Next Article in Journal
Effects of CuZnAl Particles on Properties and Microstructure of Sn-58Bi Solder
Next Article in Special Issue
Enhancing the Compatibility of Poly (1,4-butylene adipate) and Phenoxy Resin in Blends
Previous Article in Journal
Structure and Thermoelectric Properties of Bi2−xSbxTe3 Nanowires Grown in Flexible Nanoporous Polycarbonate Templates
Previous Article in Special Issue
Fabrication of Polymeric Antireflection Film Manufactured by Anodic Aluminum Oxide Template on Dye-Sensitized Solar Cells
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

On the Morphology of the SDS Film on the Surface of Borosilicate Glass

Department of Applied Chemistry, National Chia Yi University, Chiayi City 60004, Taiwan
*
Author to whom correspondence should be addressed.
Materials 2017, 10(5), 555; https://doi.org/10.3390/ma10050555
Submission received: 11 April 2017 / Revised: 15 May 2017 / Accepted: 17 May 2017 / Published: 19 May 2017
(This article belongs to the Special Issue Selected Papers from IEEE ICASI 2017)

Abstract

:
Surfactant films on solid surfaces have attracted much attention because of their scientific interest and applications, such as surface treatment agent, or for micro- or nano-scale templates for microfluidic devices. In this study, anionic surfactant sodium dodecyl sulfate (SDS) solutions with various charged inorganic salts was spread on a glass substrate and dried to form an SDS thin film. Atomic force microscopy (AFM) was employed to observe the micro-structure of the SDS thin film. The effects of inorganic salts on the morphology of the SDS film were observed and discussed. The results of experiments demonstrated that pure SDS film formed patterns of long, parallel, highly-ordered stripes. The existence of the inorganic salt disturbed the structure of the SDS film due to the interaction between the cationic ion and the anionic head groups of SDS. The divalent ion has greater electrostatic interaction with anionic head groups than that of the monovalent ion, and causes a gross change in the morphology of the SDS film. The height of the SDS bilayer measured was consistent with the theoretical value, and the addition of the large-sized monovalent ion would lead to lowering the height of the adsorbed structures.

1. Introduction

Surfactants are widely used as chemical ingredients in cleaning agents, emulsifiers, pigments, inks, anti-foaming agents, etc. When the surfactant solution is dribbled on a solid substrate, the solvent will evaporate, and the remaining particles will form various patterns on the surface. The morphology of the surfactant on the solid substrate depends on many factors, such as (i) the hydrophilic/hydrophobic property of the surface; (ii) the concentration of the surfactant; (iii) ionic functional groups of the surfactant and the surface charge; and (iv) counter-ions [1,2]. Due to scientific interest and promising applications (e.g., surface treatment agent [3,4] or micro- or nano-scale templates for microfluidic devices [5,6,7,8]), the design of the assembly structure has attracted much attention. Over the few past decades, many works have studied the morphology and the structure of ionic surfactants on the various substrates, including graphite, mica, silica, and metal [9,10,11,12,13,14,15,16,17,18,19,20,21,22,23,24,25,26,27]. The results of previous studies demonstrated that ionic surfactants could form flat sheets or semi-cylindrical structures on hydrophobic substrates via the van der Waals force, whereas the ionic surfactants would aggregate into the shape of a bilayer, cylinder, or sphere on the hydrophilic substrate through electrostatic interaction.
Many researchers are interested in the effect of the ionic strength or the counter-ion on the organization of ionic surfactant molecules. Some studies have shown that the salts had an impact on the morphology of the ionic surfactant on the various surfaces when the ionic surfactant and the surface contained opposite charges [28]. Ducker et al. studied the influence of monovalent electrolytes on cetyltrimethylammonium bromide (CTAB) aggregates on mica [29]. The CTAB formed a flat sheet structure on the surface. With the addition of HBr and KBr to the system, the structure of the aggregate would transform into a cylindrical structure. Metal halide (CsBr, CsCl, KCl, LiCl, LiBr) salts could induce the transformation of the aggregate of CTAC on mica from bilayers to cylindrical micelles to globular micelles with a variation in concentration [30]. According to these studies, mica can bind cations because of its negative lattice sites. In the presence of salts, excess cations compete with positively-charged head groups of the surfactant to occupy the lattice sites and reduce the density of the surfactant on the surface. Thus, the shapes of the surfactant aggregates are transformed.
The effect of salt on the morphology of the ionic surfactant adsorbed on the low-charge surface was studied. Ducker et al. used atomic force microscopy (AFM) to study the influence of NaCl on the aggregated structure of SDS on the graphite–solution interface [31]. The addition of NaCl to the system did not change the morphology of adsorbed surfactant, but it reduced the repulsive interactions between the negatively-charged head groups and resulted in a lower space between hemicylinders. The same result was evidenced by the study of molecular dynamics simulation [32]. For the divalent ions (Mg2+, Mn2+, and Ca2+), the adsorbed structures are very similar to the results observed in the presence of only monovalent counter ions. The high electric charge would enhance the adsorption density and did not change the shape of the aggregation conspicuously [33]. From the results of these studies, the hydrophobic tail groups of the ionic surfactant adsorbed on graphite by the van der Waals force and the addition of salts in SDS solutions does not greatly change the structures of adsorbed aggregate on graphite.
As discussed previously, studies mainly discussed the effect of salts on the morphology or the transformation of the structure of the surfactant with the opposite charge of the surface, with little concern for the stacking of the surfactant and the effect of salts on the surfactant self-assembly on the surface with the same charge of the surfactant. In this study, the effect of salts on the stacking of the anionic surfactant on the negatively-charged surface was observed and discussed. Thin films of the anionic surfactant SDS with various charged inorganic salts were prepared on borosilicate glass, which is a hydrophilic and negatively-charged surface. AFM was employed to observe the structure of these films. The effects of various salts on the morphology of the SDS film are discussed.

2. Results

The morphology of the thin films are presented in three types of AFM image, which include the error signal image, the height image, and the 3D reconstruction. The height image displays the height of the surface with various colors. The 3D height image is useful for determining three-dimensional patterns of molecule accumulation.

2.1. Structure of the SDS Aggregate

Figure 1a,b show the AFM surface height images and cross-section profiles of the morphology of SDS aggregates on the glass slide. Whether the concentration of SDS is 2 mM or 8.1 mM, the structure of the SDS molecules appear as linear and parallel stripes. The cross-section height profiles are along the black line in the AFM height image. This provides the height variation over the SDS aggregate structure. For the 2 mM SDS concentration, the adsorbed structures of 0.15–0.35 μm height and 3–8 μm width were observed. At the concentration of 8.1 mM (the critical micelle concentration (CMC) of the SDS solution), the adsorbed structures feature similar results. The height and the width of the structures are about 0.4–0.8 μm and 5–8 μm, respectively. The maximum height in these two samples are approximately 333 nm and 710 nm, respectively. These two images show that every stripe forms a flat layer and the distance between the stripes is about 2 μm.
Figure 1a,b are enlarged and shown in Figure 2a,b, respectively. The edge of the parallel structure is smooth. Figure 2c is an AFM error signal image from Figure 2b. It is clear that SDS molecules self-assembled to form an ordered structure on borosilicate glass through layer-by-layer deposition. We also observed that the formation of the layer had an orientation outwards (indicated by the white arrow in Figure 2c). This phenomenon was assigned to the outward capillary flow during evaporation [34]. On the basis of the results, it is concluded that the height of the adsorbed structures are affected by the surfactant concentration, but the morphology and the aggregate structure do not change.

2.2. The Effect of the Cations on the Structure

For further understanding of the influence of the cations on the morphology of the SDS film, we prepared 8.1 mM SDS solutions with 8.1 mM alkali chloride (Na+, K+) or alkaline earth chloride (Mg2+, Ca2+) to form a thin film. Figure 3a,b show the results of the SDS-monovalent ion films. When SDS coexisted with monovalent ions, the transformation from the linear stripe to the rice plant shape was obtained. The SDS molecules in the flat layer structures stretched out, and the space between stripes decreased. The maximum height of the structure in SDS-NaCl and SDS-KCl are 344 nm and 235 nm, which are lower than that of the SDS film (710 nm). When SDS was mixed with the divalent cation, SDS molecules assembled in a disorderly manner and no regular structure was observed, as shown in Figure 3c,d. The results demonstrated that the existence of the inorganic salt would interfere with the structure of the SDS film. With enough electrolytes in the system, the counter-ions dominate in the Stern and diffuse layers, and hence reduce the repulsive interaction (increasing the attractive interaction) between DS- molecules, so the counter-ions are more susceptible than co-ions. It is well-known that the valence and the concentration of counter-ions play an important role in the stability of the colloid system. In our case, all concentrations of SDS and electrolyte solutions were constant at 8.1 mM. Thus, the principal reason for the influence was ascribed to the valence of the counter ions. The phenomenon that SDS molecules aggregate intensely with the addition of multivalent ions can be formalized in the Schultz–Hardy rule for the critical coagulation concentration, as given in Equation (1):
C . C . C .       1 z   6
where the critical coagulation concentration (C. C. C.) is defined as the minimum concentration of colloidal particles for coagulation and z is the valence of the counter-ions [35,36]. For z = 1 and 2, the ratio of the CCCs value are thus 1 and 0.0156. This means that colloid particles aggregate with each other at a lower concentration of higher-valence counter-ions. In other words, at the same concentration of electrolytes, high-valence counter-ions could result in a greater coagulation behavior. The divalent ion has much more electrostatic interaction with anionic head groups than that of the monovalent ion, so it causes a significant impact on changing the morphology of the SDS film.

2.3. The Effect of Anions on the Structure

From the above experiments, the regular stripe structure of SDS was affected slightly by the addition of Na+ or K+ ions. To further understand whether the SDS structure could be influenced by the anions, the thin films from 8.1 mM SDS in the presence of 8.1 mM sodium inorganic salt (NaCl, NaI, or NaNO2) solutions were prepared, as shown in Figure 4. It was found that the maximum height of the structure in SDS-NaCl, SDS-NaI, and SDS-NaNO2 is 338 nm, 276 nm, and 163 nm, respectively. They are much lower than the height of the pure SDS film. It is clear that SDS structures near the periphery of the flat layer stretched out and a branched pattern was obtained. The results are very similar to that observed in the presence of NaCl and KCl.

2.4. Formation of SDS Multilayers

We can observe the stacking formation of the aggregation by using AFM cross-section profile and 3D reconstruction image. The film structure formed by using the 8.1 mM SDS solution was shown in Figure 5. It can clearly be seen in the 3D reconstruction image (Figure 5c) that the SDS adsorption on borosilicate glass was stacked in layers. The cross-section of an indentation site in the AFM height image (Figure 5b) shows that the thicknesses of the SDS layers are approximately 10, 15, or 25 nm. The structure of the SDS-NaCl film is represented in Figure 6. The 3D reconstruction image—which is on the periphery of the aggregation structure—shows that the SDS molecules in the flat layer structures extended laterally and had the lower space between structures. The cross-section profile reveals that the thicknesses of the aggregated layers are approximately 10, 15, or 25 nm, which is similar to the result of SDS film.
It is known from the previous results that the low concentration of the SDS solution would cause a lowering of the height of the adsorbed structure from 0.7 μm to 0.2 μm. Without changing the concentration of SDS, the addition of the monovalent ions could also cause a similar result. It is interesting to note the effect of the large-volume cations on the height of the SDS adsorbed film. The film structure formed by using the solution with 8.1 mM SDS-CsCl was recorded by AFM, as shown in Figure 7. The branched pattern was observed and the maximum height of the film decreased to 33.9 nm, which is far lower than that of the other SDS-monovalent ion system. The 3D reconstruction image (Figure 7c) shows that the SDS structure was in the form of lamellae. It is clear that the SDS adsorption on borosilicate glass was stacked in layers. The cross-section of an indentation site in the Figure 7a depicts that the thickness of the SDS layers is approximately 5 nm. According to previous literature, the hydrophobic part of one SDS bilayer at low water content (1:8 water:SDS) is about 4 nm, and each sulfate group has 0.6 nm length [22,37,38]. Hence, the result corresponds to the height of one surfactant bilayer.

3. Discussion

In previous literature, the SDS formed hemicylindrical structure on the graphite surface since the hydrophobic substrates interact with the carbon chains through van der Waals forces [19,31]. According to the AFM results mentioned above, we observed the stacking formation and the morphology of the aggregates, which is similar to the aggregation of SDS on the mica and ZnSe surface [22,23]. These observations provide some information to postulate the mechanism of the adsorbed process as represented in Figure 8. It is well-known that borosilicate glass is a negatively-charged surface with hydrophilic properties, and the DS- has a negatively-charged head group. Figure 8a gives the possible mechanism for the formation of the SDS film. When the SDS solution is dropped on the glass surface, the negatively-charged sites of the borosilicate glass binds the cations through attractive electrostatic interaction [30]. The negative DS- head group adsorbs on the Na+ ion layer, and the hydrophobic carbon chain of the SDS is upward. Then, the hydrophobic carbon chains of the SDS link together by the van der Waals force to form a deposited bilayer. In the drying process, the two parallel and negatively-charged surfaces are forced to approach mutually and create a thin layer between the two surfaces. This thin layer has the potential for counter ions to compensate the charge repulsion. Thus, Na+ ions penetrate into the negative interface between the DS- head groups to compensate for the charge density and result in a bilayer [22]. Finally, a lamellar structure of stacking bilayers forms.
Ducker et al.’s study indicates that ionic strength has an influence on aggregate space [31]. The space between aggregates can be controlled by Coulombic interactions. When the salt concentration increased (high ionic strength), excess cations reduced repulsive interactions between headgroups and decreased the space between stripes. SDS molecules were attracted by the excess monovalent cations and extended laterally instead of stacking upward, which caused the stripe shape of SDS to change to the rice plant/leafy shapes and the reduction of the stack thickness, as shown in Figure 8b. Thus, the height of the structure is much lower than that of the pure SDS film. Since the large size of cesium ions results in a lower charge density, the electrostatic interaction force between these ions and the substrate is poor. Thus, the ions prefer to spread with the solvent to flow in preference of binding onto the liquid–solid interface. The SDS molecules are also susceptible to movement, giving rise to a wider range of diffusion. The mutual attractive force between SDS molecules for stacking is low in this case. Hence, we still obtain the SDS bilayer by adding the larger ions without decreasing the SDS concentration.

4. Materials and Methods

All water in the experiment was pre-treated by a Milli-Q system and had a conductivity of 18 MO cm−1. Sodium dodecyl sulfate was purchased from Sigma (purity, 92.5–100.5%). NaCl (J.T. Baker, 99.7%), KCl (Choneye pure chemicals, 98%), CsCl (Merk, 99.5%), CaCl2·2H2O (Hayashi Japan, 99.7%), MgCl2 (Honeywell Riedel-de Haen chemicals, 99%), NaI (Choneye pure chemicals, 99%), and NaNO2 (Showa chemical, 98.5%) were used as the electrolyte additives. SDS was prepared at 2 mM and 8.1 mM. SDS-inorganic salt aqueous solutions were prepared at 8.1 mM.
The borosilicate glass slide was cleaned with 75% ethanol to remove possible organic impurities and then rinsed with ultrapure water from the Milli-Q system before use. A drop of solution with a volume of 15 μL was transferred to the glass surface with a pipette. The borosilicate glass with the solution drop was kept at 25 °C and a humidity of 60% for 24 h. The water was evaporated, and the surfactant film formed. All films were imaged by atomic force microscopy (JPK, Axiovert 200, Berlin, Germany) in intermittent contact mode. The AFM probes were Tap 150Al-G silicon probes, which were purchased from Budget Sensors.

5. Conclusions

In this study, the self-aggregation of sodium dodecyl sulfate with inorganic salts on the surface of the borosilicate glass was investigated by AFM. The results of the experiments demonstrated that pure SDS film formed patterns of long, parallel, highly-ordered stripes. The existence of inorganic salt disturbed the structure of the SDS film due to the interaction between cationic ions and the anionic head groups of SDS. The branch pattern was obtained by adding the monovalent ion. The divalent ion has greater electrostatic interaction with anionic head groups than that of the monovalent ion, and has a greater effect in changing the morphology of the SDS film.
The addition of a large-sized monovalent ion led to a lowering of the height of the adsorbed structures without adjusting the SDS concentration. By using CsCl, a lamellar structure was obtained. It was evidenced that SDS molecules were self-assembled on borosilicate glass through layer-by-layer deposition. The height of the lamella (about 5 nm) was in agreement with the thickness of an SDS bilayer that was estimated from theories in the literature.

Acknowledgments

National Chiayi University is acknowledged for supporting this study.

Author Contributions

Maw-Tien Lee designed the experiments; Zih-Yao Shen performed the experiments; Maw-Tien Lee and Zih-Yao Shen analyzed the data; and Maw-Tien Lee and Zih-Yao Shen wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Atkin, R.; Craig, V.; Wanless, E.J.; Biggs, S. Mechanism of cationic surfactant adsorption at the solid–aqueous interface. Adv. Colloid Interface Sci. 2003, 103, 219–304. [Google Scholar] [CrossRef]
  2. Paria, S.; Khilar, K.C. A review on experimental studies of surfactant adsorption at the hydrophilic solid–water interface. Adv. Colloid Interface Sci. 2004, 110, 75–95. [Google Scholar] [CrossRef] [PubMed]
  3. Lal, S.; Gautam, D.; Razeeb, K.M. The impact of surfactant sodium dodecyl sulfate on the microstructure and thermoelectric properties of p-type (Sb1−xBix)2Te3 electrodeposited films. ECS J. Solid State Sci. Technol. 2017, 6, N3017–N3021. [Google Scholar] [CrossRef]
  4. Naylor, A.J.; Koukharenko, E.; Nandhakumar, I.S.; White, N.M. Surfactant-mediated electrodeposition of bismuth telluride films and its effect on microstructural properties. Langmuir 2012, 28, 8296–8299. [Google Scholar] [CrossRef] [PubMed]
  5. Jiang, H.; Jelinek, R. Dramatic shape modulation of surfactant/diacetylene microstructures at the air–water interface. Chem. Eur. J. 2014, 20, 16747–16752. [Google Scholar] [CrossRef] [PubMed]
  6. Plawsky, J.; Fedorov, A.; Garimella, S.; Ma, H.; Maroo, S.; Chen, L.; Nam, Y. Nano-and microstructures for thin-film evaporation—A review. Nanoscale Microscale Thermophys. Eng. 2014, 18, 251–269. [Google Scholar] [CrossRef]
  7. Fatona, A.; Chen, Y.; Reid, M.; Brook, M.A.; Moran-Mirabal, J.M. One-step in-mould modification of pdms surfaces and its application in the fabrication of self-driven microfluidic channels. Lab Chip 2015, 15, 4322–4330. [Google Scholar] [CrossRef] [PubMed]
  8. Sharma, S.; Yadav, N.; Chowdhury, P.K.; Ganguli, A.K. Controlling the microstructure of reverse micelles and their templating effect on shaping nanostructures. J. Phys. Chem. B 2015, 119, 11295–11306. [Google Scholar] [CrossRef] [PubMed]
  9. Manne, S.; Cleveland, J.; Gaub, H.; Stucky, G.; Hansma, P. Direct visualization of surfactant hemimicelles by force microscopy of the electrical double layer. Langmuir 1994, 10, 4409–4413. [Google Scholar] [CrossRef]
  10. Manne, S.; Gaub, H.E. Molecular organization of surfactants at solid-liquid interfaces. Science 1995, 270, 1480. [Google Scholar] [CrossRef]
  11. Ducker, W.A.; Grant, L.M. Effect of substrate hydrophobicity on surfactant surface−aggregate geometry. J. Phys. Chem. 1996, 100, 11507–11511. [Google Scholar] [CrossRef]
  12. Lamont, R.; Ducker, W. Organized structure of lithium perfluorooctanesulfonate at the graphite–solution interface. J. Colloid Interface Sci. 1997, 191, 303–311. [Google Scholar] [CrossRef] [PubMed]
  13. Johnson, R.; Nagarajan, R. Modeling self-assembly of surfactants at solid–liquid interfaces. II. Hydrophilic surfaces. Coll. Surf. A Physicochem. Eng. Asp. 2000, 167, 21–30. [Google Scholar] [CrossRef]
  14. Johnson, R.A.; Nagarajan, R. Modeling self-assembly of surfactants at solid/liquid interfaces. I. Hydrophobic surfaces. Coll. Surf. A Physicochem. Eng. Asp. 2000, 167, 31–46. [Google Scholar] [CrossRef]
  15. Warr, G.G. Surfactant adsorbed layer structure at solid/solution interfaces: Impact and implications of AFM imaging studies. Curr. Opin. Colloid Interface Sci. 2000, 5, 88–94. [Google Scholar] [CrossRef]
  16. Xu, S.L.; Wang, C.; Zeng, Q.D.; Wu, P.; Wang, Z.G.; Yan, H.K.; Bai, C.L. Self-assembly of cationic surfactants on a graphite surface studied by STM. Langmuir 2002, 18, 657–660. [Google Scholar] [CrossRef]
  17. Ferrari, M.; Ravera, F.; Viviani, M.; Liggieri, L. Characterization of surfactant aggregates at solid–liquid surfaces by atomic force microscopy. Coll. Surf. A Physicochem. Eng. Asp. 2004, 249, 63–67. [Google Scholar] [CrossRef]
  18. Tulpar, A.; Ducker, W.A. Surfactant adsorption at solid–aqueous interfaces containing fixed charges: Experiments revealing the role of surface charge density and surface charge regulation. J. Phys. Chem. B 2004, 108, 1667–1676. [Google Scholar] [CrossRef]
  19. Domínguez, H. Self-aggregation of the sds surfactant at a solid–liquid interface. J. Phys. Chem. B 2007, 111, 4054–4059. [Google Scholar] [CrossRef] [PubMed]
  20. Schniepp, H.C.; Shum, H.C.; Saville, D.A.; Aksay, I.A. Surfactant aggregates at rough solid–liquid interfaces. J. Phys. Chem. B 2007, 111, 8708–8712. [Google Scholar] [CrossRef] [PubMed]
  21. Chen, M.; Burgess, I.; Lipkowski, J. Potential controlled surface aggregation of surfactants at electrode surfaces—A molecular view. Surf. Sci. 2009, 603, 1878–1891. [Google Scholar] [CrossRef]
  22. Bernardes, J.S.; Rezende, C.A.; Galembeck, F. Morphology and self-arraying of SDS and DTAB dried on mica surface. Langmuir 2010, 26, 7824–7832. [Google Scholar] [CrossRef] [PubMed]
  23. Gao, X.; Chorover, J. Adsorption of sodium dodecyl sulfate (SDS) at ZnSe and α-Fe2O3 surfaces: Combining infrared spectroscopy and batch uptake studies. J. Colloid Interface Sci. 2010, 348, 167–176. [Google Scholar] [CrossRef] [PubMed]
  24. Karlsson, P.M.; Anderson, M.W.; Palmqvist, A.E. Adsorption of sodium dodecyl sulfate and sodium dodecyl phosphate at the surface of aluminium oxide studied with AFM. Corros. Sci. 2010, 52, 1103–1105. [Google Scholar] [CrossRef]
  25. Seiedi, O.; Rahbar, M.; Nabipour, M.; Emadi, M.A.; Ghatee, M.H.; Ayatollahi, S. Atomic force microscopy (afm) investigation on the surfactant wettability alteration mechanism of aged mica mineral surfaces. Energy Fuels 2010, 25, 183–188. [Google Scholar] [CrossRef]
  26. Zhang, H.; Wang, Y.E.; Fan, Q.; Zuo, Y.Y. On the low surface tension of lung surfactant. Langmuir 2011, 27, 8351. [Google Scholar] [CrossRef] [PubMed]
  27. Song, S.H.; Koelsch, P.; Weidner, T.; Wagner, M.S.; Castner, D.G. Sodium dodecyl sulfate adsorption onto positively charged surfaces: Monolayer formation with opposing headgroup orientations. Langmuir 2013, 29. [Google Scholar] [CrossRef] [PubMed]
  28. Liu, J.F.; Ducker, W.A. Surface-induced phase behavior of alkyltrimethylammonium bromide surfactants adsorbed to mica, silica, and graphite. J. Phys. Chem. B 1999, 103, 8558–8567. [Google Scholar] [CrossRef]
  29. Ducker, W.A.; Wanless, E.J. Adsorption of hexadecyltrimethylammonium bromide to mica: Nanometer-scale study of binding-site competition effects. Langmuir 1999, 15, 160–168. [Google Scholar] [CrossRef]
  30. Lamont, R.E.; Ducker, W.A. Surface-induced transformations for surfactant aggregates. J. Am. Chem. Soc. 1998, 120, 7602–7607. [Google Scholar] [CrossRef]
  31. Wanless, E.J.; Ducker, W.A. Organization of sodium dodecyl sulfate at the graphite−solution interface. J. Phys. Chem. 1996, 100, 3207–3214. [Google Scholar] [CrossRef]
  32. Domínguez, H. Structure of the sodium dodecyl sulfate surfactant on a solid surface in different nacl solutions. Langmuir 2009, 25, 9006–9011. [Google Scholar] [CrossRef] [PubMed]
  33. Wanless, E.J.; Ducker, W.A. Weak influence of divalent ions on anionic surfactant surface-aggregation. Langmuir 1997, 13, 1463–1474. [Google Scholar] [CrossRef]
  34. Deegan, R.D.; Bakajin, O.; Dupont, T.F.; Huber, G.; Nagel, S.R.; Witten, T.A. Capillary flow as the cause of ring stains from dried liquid drops. Nature 1997, 389, 827–829. [Google Scholar] [CrossRef]
  35. Goodwin, J. Colloids and Interfaces with Surfactants and Polymers: An Introduction, 1st ed.; John Wiley & Sons Ltd: West Sussex, UK, 2004. [Google Scholar]
  36. Cosgrove, T. Colloid Science: Principles, Methods and Applications, 1st ed.; Wiley-Blackwell: Oxford, UK, 2005. [Google Scholar]
  37. Edward, J.T. Molecular volumes and the stokes-einstein equation. J. Chem. Educ. 1970, 47, 261. [Google Scholar] [CrossRef]
  38. Coiro, V.; Manigrasso, M.; Mazza, F.; Pochetti, G. Structure of a triclinic phase of sodium dodecyl sulfate monohydrate. A comparison with other sodium dodecyl sulfate crystal phases. Acta Crystallogr. Sect. C Cryst. Struct. Commun. 1987, 43, 850–854. [Google Scholar] [CrossRef]
Figure 1. Atomic force microscopy (AFM) images (50 μm × 50 μm) and cross-section height profiles at: (a) 2 mM; and (b) 8.1 mM.
Figure 1. Atomic force microscopy (AFM) images (50 μm × 50 μm) and cross-section height profiles at: (a) 2 mM; and (b) 8.1 mM.
Materials 10 00555 g001
Figure 2. AFM images (10 μm × 10 μm) (a) at 2 mM and (b) at 8.1 mM; and (c) AFM error signal image from (b).
Figure 2. AFM images (10 μm × 10 μm) (a) at 2 mM and (b) at 8.1 mM; and (c) AFM error signal image from (b).
Materials 10 00555 g002
Figure 3. AFM images of SDS-inorganic salt aggregates on the surface of the glass: (a) SDS-NaCl; (b) SDS-KCl; (c) SDS-MgCl2; and (d) SDS-CaCl2.
Figure 3. AFM images of SDS-inorganic salt aggregates on the surface of the glass: (a) SDS-NaCl; (b) SDS-KCl; (c) SDS-MgCl2; and (d) SDS-CaCl2.
Materials 10 00555 g003
Figure 4. AFM images of SDS-inorganic salt aggregates on the surface of the glass: (a) SDS-NaCl; (b) SDS-NaI; and (c) SDS-NaNO2.
Figure 4. AFM images of SDS-inorganic salt aggregates on the surface of the glass: (a) SDS-NaCl; (b) SDS-NaI; and (c) SDS-NaNO2.
Materials 10 00555 g004
Figure 5. AFM result of SDS aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Figure 5. AFM result of SDS aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Materials 10 00555 g005
Figure 6. AFM result of SDS-NaCl aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Figure 6. AFM result of SDS-NaCl aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Materials 10 00555 g006
Figure 7. AFM result of SDS-CsCl aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Figure 7. AFM result of SDS-CsCl aggregates of the surface of the glass: (a) height image; (b) cross-section height profiles along the line in (a); and (c) 3D reconstruction image.
Materials 10 00555 g007
Figure 8. Schematic representation of possible mechanisms for surfactant adsorption on a glass slide: (a) SDS; and (b) SDS-monovalent ions.
Figure 8. Schematic representation of possible mechanisms for surfactant adsorption on a glass slide: (a) SDS; and (b) SDS-monovalent ions.
Materials 10 00555 g008

Share and Cite

MDPI and ACS Style

Shen, Z.-Y.; Lee, M.-T. On the Morphology of the SDS Film on the Surface of Borosilicate Glass. Materials 2017, 10, 555. https://doi.org/10.3390/ma10050555

AMA Style

Shen Z-Y, Lee M-T. On the Morphology of the SDS Film on the Surface of Borosilicate Glass. Materials. 2017; 10(5):555. https://doi.org/10.3390/ma10050555

Chicago/Turabian Style

Shen, Zih-Yao, and Maw-Tien Lee. 2017. "On the Morphology of the SDS Film on the Surface of Borosilicate Glass" Materials 10, no. 5: 555. https://doi.org/10.3390/ma10050555

APA Style

Shen, Z. -Y., & Lee, M. -T. (2017). On the Morphology of the SDS Film on the Surface of Borosilicate Glass. Materials, 10(5), 555. https://doi.org/10.3390/ma10050555

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop