Article

Effect of (Tb+Y)/Al ratio on Microstructure Evolution and Densification Process of (Tb0.6Y0.4)3Al5O12 Transparent Ceramics

1
Guangdong Engineering Technology Research Center of Efficient Green Energy and Environmental Protection Materials, Guangdong Key Laboratory of Quantum Engineering and Quantum Materials, School of Physics & Telecommunication Engineering, South China Normal University, Guangzhou 510006, China
2
State Key Laboratory of High Performance Ceramics and Superfine Microstructure, Shanghai Institute of Ceramics, Chinese Academy of Sciences, Shanghai 200050, China
3
Key Laboratory of Transparent Opto-functional Inorganic Materials, Shanghai Institute of Ceramics, Chinese Academy of Sciences, Shanghai 201899, China
4
Center of Materials Science and Optoelectronics Engineering, University of Chinese Academy of Sciences, Beijing 100049, China
*
Authors to whom correspondence should be addressed.
Materials 2019, 12(2), 300; https://doi.org/10.3390/ma12020300
Submission received: 24 December 2018 / Revised: 9 January 2019 / Accepted: 15 January 2019 / Published: 18 January 2019

Abstract

:
(Tb0.6Y0.4)3Al5O12 transparent ceramics were successfully fabricated by solid-state reactive sintering using Tb4O7, Y2O3, and α-Al2O3 powders as raw materials. The effect of (Tb+Y)/Al ratio on microstructure evolution and densification process was investigated in detailed. The results showed that the grain growth kinetics were significantly affected by (Tb+Y)/Al ratio. Al-rich and Tb-rich phases appeared in part of the samples of different ratios. Particularly, excess aluminum increased the diffusing process, leading to a higher densification rate, while samples with excess terbium ratios displayed a smaller grain size and lower relative density. The optical quality was highly related to the amount of the secondary phase produced by different (Tb+Y)/Al ratios. Finally, (Tb0.6Y0.4)3Al5O12 transparent ceramics have been fabricated through pre-sintering in vacuum, followed by hot isostatic sintering (HIP), and the best transmittance of sample with a 4 mm thickness was approximately 78% at 1064 nm.

1. Introduction

Magneto-optical material, including glass, single crystal, and transparent ceramic, is the crucial constitution of the optical isolators in high-power laser systems [1,2,3]. At present, due to the advantages of large Verdet constant, high thermal conductive, and low absorption, Tb3Ga5O12 (TGG) is one of the most commonly used commercial magneto-optical material of Faraday isolators [4,5,6]. Compared to TGG, Tb3Al5O12 (TAG) has a higher Verdet constant, which makes it a highly sought magneto-optical isolator material for future applications [7]. However, it is difficult to obtain TAG single crystals, due to incongruent melting [8,9,10]. Although many efforts have been devoted to solving this problem, the size of crystals is still too limited to meet the requirement of practical application [11,12]. This phenomenon can be effectively avoided by fabricating TAG transparent ceramic below the phase transition point, thanks to the cubic structure.
TAG transparent ceramic has been studied for many years since it was firstly reported in 2011 [13]. A large number of studies have been done investigating the preparation method, ion doping, and magneto-optical property improvements. More importantly, it was found that Y-doping can avoid strain generation and crack initiation during the sintering process. Chen et al. [14] successfully fabricated (Tb1−xRx)3Al5O12 (R = Y, Ce) ceramics by a two-step sintering method, and confirmed that Y3+ addition improved the optical quality of the TAG ceramics. Duan et al. [15] found Y-doping can optimize the microstructure of the TAG transparent ceramics and achieve a smaller average grain size. In 2017, Ikesue et al. [16] produced (Tb1−xYx)3Al5O12 transparent ceramics with ultralow optical loss for practical applications, promoting the commercial development of TAG transparent ceramics.
Even though most former studies have claimed that highly transparent TAG or TAG-based ceramics were fabricated, there was still numerous scatters that existed in the samples (pores, second phases, impurities, grain boundaries) which limited further improvement of the transmittance. Generally, in order to avoid the second phase, the ratio of RE/Al (RE is rare earth, such as Y, Lu, Dy) must be carefully controlled as 3/5, according to the binary phase diagram of RE2O3-Al2O3. Much research has been devoted to understanding the effect of composition deviation on several common garnet structures. Hu et al. [17] found that excess lutetium restrained abnormal grain growth by the impurity drag effect, while excess Al2O3 pinned in the grain boundary limited the fast migration of grain boundaries in Pr: LuAG transparent ceramics. Stanek et al. [18] studied the variation of lattice parameter with stoichiometry deviation, and non-stoichiometry in YAG proceeded through cation antisite defects, which would be a theoretical foundation in vacancy diffusion during the densification process. Liu et al. [19] investigated that a small excess of yttrium was tolerable for the optical quality of ceramics compared with excess alumina. They deduced that the average grain size abruptly decreased, and the porosity increased with the increasing of both excess Al2O3 and Y2O3. However, related works have not been carried out in TAG ceramic system, though it would be meaningful for obtaining transparent ceramics with excellent magneto-optical properties.
Generally, Tb4O7 instead of Tb2O3 is usually used as the raw material to prepare TAG transparent ceramics, owning to the instability of Tb2O3 at room temperature [20,21]. However, the precise contents of Tb3+ and Tb4+ in Tb4O7 powder can be hardly measured. In other words, Tb4O7 should actually be described as Tb4O7±x, making precise control of Tb/Al ratios impossible. Therefore, investigate different ratios will be significant for fabrication of high optical quality ceramics. In this paper, (Tb0.6Y0.4)3Al5O12 transparent ceramics were fabricated by reactive sintering in vacuum, followed by hot isostatic sintering (HIP) treatment and Tb4O7, Y2O3, and α-Al2O3 were used as raw powders. The effect of (Tb+Y)/Al ratio on the phase formation, densification process, and microstructure evolution was elaborately investigated.

