.C.; Kankare, J. Correlation between the lowest triplet state energy level of the ligand and lanthanide(III) luminescence quantum yield. J. Lumin. 1997, 75, 149–169. [Google Scholar] [CrossRef]
  12. Yang, C.; Fu, L.M.; Wang, Y.; Zhang, J.P.; Wong, W.T.; Ai, X.C.; Qiao, Y.F.; Zou, B.S.; Gui, L.L. A highly luminescent europium complex showing visible-light-sensitized red emission: Direct observation of the singlet pathway. Angew. Chem. Int. Ed. 2004, 116, 5119. [Google Scholar] [CrossRef]
  13. Kasprzycka, E.; Trush, V.A.; Amirkhanov, V.M.; Jerzykiewicz, L.; Malta, O.L.; Legendziewicz, J.; Gawryszewska, P. Contribution of energy transfer from the singlet state to the sensitization of Eu3+and Tb3+ luminescence by sulfonylamidophosphates. Chem.—Eur. J. 2017, 23, 1318–1330. [Google Scholar] [CrossRef] [PubMed]
  14. Miyazaki, S.; Miyata, K.; Sakamoto, H.; Suzue, F.; Kitagawa, Y.; Hasegawa, Y.; Onda, K. Dual energy transfer pathways from an antenna ligand to lanthanide ion in trivalent europium complexes with phosphine oxide bridges. J. Phys. Chem. A 2020, 124, 6601–6606. [Google Scholar] [CrossRef] [PubMed]
  15. Do Nascimento, J.F.S.; de Arau’jo, A.M.U.; Kulesza, J.; de Farias Monteiro, A.F.; Ju´nior, S.A.; Barros, B.S. Solid-state tunable photoluminescence in gadolinium-organic frameworks: Effect of the Eu3+ content and co-doping with Tb3+. New J. Chem. 2018, 42, 5514–5522. [Google Scholar] [CrossRef]
  16. Nosov, V.G.; Kupryakov, A.S.; Kolesnikov, I.E.; Vidyakina, A.A.; Tumkin, I.I.; Kolesnik, S.S.; Ryazantsev, M.N.; Bogachev, N.A.; Skripkin, M.Y.; Mereshchenko, A.S. Heterometallic Europium(III)–lutetium(III) terephthalates as bright luminescent antenna MOFs. Molecules 2022, 27, 5763. [Google Scholar] [CrossRef] [PubMed]
  17. Utochnikova, V.V.; Grishko, A.Y.; Koshelev, D.S.; Averin, A.A.; Lepnev, L.S.; Kuzmina, N.P. Lanthanide heterometallic terephthalates: Concentration quenching and the principles of the “multiphotonic emission”. Opt. Mater. 2017, 74, 201–208. [Google Scholar] [CrossRef]
  18. Alammar, T.; Hlova, I.Z.; Gupta, S.; Biswas, A.; Ma, T.; Zhou, L.; Balema, V.; Pecharsky, V.K.; Mudring, A.-V. Mechanochemical synthesis, luminescent and magnetic properties of lanthanide benzene-1,4-dicarboxylate coordination polymers (Ln0.5Gd0.5)2(1,4-BDC)3(H2O)4; Ln = Sm, Eu, Tb. New J. Chem. 2020, 44, 1054–1062. [Google Scholar] [CrossRef]
  19. Do Nascimento, J.F.S.; Barros, B.S.; Kulesza, J.; de Oliveira, J.B.L.; Pereira Leite, A.K.; de Oliveira, R.S. Influence of synthesis time on the microstructure and photophysical properties of Gd-MOFs doped with Eu3+. Mater. Chem. Phys. 2017, 190, 166–174. [Google Scholar] [CrossRef]
  20. Reineke, T.M.; Eddaoudi, M.; Fehr, M.; Kelley, D.; Yaghi, O.M. From condensed lanthanide coordination solids to microporous frameworks having accessible metal sites. J. Am. Chem. Soc. 1999, 121, 1651–1657. [Google Scholar] [CrossRef]
  21. Holland, T.J.B.; Redfern, S.A.T. Unit cell refinement from powder diffraction data: The use of regression diagnostics. Mineral. Mag. 1997, 61, 65–77. [Google Scholar] [CrossRef]
  22. Pawley, G.S. Unit-cell refinement from powder diffraction scans. J. Appl. Crystallogr. 1981, 14, 357–361. [Google Scholar] [CrossRef]
  23. Shannon, R.D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crystallogr. Sect. A 1976, 32, 751–767. [Google Scholar] [CrossRef]
  24. Denton, A.R.; Ashcroft, N.W. Vegard’s law. Phys. Rew. A 1991, 43, 3161. [Google Scholar] [CrossRef] [PubMed]
  25. Batten, S.R.; Champness, N.R.; Chen, X.-M.; Garcia-Martinez, J.; Kitagawa, S.; Öhrström, L.; O’Keeffe, M.; Suh, M.P.; Reedijk, J. Terminology of metal–organic frameworks and coordination polymers (IUPAC Recommendations 2013). Pure Appl. Chem. 2013, 85, 1715–1724. [Google Scholar] [CrossRef]
  26. Costa, B.A.; Nunes, W.D.G.; Bembo, L.H.; Siqueira, A.B.; Caires, F.; Leles, M.I.G.; Ionashiro, E.Y. Study of thermoanalytical behavior of heavier lanthanides terephthalates in air atmosphere. J. Therm. Anal. Calorim. 2018, 134, 1205–1210. [Google Scholar] [CrossRef]
  27. Nunes, W.D.G.; Teixeira, J.A.; Do Nascimento, A.L.C.S.; Caires, F.J.; Ionashiro, E.Y.; Ionashiro, M. A comparative study on thermal behavior of solid-state light trivalent lanthanide isonicotinates in dynamic dry air and nitrogen atmospheres. J. Therm. Anal. Calorim. 2016, 125, 397–405. [Google Scholar] [CrossRef]
  28. Daiguebonne, C.; Kerbellec, N.; Guillou, O.; Bünzli, J.C.; Gumy, F.; Catala, L.; Mallah, T.; Audebrand, N.; Gérault, Y.; Bernot, K.; et al. Structural and Luminescent Properties of Micro- and Nanosized Particles of Lanthanide Terephthalate Coordination Polymers. Inorg. Chem. 2008, 47, 3700–3708. [Google Scholar] [CrossRef]
  29. Kolesnikov, I.E.; Kolokolov, D.S.; Kurochkin, M.A.; Voznesenskiy, M.A.; Osmolowsky, M.G.; Lähderanta, E.; Osmolovskaya, O.M. Morphology and doping concentration effect on the luminescence properties of SnO2:Eu3+ nanoparticles. J. Alloys Compd. 2020, 822, 153640. [Google Scholar] [CrossRef]
  30. Haquin, V.; Etienne, M.; Daiguebonne, C.; Freslon, S.; Calvez, G.; Bernot, K.; Le Pollès, L.; Ashbrook, S.E.; Mitchell, M.R.; Bünzli, J.-C.; et al. Color and brightness tuning in heteronuclear lanthanide terephthalate coordination polymers. Eur. J. Inorg. Chem. 2013, 2013, 3464–3476. [Google Scholar] [CrossRef]
  31. Kolesnikov, I.E.; Povolotskiy, A.V.; Mamonova, D.V.; Kolesnikov, E.Y.; Kurochkin, A.V.; Lähderanta, E.; Mikhailov, M.D. Asymmetry ratio as a parameter of Eu3+ local environment in phosphors. J. Rare Earths 2018, 36, 474–481. [Google Scholar] [CrossRef]
Figure 1. The XRD patterns of selected (EuxM1−x)2bdc3·4H2O (M = Gd, La, Y; x = 0, 0.5, 1) and the simulated XRD pattern of Eu2(1,4-bdc)3·4H2O single-crystal structure were taken from ref. [20] (a). The crystal structure of Eu2(1,4-bdc)3·4H2O (b).
Figure 1. The XRD patterns of selected (EuxM1−x)2bdc3·4H2O (M = Gd, La, Y; x = 0, 0.5, 1) and the simulated XRD pattern of Eu2(1,4-bdc)3·4H2O single-crystal structure were taken from ref. [20] (a). The crystal structure of Eu2(1,4-bdc)3·4H2O (b).
Molecules 29 03558 g001
Figure 2. Eu3+ concentration dependence of unit cell volume (Vuc) refined for (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Figure 2. Eu3+ concentration dependence of unit cell volume (Vuc) refined for (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Molecules 29 03558 g002
Figure 3. SEM images of (Eu0.5M0.5)2(1,4-bdc)3∙4H2O (M = Gd, La, Y).
Figure 3. SEM images of (Eu0.5M0.5)2(1,4-bdc)3∙4H2O (M = Gd, La, Y).
Molecules 29 03558 g003
Figure 4. FTIR spectra of (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu).
Figure 4. FTIR spectra of (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu).
Molecules 29 03558 g004
Figure 5. TGA curves of selected heterometallic (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and homometallic M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu) terephthalates measured in the temperature range of 35–200 °C.
Figure 5. TGA curves of selected heterometallic (Eu0.5M0.5)2(1,4-bdc)3·4H2O (M = Y, Gd, La) and homometallic M2(1,4-bdc)3·4H2O (M = Y, Gd, La, Eu) terephthalates measured in the temperature range of 35–200 °C.
Molecules 29 03558 g005
Figure 6. The normalized emission spectra of (EuxM1−x)2(1,4-bdc)3∙4H2O (M = Gd, La, Y) at selected Eu3+ concentrations (given in legend) upon 300 nm excitation.
Figure 6. The normalized emission spectra of (EuxM1−x)2(1,4-bdc)3∙4H2O (M = Gd, La, Y) at selected Eu3+ concentrations (given in legend) upon 300 nm excitation.
Molecules 29 03558 g006
Figure 7. The 615 nm photoluminescence decay curves of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, La, Gd; x = 0.01, 0.1).
Figure 7. The 615 nm photoluminescence decay curves of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Y, La, Gd; x = 0.01, 0.1).
Molecules 29 03558 g007
Figure 8. Photoluminescence quantum yield (PLQY) (a), quantum efficiency (η) 5D0 of Eu3+ (b), and quantum yield of 5D0 formation (c) of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Figure 8. Photoluminescence quantum yield (PLQY) (a), quantum efficiency (η) 5D0 of Eu3+ (b), and quantum yield of 5D0 formation (c) of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Molecules 29 03558 g008
Figure 9. Asymmetric ratios of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Figure 9. Asymmetric ratios of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y).
Molecules 29 03558 g009
Figure 10. The emission spectra of Gd2(1,4-bdc)3∙4H2O and Y2(1,4-bdc)3∙4H2O upon 300 nm excitation.
Figure 10. The emission spectra of Gd2(1,4-bdc)3∙4H2O and Y2(1,4-bdc)3∙4H2O upon 300 nm excitation.
Molecules 29 03558 g010
Table 1. The observed 5D0 lifetime of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y; x = 0.01, 0.1).
Table 1. The observed 5D0 lifetime of (EuxM1−x)2(1,4-bdc)3·4H2O (M = Gd, La, Y; x = 0.01, 0.1).
EuxM1−xτ(5D0), ms
Eu0.01Gd0.990.48 ± 0.01
Eu0.1Gd0.90.46 ± 0.01
Eu0.01La0.990.44 ± 0.01
Eu0.1La0.90.43 ± 0.01
Eu0.01Y0.990.47 ± 0.01
Eu0.1Y0.90.45 ± 0.01
Eu0.44 ± 0.01
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Butorlin, O.S.; Petrova, A.S.; Toikka, Y.N.; Kolesnikov, I.E.; Orlov, S.N.; Ryazantsev, M.N.; Bogachev, N.A.; Skripkin, M.Y.; Mereshchenko, A.S. The Structure and Optical Properties of Luminescent Europium Terephthalate Antenna Metal–Organic Frameworks Doped by Yttrium, Gadolinium, and Lanthanum Ions. Molecules 2024, 29, 3558. https://doi.org/10.3390/molecules29153558

AMA Style

Butorlin OS, Petrova AS, Toikka YN, Kolesnikov IE, Orlov SN, Ryazantsev MN, Bogachev NA, Skripkin MY, Mereshchenko AS. The Structure and Optical Properties of Luminescent Europium Terephthalate Antenna Metal–Organic Frameworks Doped by Yttrium, Gadolinium, and Lanthanum Ions. Molecules. 2024; 29(15):3558. https://doi.org/10.3390/molecules29153558

Chicago/Turabian Style

Butorlin, Oleg S., Anna S. Petrova, Yulia N. Toikka, Ilya E. Kolesnikov, Sergey N. Orlov, Mikhail N. Ryazantsev, Nikita A. Bogachev, Mikhail Yu. Skripkin, and Andrey S. Mereshchenko. 2024. "The Structure and Optical Properties of Luminescent Europium Terephthalate Antenna Metal–Organic Frameworks Doped by Yttrium, Gadolinium, and Lanthanum Ions" Molecules 29, no. 15: 3558. https://doi.org/10.3390/molecules29153558

APA Style

Butorlin, O. S., Petrova, A. S., Toikka, Y. N., Kolesnikov, I. E., Orlov, S. N., Ryazantsev, M. N., Bogachev, N. A., Skripkin, M. Y., & Mereshchenko, A. S. (2024). The Structure and Optical Properties of Luminescent Europium Terephthalate Antenna Metal–Organic Frameworks Doped by Yttrium, Gadolinium, and Lanthanum Ions. Molecules, 29(15), 3558. https://doi.org/10.3390/molecules29153558

Article Metrics