Next Article in Journal
New Insights into ZIF-90 Synthesis
Next Article in Special Issue
Mechanistic Study of Atomic Oxygen Erosion on Polyimide Under Electric Fields: A Molecular Dynamics and Density Functional Theory Approach
Previous Article in Journal
Experimental Study on Combined Microwave–Magnetic Separation–Flotation Coal Desulfurization
Previous Article in Special Issue
Effect of Particle Heterogeneity in Catalytic Copper-Containing Single-Chain Polymeric Nanoparticles Revealed by Single-Particle Kinetics
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Rheological Property Modification of a Molten-State Polyamide through the Addition of an α-Olefin–Maleic Anhydride Copolymer

1
Materials Chemistry Frontiers Research Area, Japan Advanced Institute of Science and Technology, 1-1 Asahidai, Nomi 923-1292, Ishikawa, Japan
2
Performance Additives Group, C&A Hiroshima, Coating & Additives R&D Center, Mitsubishi Chemical Corporation, 20-1 Miyukicho, Otake 739-0693, Hiroshima, Japan
*
Author to whom correspondence should be addressed.
Molecules 2024, 29(16), 3730; https://doi.org/10.3390/molecules29163730
Submission received: 13 July 2024 / Revised: 5 August 2024 / Accepted: 5 August 2024 / Published: 6 August 2024
(This article belongs to the Special Issue Exclusive Feature Papers in Macromolecular Chemistry)

Abstract

:
The rheological properties of a polyamide (PA) resin with low crystallinity were modified by melt-mixing it with a small amount of an alternative α-olefin–maleic anhydride copolymer as a reactive compound. Because PA has a low melting point, rheological characterization was performed over a wide temperature range. Owing to the reaction between PA and the alternative α-olefin–maleic anhydride copolymer, the blend sample behaved as a long-chain branched polymer in the molten state. The thermo-rheological complexity was obvious owing to large flow activation energy values in the low modulus region, i.e., the rheological time–temperature superposition principle was not applicable. The primary normal stress difference under steady shear was greatly increased in the wide shear rate range, leading to a large swell ratio at the capillary extrusion. Furthermore, strain hardening in the transient elongational viscosity, which is responsible for favorable processability, was clear. Because this is a simple modification method, it will be widely employed to modify the rheological properties of various polyamide resins.

1. Introduction

It is essential that engineering plastics including polyamides are able to undergo various processing operations besides injection molding. Most engineering plastics have a narrow molecular weight distribution and no long-chain branches. Therefore, during processes in which a molten resin with a free surface is deformed, it is necessary to modify the rheological properties of the resin to provide strain hardening in transient elongational viscosity. Such processes include foaming, blow molding, thermoforming, T-die casting, and tubular-blown film processing. Various techniques have been proposed to achieve this modification: (1) the addition of an ultra-high molecular-weight fraction [1,2,3], (2) the incorporation of long-chain branches [4,5,6], (3) the addition of flexible nanofibers [7,8,9], (4) the addition of a critical gel [10,11], (5) the addition of a comb-shaped block copolymer in an immiscible polymer blend [12,13], (6) blending with an immiscible long-chain branched polymer [14,15], and (7) making a multi-layered structure [16].
Polyamides are engineering plastics with high mechanical toughness, abrasion resistance, heat resistance, oil resistance, and gas barrier properties [17,18,19]. They are therefore potentially very useful for various products such as films, bottles, and foams. Reaction at the amide groups of polyamides is a good method of providing long-chain branches and therefore strain hardening in elongational viscosity [20]. Among various chain extenders [21,22,23,24,25,26,27,28,29], maleic anhydride is one of the most appropriate reactive compounds. Maleic anhydride graft copolymers such as polypropylene–graft–maleic anhydride (PP-g-MAH) are widely available and are used as compatibilizers for blends comprising polypropylene (PP) and polyamides [30,31,32]. This is logical because the polymer chains of the graft copolymer are localized at the boundary between the two phases and reduce the possibility of the coalescence of dispersed droplets [33,34]. However, such a graft copolymer is not appropriate for the rheological modification of a polyamide resin because one component of the graft copolymer, e.g., PP in PP-g-MAH, is immiscible with the polyamide resin. Therefore, PP exists as a dispersed phase. An alternative copolymer of α-olefin and maleic anhydride (O-MAH, shown in Figure 1), which reacts readily with polyamides, is a good candidate of a rheology modifier because the α-olefin component in the alternative copolymer must be impossible to show phase separation. In fact, Li et al. employed O-MAH to modify polyamide 6 (PA6) and confirmed that its foaming processability was improved [29].
However, it is not easy to characterize the rheological properties of conventional polyamides such as PA6 and polyamide 66 (PA66), especially in the low frequency region, owing to severe thermal degradation beyond their melting points [35,36,37,38]. Elongational viscosity is also difficult to evaluate [20,39,40]. Therefore, in the present study, a copolyamide resin with low crystallinity, denoted as PA, was used for the evaluation of basic rheological properties at relatively low temperatures. Subsequently, the effect of the addition of O-MAH on the rheological properties of the polyamide was discussed in detail. In particular, thermo-rheological simplicity/complexity and transient elongational viscosity were evaluated in detail because they are known to be sensitive to long-chain branch structures [4,5,6,41]. The results obtained herein will be widely available to inform modification of the rheological properties and processabilities of various polyamide resins.

2. Results and Discussion

Figure 2 shows the IR spectra of O-MAH, PA, and their blends. Stretching vibrations attributable to the carbonyl groups of O-MAH were detected at 1780 and 1850 cm−1 [29]. These peaks disappeared in PA/O-MAH (30/1), demonstrating that all the maleic anhydride in O-MAH had reacted with the amide groups in the PA during mixing and compression molding. In the previous study [29], it was confirmed that the bands of amide groups became weak after melt-mixing. In this study, however, it was not obvious because of the strong intensity. Although exposure to high temperature results in the dehydration of amide bonds in polyamide resins [42], it hardly occurred in this experiment because of the low temperature mixing at 140 °C. In fact, the PA sample in Figure 2 had the same thermal history. The stretching vibrations in PA/O-MAH (90/10) weakened but did not disappear. Although some of the maleic anhydride reacted with the PA, some remained in the blend. It suggested that 10 wt% of O-MAH was too much for the present PA sample. Subsequently, therefore, we employed only PA/O-MAH (30/1) as the blend sample because further reactions barely occurred during the rheology measurements.
The light transmittance of each 0.3 mm-thick PA and PA/O-MAH (30/1) film was evaluated using a UV-vis spectrometer, and the results are shown in Figure 3. Photographs of the films are also shown in the figure. The light transmittance increased with wavelength, indicating light absorption in the short wavelength range [35]. Considering that approximately 10% of the light transmittance was lost by surface reflection [43,44], both films were relatively transparent, as demonstrated by the photographs. This must have been due to the lower light scattering of the crystalline structure of PA [45,46,47]. Moreover, the O-MAH addition hardly affected the transparency. The result suggested that the extent of phase separation, if any, must have been small in the blend, and we could not detect any phase-separated structure in the blend by electron microscopy.
The DSC heating and cooling curves are shown in Figure 4. The heating/cooling rate was 10 °C min−1. There was an endothermic melting peak at approximately 105 °C in the DSC curve of pure PA, and the heat of fusion of 36.7 J g−1. Assuming that these crystals were composed of the main component in PA, i.e., polyamide 6 (PA6), the crystallinity was calculated to be 19% (the heat of fusion of perfect PA6 crystals was reported to be 230 J g−1) [48]. Because PA crystallization occurred slowly, no crystallization peak was detected at this cooling rate. In the case of pure O-MAH, a main melting peak was detected at approximately 76 °C, with a weak broad/shoulder peak at approximately 55 °C. These melting peaks can be attributed to the crystallinity of the α-olefin, as reported previously [49,50,51,52]. There was a clear crystallization peak at 62 °C in the cooling curve. The PA/O-MAH (30/1) film produced two peaks in the heating curve at approximately 80 °C and 107 °C. The PA crystallinity was reduced by adding O-MAH. Moreover, a crystallization peak was absent from the curve generated by the blend film.
Figure 5 shows the temperature dependencies of the tensile storage modulus E′, loss modulus E″, and loss tangent tan δ of the PA and PA/O-MAH (30/1) films. There was a peak in the E″ curve at approximately −60 °C (−100 °C to −30 °C), which can be attributed to localized segmental motion [53,54]. This relaxation mode was not affected by the addition of O-MAH. The E′ values decreased from approximately 20 °C owing to the glass-to-rubber transition of PA. Correspondingly, there was a peak in the E″ curve as well as the tan δ curve. The peak temperature of E″, i.e., the glass transition temperature Tg, of the PA film was approximately 30 °C, which was lower than that of PA6 [35]. The Tg of the PA/O-MAH (30/1) film was slightly lower. The decrease in the Tg following the addition of O-MAH was presumably attributable to its lower crystallinity, which increased segmental motion. The E′ decreased gradually, indicating that the PA was not fully amorphous, as shown in Figure 4. Beyond 100 °C, E′ dropped abruptly owing to the melting of the PA crystals. The E′ decrease occurred at 85 °C in the blend film. This must be attributed to the melting of the O-MAH crystals.
To understand the basic characteristics of PA in the molten state, we evaluated the relationship between pressure and specific volume at 230 °C. As shown in Figure 6, a straight line was obtained. The slope provided the bulk modulus K, which was 1.47 GPa and was determined by the following relationship [55]:
K = P Δ V / V 0 ,
where V0 is the volume at P = 0.
The melt density ρ at atmospheric pressure was calculated to be 954 kg m−3.
The master curves of the angular frequency dependency of the oscillatory shear moduli, such as shear storage modulus G′ and loss modulus G″, of PA and PA/O-MAH (30/1) are shown in Figure 7. The reference temperature was 230 °C. Although the time–temperature superposition principle was not applicable to PA/O-MAH (30/1), as explained in detail later, the apparent flow activation energy ΔEa was roughly calculated according to the Arrhenius equation, and was determined to be 72.4 kJ mol−1 for PA/O-MAH (30/1). This value was almost the same as that of pure PA, i.e., 72.5 kJ mol−1. The measurement was also performed at 130 °C in the present experiment. There were no crystals at that temperature because the time–temperature superposition principle was applicable to PA.
As shown in Figure 7, the rheological terminal region was clearly detected in PA. The slopes of G′ and G″ in the low-frequency region were 2 and 1, respectively. The zero-shear viscosity η0 and the steady-state shear compliance Je0 were calculated using the following equations [55]:
η 0 = lim ω 0 G ω ,
J e 0 = lim ω 0 G G ,
The rheological terminal parameters at 230 °C were as follows: η0 = 53.4 Pa s and Je0 = 1.1 × 10−5 Pa−1. For PA/O-MAH, neither parameter was obtained in the measurement range, suggesting a long-time relaxation mechanism.
As is well known, the rubbery plateau modulus GN0 of a simple polymer melt can be calculated using the following equation [55]:
G N 0 = 2 π a G d ln ω ,
where a is the angular frequency at the upper limit of the terminal region. The value of G N 0 is usually obtained by doubling the numerical integration of G″ from ln = −∞ to the maximum of G″. The G N 0 of PA is 2.1 MPa. Because the melt density, ρ, was known, the average molecular weight between entanglement coupling by points, i.e., Me, can be calculated from G N 0 [55]:
M e = ρ R T G N 0 ,
where R is the gas constant.
The Me value of the PA used in the present study was 1900. This value is close to those of other aliphatic polyamide resins, such as PA6 (Me = 2490) and PA66 (Me = 2000) [56].
Considering the thermo-rheological complexity detected in PA/O-MAH (30/1), the van Gurp–Palmen plot, i.e., loss angle δ versus absolute value of complex shear modulus |G*|, is shown in Figure 8. A curve that was typical of most simple polymer liquids was obtained for PA without deviation at any temperature. In contrast, PA/O-MAH (30/1) exhibited a significantly different trend. Although it was possible to superimpose the data obtained at various temperatures onto each other in the high |G*| region, the deviation was obvious in the low |G*| region. The δ value decreased as the measurement temperature decreased. This phenomenon has often been detected in long-chain branched polymers owing to the large activation energy in the low modulus region [57,58]. Therefore, the present results demonstrated that the reactions between PA and O-MAH generated long-chain branches.
Figure 9 shows the shear rate γ ˙ dependence of shear stress σ and primary normal stress difference N1 at 130 °C. Both σ and N1 increased with increasing γ ˙ for the samples. In addition, the values of N1 for PA/O-MAH (30/1) were much higher than those for pure PA over the whole shear-rate region. Furthermore, it should be noted that the order of σ and N1 was reversed, i.e., σ > N1 for PA and σ < N1 for the blend, demonstrating that the addition of O-MAH greatly enhanced elasticity over viscosity. This behavior was clearly confirmed by the right figure.
In the high shear rate region, a capillary rheometer was employed to evaluate the steady-state shear viscosity η and the appearance of the extruded strands. In the present study, neither Bagley nor Rabinowitsch corrections were performed. As shown in Figure 10, the steady-state shear viscosity was enhanced to some degree by the addition of O-MAH. However, flow instabilities such as shark-skin failure and volumetric gross melt fracture were absent over the whole shear rate range. This result suggested that the applied shear stress at die exit and elongational stress at die entry were still lower than their critical onset values of flow instabilities [6,59,60,61].
As revealed by the photographs, the diameters of the extruded strands of PA/O-MAH (30/1) were much larger than those of PA, demonstrating that the melt elasticity was greatly increased by the addition of O-MAH. These results corresponded with those in Figure 9.
Figure 11 shows the growth curves of the uniaxial elongational viscosity ηE+ at 130 °C of PA/O-MAH (30/1). It was impossible to evaluate the ηE+ of pure PA owing to its severe downward deformation due to gravitational force. The numerals in the figure represent the elongational strain rates, ε ˙ . Since the vertical and horizontal axes are proportional to stress and strain, respectively, they are basically stress–strain curves in double-logarithm plots [14]. There was marked strain hardening, i.e., sudden increase in ηE+, even at a low strain rate. This is typical for a polymer melt with a well-developed long-chain branch structure [4,5,6,30,59,60]. Chain stretching between branch points is responsible for strain hardening. The figure demonstrated that the strain to show the upward departure was around 0.5, which was independent of the strain rates. As mentioned in the introduction, such rheological properties are essential for various processing operations.

3. Materials and Methods

A polyamide resin with low crystallinity (PA) was used. Its chemical composition was as follows: PA6 = 55 mol%, PA66 = 13 mol%, and PA610 = 32 mol%. Its number and weight average molecular weights were characterized by size exclusion chromatography using poly(methyl methacrylate) as the standard, and were 1.14 × 104 Da and 2.46 × 104 Da, respectively. An alternative α-olefin–maleic anhydride copolymer (O-MAH; DIACARNA 30M; Mitsubishi Chemical Corp., Tokyo, Japan) was employed and is depicted in Figure 1 [29].
Before melt-mixing, the PA and O-MAH were dried under vacuum for 4 h at 65 °C. They were then melt-mixed using an internal batch mixer (Labo Plastomill; Toyo Seiki Seisaku-sho Ltd., Tokyo, Japan) at 140 °C for 3 min. The blade rotation speed was 30 rpm. The PA/O-MAH weight fractions were 100/0, 30/1, and 90/10. The obtained blends were compressed into flat films using a compression-molding machine at 140 °C for 1 min, and subsequently cooled at 30 °C for 3 min.
The reaction of O-MAH was evaluated by attenuated total reflectance Fourier-transform infrared (ATR-IR) spectroscopy (Spectrum100; PerkinElmer Co., Ltd., Waltham, MA, USA) from 400 to 4000 cm−1. KRS-5, i.e., thallium bromoiodide, was used as an ATR crystal. The accumulation count and the resolution were 16 times and 4 cm−1, respectively.
The light transmittance of each film (0.3 mm thick) was measured at 25 °C using a UV-Vis spectrometer (Lambda 25; PerkinElmer Co., Ltd., Waltham, MA, USA) within the wavelength range of 200 to 800 nm.
Thermal analysis was conducted using a differential scanning calorimeter (DSC) (DSC8500; PerkinElmer Co., Ltd., Waltham, MA, USA) under a nitrogen atmosphere. Each sample was placed in an aluminum pan and heated from 25 to 140 °C at a rate of 10 °C min−1, then cooled at 10 °C min−1. Each sample weighed approximately 5 mg.
The temperature dependencies of the tensile storage moduli E′, loss modulus E″, and loss tangent tan δ were evaluated from −80 to 140 °C using a dynamic mechanical analyzer (Rheogel-E4000; UBM Co., Ltd., Muko, Japan). The measurements were performed at a frequency of 10 Hz within the linear viscoelastic region. The heating rate was 2 °C min−1. Rectangular samples cut from the compression-molded films (5 mm wide, 7 mm long, and 1 mm thick) were employed for the measurements.
The melt density of the PA was measured under various pressures using a pressure–volume–temperature (PVT) measuring machine (PVT Test system; Toyo Seiki Seisaku-sho Ltd., Tokyo, Japan) at 230 °C.
The angular frequency dependencies of the shear storage and loss moduli (G′ and G″, respectively) were evaluated at various temperatures using a rotational rheometer (AR2000ex; TA Instruments, Inc., New Castle, DE, USA) with a cone-and-plate geometry. The diameter of the cone was 25 mm and the cone angle was 4°. The shear stress and primary normal stress difference under steady shear were also measured using this machine at 130 °C. The transient uniaxial elongational viscosity was evaluated using the rheometer equipped with a universal testing platform (SEG2-G; Xpansion Instruments LLC, Tallmadge, OH, USA) at 130 °C. Rectangular specimens (10 mm wide, 15 mm long, and 1 mm thick) were used for the measurements.
Capillary extrusion was performed using a pressure-driven capillary rheometer (140-SAS-2002; Yasuda-Seiki Seisaku-sho Ltd., Nishinomiya, Japan) at 130 °C to evaluate the steady-state shear viscosity and the extrusion processability. A circular die with a length of 10 mm and a diameter of 1 mm was employed. The entrance angle of the die was 180°.

4. Conclusions

Polyamide resins generally have a narrow molecular weight distribution and no long-chain branches. These properties cause difficulties in various processing operations due to poor melt elasticity, including an absence of strain hardening in the transient elongational viscosity. In the present study, the rheological properties were evaluated over a wide temperature range using a polyamide resin with low crystallinity. The basic viscoelastic properties of the pure PA, such as the GN0 and Me, were also determined. The present study verified that the addition of O-MAH successfully modified the rheological properties of the resin through chemical reactions between the amide groups and the maleic anhydride groups. Because O-MAH is not a block copolymer, macroscopic phase separation, which causes light scattering, was not detected. The addition of O-MAH provided a PA with long-chain branches. Consequently, the melt elasticity, i.e., the primary normal stress difference and strain hardening in the transient elongational viscosity, was greatly enhanced. Although the shear viscosity increased to some degree, the extrusion performance was good and there were no flow instabilities. O-MAH is a solid at room temperature and is easy to handle. Therefore, the technique described herein can be applied to various processing operations without any difficulty.

Author Contributions

Conceptualization, M.Y. (Misaki Yamaguchi). and M.Y. (Masayuki Yamaguchi); methodology, X.M., Q.-V.D. and T.N.; validation, X.M. and M.Y. (Masayuki Yamaguchi); formal analysis, X.M.; writing—original draft preparation, X.M.; writing—review and editing, M.Y. (Masayuki Yamaguchi). All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

Data will be available upon request.

Acknowledgments

We thank Frank Kitching from Edanz (https://jp.edanz.com/ac (accessed on 12 July 2024) for editing the draft of this manuscript. Furthermore, we appreciate the technical support from Tosoh Analysis and Research Center Co., Ltd. and DJK Corp.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Münstedt, H. Dependence of the elongational behavior of polystyrene melts on molecular weight and molecular weight distribution. J. Rheol. 1980, 24, 847–867. [Google Scholar] [CrossRef]
  2. Linster, J.J.; Meissner, J. Melt elongation and structure of linear polyethylene (HDPE). Polym. Bull. 1986, 16, 187–194. [Google Scholar] [CrossRef]
  3. Sugimoto, M.; Masubuchi, Y.; Takimoto, J.; Koyama, K. Melt rheology of polypropylene containing small amounts of high-molecular-weight chain. 2. Uniaxial and biaxial extensional flow. Macromolecules 2001, 34, 6056–6063. [Google Scholar] [CrossRef]
  4. Hingmann, R.; Marczinke, B.L. Shear and elongational flow properties of polypropylene melts. J. Rheol. 1994, 38, 573–587. [Google Scholar] [CrossRef]
  5. Yamaguchi, M.; Todd, D.B.; Gogos, C.G. Rheological properties of LDPE processed by conventional processing machines. Adv. Polym. Technol. 2003, 22, 179–187. [Google Scholar] [CrossRef]
  6. Wagner, M.H.; Kheirandish, S.; Stange, J.; Münstedt, H. Modeling elongational viscosity of blends of linear and long-chain branched polypropylenes. Rheol. Acta 2006, 46, 211–221. [Google Scholar] [CrossRef]
  7. Yokohara, T.; Nobukawa, S.; Yamaguchi, M. Rheological properties of polymer composites with flexible fine fibers. J. Rheol. 2011, 55, 1205–1218. [Google Scholar] [CrossRef]
  8. Yamaguchi, M.; Fukuda, K.; Yokohara, T.; Ali, M.A.B.M.; Nobukawa, S. Modification of rheological properties under elongational flow by addition of polymeric fine fibers. Macromol. Mater. Eng. 2012, 297, 654–658. [Google Scholar] [CrossRef]
  9. Rizvi, A.; Andalib, Z.K.M.; Park, C.B. Fiber-spun polypropylene/polyethylene terephthalate microfibrillar composites with enhanced tensile and rheological properties and foaming ability. Polymer 2017, 110, 139–148. [Google Scholar] [CrossRef]
  10. Yamaguchi, M.; Miyata, H. Strain hardening behavior in elongational viscosity for binary blends of linear polymer and crosslinked polymer. Polym. J. 2000, 32, 164–170. [Google Scholar] [CrossRef]
  11. Yamaguchi, M.; Suzuki, K. Rheological properties and foam processability for blends of linear and crosslinked polyethylenes. J. Polym. Sci. Part B Polym. Phys. 2001, 39, 2159–2167. [Google Scholar] [CrossRef]
  12. Tsou, A.H.; Lopez-Barron, C.R.; Jiang, P.; Crowther, D.J.; Zeng, Y. Bimodal poly(ethylene-cb-propylene) comb block copolymers from serial reactors: Synthesis and applications as processability additives and blend compatibilizers. Polymer 2016, 104, 72–82. [Google Scholar] [CrossRef]
  13. Lopez-Barron, C.R.; Tsou, A.H. Strain hardening of polyethylene/polypropylene blends via interfacial reinforcement with poly(ethylene-cb-propylene) comb block copolymer. Macromolecules 2017, 50, 2986–2995. [Google Scholar] [CrossRef]
  14. Fujii, Y.; Nishikawa, R.; Phulkerd, P.; Yamaguchi, M. Modifying the rheological properties of polypropylene under elongational flow by adding polyethylene. J. Rheol. 2019, 63, 11–18. [Google Scholar] [CrossRef]
  15. Kugimoto, D.; Kouda, S.; Yamaguchi, M. Modification of poly(lactic acid) rheological properties using ethylene–vinyl acetate copolymer. J. Polym. Environ. 2021, 29, 121–129. [Google Scholar] [CrossRef]
  16. Jordan, A.M.; Lee, B.; Kim, K.; Ludtke, E.; Lhost, O.; Jaffer, S.A.; Bates, F.S.; Macosko, C.W. Rheology of polymer multilayers: Slip in shear, hardening in extension. J. Rheol. 2019, 63, 751–761. [Google Scholar] [CrossRef]
  17. Aharoni, S.M. n-Nylons: Their Synthesis, Structure, and Properties; Wiley: New York, NY, USA, 1997. [Google Scholar]
  18. Deopura, B.L.; Alagirusamy, R.; Joshi, M.; Gupta, B. Polyesters and Polyamides; CRC Press: Boca Raton, FL, USA, 2008. [Google Scholar]
  19. García, J.M.; García, F.C.; Serna, F.; de la Peña, J.L. High-performance aromatic polyamides. Prog. Polym. Sci. 2010, 35, 623–686. [Google Scholar] [CrossRef]
  20. Xu, M.; Lu, J.; Zhao, j.; Wei, L.; Liu, T.; Zhao, L.; Park, C.B. Rheological and foaming behaviors of long-chain branched polyamide 6 with controlled branch length. Polymer 2021, 224, 123730. [Google Scholar] [CrossRef]
  21. Xanthos, M. Reactive Extrusion: Principles and Practice; Hanser Publishers: Munich, Germany, 1992. [Google Scholar]
  22. Lu, C.; Chen, T.; Zhao, X.; Ren, X.; Cai, X. Chemical modification of polyamide-6 by chain extension with 2,2′-bis(2-oxazoline). J. Polym. Sci. Part B Polym. Phys. 2007, 45, 1976–1982. [Google Scholar] [CrossRef]
  23. Van Ruymbeke, E.; Slot, J.J.M.; Kapnistos, K.; Steeman, P.A.M. Structure and rheology of branched polyamide 6 polymers from their reaction recipe. Soft Matter 2013, 9, 6921–6935. [Google Scholar] [CrossRef]
  24. Bouchékif, H.; Tunc, D.; Le Coz, C.; Deffieux, A.; Desbois, P.; Carlotti, S. Controlled synthesis of crosslinked polyamide 6 using a bis-monomer derived from cyclized lysine. Polymer 2014, 55, 5991–5997. [Google Scholar] [CrossRef]
  25. Seo, Y.P.; Seo, Y. Effect of molecular structure change on the melt rheological properties of a polyamide (Nylon 6). ACS Omega 2018, 3, 16549–16555. [Google Scholar] [CrossRef] [PubMed]
  26. Xu, Z.; Lin, X.; Luo, C.; Xiao, W. The application of a tri-functional epoxy resin as a crosslinking agent in extruded polyamide-6 foam. Polym. Sci. Ser. B 2019, 61, 574–581. [Google Scholar]
  27. Ozmen, S.C.; Ozkoc, G.; Serhatli, E. Thermal, mechanical and physical properties of chain extended recycled polyamide 6 via reactive extrusion: Effect of chain extender types. Polym. Degrad. Stab. 2019, 162, 76–84. [Google Scholar]
  28. Cai, J.; Liu, Z.; Cao, B.; Guan, X.; Liu, S.; Zhao, J. Simultaneous improvement of the processability and mechanical properties of polyamide-6 by chain extension in extrusion. Ind. Eng. Chem. Res. 2020, 59, 14334–14343. [Google Scholar] [CrossRef]
  29. Li, S.; Jiang, T.; Zeng, X.; Zhu, N.; Shen, C.; Gong, W.; Zhang, C.; He, L. The effect of α-olefin–maleic anhydride copolymer on the rheological and crystalline properties and microcellular foaming behavior of polyamide 6. Polymers 2013, 15, 2056. [Google Scholar] [CrossRef] [PubMed]
  30. Park, S.J.; Kim, B.K.; Jeong, H.M. Morphological, thermal and rheological properties of the blends polypropylene/nylon-6, polypropylene/nylon-6/(maleic anhydride-g-polypropylene) and (maleic anhydride-g-polypropylene)/nylon-6. Eur. Polym. J. 1990, 26, 131–136. [Google Scholar] [CrossRef]
  31. Nishio, T.; Suzuki, Y.; Kojima, K.; Kakugo, M. Morphology of maleic anhydride grafted polypropylene and polyamide alloy produced by reactive processing. J. Polym. Eng. 1991, 10, 123–150. [Google Scholar] [CrossRef]
  32. Grossman, R.F.; Lutz, J.T., Jr. Polymer Modifiers and Additives (Plastics Engineering); CRC Press: Boca Raton, FL, USA, 2000. [Google Scholar]
  33. Sundararaj, U.; Macosko, C.W. Drop breakup and coalescence in polymer blends: The effects of concentration and compatibilization. Macromolecules 1995, 28, 2647–2657. [Google Scholar]
  34. Hua, G.H.; Hoppe, S.; Feng, L.F.; Fonteix, C. Reactive Compounding. In Mixing and Compounding of Polymers, 2nd ed.; Manas-Zloczower, I., Ed.; Hanser: Munich, Germany, 2009; Chapter 27. [Google Scholar]
  35. Achhammer, B.G.; Reinhart, F.W.; Kline, G.M. Mechanism of the degradation of polyamides. J. Appl. Polym. Sci. 1951, 1, 301–332. [Google Scholar]
  36. Esmaeili, N.; Kandola, B.K.; Ebdon, J.R.; Horrocks, A.R. Comparison of the effects of antimony trioxide and zinc, calcium and copper stannates on the thermal degradation of polyamide-6,6. Polym. Degrad. Stab. 2023, 214, 110402. [Google Scholar] [CrossRef]
  37. Hirschberg, V.; Rodrigue, D. Recycling of polyamides: Processes and conditions. J. Polym. Sci. 2023, 61, 1937–1958. [Google Scholar] [CrossRef]
  38. Kurima, A.; Nguyen, T.A.; Kinashi, K.; Sakai, W.; Tsutsumi, N. Direct observation of the thermo-oxidative degradation of PA66 by spin-trapping ESR analysis. Polym. Degrad. Stab. 2023, 215, 110429. [Google Scholar] [CrossRef]
  39. Laun, H.M.; Schmidt, G. Rheotens tests and viscoelastic simulations related to high-speed spinning of Polyamide 6. J. Non-Newton. Fluid Mech. 2015, 222, 45–55. [Google Scholar] [CrossRef]
  40. Luo, M.; Liu, B.; Li, T.; Xu, J.; Zhu, N.; Zeng, X.; Jiang, T.; He, L. Effect of viscosity on foaming behavior and surface quality of foamed polyamide 6. J. Appl. Polym. Sci. 2023, 140, e54588. [Google Scholar] [CrossRef]
  41. Yamaguchi, M.; Wagner, M.H. Impact of processing history on rheological properties for branched polypropylene. Polymer 2006, 47, 3629–3635. [Google Scholar] [CrossRef]
  42. Ganesan, M.; Nagaraaj, P. Recent developments in dehydration of primary amides to nitriles. Org. Chem. Front. 2020, 7, 3792–3814. [Google Scholar] [CrossRef]
  43. Born, M.; Wolf, E. Principles of Optics, 7th ed.; Cambridge University Press: Cambridge, UK, 1999. [Google Scholar]
  44. Takahashi, S.; Okada, H.; Yamaguchi, M. Optical properties of polymer blends composed of poly(methyl methacrylate) and ethylene-vinyl acetate copolymer. Eur. Polym. J. 2012, 48, 974–980. [Google Scholar] [CrossRef]
  45. Keane, J.; Stein, R.S. The scattering of light from thin polymer films. II. Scattering from polyethylene. J. Polym. Sci. 1956, 20, 327–350. [Google Scholar] [CrossRef]
  46. Norris, F.H.; Stein, R.S. The scattering of light from thin polymer films. IV. Scattering from oriented polymers. J. Polym. Sci. 1958, 22, 87–114. [Google Scholar] [CrossRef]
  47. Tenma, M.; Yamaguchi, M. Structure and properties of injection-molded polypropylene with sorbitol-based clarifier. Polym. Eng. Sci. 2007, 47, 1441–1446. [Google Scholar] [CrossRef]
  48. Menczel, J.D.; Prime, R.B. Thermal Analysis of Polymers; Wiley: New York, NY, USA, 2009. [Google Scholar]
  49. Greenberg, S.A.; Alfey, T. Side chain crystallization of n-alkyl polymethacrylates and polyacrylates. J. Am. Chem. Sci. 1954, 76, 6280–6285. [Google Scholar] [CrossRef]
  50. Russell, K.E.; McFaddin, D.C.; Hunter, B.K.; Heyding, R.D. Crystallization of side chains in copolymers of ethylene and 1-alkenes. J. Polym. Sci. Part B Polym. Phys. 1996, 34, 2447–2458. [Google Scholar] [CrossRef]
  51. Janicek, M.; Cermak, R.; Obadai, M.; Piel, C.; Ponizil, P. Ethylene copolymers with crystallizable side chains. Macromolecules 2011, 44, 6759–6766. [Google Scholar] [CrossRef]
  52. Kitphaitun, S.; Takeshita, H.; Nomura, H. Analysis of ethylene copolymers with long-chain α-olefins (1-dodecene, 1-tetradecene, 1-hexadecene): A transition between mein chain crystallization and side chain crystallization. ACS Omega 2022, 7, 6900–6910. [Google Scholar] [CrossRef]
  53. Hayakawa, R.; Wada, Y. Theory of the local mode relaxation in the glassy state of polymers. J. Polym. Sci. Part B Polym. Phys. 1974, 12, 2119–2134. [Google Scholar] [CrossRef]
  54. Ishisaki, A.; Kawagoe, M. Examination of the time-water content superposition on the dynamic viscoelasticity of moistened polyamide 6 and epoxy. J. Appl. Polym. Sci. 2004, 93, 560–567. [Google Scholar] [CrossRef]
  55. Ferry, J.D. Viscoelastic Properties of Polymers, 3rd ed.; Wiley: Hoboken, NJ, USA, 1980. [Google Scholar]
  56. Wu, S. Chain structure and entanglement. J. Polym. Sci. Part B Polym. Phys. 1989, 27, 723–741. [Google Scholar] [CrossRef]
  57. Raju, V.R.; Rachapudy, H.; Graessley, W.W. Properties of amorphous and crystallizable hydrocarbon polymers. IV. Melt rheology of linear and star-branched hydrogenated polybutadiene. J. Polym. Sci. Part B Polym. Phys. 1979, 17, 1223–1235. [Google Scholar] [CrossRef]
  58. Carella, J.M.; Gotro, J.T.; Graessley, W.W. Thermorheological effects of long-chain branching in entangled polymer melts. Macromolecules 1986, 19, 659–667. [Google Scholar] [CrossRef]
  59. Meller, M.; Luciani, A.; Sarioglu, A.; Manson, J.A.E. Flow through a convergence. Part 1: Critical conditions for unstable flow. Polym. Eng. Sci. 2002, 42, 611–633. [Google Scholar] [CrossRef]
  60. Yamaguchi, M.; Miyata, H.; Tan, V.; Gogos, C.G. Relation between molecular structure and flow instability for ethylene/α-olefin copolymers. Polymer 2002, 43, 5249–5255. [Google Scholar] [CrossRef]
  61. Allal, A.; Vergnes, B. Molecular design to eliminate sharkskin defect for linear polymers. J. Non-Newton. Fluid Mech. 2007, 146, 45–50. [Google Scholar] [CrossRef]
Figure 1. Chemical structure of the alternative α-olefin–maleic anhydride copolymer (O-MAH).
Figure 1. Chemical structure of the alternative α-olefin–maleic anhydride copolymer (O-MAH).
Molecules 29 03730 g001
Figure 2. ATRIR spectra of the samples.
Figure 2. ATRIR spectra of the samples.
Molecules 29 03730 g002
Figure 3. Light transmittance as a function of the wavelength of PA and PA/O-MAH (30/1) films (0.3 mm thick). Photographs of the films are shown on the right.
Figure 3. Light transmittance as a function of the wavelength of PA and PA/O-MAH (30/1) films (0.3 mm thick). Photographs of the films are shown on the right.
Molecules 29 03730 g003
Figure 4. DSC heating (left) and cooling (right) curves at 10 °C min−1 produced by PA, O-MAH, and PA/O-MAH (30/1).
Figure 4. DSC heating (left) and cooling (right) curves at 10 °C min−1 produced by PA, O-MAH, and PA/O-MAH (30/1).
Molecules 29 03730 g004
Figure 5. Temperature dependencies of the tensile storage modulus E′, loss modulus E″, and loss tangent tan δ at 10 Hz of the PA and PA/O-MAH (30/1) films.
Figure 5. Temperature dependencies of the tensile storage modulus E′, loss modulus E″, and loss tangent tan δ at 10 Hz of the PA and PA/O-MAH (30/1) films.
Molecules 29 03730 g005
Figure 6. Specific volume of PA as a function of pressure, P, at 230 °C.
Figure 6. Specific volume of PA as a function of pressure, P, at 230 °C.
Molecules 29 03730 g006
Figure 7. Master curves of oscillatory shear storage modulus G′ and loss modulus G″ of PA (left) and PA/O-MAH (30/1) (right) at the reference temperature, Tr, of 230 °C.
Figure 7. Master curves of oscillatory shear storage modulus G′ and loss modulus G″ of PA (left) and PA/O-MAH (30/1) (right) at the reference temperature, Tr, of 230 °C.
Molecules 29 03730 g007
Figure 8. van Gurp–Palmen plots of PA and PA/O-MAH (30/1). The data were obtained at 130, 140, 170, 200, and 230 °C.
Figure 8. van Gurp–Palmen plots of PA and PA/O-MAH (30/1). The data were obtained at 130, 140, 170, 200, and 230 °C.
Molecules 29 03730 g008
Figure 9. (Left) Shear stress σ and primary normal stress difference N1 as a function of shear rate γ ˙ ; and (right) N1 versus σ for PA and PA/O-MAH (30/1) at 130 °C.
Figure 9. (Left) Shear stress σ and primary normal stress difference N1 as a function of shear rate γ ˙ ; and (right) N1 versus σ for PA and PA/O-MAH (30/1) at 130 °C.
Molecules 29 03730 g009
Figure 10. Steady-state shear viscosity η of PA and PA/O-MAH (30/1) at 130 °C. The photographs show strands extruded at 560 and 1000 s−1 through a circular die with a diameter of 1 mm.
Figure 10. Steady-state shear viscosity η of PA and PA/O-MAH (30/1) at 130 °C. The photographs show strands extruded at 560 and 1000 s−1 through a circular die with a diameter of 1 mm.
Molecules 29 03730 g010
Figure 11. Growth curves of the transient elongational viscosity ηE+ of PA/O-MAH (30/1) at 130 °C. The numerals in the figure represent the strain rates, ε ˙ .
Figure 11. Growth curves of the transient elongational viscosity ηE+ of PA/O-MAH (30/1) at 130 °C. The numerals in the figure represent the strain rates, ε ˙ .
Molecules 29 03730 g011
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Mei, X.; Do, Q.-V.; Narita, T.; Yamaguchi, M.; Yamaguchi, M. Rheological Property Modification of a Molten-State Polyamide through the Addition of an α-Olefin–Maleic Anhydride Copolymer. Molecules 2024, 29, 3730. https://doi.org/10.3390/molecules29163730

AMA Style

Mei X, Do Q-V, Narita T, Yamaguchi M, Yamaguchi M. Rheological Property Modification of a Molten-State Polyamide through the Addition of an α-Olefin–Maleic Anhydride Copolymer. Molecules. 2024; 29(16):3730. https://doi.org/10.3390/molecules29163730

Chicago/Turabian Style

Mei, Xianzhu, Quoc-Viet Do, Takaaki Narita, Misaki Yamaguchi, and Masayuki Yamaguchi. 2024. "Rheological Property Modification of a Molten-State Polyamide through the Addition of an α-Olefin–Maleic Anhydride Copolymer" Molecules 29, no. 16: 3730. https://doi.org/10.3390/molecules29163730

APA Style

Mei, X., Do, Q. -V., Narita, T., Yamaguchi, M., & Yamaguchi, M. (2024). Rheological Property Modification of a Molten-State Polyamide through the Addition of an α-Olefin–Maleic Anhydride Copolymer. Molecules, 29(16), 3730. https://doi.org/10.3390/molecules29163730

Article Metrics