2. Materials and Methods

2.1. Experimental Procedure

(Tb0.6Y0.4)3Al5O12 transparent ceramics with different (Tb+Y)/Al mole ratios (0.5964, 0.6000, 0.6036, 0.6073, and 0.6110) were fabricated with high-purity commercial Tb4O7 (99.99%, Jiahua Corp. Ltd., Jiangyin, China), Y2O3 (99.99%, Jiahua Corp. Ltd., Jiangyin, China), and α-Al2O3 (99.99%, Sumitomo Chemicals, Tokyo, Japan) powders. The particle sizes of three raw powders were 2, 1, and 0.2 μm, respectively. Meanwhile, 0.5 wt % TEOS (99.99%, Alfa Aesar Company, Beijing, China) and 0.1 wt % MgO (99.99%, Alfa Aesar Company, Beijing, China) were added as sintering aids. The powder mixtures was dispersed in 99.99% ethyl alcohol and ball-milled in nylon tank for 15 h. Then, the slurries were dried at 80 °C in oven for 24 h and sieved through a 100-mesh screen. After this, they were uniaxially pressed into plates in Φ 12 mm stainless steel molds at 20 MPa and cold isostatic pressing at 200 MPa for 5 min. In order to remove organics, plates were calcined at 800 °C for 6 h in a muffle furnace. The green bodies were pre-sintered at varieties temperatures (from 950 to 1550 °C) in a vacuum furnace (ZW-50-20, Chenrong Corp. Ltd., Shanghai, China) under a vacuum level of ~10−3 Pa for 4 h, followed by HIP at 1600 °C under 196 MPa Ar atmosphere. Finally, all samples were annealed at 1350 °C for 10 h in a muffle furnace (SSX-2-16, Yifeng Corp. Ltd., Shanghai, China), and mirror-polished to 4 mm on double sides.

2.2. Characterization

The phase compositions of pre-sintering plates were identified by X-ray diffraction (XRD; D2, Bruker, Hamburg, Germany) with Cu Kα radiation. The microstructures of the ceramics were characterized by scanning electron microscopy (SEM; JSM-6510, JEOL, Akishima, Japan). The element mapping was conducted with energy dispersive spectroscopy (EDS; SwiftED3000, HITACHI, Tokyo, Japan). The densities of the transparent ceramics were measured by Archimedes method. The in-line transmittances of the polished samples were measured by UV–vis–NIR spectrophotometer (Lambda 950; Perkin-Elmer, Waltham, MA, USA).

3. Results and Discussion

3.1. Phase Formation Process

The X-ray diffraction patterns in Figure 1 demonstrate the phase formation of the pre-sintered samples with 0.6000 ratio. The results confirm that Tb and Y react with Al2O3 and form a solid solution of yttrium terbium aluminum garnet (YTbAG). Specifically, Tb4O7 deoxygenates to Tb2O3 beyond 950 °C and Tb2O3, Y2O3, and Al2O3 can be detected at this temperature. Yttrium terbium aluminum monoclinic phase (YTbAM) forms at 1050 °C while the diffractions of raw powders still exist. With the temperature increasing, YTbAM and yttrium terbium aluminum perovskite phase (YTbAP) simultaneously appear at 1150 °C, and the diffraction intensity of YTbAM decreases. Meanwhile, YTbAP and some YTbAG are detected at 1250 °C while YTbAM has disappeared. When the temperature reaches 1350 °C, a pure YTbAG phase is generated and all peaks match well with TAG standard card (PDF#17-0735). No residual intermediate phases remain to be detected. In summary, YTbAM, YTbAP, and YTbAG appear in order with the reaction processing, which can be described by the formulas
Tb4O7 → Tb2O3 + O2 (beyond 950 °C),
Tb2O3 + Y2O3 + Al2O3 → YTbAM (950–1050 °C),
YTbAM + Al2O3 → YTbAP (1050–1250 °C),
YTbAP + Al2O3 → YTbAG (1250–1350 °C).

3.2. Densification and Microstructure

The relationship between relative density and pre-sintering temperature is shown in Figure 2. This indicated that the relative densities improved simultaneously with the increase of temperature for all samples. A rapid densification process between 1350 and 1450 °C can be observed, and the rate slows down from 1450 to 1550 °C. The density fluctuations tend to be flat when the temperature continues to increase. Regularly, the relative density decreases with the ratio of (Tb+Y)/Al increasing. The relative density of the 0.5964 ratio sample is 78%, while it is just 71% for the 0.6110 ratio sample at 1350 °C. Density distinction among different ratio samples constantly decreases as the pre-sintering temperature rises further. Finally, all of the densities with the different (Tb+Y)/Al ratios are almost coincident at 1550 °C, and they are above 99%.
Figure 3 shows the thermal etching surface of the as-prepared ceramics with different (Tb+Y)/Al ratios (0.5964, 0.6000, 0.6036, 0.6073, and 0.6110) pre-sintered from 1350 to 1500 °C. It is clearly observed that the average grain size of ceramics increases and the porosity decreases with the sintering temperature increasing, regardless of (Tb+Y)/Al ratios. Open pores can be easily observed at 1350 °C which change to being closed around 1400 °C. When the sintering temperature reaches 1450 °C, the samples possess uniform grains as well as high density. The microstructure evolution as well as porosity changes are consistent with the results displayed in Figure 2. It is worth mentioning that second phases at grain boundaries appear in part of the (Tb+Y)/Al ratio samples (0.5964, 0.6000, 0.6073, and 0.6110) when the sintering temperature reaches 1450 °C, and they are marked with red circles. For samples with (Tb+Y)/Al ratios of 0.5964 and 0.6000, the residual pores and average grain size are obviously larger than those samples with other ratios (0.6073 and 0.6110) below 1450 °C. The density distinction decreases with continually increasing temperature. However, for the sample with (Tb+Y)/Al ratio of 0.6036, the grain boundaries are clean and free from second phases and abnormal grains at each temperature. Unluckily, intergranular pores appear at 1500 °C and are unable to be removed by HIP treatment.
SEM micrograph and the corresponding EDS mapping images of various elements of the pre-sintered sample with two (Tb+Y)/Al ratios (0.6000 and 0.6073) are shown in Figure 4. Figure 4a indicates that Al2O3 second phases are detected in the sample with a ratio of 0.6000. Due to the lower atomic number, it looks darker. Meanwhile, Tb and Y disappear in this area. The mapping result of 0.6073 ratio is showed in Figure 4b, and excess Tb second phases exist in the bright area. Surprisingly, an interesting phenomenon occurs that the content of Si is also enriched. This may be caused by generation of a terbium silicate compound. Similar results were already reported in Nd: YAG transparent ceramics [22,23].
The rare earth-controlled densification and average grain size were already discovered in YAG [24,25]. In this investigation, it can be explained that (Tb+Y)/Al ratios affect the sintering behavior via generating structural defects which can promote or inhibit densification and grain growth, relying on their atoms’ diffusion kinetics. When excess Al reacts with terbium in the system, it generates a high concentration of vacancies, which increases the diffusion rate during the sintering process. The second phase does not produce a pinning effect, and the grain boundaries migrate, sequentially, with higher temperature. When Tb is in excess, it consumes the bulk concentration of rare earth vacancies so that the diffusion kinetics of rare earth species would be limited. This also indicates that excess terbium hinders the grain growth which is significantly effective at lower temperatures.
HIP treatment is a typical method in fabricating optical ceramics, because it can remove residual intergranular pores and further improve the densification. There is more suitable microstructure of pre-sintering ceramics before HIP due to no intragranular pores, higher relative density, and smaller grain size. Therefore, the microstructures of samples pre-sintered at 1450 °C and treated by 1600 °C HIP are displayed in Figure 5. It can be seen that residual pores are removed through HIP treatment. At the same time, the average grain size also obviously grows despite the second phases remain in some samples.

3.3. Optical Quality

Figure 6 shows the in-line transmittance curves of samples pre-sintered at 1450 °C followed by 1600 °C HIP treatment. Specifically, excess aluminum enormously affects the transmittance both in the visible and near-infrared region, while the transmittance lines of excess terbium samples are lower than the sample with 0.6036 ratio, and it decreases quickly along with the wavelength decreasing. Actually, this phenomenon is explained by the Mie scattering caused by residual pores [26]. The absorption peak at 484 nm is attributed to the Tb3+: 7F65D4 transition. The best optical quality sample, whose transmittance reaches 78% at 1064 nm, is obtained by a (Tb+Y)/Al ratio of 0.6036. Macroscopic observations of (Tb0.6Y0.4)3Al5O12 transparent ceramics with different (Tb+Y)/Al ratios are displayed inside. The samples with 0.6036, 0.6073, and 0.6110 ratios are transparent, with words being clearly seen below the photograph, while 0.5964 and 0.6000 ratio samples are opaque. The bright yellow appearance is connected with the valence state of terbium.

4. Conclusions

(Tb0.6Y0.4)3Al5O12 transparent ceramics were fabricated by vacuum pre-sintering and HIP treatment. Due to the uncertain volume of terbium in Tb4O7 raw powders, the influence of different (Tb+Y)/Al ratios on the densification process and optical properties of (Tb0.6Y0.4)3Al5O12 transparent ceramics were studied in detail. Meanwhile, results indicated that excess aluminum ((Tb+Y)/Al = 0.5964 and 0.6000) made the densification process faster, while excess terbium ((Tb+Y)/Al = 0.6073 and 0.6110) caused decay and hindered grain growth. More importantly, the excess aluminum or terbium caused second phases to appear, which seriously affected the sample optical properties. Finally, transparent ceramic with (Tb+Y)/Al = 0.6036 pre-sintered at 1450 °C in vacuum, followed by HIP treatment at 1600 °C, resulted in better optical quality and a transmittance of up to 78% at 1064 nm in a sample of 4 mm thickness was obtained.

Author Contributions

Z.W., Y.W., J.Z. and S.W. designed the project; Z.W., J.W. and D.W. performed the experiments; Z.W., J.Z. and D.H. analyzed the data and wrote the manuscript.

Funding

This work was supported by funding from National Key R&D Program of China (No. 2017YFB0310500).

Acknowledgments

Thanks for the memorable time spending in South China Normal University and Shanghai Institute of Ceramics, Chinese Academy of Sciences.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Víllora, E.G.; Molina, P.; Nakamura, M.; Shimamura, K.; Hatanaka, T.; Funaki, A.; Naoe, K. Faraday rotator properties of Tb3[Sc1.95Lu0.05](Al3)O12, a highly transparent terbium-garnet for visible-infrared optical isolators. Appl. Phys. Lett. 2011, 99, 011111. [Google Scholar] [CrossRef]
  2. Vasyliev, V.; Molina, P.; Nakamura, M.; Víllora, E.G.; Shimamura, K. Magneto-optical properties of Tb0.81Ca0.19F2.81 and Tb0.76Sr0.24F2.76 single crystals. Opt. Mater. 2011, 33, 1710–1714. [Google Scholar] [CrossRef]
  3. Mansell, J.D.; Hennawi, J.; Gustafson, E.K.; Fejer, M.M.; Byer, R.L.; Clubley, D.; Yoshida, S.; Reitze, D.H. Evaluating the effect of transmissive optic thermal lensing on laser beam quality with a shack-hartmann wave-front sensor. Appl. Opt. 2001, 40, 366–374. [Google Scholar] [CrossRef] [PubMed]
  4. Barati, M.; Vahdani, M.R.K.; Rezaei, G. Lower-lying states of hydrogenic impurity in lens-shaped and semi-lens-shaped quantum dots. J. Phys. Condens. Matter 2007, 19, 136208. [Google Scholar] [CrossRef]
  5. Ikesue, A.; Yoshida, K.; Yamamoto, T.; Yamaga, I. Optical Scattering Centers in Polycrystalline Nd: YAG Laser. J. Am. Ceram. Soc. 1997, 80, 6. [Google Scholar]
  6. Ivanov, I.; Bulkanov, A.; Khazanov, E.; Mukhin, I.B.; Palashov, O.V.; Tsvetkov, V.; Popov, P. Terbium gallium garnet for high average power Faraday isolators: Modern aspects of growing and characterization. In Proceedings of the European Conference on Lasers & Electro-Optics & the European Quantum Electronics Conference Cleo Europe-EQEC, Munich, Germany, 14–19 June 2009. [Google Scholar]
  7. Ganschow, S.; Klimm, D.; Reiche, P.; Uecker, R. On the Crystallization of Terbium Aluminum Garnet. Cryst. Res. Technol. 2010, 34, 615–619. [Google Scholar] [CrossRef]
  8. Ganschow, S.; Klimm, D.; Epelbaum, B.M.; Yoshikawa, A.; Doerschel, J.; Fukuda, T. Growth conditions and composition of terbium aluminum garnet single crystals grown by the micro pulling down technique. J. Cryst. Growth 2001, 225, 454–457. [Google Scholar] [CrossRef]
  9. Geho, M.; Sekijima, T.; Fujii, T. Growth mechanism of incongruently melting terbium aluminum garnet (Tb3Al5O12; TAG) single crystals by laser FZ method. J. Cryst. Growth 2005, 275, e663–e667. [Google Scholar] [CrossRef]
  10. Geho, M.; Sekijima, T.; Fujii, T. Growth of terbium aluminum garnet (Tb3Al5O12; TAG) single crystals by the hybrid laser floating zone machine. J. Cryst. Growth 2004, 267, 188–193. [Google Scholar] [CrossRef]
  11. Shimamura, K.; Kito, T.; Castel, E.; Latynina, A.; Molina, P.; Víllora, E.G.; Mythili, P.; Veber, P.; Chaminade, J.-P.; Funaki, A.; et al. Growth of Tb3[Sc2−xLux](Al3)O12 Single Crystals for Visible-Infrared Optical Isolators. Cryst. Growth Des. 2010, 10, 3466–3470. [Google Scholar] [CrossRef]
  12. Chani, V.I.; Yoshikawa, A.; Machida, H.; Fukuda, T. Melt growth of (Tb, Lu)3Al5O12 mixed garnet fiber crystals. J. Cryst. Growth 2000, 212, 469–475. [Google Scholar] [CrossRef]
  13. Lin, H.; Zhou, S.; Teng, H. Synthesis of Tb3Al5O12 (TAG) transparent ceramics for potential magneto-optical applications. Opt. Mater. 2011, 33, 1833–1836. [Google Scholar] [CrossRef]
  14. Chen, C.; Zhou, S.; Lin, H.; Yi, Q. Fabrication and performance optimization of the magneto-optical (Tb1−xRx)3Al5O12 (R = Y, Ce) transparent ceramics. Appl. Phys. Lett. 2012, 101, 131908. [Google Scholar] [CrossRef]
  15. Duan, P.; Liu, P.; Xu, X.; Wang, W.; Wan, Z.; Zhang, S.; Wang, Y.; Zhang, J. Fabrication and properties of (TbxY1−x)3Al5O12, transparent ceramics by hot isostatic pressing. Opt. Mater. 2017, 72, 58–62. [Google Scholar] [CrossRef]
  16. Aung, Y.L.; Ikesue, A. Development of optical grade (TbxY1−x)3Al5O12 ceramics as Faraday rotator material. J. Am. Ceram. Soc. 2017, 100, 4081–4087. [Google Scholar] [CrossRef]
  17. Hu, Z.; Chen, X.; Dai, J.; Chen, H.; Shi, Y.; Kou, H.; Xie, T.; Yang, Z.; Wu, L.; Pan, Y.; et al. The influences of stoichiometry on the sintering behavior, optical and scintillation properties of Pr: LuAG ceramics. J. Eur. Ceram. Soc. 2018, 38, 4252–4259. [Google Scholar] [CrossRef]
  18. Stanek, C.R.; Mc Clellan, K.J.; Patel, A.P.; Levy, M.R.; Grimes, R.W.; Gaume, R.M.; Feigelson, R.S. Mechanisms of nonstoichiometry in Y3Al5O12. Appl. Phys. Lett. 2008, 93, R19. [Google Scholar]
  19. Liu, J.; Cheng, X.; Li, J.; Xie, T.; Ivanov, M.; Ba, X.; Chen, H.; Liu, Q.; Pan, Y.; Guo, J. Influence of non-stoichiometry on solid-state reactive sintering of YAG transparent ceramics. J. Eur. Ceram. Soc. 2015, 35, 3127–3136. [Google Scholar] [CrossRef]
  20. Ikesue, A.; Aung, Y.L.; Makikawa, S.; Yahagi, A. Polycrystalline (TbxY1–x)2O3 Faraday rotator. Opt. Lett. 2017, 42, 4399–4401. [Google Scholar] [CrossRef]
  21. Burnham, D.A.; Eyring, L.R.; Kordis, J. High-temperature x-ray diffraction studies of the terbium oxide-oxygen and mixed cerium terbium oxide-oxygen systems. J. Phys. Chem. 1968, 72, 4424–4431. [Google Scholar] [CrossRef]
  22. Maıˆtre, A.; Sallé, C.; Boulesteix, R.; Baumard, J.F.; Rabinovitch, Y. Effect of Silica on the Reactive Sintering of Polycrystalline Nd: YAG Ceramics. J. Am. Ceram. Soc. 2008, 91, 406–413. [Google Scholar] [CrossRef]
  23. Lee, S.-H.; Kupp, E.R.; Stevenson, A.J.; Anderson, J.M.; Messing, G.L.; Li, X.; Dickey, E.C.; Dumm, J.Q.; Simonaitis-Castillo, V.K.; Quarles, G.J. Hot Isostatic Pressing of Transparent Nd: YAG Ceramics. J. Am. Ceram. Soc. 2009, 92, 8. [Google Scholar] [CrossRef]
  24. Boulesteix, R.; Maitre, A.; Baumard, J.; Sallé, C.; Rabinovitch, Y. Mechanism of the liquid phase sintering for Nd: YAG ceramics. Opt. Mater. 2009, 31, 711–715. [Google Scholar] [CrossRef]
  25. Kuklja, M.M. Defects in yttrium aluminum perovskite and garnet crystals: Atomistic study. J. Phys. Condens. Matter 2000, 12, 2953. [Google Scholar] [CrossRef]
  26. Liu, W.; Jiang, B.; Zhang, W.; Li, J.; Zhou, J.; Zhang, D.; Pan, Y.; Guo, J. Influence of heating rate on optical properties of Nd: YAG laser ceramic. Ceram. Int. 2010, 36, 2197–2201. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of (Tb0.6Y0.4)3Al5O12 pre-sintered every 100 °C from 950 to 1350 °C, in vacuum.
Figure 1. XRD patterns of (Tb0.6Y0.4)3Al5O12 pre-sintered every 100 °C from 950 to 1350 °C, in vacuum.
Materials 12 00300 g001
Figure 2. Relationship between relative density and pre-sintering temperature with different (Tb+Y)/Al ratios.
Figure 2. Relationship between relative density and pre-sintering temperature with different (Tb+Y)/Al ratios.
Materials 12 00300 g002
Figure 3. SEM micrographs of the thermal etching surface of different (Tb+Y)/Al ratio samples (AE represent 0.5964, 0.6000, 0.6036, 0.6073 and 0.6110) pre-sintered at different temperatures (1 to 4 represent 1350, 1400, 1450, and 1500 °C).
Figure 3. SEM micrographs of the thermal etching surface of different (Tb+Y)/Al ratio samples (AE represent 0.5964, 0.6000, 0.6036, 0.6073 and 0.6110) pre-sintered at different temperatures (1 to 4 represent 1350, 1400, 1450, and 1500 °C).
Materials 12 00300 g003
Figure 4. Energy dispersive spectroscopy of two ratios pre-sintered at 1450 °C: (a) 0.6000, (b) 0.6073.
Figure 4. Energy dispersive spectroscopy of two ratios pre-sintered at 1450 °C: (a) 0.6000, (b) 0.6073.
Materials 12 00300 g004
Figure 5. SEM images of different (Tb+Y)/Al ratio samples (AE represent 0.5964, 0.6000, 0.6036, 0.6073 and 0.6110) pre-sintered at 1450 °C and with 1600 °C HIP treatment.
Figure 5. SEM images of different (Tb+Y)/Al ratio samples (AE represent 0.5964, 0.6000, 0.6036, 0.6073 and 0.6110) pre-sintered at 1450 °C and with 1600 °C HIP treatment.
Materials 12 00300 g005
Figure 6. Transmittances of different (Tb+Y)/Al ratios pre-sintered at 1450 °C and with 1600 °C HIP treatment (4 mm thickness); Macroscopic observations of (Tb0.6Y0.4)3Al5O12 with different (Tb+Y)/Al ratios are displayed inside: from left to right (0.5964, 0.6000, 0.6036, 0.6073, and 0.6110).
Figure 6. Transmittances of different (Tb+Y)/Al ratios pre-sintered at 1450 °C and with 1600 °C HIP treatment (4 mm thickness); Macroscopic observations of (Tb0.6Y0.4)3Al5O12 with different (Tb+Y)/Al ratios are displayed inside: from left to right (0.5964, 0.6000, 0.6036, 0.6073, and 0.6110).
Materials 12 00300 g006

Share and Cite

MDPI and ACS Style

Wan, Z.; Wang, Y.; Zhang, J.; Wang, S.; Han, D.; Wang, J.; Wang, D. Effect of (Tb+Y)/Al ratio on Microstructure Evolution and Densification Process of (Tb0.6Y0.4)3Al5O12 Transparent Ceramics. Materials 2019, 12, 300. https://doi.org/10.3390/ma12020300

AMA Style

Wan Z, Wang Y, Zhang J, Wang S, Han D, Wang J, Wang D. Effect of (Tb+Y)/Al ratio on Microstructure Evolution and Densification Process of (Tb0.6Y0.4)3Al5O12 Transparent Ceramics. Materials. 2019; 12(2):300. https://doi.org/10.3390/ma12020300

Chicago/Turabian Style

Wan, Zhong, Yinzhen Wang, Jian Zhang, Shiwei Wang, Dan Han, Junping Wang, and Dewen Wang. 2019. "Effect of (Tb+Y)/Al ratio on Microstructure Evolution and Densification Process of (Tb0.6Y0.4)3Al5O12 Transparent Ceramics" Materials 12, no. 2: 300. https://doi.org/10.3390/ma12020300

APA Style

Wan, Z., Wang, Y., Zhang, J., Wang, S., Han, D., Wang, J., & Wang, D. (2019). Effect of (Tb+Y)/Al ratio on Microstructure Evolution and Densification Process of (Tb0.6Y0.4)3Al5O12 Transparent Ceramics. Materials, 12(2), 300. https://doi.org/10.3390/ma12020300

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop