Review

Comprehensive Review of Polymer Architecture for All-Solid-State Lithium Rechargeable Batteries

Center of Excellence in Transportation Electrification and Energy Storage (CETEES), Hydro-Québec, 1806, Lionel-Boulet Blvd., Varennes, QC J3X 1S1, Canada
*
Author to whom correspondence should be addressed.
Materials 2020, 13(11), 2488; https://doi.org/10.3390/ma13112488
Submission received: 24 April 2020 / Revised: 27 May 2020 / Accepted: 27 May 2020 / Published: 29 May 2020

Abstract

:
Solid-state batteries are an emerging option for next-generation traction batteries because they are safe and have a high energy density. Accordingly, in polymer research, one of the main goals is to achieve solid polymer electrolytes (SPEs) that could be facilely fabricated into any preferred size of thin films with high ionic conductivity as well as favorable mechanical properties. In particular, in the past two decades, many polymer materials of various structures have been applied to improve the performance of SPEs. In this review, the influences of polymer architecture on the physical and electrochemical properties of an SPE in lithium solid polymer batteries are systematically summarized. The discussion mainly focuses on four principal categories: linear, comb-like, hyper-branched, and crosslinked polymers, which have been widely reported in recent investigations as capable of optimizing the balance between mechanical resistance, ionic conductivity, and electrochemical stability. This paper presents new insights into the design and exploration of novel high-performance SPEs for lithium solid polymer batteries.

1. Introduction

As a major portable power source, lithium-ion batteries (LIBs) are widely used in consumer electronics as well as electric vehicles (EVs). Because they present a higher power density than conventional secondary batteries such as Ni-Cd batteries, and a higher energy density than capacitors, like shown in Figure 1 [1,2,3,4,5]. Currently, most of the LIBs utilize liquid electrolytes because of their high ionic conductivity at ambient temperature. However, the safety issues of liquid electrolytes, such as the flammability and leakage, are hindering the development of LIBs [6]. The appearance of gelled polymer electrolytes (GPEs), in which liquid solvent is immobilized in a polymer matrix [7], can reduce the risk of leakage, but not the flammability. An SPE is defined as an ion-conductive phase composed of salt and salt-solvating macromolecules [8,9]. Compared with conventional lithium-ion batteries with a liquid electrolyte, using SPEs can enhance the energy density and safety of batteries [10,11]. Ever since PEO/alkali salt complex as a polymer electrolyte in lithium batteries was first reported in 1978 [12], the use of this type of electrolyte has captured the interest of researchers worldwide. In the 1980s, an exploration period for SPEs, the investigations were focused on ion transport mechanism and ionic conductivity enhancement as well as the production of lithium secondary batteries. Hydro-Québec and two French laboratories reported the first 3 V lithium secondary battery with a PEO electrolyte in 1985 [13]. Chatani et al. [14] published the first full crystallographic determination of a PEO/salt complex in 1987. The 1990s and 2000s represented a fast development period of LIBs, including electrode and electrolyte materials [15]. In 1991, the successful commercialization of LIB by Sony initiated a steep increase in the production of portable electronics, which accelerated the development of high energy density LIBs. In the same period, lithium-polymer battery technology was also developed for electric vehicle applications. In 1998, 3M (Rogers, AR, USA), Hydro-Québec and Argonne National Laboratories developed a lithium polymer battery of 119 Ah for EVs [16]. In recent years, the emergence of numerous new host polymers and salts has also given impetus to the development of solid polymer electrolytes.
In view of the current global climate situation, it is urgent to develop zero-emission power sources to reduce greenhouse effects. The first candidates for such power sources are all solid-state lithium polymer batteries (ASSLPBs). This is because they exhibit balanced characteristics of safety, energy density, power density, and cost compared with other batteries [17,18]. In 2011, the first commercial EV (Bluecar®) equipped ASSLPB as a power source appeared in Paris [19]. Today, the widespread diffusion of EVs all over the world irritates the battery technology improvement. Accordingly, to achieve high power performance, this research is focused on the development of battery materials. In their present state, ASSLPBs generally consist of a metallic lithium anode, a lithium iron phosphate (LFP) or nickel-manganese-cobalt (NMC) cathode, an SPE, and an insulated separator, as illustrated in Figure 2. In the SPE, the lithium ions are set in motion when the battery is charged or discharged. Compared with ceramic electrolytes, SPEs exhibit a lower interfacial impedance with electrodes because of their better flexibility and interfacial adhesion. Currently, SPEs are not only employed in lithium batteries but also in other energy accumulators, such as fuel cells [20], dye-sensitized solar cells [21], and supercapacitors [22]. Despite the many advantages that SPEs afford over liquid and ceramic electrolytes, they also exhibit certain disadvantages, such as lower ionic conductivity at low temperatures (<50 °C) and poor electrochemical stability at high voltage levels (>4.5 V). To overcome these limitations, considerable efforts have therefore been devoted to their investigation. An ideal SPE should be easy to fabricate and inexpensive, as well as possess high ionic conductivity at a wide temperature range, high chemical and electrical stability, and good mechanical strength and flexibility.
Many excellent reviews have summarized the development of SPEs, including PEO-based SPEs [23,24,25], poly(ionic liquid) (PIL) SPEs [26,27], composite SPEs [28,29], single lithium-ion conducting SPEs [30], and SPE additives and salts [31,32]. This paper focuses on the influence of polymer architecture on the physical and electrochemical properties of SPEs in ASSLPBs, which is yet to be reviewed. To optimize the balance between mechanical resistance, ionic conductivity, and electrochemical stability, four principal categories, which have been widely elaborated in recent investigations, are examined: linear, comb-like, hyper-branched, and crosslinked polymers. In view of the various ion transport mechanisms, the discussion centers on two types of electrolytes: PEO-based and PIL SPEs. It is assumed that this review will provide new insights into the design of novel high-performance SPEs for ASSLPBs.

2. Theoretical Background

Before polymer architecture is discussed, the ion transport mechanism of SPEs is briefly reviewed herein. As known, most polymers are recognized as poor ionic conductors. The ionic conductivity of a polymer electrolyte generally emanates from the contributions of all free ions of dissolved salts or polymeric salts, as expressed by:
σ = n i q i μ i
where ni is the ion concentration (number of ions per unit volume); qi is the ion charge; μi is the ion mobility (average ion velocity), which can be further described by the following Einstein relationship:
μ = D q k B T
where D is the diffusion constant; kB is Boltzmann constant; T is the absolute temperature. The ionic conductivity of a given polymer electrolyte is therefore mainly associated with ion concentration and temperature.
Solid polymer electrolytes can be categorized into salt-polymer complex electrolytes and single-ion polymer electrolytes (polymeric salts) according to their composition. In the former, lithium salts are dissolved in polymer matrices containing atoms or functional groups that are capable of coordinating with cations. It is found that only oxygen, nitrogen, and sulfur atoms can form the coordination bond with lithium ions [33]. The stability of lithium complexes decreases in the following order: O > N > S. Single-ion polymer electrolytes typically consist of polymerized anions and mobile lithium cations or an anion acceptor [34]. In fact, both this type of polymer electrolytes and PILs can be considered as polyelectrolytes in which polymer chains bear dissociating groups in their repeat units [35].
When a non-ionic polymer is used as an ion-solvating medium in salt-polymer complex electrolytes (e.g., PEO), lithium cations transfer by hopping between any two adjacent coordinating sites located in the intra-chain and inter-chain in an electric field, as shown in Figure 3.
The dynamics of cations is linked to the polymer segmental motion in the amorphous state above the glass transition temperature (Tg) of the polymer. No evident ion motion has been observed in the crystalline and amorphous sections at temperatures below Tg [36,37]. In this case, the relationship between temperature and ion conductivity can be described by the non-linear Vogel–Fulcher–Tammann (VFT) equation:
σ = σ 0 e x p ( B T T 0 )
where σ0 is the pre-exponential parameter and B is the pseudo-activation energy; T0 is an empirically determined temperature (10–50 °C) that is below Tg.
In another case, the Li+ transport is less dependent on the segmental motion. The conduction mechanism follows Arrhenius model:
σ = σ 0 e x p ( E 0 k B T )
where E0 is the activation energy and kB is the Boltzmann constant. The relationship between ion conductivity and 1/T is linear, and the activation energy E0 can be determined by finding the slop of Arrhenius plots.
Compared to non-ionic polymers, ionic hosts, such as PILs, have a higher dielectric constant and electrochemical stability; most PILs have a measure of ion conductivity. In ionic liquid electrolytes, the Li+ cation transport occurs by anion exchange with its adjacent coordinating sites during Li+ movement via electrostatic interaction [38], which is similar to vehicular mechanism [39]. With regard to PILs, most studies on ion transport focus on pure polymer without lithium salt addition [40]; however, the lithium cation transport mechanism in PILs has not been reported.
As mentioned, the cations and anions in salt-polymer complex electrolytes are all mobile. This usually reduces the transference number, which is defined as the ratio of the electric current derived from the cation to the total electric current, thereby leading to concentration polarization. In order to increase this number, the counterpart of lithium cation can be attached to the macromolecular chains by a covalent bond or an anion acceptor. Computer simulations and experimental results demonstrate that the cation transport in this case also occurs through ion hopping among anion sites and considerably depends on the rotation of polymer segments. A higher ionic conductivity can be obtained for a single-ion polymer electrolyte with a lower Tg, such as salt-polymer electrolytes. Despite the high cation transference number in a single-ion polymer electrolyte, however, its ionic conductivity is lower than that of salt-polymer electrolyte because of the insufficient dissociation of Li+ ions in such electrolytes.
Overall, regardless of the electrolyte system, the ion transport is mainly linked to polymer segmental mobility, i.e., the Tg of polymer host. Another important factor that varies with the electrolyte architecture is its mechanical strength. When metallic lithium is used as the battery anode, high tensile modulus electrolytes can inhibit the nucleation and growth of lithium dendrites which often cause a battery short-circuit [41,42]. In the following sections, the architecture of the polymer host used in SPEs and its effect on ion mobility, as well as its mechanical properties and electrochemical stability, are summarized.

3. PEO-Based SPEs

3.1. Linear Polymer

The simplest polymer structure is a linear chain, and initial investigations of SPEs started with a linear PEO. Wright et al. first discovered the ionic conductivity of PEO/alkali salts in 1973 [43]. Five years later, M. Armand proposed the use of this complex as an electrolyte in secondary lithium batteries [10]. In the past 40 years, it has been demonstrated that PEO, which is the most frequently studied polymer host, has good ionic conductivity in an amorphous state and electrochemical stability. It also has an excellent compatibility with other organic or inorganic materials, which is crucial for a polymer to be regarded as the best candidate for SPEs. The advantages and disadvantages of PEO-based electrolytes have already been reported by certain articles [23,24]; hence, these are not repeated here.
In addition to PEO, polymers that contain oxygen or nitrogen atoms (e.g., polyethers, polycarbonates, polyesters, and polynitriles) as solvating hosts of lithium salts have been investigated. However, the degradation of polycarbonates and polyesters [44] and the low ionic conductivity of lithium cation in polynitriles [45] limit their further application.
Although other polyethers, such as poly(propylene oxide) [46,47], polytetrahydrofuran [48], and poly(1,3-dioxolane) [49,50], have also exhibited physical and electrochemical properties similar to those of PEO, these have not been widely investigated because of the dearth of products with high molecular weights.
At present, as the demands of the battery market continue to increase, there remain three main problems in PEO-based SPEs that should be resolved. These include low ionic conductivity at low temperatures, low transference number, and relatively narrow electrochemical window when a high-voltage cathode is used. To overcome the foregoing, various strategies have been conceived, including the addition of organic plasticizers [51], inorganic fillers [52], natural fibers [53], and ceramic particles [54] to SPEs. The use of PEO-based polymer blends and copolymers has also been explored, and a recent review has summarized the benefits of employing PEO-based block copolymer electrolytes for lithium batteries [55]. The incorporation of different polymer segments can enhance not only the ionic conductivity but also the mechanical properties of PEO. Furthermore, copolymers with a single-lithium ion block have been observed to exhibit a higher transference number.
Another effective approach that affects the electrochemical properties of PEO-based electrolytes is modifying the polymer host architecture. Three structures are discussed in the succeeding paragraphs.

3.2. Comb-Like Polymer

Typically, the operational temperature of linear PEO-based SPEs is approximately 80 °C, which exceeds the PEO melting temperature. Under this condition, the PEO’s mechanical resistance is considerably inadequate to alleviate the growth of lithium metal dendrites during cycling [56]. Based on this, many comb-like polymers with side oligo(ethylene oxide) chains, acting as lithium cation coordinating sites, were synthesized, and the influence of the main polymer chain structure and grafting degree on ionic conductivity and mechanical strength has been investigated. Table 1 summarizes the common main polymer backbone and some of the electrochemical results.
Polyphosphazene [57,58] and polysiloxane are generally used as the main polymer chains for oxyethylene-grafted polymer electrolytes. The benefits afforded by these main chains result from their thermal stability, high dielectric constant, and flexibility. Oxyethylene-grafted polyphosphazenes (MEEPs) are usually synthesized with alkoxide-end oligo(ethylene oxide) and poly(chlorophosphazene) (Figure 4). In literature, however, only extremely short grafted side chains are reported [59,60]. The MEEPs are amorphous with a Tg less than −60 °C [61], indicating good segmental mobility. Consequently, MEEP-based SPEs exhibit a considerably higher conductivity than PEOs at room temperature [62]. However, MEEPs undergo viscous flow under pressure because of the lack of dimensional stability and mechanical resistance.
Polymers, being considerably similar to MEEPs (with polysiloxane as backbone and side PEO chains), are also amorphous with a low Tg value of less than −60 °C. In view of this, polymers also have a good ionic conductivity at room temperature but insufficient mechanical strength [63]; hence, polysiloxane-based SPEs usually have a crosslinking structure. Their mechanical and electrochemical properties are discussed in the section on crosslinked polymers. Borodin et al. presented a report on the mechanism of lithium cation transport in an all-ethylene oxide (EO) comb-like polymer in which a considerably flexible main chain was used [64]. Their study clearly illustrates the occurrence of ion transport in the main and side chains—Li+ cations have the highest and lowest probabilities of being coordinated by EOs near the polyepoxide ether polymer backbone and at the side chain ends, respectively. The most mobile Li+ cations hop from a side chain to another without being complexed by the backbone.
Compared with flexible backbones, a methacrylate polymer main chain is considerably stronger. Poly(ethylene glycol) methacrylate (PEGMA) is the most widely used monomer in the preparation of comb-like polymers with ethylene oxide-containing side groups. The PEGMA homopolymer is amorphous and has a good mechanical resistance. Recently, Yao et al. reported a high-conductivity SPE based on poly(ethylene glycol) methyl ether methacrylate (PEGMEM) [65]. Three comb-like polymer-bearing side poly(ethylene glycol) (PEG) chains with different molecular weights are prepared by ultraviolet (UV) polymerization. Optimal electrochemical results are obtained for the SPE with LiTFSI salt and a 950 g∙mol−1 PEGMEM. The SPE exhibits a high conductivity of 1.44 × 10−4 S∙cm−1 at 30 °C with EO/Li+ = 18:1. In a previous report, Zhang et al. studied the physicochemical and electrochemical behaviors of linear PEO in the presence of lithium bis(fluorosulfonyl)imide (LiFSI) and LiTFSI salts [66]. The SPE membranes prepared by solution casting with PEO/LiFSI and PEO/LiTFSI at an EO/Li+ = 20:1 exhibit crystallinities of 44% and 47%, respectively, resulting in a decrease in the conductivity of SPEs at 60 °C. A comparison of ionic conductivity as a function of temperature between linear and comb-like polymers is shown in Figure 5. Ignoring the slight difference in Li+ concentration, the conductivities in both cases are similar, i.e., above 60 °C. The SPE with a comb-like PEO host, however, exhibits a better conductivity at a lower temperature. Moreover, they all show an electrochemical window (>5 V) and a low transference number (<0.3). In another investigation based on a PEG-grafted SPE, Thelakkat et al. revealed the influence of PEG content on the ionic conductivity [67]. With an EO/Li+ = 16:1, the ionic conductivity increases with the side chain length because of the increasing amount of dissolved Li+; this observation is similar to the results reported by Yao. However, the anodic breakdown potential is found to be ∼3.5 V vs. Li/Li+ because of the electrolyte decomposition by oxidation; this value is lower than that described above. This is probably because of the difference in experimental conditions under which they have been obtained.
In addition to the methacrylate polymer backbone, other rigid polymers are also used as the main chain. Song et al. reported the effects of grafting degree and side chain lengths on the ionic conductivity using an acrylonitrile-butadiene copolymer backbone with low molecular weight side PEO chains [68]. They found that its degree of crystallinity is significantly reduced, and the mechanical strength is significantly improved compared with those of a linear PEO. The conductivity varies with the side chain length and grafting degree. The maximum conductivity exceeds 10−5 S·cm−1 at room temperature. Using ring-opening metathesis polymerization, a PEO-grafted polynorbornene with different side chain lengths is synthesized [67]. It exhibits a lower conductivity than a methacrylate backbone polymer because its non-conductive hydrocarbon content in the main chain is higher; similar results are obtained for comb-like PEO−mimetic polypeptoids [69]. In a poly(ether ether ketone)-based comb-like copolymer with short side PEO chains [70], it is also observed that the non-conductive backbone only affects its mechanical resistance, rather than significantly improving its electrochemical properties. In the foregoing examples, only short side chains are grafted. Zardalidis et al. studied the physicochemical and electrochemical properties of poly(hydroxylstyrene) with long side PEO chains [71]. The copolymer exhibits a similar electrochemical behavior as the linear PEO because of the crystallization of PEO chains but a better mechanical strength. Because of the incorporation of rigid main chain, the highest storage modulus (G’) obtained at 80 °C reaches 108 Pa, much better than that of linear PEO (Mw = 22 kg·mol−1) at the same temperature [72]. It is also found that G’ decreases with the salt concentration. In addition to side PEO chains, Aldalur et al. successfully grafted other ethylene oxide-containing polymers, such as Jeffamine® (diamine-poly(oxyethylene-co-oxypropylene)), to a main poly(ethylene-alt-maleic anhydride) chain [73,74]. The degree of crystallinity of this polymer decreases with the side chain length similar to that of the side PEO chain copolymer. The ionic conductivity (4.5 × 10−5 S∙cm−1) of SPE with Jeffamine-based matrix at room temperature is considerably better than that with a linear PEO.
In conclusion, PEO-based comb-like polymers usually comprised of short PEO chains and a hard backbone, which enhances mechanical strength. The SPEs that constitute such a polymer demonstrate a higher ionic conductivity and a better mechanical resistance compared with linear PEO-based SPEs; however, they exhibit similar transference numbers (< 0.5). The electrochemical stability of these materials is overestimated because it is usually measured by cyclic voltammetry using a symmetric cell with smooth metallic electrodes, which is different from real electrode composition. On the other hand, many poly(ethylene oxide) methacrylate (PEOMA)-based block copolymers with an amorphous block, such as polystyrene [76], poly(n-butyl methacrylate) [77], and poly(methyl methacrylate) [78], are synthesized. The derived results are similar to those of the above mentioned comb-like polymers. In contrast, combining a single-ion transport block with a PEOMA block can improve not only its mechanical properties but also increase its transference number. The single-ion conducting copolymer, i.e., lithium poly[(4-styrenesulfonyl) (trifluoromethanesulfonyl)imide-co-methoxy-polyethylene glycol acrylate], reported by Zhou et al. [79] exhibits the highest ionic electrolyte conductivities of 7.6 × 10−6 S∙cm−1 at 25 °C and 10−4 S∙cm−1 at 60 °C with an EO/Li+ = 20.5/1; the transference number (>0.9) approaches unity. In another report [80], a single ion-conducting copolymer composed of poly(lithium 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethylsulfonyl)imide) and poly(ethylene glycol) methyl ether methacrylate blocks exhibits similar conductivities of 2.3 × 10−6 S∙cm−1 at 25 °C and 1.2 × 10−5 S∙cm−1 at 55 °C with an EO/Li+ = 36/1; the transference number is 0.83.

3.3. Hyper-Branched Polymer

Different from two-dimensional block copolymers or comb-like copolymer electrolytes, hyper-branched polymers have a globular structure with mobile polymer branches. This type of structure can also suppress PEO crystallization and improve the ionic conductivity and mechanical strength of SPEs. In 2009, Niitani et al. designed a star-shaped copolymer electrolyte with a hyper-branched polystyrene core and poly(poly(ethylene glycol) methyl ether methacrylate) (PPEGMA) arms [81]. Transmission electron microscopy (TEM) and atomic force microscopy (AFM) show that this copolymer forms a well-ordered spherical micro-phase separation structure, in which the star polymers are systematically ordered to form the PPEGMA continuous phase. As a result of the polymer’s unique morphology, the SPEs that contain lithium bis(pentafluoroethanesulfonyl)imide salts exhibit high ionic conductivities, i.e., 10−4 S∙cm−1 at 30 °C and 10−5 S cm−1 at 5 °C with EO/Li+ = 33/1. Another star-shaped copolymer based on PS and PPEGMA is synthesized by atom transfer radical polymerization [82]. The ionic conductivity increases with the chain length of PEGMA and reaches 8 × 10−5 S∙cm−1 at 25 °C with EO/Li+ = 30/1.
Recently, Zhang et al. synthesized a similar core–shell hyper-branched copolymer [83] with hyper-branched polystyrene (HBPS) as core and poly(methyl methacrylate)-block-poly(poly(ethylene glycol) methyl ether methacrylate) (PMMA-b-PPEGMA) as arms (Figure 6). The ionic conductivities of the polymer electrolyte composed of HBPS-(PMMA-b-PPEGMA)x and LiTFSI are 8.3 × 10−5 S∙cm−1 at 30 °C (PPEGMA content: 83.7%) and 2.0 × 10−4 S∙cm−1 at 80 °C (PPEGMA content: 51.6%) with a transference number of up to 0.31. Furthermore, the electrolyte exhibited good interfacial compatibility in a symmetric Li/SPE/Li cell. Subsequently, the authors studied the electrochemical behaviors of the composite polymer electrolyte with HBPS-(PMMA-b-PPEGMA)30 (PPEGMA content: 69.56%), ionic liquid, and LiTFSI [84]. In the presence of ionic liquid, the electrolytes exhibited better ionic conductivities but a considerably lower transference number.
In contrast to the hard core–soft arm structure, Yao et al. reported a hyper-branched polymer structure with the PEO as star core and the linear polystyrene (PS) as arms (hyper-branched PPEGMAm-s-PSn (hbPPEGMAm-s-PSn)), as illustrated in Figure 7 [85]. The authors found that the self-assembly of rigid PS arms during phase separation increases the copolymer’s mechanical strength. The highest storage modulus reaches 1.4 MPa for hbPPEGMA25-b-PS179 at 60 °C. The PEGMA chain length affects its segmental motion in the core. The room-temperature ionic conductivities of hbPPEGMAm-s-PSn SPEs are 5−16 times higher than those of PEO20k and PEO35k SPEs and 2−7 times that of the linear PPEGMA50-b-PS179 SPE. An all-solid-state Li/LiFePO4 battery based on the hyper-branched SPE achieves a stable capacity of 142 mAh∙g−1 at 0.2 C.
The branched PEO chains of comb-like and hyper-branched polymer electrolytes are both mobile, and it is this similarity that contributes to the ion transport. In a network structure, crosslinked polymer chains can effectively suppress PEO crystallization, increase thermal and mechanical stabilities, and mitigate the growth of lithium dendrites.

3.4. Crosslinked Polymer

In network electrolytes formed by linear PEO chains or corresponding block copolymers without a liquid additive, the ionic conductivity depends on the crosslinking degree and chain length between adjacent junction points [86,87]. Moreover, the ionic conduction mechanism also depends on the mesh size of polymer networks [88]. When this size is small enough, the Li+ transport follows Arrhenius model rather than VFT model. In this case, ions jump to the nearest vacant sites. In contrast, when comb-like copolymers with side PEO chains are crosslinked, the PEO chain mobility is better than that of the linear counterpart, resulting in a better ion transport. The network’s mechanical strength varies with the backbone structure and crosslinking degree. H. Kawakami et al. found that linear PEG-based crosslinked network exhibits a much higher stress modulus (6.84 MPa) than PEO (0.55 MPa) with similar molecular mass to the network precursor at ambient temperature [86]. As mentioned, when polysiloxane or polyphosphazene is used as the backbone with the side PEO chain, the network is more flexible than the methacrylate or styrene backbone. The ionic conductivity is mainly tuned by the PEO segment content and mobility as well as the amount of liquid additives introduced. The crosslinking structure is usually obtained through physical means (e.g., micro-phase separation, H-bonding and chain entanglement) or chemical techniques (e.g., copolymerization with a difunctional or multifunctional crosslinker).
Numerous PEO-based block copolymers can form an ion-conducting pathway during the micro-phase separation [89,90,91,92]. Depending on the nature and length ratio of blocks, micro-phases with different morphologies are formed by the copolymer self-assembly. Balsara et al. studied the relationship between ion transport and morphology and the effect of nanoparticle addition on the micro-phase transition [93]. Figure 8 shows the dependence of the ideal morphology factor, fideal, on the conductive phase morphology; a bicontinuous morphology provides the best ion transport. The authors also observed that the addition of 2 wt% polyethylene glycol polyhedral oligomeric silsesquioxane (PEO-POSS) nanoparticles into the PS-b-PEO copolymer causes a lamellar-to-bicontinuous phase transition, leading to a remarkable increase in the ionic conductivity. This type of phase transition that induces the increase in ionic conductivity is also observed in a PEO/PS/PS-b-PEO ternary system [94]. The total homopolymer volume fraction varies from 0 to 0.70, and the ratio, r = [Li+]/[EO], is maintained at 0.06. It is found that the increase in conductivity through the order−disorder transition is most probably caused by the elimination of grain boundaries. In either the disordered or ordered state, the conductivity decreases as the total amount of homopolymer increases.
Using the same approach, Chopade et al. synthesized a PEO-b-PS-based polymer electrolyte through polymerization-induced micro-phase separation (Figure 9) [95]. In this material, the non-conductive phase is chemically crosslinked, thus yielding a higher mechanical strength. The addition of succinonitrile plasticizer allows the electrolyte to reach an excellent conductivity that even exceeds 10−4 S∙cm−1 at room temperature.
Recently, Wu et al. reported a self-healing solid polymer electrolyte (SHSPE) that is crosslinked by the dynamic intermolecular hydrogen bond between urea and ester groups located in the PEO chains [96]. The authors indicated that the inter-chain hydrogen bond and attractive Coulombic forces among the ions in the lithium salt facilitate fast self-healing. This means that the self-healing rate is considerably affected by the lithium salt concentration. As a result of the fast self-healing capability, a high electrolyte mechanical stability is enabled after damage. The optimized SHSPE with high ionic conductivity (1.9 × 10−4 S∙cm−1), low electronic conductivity (1.87 × 10−8 S·cm−1), and high Li-ion transference number (0.44) at room temperature is stable up to 5 V (vs. Li+/Li). Moreover, using the SHSPE, full batteries with a lithium metal anode and an LFP or NCM cathode exhibit good performance. The lithium storage capacities in both cases reach 147.9 mAh∙g−1 (Li/SHSPE/LFP battery) and 170.6 mAh∙g−1 (Li/SHSPE/NCM battery) at 0.1 C. The extremely low polarization between the charge and discharge plateaus of the Li/SHSPE/LFP battery after 20 cycles at 0.1 C indicate the excellent compatibility and stability between the SHSPE and electrodes.
Poly(ethylene glycol) dimethacrylate (PEGDMA) and diacrylate (PEGDA) are the most widely used monomers for the chemical crosslinking of polymer electrolytes. The networks are typically prepared by free radical photo-polymerization or thiol-ene reaction. Zhang et al. demonstrated a facile approach by UV irradiation to prepare a flexible PEO-based crosslinked electrolyte (PTT) consisting of linear PEO, tetraglyme (TEGDME), and tetraethylene glycol dimethacrylate (TEGDMA) (Figure 10) [97]. The SPE exhibits superior electrochemical properties with high ionic conductivity (2.7 × 10−4 S∙cm−1 at 24 °C), high transference number (0.56), wide electrochemical stability window that exceeds 5 V (Li+/Li), and low interfacial resistance; similar SPEs have also been reported [98,99]. In the work of Choudhury et al. [98], the crosslinked polymer matrix comprised of PEGDMA and bis(2-methoxyethyl) ether (diglyme), and the Tg and mechanical strength were found to increase with the PEGDMA content as shown in Figure 11. The authors observed that the materials behaved as single-phase soft solids at a critical PEGDMA content of 40%. At this point, the barrier to ionic transport in the oligoether is sufficiently low to produce high ionic conductivity; however, the oligoether is also prevented from exhibiting large-scale convective motions by interacting with network chain segments. At the same time, the authors indicated that the membranes with high crosslinking degree (>40%) are able to completely suppress electroconvective instability. In another report [100], Khurana et al. synthesized a series of cross-linked polyethylene/poly(ethylene oxide) SPEs with high ionic conductivity (>1.0 × 10−4 S/cm) at 25 °C and a relatively low storage modulus (G′ ≈ 1.0 × 105 Pa) at 90 °C. In lithium dendrite tests, using symmetric Li/SPE/Li cell, they found that low-modulus cross-linked SPEs exhibit remarkable dendrite growth resistance compared with a linear PEO standard (Mw = 900 kg·mol−1). This result suggests that a high-modulus SPE is not a requirement for dendrite nucleation and growth. Furthermore, when single-ion segments are incorporated into an SPE network, the transference number improves. Nevertheless, the use of a liquid plasticizer remains advantageous for ion conduction and improving the flexibility of the SPE membrane [101,102].
In addition to the linear PEO-based networks, crosslinked comb-like polymer electrolytes have also been studied; PEO-grafted polysiloxane is one of the most frequently investigated polymers because of the excellent mechanical and thermal stabilities of siloxane backbone. To prepare this type of network, the polymer chains are commonly crosslinked among themselves or through the addition of a crosslinker. Jiang et al. prepared a comb-like polysiloxane network by photo-polymerization (Figure 12) [103]. They found that the network chain structure has a significant effect on the ionic conductivity and mechanical properties of the electrolyte, and rich PEO side chains enhance conductivity and flexibility. The SPEs exhibit maximum conductivity and tensile strength of 1.01 × 10−4 S∙cm−1 and 0.66 MPa at 30 °C, respectively.
Oh et al. synthesized a crosslinked mono-comb-type poly(siloxane-g-ethylene oxide) electrolyte using PEGDMA as a crosslinker [104]. A maximum ionic conductivity of 1.33 × 10−4 S∙cm−1 at 25 °C is obtained, indicating that the crosslinking method has no significant effect on the properties of this type of SPEs.
An epoxy group is also employed to prepare a network structure. Daigle et al. prepared a crosslinked SPE composed of a poly(poly(ethylene glycol) methacrylate-co-glycidyl methacrylate) copolymer [105]; the polymer chains were crosslinked through amino-epoxy polymerization. The obtained SPE exhibited excellent electric stability and mechanical resistance. Grewal et al. synthesized free-standing polydimethylsiloxane-based crosslinked network solid polymer electrolytes via in situ thiol-epoxy polymerization [106]. In the presence of lithium salt and base catalyst, poly(ethylene glycol) diglycidyl ether, mercapto-terminated polydimethylsiloxane, and pentaerythritol tetrakis (3-mercaptopropionate) were copolymerized at the stoichiometric ratio. Without a liquid plasticizer, the crosslinked SPEs exhibited the following: Ionic conductivities between 1.5 × 10−6 S∙cm−1 at room temperature and 1.6 × 10−4 S∙cm−1 at 90 °C; lithium ion transference number of 0.15–0.20; electrochemical window of up to 5.3 V (vs. Li+/Li); thermal resistance of approximately 254.5 °C; maximum tensile strength of approximately 1.6 MPa.
A number of SPEs that employ different node groups also exhibit similar electrochemical and mechanical properties. In conclusion, the crosslinking structure affords a stronger mechanical support, and the lithium cation transport in the PEO-based network mainly depends on chain segmental motion and hopping between adjacent coordinating sites.

3.5. Discussion

After 40 years of development, both the ionic conduction mechanism and practical applications of PEO-based electrolytes have remarkably improved. A significant number of research articles pertaining to PEO-based SPEs have been published, and many factors affecting the performance of this type of SPEs have been investigated. Herein, some effects of polymer architecture on the mechanical and electrochemical properties are summarized (Figure 13), and linear, comb-like, hyper-branched, and crosslinked structures are discussed. Without the addition of any plasticizers, the SPEs with a comb-like or hyper-branched structure exhibit better ionic conductivity at a low temperature compared to that with a linear PEO; the foregoing is attributed to crystallinity reduction or suppression. Moreover, the mechanical strength is enhanced when an amorphous hard backbone is incorporated. With regard to crosslinked SPEs, the crosslinking degree and PEO segment length perform important functions in improving ionic conductivity and mechanical flexibility. In the presence of a liquid additive, the SPEs with a crosslinking structure exhibit excellent ionic conductivity at room temperature as well as good thermal and electrochemical stabilities.
Furthermore, the incorporation of single-ion segments into these structures can significantly increase the transference number of SPEs from 0.2 to unity. The decomposition mechanism is mainly related to an oxidation reaction of the polymer electrolyte with active materials [107]. The electrochemical stability of SPEs is usually tested by cyclic voltammetry using a symmetric cell with metallic electrodes. Because of the absence of active electrode materials, this measurement method leads to a higher oxidation voltage than that observed in real batteries because of milder test conditions. The decomposition voltage for the PEO-based electrolyte in the presence of active electrode materials is found to be 3.8 V [108], which limits its development in high-voltage ASSLPBs. Besides, it is found that PEO thermodynamic stability on the lithium metal surface mainly relies on its molecular mass [109,110]. A complex architecture often gives a very high molecular mass, therefore, corresponding SPEs exhibit a better stability.

4. PIL-Based SPEs

In recent years, the use of ionic liquid (IL) as the ion-conducting medium in lithium batteries has attracted further interest because of its salt solvating capacity, thermal and chemical stabilities. The commonly used cations and anions of ILs have been summarized in several reviews [26,111,112,113,114,115]. Polymeric ionic liquid, sometimes referred to as polymerized ionic liquid or poly(ionic liquid) (PIL), is a macromolecule with ionic liquid units that combines the advantages of ILs and mechanical strength of polymers. In previous years, many of the factors that affect the ion transport in PILs have been investigated. These include the nature of counter-ion [116,117], nature and length of spacer between the main chain and IL moieties [118], and polymer molecular weight [119]. This review is focused on the effects of PIL architecture on the ionic conductivity and electrochemical stability of PIL-based SPEs. Despite the variety of PILs, only imidazolium-based PILs, which are most frequently studied, are considered as an example.
Before the properties of PIL-based SPEs are discussed, the effects of architecture on the ion transport in pure PILs are briefly presented. For this type of polymer, IL units can be incorporated into the chain backbone or pendant; their position affects the properties of polymers. Kuray et al. recently investigated the morphology, conductivity, and rheology of imidazolium-based pendant and backbone PILs (P-PIL and B-PIL, respectively) [120]. Figure 14 shows the structure of PILs and their ionic conductivities as a function of temperature. The authors found that B-PILs have a considerably lower Tg than P-PILs with the same counter-anions and also exhibit a higher ionic conductivity on an absolute temperature scale. The conductivity of P-PILs is higher when scaled to Tg or below Tg. This is attributed to the movement of the counter-anions among the side chains in P-PILs (difference in the decoupling degree). Moreover, they found that the ion transport for B-PILs is linked to the segmental motions of polymer chains, whereas that for P-PILs is decoupled from the segmental dynamics at a temperature close to Tg.
Delhorbe et al. systematically investigated the effect of the side alkyl chain length in the imidazolium-based P-PILs on the physicochemical properties and ionic conductivity based on 1-alkyl-3-vinylimidazolium bis(trifluoromethane)sulfonimide-derived homopolymers with various alkyl chain lengths (−C nH2n+1 (n = 2, 4, 6, 8, 10)) [121]. They revealed that the charge transport in PILs is determined by the segmental motion of the polymer backbone and charge carrier density as well as the self-assembly nanostructure of such PILs, specifically the backbone-to-backbone correlation distance. The low viscosity and Tg favor ion conduction, and the decrease in the backbone-to-backbone correlation distance enhances conductivity. On the other hand, in the presence of LiTFSI with a molar ratio of [Imidazolium+]:[Li+] = 3:1, they found that the ion transport in PILs also depends on the parameters described above. However, the authors have not identified the lithium cation transport in this system.
The membrane of most PILs is extremely brittle because of insufficient chain flexibility. As a result, the majority of PIL-based SPEs contain a liquid plasticizer, which also aids ion mobility. In a previous study of Hirano et al. [122], the SPE membranes are prepared with a PIL/IL/Li salt ternary system. Poly(1-ethyl-3-vinylimidazolium bis(trifluoromethanesulfonylimide)) (P(EtVIm-TFSI)) is used as the polymer host, and the mixture of 1,2-dimethyl-3-ethoxyethyl imidazolium bis(trifluoromethanesulfonyl) imide (IM(2o2)11TFSI) and LiTFSI is added as the liquid plasticizer. It is found that the ionic conductivity increases with the amount of IM(2o2)11TFSI. With a 65% ionic liquid content, the ionic conductivity reaches 1.89 × 10−5 S∙cm−1 at 25 °C and 1.84 × 10−4 S∙cm−1 at 60 °C; however, the mechanical resistance is compromised.
In comparison to linear PILs, the network structure has a higher charge density. Zhang et al. synthesized polymeric ionic networks (PINs) using hexakis(bromomethyl)benzene and 4,4-bipyridine by nucleophilic substitution reaction or a star-shaped imidazolium monomer by free radical polymerization [123]. In the PIN and LiTFSI mixture, it is possible that the crystalline structure of LiTFSI disappears because of the strong electrostatic interaction. Moreover, when the LiTFSI and PINs have the same anion, the LiTFSI ion pair configuration may be restructured. Using PINs as polymer hosts and LiTFSI in 1-ethyl-3-methylimidazolium bis(trifluoromethane)sulfonimide (EMIM-TFSI) (0.5 mol∙kg−1) as plasticizer, a six-arm imidazolium monomer-based network SPE exhibits the best ionic conductivity of up to 5.32 × 10−3 S∙cm−1 at 22 °C and good mechanical properties. Such a high ionic conductivity at room temperature is also observed in other PIL network-based SPEs [124,125]. These results indicate that the network affords higher charge density and better mechanical strength than a linear architecture that enhances the ionic conductivity of PIL-based SPEs.

5. Perspectives

In this review, the effects of polymer architecture on the performance of polymer electrolytes are summarized. With the development of all-solid-state batteries, however, the traditional solid polymer electrolytes (e.g., PEO and polycarbonates) are incapable of satisfying the required high energy density and high voltage. In order to improve the mechanical strength and electrochemical performance of electrolytes, three basic strategies are typically implemented for designing new materials: (1) The use of a highly crosslinked structure; (2) the combination of macromolecules and small molecules (e.g., ionic liquid); (3) the use of organic/inorganic hybrid materials.
From the perspective of polymer architecture, a highly crosslinked matrix with mobile Li+ coordination sites can yield a stable structure to satisfy the demand for high-performance batteries. Indeed, battery performance is a result of electrode and electrolyte cooperation; hence, a good electrolyte design that is suitable for desired electrode materials is necessary.

Author Contributions

X.Z.: conceptualization, data curation, writing—original draft. J.-C.D.: editing. K.Z.: editing and supervision. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the funding from Center of Excellence in Transportation Electrification and Energy Storage (CETEES), Hydro-Québec.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Burke, A.; Miller, M. The power capability of ultracapacitors and lithium batteries for electric and hybrid vehicle applications. J. Power Sources 2011, 196, 514–522. [Google Scholar] [CrossRef]
  2. Cairns, E.J.; Albertus, P. Batteries for electric and hybrid-electric vehicles. Annu. Rev. Chem. Biomol. Eng. 2010, 1, 299–320. [Google Scholar] [CrossRef]
  3. Frackowiak, E. Carbon materials for supercapacitor application. Phys. Chem. Chem. Phys. 2007, 9, 1774–1785. [Google Scholar] [CrossRef] [PubMed]
  4. Jeżowski, P.; Crosnier, O.; Deunf, E.; Poizot, P.; Béguin, F.; Brousse, T. Safe and recyclable lithium-ion capacitors using sacrificial organic lithium salt. Nat. Mater. 2018, 17, 167–173. [Google Scholar] [CrossRef] [PubMed]
  5. Padbury, R.; Zhang, X.W. Lithium–oxygen batteries—Limiting factors that affect performance. J. Power Sources 2011, 196, 4436–4444. [Google Scholar] [CrossRef]
  6. Marcinek, M.; Syzdek, J.; Marczewski, M.; Piszcz, M.; Niedzicki, L.; Kalita, M.; Plewa-Marczewska, A.; Bitner, A.; Wieczorek, P.; Trzeciak, T.; et al. Electrolytes for Li-ion transport—Review. Solid State Ion. 2015, 276, 107–126. [Google Scholar] [CrossRef]
  7. Murata, K.; Izuchi, S.; Yoshihisa, Y. An overview of the research and development of solid polymer electrolyte batteries. Electrochim. Acta 2000, 45, 1501–1508. [Google Scholar] [CrossRef]
  8. Bruce, P.G.; Vincent, C.A. Polymer electrolytes. J. Chem. Soc. Faraday Trans. 1993, 89, 3187–3203. [Google Scholar] [CrossRef]
  9. Sequeira, C.; Santos, D. Polymer Electrolytes-Fundamentals and Applications; Woodhead Publishing: Sawston, UK, 2010; ISBN 978-1-84569-772-3. [Google Scholar]
  10. Amine, K. Batteries: Polymers switch for safety. Nat. Energy 2016, 1, 15018. [Google Scholar] [CrossRef]
  11. Wang, Q.; Jiang, L.; Yu, Y.; Sun, J. Progress of enhancing the safety of lithium ion battery from the electrolyte aspect. Nano Energy 2019, 55, 93–114. [Google Scholar] [CrossRef]
  12. Armand, M.B.; Chabagno, J.M.; Duclot, M. Polymeric solid electrolytes. In Proceedings of the Second International Meeting on Solid Electrolytes, St Andrews, Scotland, 20–22 September 1978. [Google Scholar]
  13. Gauthier, M.; Fauteux, D.; Vassort, G.; Bélanger, A.; Duval, M.; Ricoux, P.; Chabagno, J.-M.; Muller, D.; Rigaud, P.; Armand, M.B.; et al. Assessment of polymer-electrolyte batteries for EV and ambient temperature applications. J. Electrochem. Soc. 1985, 132, 1333–1340. [Google Scholar] [CrossRef]
  14. Chatani, Y.; Okamura, S. Crystal structure of poly(ethylene oxide)—Sodium iodide complex. Polymer 1987, 28, 1815. [Google Scholar] [CrossRef]
  15. Zhang, H.; Li, C.M.; Eshetu, G.G.; Laruelle, S.; Grugeon, S.; Zaghib, K.; Julien, C.; Mauger, A.; Guyomard, D.; Rojo, T.; et al. From solid-solution electrodes and the Rocking-Chair concept to today’s batteries. Angew. Chem. Int. Ed. 2020, 59, 534–538. [Google Scholar] [CrossRef] [PubMed]
  16. Letourneau, C.; Gauthier, M.; Belanger, A.; Kuller, D.; Hoffman, J. Lithium polymer battery pack design. In Proceedings of the 14th International Electric Vehicle Symposium and Exposition (EVS—14), Orlando, FL, USA, 15–17 December 1997. [Google Scholar]
  17. Zeng, X.-Q.; Li, M.; Abd El-Hady, D.; Alshitari, W.; Al-Bogami, A.S.; Lu, J.; Amine, K. Commercialization of lithium battery technologies for electric vehicles. Adv. Energy Mater. 2019, 9, 1900161. [Google Scholar] [CrossRef]
  18. Randau, S.; Weber, D.A.; Kötz, O.; Koerver, R.; Braun, P.; Weber, A.; Ivers-Tiffée, E.; Adermann, T.; Kulisch, J.; Zeier, W.G.; et al. Benchmarking the performance of all-solid-state lithium batteries. Nat. Energy 2020, 5, 259–270. [Google Scholar] [CrossRef]
  19. History: Over 20 Years of Research and Development to Produce a Unique Technology: LMP®. Available online: https://www.blue-solutions.com/en/blue-solutions/company/presentation/histoire/ (accessed on 28 May 2020).
  20. Springer, T.E.; Zawodzinski, T.A.; Gottesfeld, S. Polymer electrolyte fuel cell model. J. Electrochem. Soc. 1991, 138, 2334–2342. [Google Scholar] [CrossRef]
  21. Su’ait, M.S.; Rahman, M.Y.A.; Ahmad, A. Review on polymer electrolyte in dye-sensitized solar cells. Sol. Energy 2015, 115, 452–470. [Google Scholar] [CrossRef]
  22. Alexandre, S.A.; Silva, G.G.; Santamaría, R.; Trigueiro, J.P.C.; Lavall, R.L. A highly adhesive PIL/IL gel polymer electrolyte for use in flexible solid state supercapacitors. Electrochim. Acta 2019, 299, 789–799. [Google Scholar] [CrossRef]
  23. Xue, Z.; He, D.; Xie, X. Poly(ethylene oxide)-based electrolytes for lithium-ion batteries. J. Mater. Chem. A 2015, 3, 19218–19253. [Google Scholar] [CrossRef]
  24. Arya, A.; Sharma, A.L. Insights into the use of polyethylene oxide in energy storage/conversion devices: A critical review. J. Phys. D Appl. Phys. 2017, 50, 443002. [Google Scholar] [CrossRef]
  25. Cheng, S.; Smith, D.M.; Pan, Q.; Wang, S.; Li, C.Y. Anisotropic ion transport in nanostructured solid polymer electrolytes. RSC Adv. 2015, 5, 48793–48810. [Google Scholar] [CrossRef]
  26. Watanabe, M.; Thomas, M.L.; Zhang, S.; Ueno, K.; Yasuda, T.; Dokko, K. Application of ionic liquids to energy storage and conversion materials and devices. Chem. Rev. 2017, 117, 7190–7239. [Google Scholar] [PubMed] [Green Version]
  27. Eshetu, G.G.; Mecerreyes, D.; Forsyth, M.; Zhang, H.; Armand, M. Polymeric ionic liquids for lithium-based rechargeable batteries. Mol. Syst. Des. Eng. 2019, 4, 294–309. [Google Scholar] [CrossRef]
  28. Keller, M.; Varzi, A.; Passerini, S. Hybrid electrolytes for lithium metal batteries. J. Power Sources 2018, 392, 206–225. [Google Scholar] [CrossRef]
  29. Dirican, M.; Yan, C.; Zhu, P.; Zhang, X. Composite solid electrolytes for all-solid-state lithium batteries. Mater. Sci. Eng. R Rep. 2019, 136, 27–46. [Google Scholar]
  30. Zhang, H.; Li, C.; Piszcz, M.; Coya, E.; Rojo, T.; Rodriguez-Martinez, L.M.; Armand, M.; Zhou, Z. Single lithium-ion conducting solid polymer electrolytes: Advances and perspectives. Chem. Soc. Rev. 2017, 46, 797–815. [Google Scholar]
  31. Zhang, H.; Eshetu, G.G.; Judez, X.; Li, C.; Rodriguez-Martínez, L.M.; Armand, M. Electrolyte additives for lithium metal anodes and rechargeable lithium metal batteries: Progress and perspectives. Angew. Chem. Int. Ed. 2018, 57, 15002–15027. [Google Scholar]
  32. Mauger, A.; Julien, C.M.; Paolella, A.; Armand, M.; Zaghib, K. A comprehensive review of lithium salts and beyond for rechargeable batteries: Progress and perspectives. Mater. Sci. Eng. R Rep. 2018, 134, 1–21. [Google Scholar] [CrossRef]
  33. Olsher, U.; Izatt, R.M.; Bradshaw, J.S.; Dalley, N.K. Coordination chemistry of lithium ion: A crystal and molecular structure review. Chem. Rev. 1991, 91, 137–164. [Google Scholar] [CrossRef]
  34. Jeong, K.; Park, S.; Lee, S.-Y. Revisiting polymeric single lithium-ion conductors as an organic route for all-solid-state lithium ion and metal batteries. J. Mater. Chem. A 2019, 7, 1917–1935. [Google Scholar] [CrossRef]
  35. Budd, P.M. Chapter 11—Polyelectrolytes. In Comprehensive Polymer Science and Supplements, 1st ed.; Pergamon Press: Oxford, UK, 1989; Volume 1, pp. 215–230. [Google Scholar]
  36. Berthier, C.; Gorecki, W.; Minier, M.; Armand, M.B.; Chabagno, J.M.; Rigaud, P. Microscopic investigation of ionic conductivity in alkali metal salts-poly(ethylene oxide) adducts. Solid State Ion. 1983, 11, 91–95. [Google Scholar] [CrossRef]
  37. Ward, I.M.; Boden, N.; Cruickshank, J.; Leng, S.A. NMR studies of ionic mobility and molecular mobility in polymer electrolytes. Electrochim. Acta 1995, 40, 2071–2076. [Google Scholar]
  38. Borodin, O.; Smith, G.D.; Henderson, W. Li+ cation environment, transport, and mechanical properties of the LiTFSI doped N-Methyl-N-alkylpyrrolidinium+TFSI- ionic liquids. J. Phys. Chem. B 2006, 110, 16879–16886. [Google Scholar] [CrossRef] [PubMed]
  39. Kreuer, K.-D.; Rabenau, A.; Weppner, W. Vehicle mechanism, a new model for the interpretation of the conductivity of fast proton conductors. Angew. Chem. Int. Ed. 1982, 21, 208–209. [Google Scholar] [CrossRef]
  40. Ganesan, V. Ion transport in polymeric ionic liquids: Recent developments and open questions. Mol. Syst. Des. Eng. 2019, 4, 280–293. [Google Scholar]
  41. Frenck, L.; Sethi, G.K.; Maslyn, J.A.; Balsara, N.P. Factors that control the formation of dendrites and other morphologies on lithium metal anodes. Front. Energy Res. 2019, 7, 115. [Google Scholar] [CrossRef] [Green Version]
  42. Barai, P.; Higa, K.; Srinivasan, V. Effect of initial state of lithium on the propensity for dendrite formation: A theoretical study. J. Electrochem. Soc. 2016, 164, A180–A189. [Google Scholar] [CrossRef] [Green Version]
  43. Fenton, D.E.; Parker, J.M.; Wright, P.V. Complexes of alkali metal ions with poly(ethylene oxide). Polymer 1973, 14, 589. [Google Scholar]
  44. Sun, B.; Xu, C.; Mindemark, J.; Gustafsson, T.; Edström, K.; Brandell, D. At the polymer electrolyte interfaces: The role of the polymer host in interphase layer formation in Li-batteries. J. Mater. Chem. A 2015, 3, 13994–14000. [Google Scholar]
  45. Yoon, H.-K.; Chung, W.-S.; Jo, N.-J. Study on ionic transport mechanism and interactions between salt and polymer chain in PAN based solid polymer electrolytes containing LiCF3SO3. Electrochim. Acta 2004, 50, 289–293. [Google Scholar] [CrossRef]
  46. Ferry, A. Ionic interactions and transport properties in methyl terminated poly(propylene glycol)(4000) complexed with LiCF3SO3. J. Phys. Chem. B 1997, 101, 150–157. [Google Scholar] [CrossRef]
  47. Ferry, A. Effects of dynamic spatial disorder on ionic transport properties in polymer electrolytes based on poly(propylene glycol)(4000). J. Chem. Phys. 1997, 107, 9168–9175. [Google Scholar] [CrossRef]
  48. Alamgir, M.; Moulton, R.D.; Abraham, K.M. Li+-conductive polymer electrolytes derived from poly(1,3-dioxolane) and polytetrahydrofuran. Electrochim. Acta 1991, 36, 773–782. [Google Scholar] [CrossRef]
  49. Sahadeo, E.; Wang, Y.; Lin, C.-F.; Li, Y.; Rubloff, G.; Lee, S.B. Mg2+ ion-catalyzed polymerization of 1,3-dioxolane in battery electrolytes. Chem. Comm. 2020, 56, 4583–4586. [Google Scholar] [CrossRef] [PubMed]
  50. Zhao, Q.; Liu, X.; Stalin, S.; Khan, K.; Archer, L. Solid-state polymer electrolytes with in-built fast interfacial transport for secondary lithium batteries. Nat. Energy 2019, 4, 365–373. [Google Scholar] [CrossRef]
  51. Wu, X.-L.; Xin, S.; Seo, H.-H.; Kim, J.; Guo, Y.-G.; Lee, J.-S. Enhanced Li+ conductivity in PEO–LiBOB polymer electrolytes by using succinonitrile as a plasticizer. Solid State Ion. 2011, 186, 1–6. [Google Scholar] [CrossRef]
  52. Johan, M.R.; Shy, O.H.; Ibrahim, S.; Mohd, Y.; Siti, M.; Hui, T.Y. Effects of Al2O3 nanofiller and EC plasticizer on the ionic conductivity enhancement of solid PEO–LiCF3SO3 solid polymer electrolyte. Solid State Ion. 2011, 196, 41–47. [Google Scholar] [CrossRef]
  53. Asghar, A.; Abdul Samad, S.; Singh Lalia, B.; Hashaikeh, R. PEG based quasi-solid polymer electrolyte: Mechanically supported by networked cellulose. J. Membr. Sci. 2012, 421, 85–90. [Google Scholar] [CrossRef]
  54. Zhang, J.; Zhao, N.; Zhang, M.; Li, Y.; Chu, P.K.; Guo, X.; Di, Z.; Wang, X.; Li, H. Flexible and ion-conducting membrane electrolytes for solid-state lithium batteries: Dispersion of garnet nanoparticles in insulating polyethylene oxide. Nano Energy 2016, 28, 447–454. [Google Scholar] [CrossRef]
  55. Phan, T.N.T.; Issa, S.; Gigmes, D. Poly(ethylene oxide)-based block copolymer electrolytes for lithium metal batteries. Polym. Int. 2019, 68, 7–13. [Google Scholar] [CrossRef] [Green Version]
  56. Rosso, M.; Brissot, C.; Teyssot, A.; Dollé, M.; Sannier, L.; Tarascon, J.-M.; Bouchet, R.; Lascaud, S. Dendrite short-circuit and fuse effect on Li/polymer/Li cells. Electrochim. Acta 2006, 51, 5334–5340. [Google Scholar] [CrossRef]
  57. Blonsky, P.M.; Shriver, D.F.; Austin, P.; Allcock, H.R. Polyphosphazene solid electrolytes. J. Am. Chem. Soc. 1984, 106, 6854–6855. [Google Scholar] [CrossRef]
  58. Allcock, H.R.; Austin, P.E.; Neenan, T.X.; Sisko, J.T.; Blonsky, P.M.; Shriver, D.F. Polyphosphazenes with etheric side groups: Prospective biomedical and solid electrolyte polymers. Macromolecules 1986, 19, 1508–1512. [Google Scholar] [CrossRef]
  59. Tonge, J.S.; Blonsky, P.M.; Shriver, D.F.; Allcock, H.R.; Austin, P.E.; Neenan, T.X.; Sisko, J.T. Effect of side-chain length and crosslinking on ionic conductivity in polyphosphazene solid electrolytes. Proc. Electrochem. Soc. 1987, 87, 533–544. [Google Scholar]
  60. Allcock, H.R.; Sunderland, N.J.; Ravikiran, R.; Nelson, J.M. Polyphosphazenes with novel architectures:  influence on physical properties and behavior as solid polymer electrolytes. Macromolecules 1998, 31, 8026–8035. [Google Scholar] [CrossRef]
  61. Allcock, H.R.; Kuharcik, S.E.; Reed, C.S.; Napierala, M.E. Synthesis of polyphosphazenes with ethyleneoxy-containing side groups:  New solid electrolyte materials. Macromolecules 1996, 29, 3384–3389. [Google Scholar] [CrossRef]
  62. Allcock, R.; O’Connor, S.J.M.; Olmeijer, D.L.; Napierala, M.E.; Cameron, C.G. Polyphosphazenes bearing branched and linear oligoethyleneoxy side groups as solid solvents for ionic conduction. Macromolecules 1996, 29, 7544–7552. [Google Scholar] [CrossRef]
  63. Oh, B.; Vissers, D.; Zhang, Z.; West, R.; Tsukamoto, H.; Amine, K. New interpenetrating network type poly(siloxane-g-ethylene oxide) polymer electrolyte for lithium battery. J. Power Sources 2003, 119, 442–447. [Google Scholar] [CrossRef]
  64. Borodin, O.; Smith, G.D. Molecular Dynamics simulations of comb-branched poly(epoxide ether)-based polymer electrolytes. Macromolecules 2007, 40, 1252–1258. [Google Scholar] [CrossRef]
  65. Wang, Z.H.; Chen, S.J.; Huang, Z.; Wei, Z.Y.; Shen, L.; Gu, H.; Xu, X.X.; Yao, X.Y. High conductivity polymer electrolyte with comb-like structure via a solvent-free UV-cured method for large-area ambient all-solid-sate lithium batteries. J. Mater. 2019, 5, 195–203. [Google Scholar] [CrossRef]
  66. Zhang, H.; Liu, C.Y.; Zheng, L.P.; Xu, F.; Feng, W.F.; Li, H.; Huang, X.J.; Armand, M.; Nie, J.; Zhou, Z.B. Lithium bis(fluorosulfonyl)imide/poly(ethylene oxide) polymer electrolyte. Electrochim. Acta 2014, 133, 529–538. [Google Scholar] [CrossRef]
  67. Rosenbach, D.; Mödl, N.; Hahn, M.; Petry, J.; Danzer, M.A.; Thelakkat, M. Synthesis and comparative studies of solvent-free brush polymer electrolytes for lithium batteries. ACS Appl. Energy Mater. 2019, 2, 3373–3388. [Google Scholar] [CrossRef]
  68. Kim, D.-W.; Park, J.-K.; Gong, M.-S.; Song, H.-Y. Effect of grafting degree and side PEO chain length on the ionic conductivities of NBR-g-PEO based polymer electrolytes. Polym. Eng. Sci. 1994, 34, 1305–1313. [Google Scholar] [CrossRef]
  69. Sun, J.; Stone, G.M.; Balsara, N.P.; Zuckermann, R.N. Structure–conductivity relationship for peptoid-based PEO–mimetic polymer electrolytes. Macromolecules 2012, 45, 5151–5156. [Google Scholar] [CrossRef]
  70. Guo, M.; Zhang, M.; He, D.; Hu, J.; Wang, X.; Gong, C.; Xie, X.; Xue, Z. Comb-like solid polymer electrolyte based on polyethylene glycol-grafted sulfonated polyether ether ketone. Electrochim. Acta 2017, 255, 396–404. [Google Scholar] [CrossRef]
  71. Zardalidis, G.; Pipertzis, A.; Mountrichas, G.; Pispas, S.; Mezger, M.; Floudas, G. Effect of polymer architecture on the ionic conductivity. Densely grafted poly(ethylene oxide) brushes doped with LiTf. Macromolecules 2016, 49, 2679–2687. [Google Scholar] [CrossRef]
  72. Glynos, E.; Pantazidis, C.; Sakellariou, G. Designing all-polymer nanostructured solid electrolytes: Advances and prospects. ACS Omega 2020, 5, 2531–2540. [Google Scholar] [CrossRef] [Green Version]
  73. Aldalur, I.; Zhang, H.; Piszcz, M.; Oteo, U.; Rodriguez-Martinez, L.M.; Shanmukaraj, D.; Rojo, T.; Armand, M. Jeffamine® based polymers as highly conductive polymer electrolytes and cathode binder materials for battery application. J. Power Sources 2017, 347, 37–46. [Google Scholar] [CrossRef]
  74. Aldalur, I.; Martinez-Ibañez, M.; Piszcz, M.; Rodriguez-Martinez, L.M.; Zhang, H.; Armand, M. Lowering the operational temperature of all-solid-state lithium polymer cell with highly conductive and interfacially robust solid polymer electrolytes. J. Power Sources 2018, 383, 144–149. [Google Scholar] [CrossRef]
  75. Kerr, J.B.; Sloop, S.E.; Liu, G.; Han, Y.B.; Hou, J.; Wang, S.E. From molecular models to system analysis for lithium battery electrolytes. J. Power Sources 2002, 110, 389–400. [Google Scholar] [CrossRef] [Green Version]
  76. Kuan, W.-F.; Remy, R.; Mackay, M.E.; Epps, T.H. Controlled ionic conductivity via tapered block polymer electrolytes. RSC Adv. 2015, 5, 12597–12604. [Google Scholar] [CrossRef] [Green Version]
  77. Harris, D.J.; Bonagamba, T.J.; Schmidt-Rohr, K.; Soo, P.P.; Sadoway, D.R.; Mayes, A.M. Solid-state NMR investigation of block copolymer electrolyte dynamics. Macromolecules 2002, 35, 3772–3774. [Google Scholar] [CrossRef]
  78. Huang, B.; Cook, C.C.; Mui, S.; Soo, P.P.; Staelin, D.H.; Mayes, A.; Sadoway, D.R. High energy density, thin-film, rechargeable lithium batteries for marine field operations. J. Power Sources 2001, 97, 674–676. [Google Scholar] [CrossRef]
  79. Feng, S.; Shi, D.; Liu, F.; Zheng, L.; Nie, J.; Feng, W.; Huang, X.; Armand, M.; Zhou, Z. Single lithium-ion conducting polymer electrolytes based on poly[(4-styrenesulfonyl)(trifluoromethanesulfonyl)imide] anions. Electrochim. Acta 2013, 93, 254–263. [Google Scholar]
  80. Porcarelli, L.; Shaplov, A.S.; Salsamendi, M.; Nair, J.R.; Vygodskii, Y.S.; Mecerreyes, D.; Gerbaldi, C. Single-ion block copoly(ionic liquid)s as electrolytes for all-solid state lithium batteries. ACS Appl. Mater. Interfaces 2016, 8, 10350–10359. [Google Scholar] [CrossRef]
  81. Niitani, T.; Amaike, M.; Nakano, H.; Dokko, K.; Kanamura, K. Star-shaped polymer electrolyte with microphase separation structure for all-solid-state lithium batteries. J. Electrochem. Soc. 2009, 156, A577–A583. [Google Scholar] [CrossRef]
  82. Ren, S.; Chang, H.; He, L.; Dang, X.; Fang, Y.; Zhang, L.; Li, H.; Hu, Y.; Lin, Y. Preparation and ionic conductive properties of all-solid polymer electrolytes based on multiarm star block polymers. J. Appl. Polym. Sci. 2013, 129, 1131–1142. [Google Scholar]
  83. Wang, A.; Xu, H.; Zhou, Q.; Liu, X.; Li, Z.; Gao, R.; Wu, N.; Guo, Y.; Li, H.; Zhang, L. A new all-solid-state hyperbranched star polymer electrolyte for lithium ion batteries: Synthesis and electrochemical properties. Electrochim. Acta 2016, 212, 372–379. [Google Scholar] [CrossRef]
  84. Wang, A.; Xu, H.; Zhou, Q.; Liu, X.; Li, Z.; Gao, R.; Liu, X.; Zhang, L. Electrochemical performances of a new solid composite polymer electrolyte based on hyperbranched star polymer and ionic liquid for lithium-ion batteries. J. Solid State Electrochem. 2017, 21, 2355–2364. [Google Scholar] [CrossRef]
  85. Chen, Y.; Shi, Y.; Liang, Y.; Dong, H.; Hao, F.; Wang, A.; Zhu, Y.; Cui, X.; Yao, Y. Hyperbranched PEO-based hyperstar solid polymer electrolytes with simultaneous improvement of ion transport and mechanical strength. ACS Appl. Energy Mater. 2019, 2, 1608–1615. [Google Scholar]
  86. Grewal, M.S.; Tanaka, M.; Kawakami, H. Bifunctional poly(ethylene glycol) based crosslinked network polymers as electrolytes for all-solid-state lithium ion batteries. Polym. Int. 2019, 68, 684–693. [Google Scholar] [CrossRef]
  87. Hasan, N.; Pulst, M.; Samiullah, M.H.; Kressler, J. Comparison of Li+-ion conductivity in linear and crosslinked poly(ethylene oxide). J. Polym. Sci. B Polym. Phys. 2019, 57, 21–28. [Google Scholar] [CrossRef] [Green Version]
  88. Carvalho, L.M.; Guégan, P.; Cheradame, H.; Gomes, A.S. Variation of the mesh size of PEO-based networks filled with TFSILi: From an Arrhenius to WLF type conductivity behavior. Eur. Polym. J. 2000, 36, 401–409. [Google Scholar]
  89. Niitani, T.; Shimada, M.; Kawamura, K.; Dokko, K.; Rho, Y.-H.; Kanamura, K. Synthesis of Li+  Ion Conductive PEO-PSt Block Copolymer Electrolyte with Microphase Separation Structure. Electrochem. Solid State Lett. 2005, 8, A385–A388. [Google Scholar]
  90. Phan, T.T.N.; Robinet, M.; Bouchet, R.; Bertin, D. PS-b-PEO-b-PS based solid polymer electrolytes for lithium rechargeable batteries. PMSE Prepr. 2008, 99, 329–330. [Google Scholar]
  91. Zhang, B.; Zhang, Y.; Zhang, N.; Liu, J.; Cong, L.; Liu, J.; Sun, L.; Mauger, A.; Julien, C.M.; Xie, H.; et al. Synthesis and interface stability of polystyrene-poly(ethylene glycol)-polystyrene triblock copolymer as solid-state electrolyte for lithium-metal batteries. J. Power Sources 2019, 428, 93–104. [Google Scholar]
  92. Young, W.-S.; Kuan, W.-F.; Epps, T.H. Block copolymer electrolytes for rechargeable lithium batteries. J. Polym. Sci. Part B Polym. Phys. 2014, 52, 1–16. [Google Scholar]
  93. Villaluenga, I.; Chen, X.C.; Devaux, D.; Hallinan, D.; Balsara, N.P. Nanoparticle-driven assembly of highly conducting hybrid block copolymer electrolytes. Macromolecules 2015, 48, 358–364. [Google Scholar] [CrossRef] [Green Version]
  94. Irwin, M.T.; Hickey, R.J.; Xie, S.; So, S.; Bates, F.; Lodge, T.P. Structure-conductivity relationships in ordered and disordered salt-doped diblock copolymer/homopolymer blends. Macromolecules 2016, 49, 6928–6939. [Google Scholar]
  95. Chopade, S.; Au, J.G.; Li, Z.; Schmidt, P.W.; Hillmyer, M.A.; Lodge, T.P. Robust polymer electrolyte membranes with high ambient-temperature lithium-ion conductivity via polymerization-induced microphase separation. ACS Appl. Mater. Interfaces 2017, 9, 14561–14565. [Google Scholar] [CrossRef]
  96. Wu, N.; Shi, Y.-R.; Lang, S.-Y.; Zhou, J.M.; Liang, J.-Y.; Wang, W.; Tan, S.-J.; Yin, Y.-X.; Wen, R.; Guo, Y.-G. Self-healable solid polymeric electrolytes for stable and flexible lithium metal batteries. Angew. Chem. Int. Ed. 2019, 58, 1–5. [Google Scholar] [CrossRef] [PubMed]
  97. Zhang, Y.; Lu, W.; Cong, L.; Liu, J.; Sun, L.; Mauger, A.; Julien, C.M.; Xie, H.; Liu, J. Cross-linking network based on Poly(ethylene oxide): Solid polymer electrolyte for room temperature lithium battery. J. Power Sources 2019, 420, 63–72. [Google Scholar] [CrossRef]
  98. Choudhury, S.; Stalin, S.; Vu, D.; Warren, A.; Deng, Y.; Biswal, P.; Archer, L.A. Solid-state polymer electrolytes for high-performance lithium metal batteries. Nat. Commun. 2019, 10, 4398. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  99. Porcarelli, L.; Gerbaldi, C.; Bella, F.; Nair, J.R. Super soft all-ethylene oxide polymer electrolyte for safe all-solid lithium batteries. Sci. Rep. 2016, 6, 19892. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  100. Khurana, R.; Schaefer, J.L.; Archer, L.A.; Coates, G.W. Suppression of lithium dendrite growth using cross-linked polyethylene/poly(ethylene oxide) electrolytes: A new approach for practical lithium-metal polymer batteries. J. Am. Chem. Soc. 2014, 136, 7395–7402. [Google Scholar] [PubMed]
  101. Porcarelli, L.; Shaplov, A.S.; Bella, F.; Nair, J.R.; Mecerreyes, D.; Gerbaldi, C. Single-ion conducting polymer electrolytes for lithium metal polymer batteries that operate at ambient temperature. ACS Energy Lett. 2016, 1, 678–682. [Google Scholar]
  102. Luo, G.; Yuan, B.; Guan, T.; Cheng, F.; Zhang, W.; Chen, J. Synthesis of single lithium-ion conducting polymer electrolyte membrane for solid-state lithium metal batteries. ACS Appl. Energy Mater. 2019, 2, 3028–3034. [Google Scholar] [CrossRef]
  103. Jiang, H.; Fang, S. All solid-state comb-like network polymer electrolytes based on poly(methylsiloxane). J. Power Sources 2006, 159, 673–678. [Google Scholar] [CrossRef]
  104. Zhang, Z.; Sherlock, D.; West, R.; West, R.; Amine, K.; Lyons, L.J. Cross-linked network polymer electrolytes based on a polysiloxane backbone with oligo(oxyethylene) side chains:  synthesis and conductivity. Macromolecules 2003, 36, 9176–9180. [Google Scholar] [CrossRef]
  105. Daigle, J.-C.; Asakawa, Y.; Vijh, A.; Hovington, P.; Armand, M.; Zaghib, K. Exceptionally stable polymer electrolyte for a lithium battery based on cross-linking by a residue-free process. J. Power Sources 2016, 332, 213–221. [Google Scholar]
  106. Grewal, M.S.; Tanaka, M.; Kawakami, H. Free-standing polydimethylsiloxane-based cross-linked network solid polymer electrolytes for future lithium ion battery applications. Electrochim. Acta 2019, 307, 148–156. [Google Scholar] [CrossRef]
  107. Xia, Y.; Fujieda, T.; Tatsumi, K.; Prosini, P.P.; Sakai, T. Thermal and electrochemical stability of cathode materials in solid polymer electrolyte. J. Power Sources 2001, 92, 234–243. [Google Scholar] [CrossRef]
  108. Xia, Y.; Tatsumi, K.; Fujieda, T.; Prosini, P.P.; Sakai, T. Solid-State Lithium-Polymer Batteries Using Lithiated MnO2 Cathodes. J. Electrochem. Soc. 2000, 147, 2050–2056. [Google Scholar] [CrossRef]
  109. Ebadi, M.; Marchiori, C.; Mindemark, J.; Brandell, D.; Araujo, C.M. Assessing structure and stability of polymer/lithium-metal interfaces from first-principles calculations. J. Mater. Chem. A 2019, 7, 8394–8404. [Google Scholar] [CrossRef]
  110. Zaghib, K.; Armand, M.; Gauthier, M. Electrochemistry of anodes in solid-state Li-ion polymer batteries. J. Electrochem. Soc. 1998, 145, 3135. [Google Scholar]
  111. Yang, Q.; Zhang, Z.; Sun, X.-G.; Hu, Y.-S.; Xing, H.; Dai, S. Ionic liquids and derived materials for lithium and sodium batteries. Chem. Soc. Rev. 2018, 47, 2020–2064. [Google Scholar] [CrossRef]
  112. Osada, I.; de Vries, H.; Scrosati, B.; Passerini, S. Ionic-liquid-based polymer electrolytes for battery applications. Angew. Chem. Int. Ed. 2016, 55, 500–513. [Google Scholar] [CrossRef]
  113. MacFarlane, D.R.; Forsyth, M.; Howlett, P.C.; Kar, M.; Passerini, S.; Pringle, J.M.; Ohno, H.; Watanabe, M.; Yan, F.; Zheng, W.; et al. Ionic liquids and their solid-state analogues as materials for energy generation and storage. Nat. Rev. Mater. 2016, 1, 15005. [Google Scholar]
  114. Appetecchi, G.B.; Montanino, M.; Passerini, S. Ionic liquid-based electrolytes for high energy, safer lithium batteries. In Ionic Liquids: Science and Applications, ACS Symposium Series; ACS Publications: Washington, DC, WA, USA, 2012; Chapter 4; Volume 1117, pp. 67–128. [Google Scholar]
  115. Armand, M.; Endres, F.; MacFarlane, D.R.; Ohno, H.; Scrosati, B. Ionic-liquid materials for the electrochemical challenges of the future. Nat. Mater. 2009, 8, 621. [Google Scholar]
  116. Ogihara, W.; Washiro, S.; Nakajima, H.; Ohno, H. Effect of cation structure on the electrochemical and thermal properties of ion conductive polymers obtained from polymerizable ionic liquids. Electrochim. Acta 2006, 51, 2614–2619. [Google Scholar] [CrossRef]
  117. Keith, J.R.; Rebello, N.J.; Cowen, B.J.; Ganesan, V. Influence of counterion structure on conductivity of polymerized ionic liquids. ACS Macro Lett. 2019, 8, 387–392. [Google Scholar] [CrossRef]
  118. Ohno, H.; Yoshizawa, M.; Ogihara, W. Development of new class of ion conductive polymers based on ionic liquids. Electrochim. Acta 2004, 50, 255–261. [Google Scholar] [CrossRef]
  119. Fan, F.; Wang, W.; Holt, A.P.; Feng, H.; Uhrig, D.; Lu, X.; Hong, T.; Wang, Y.; Kang, N.-G.; Mays, J.; et al. Effect of molecular weight on the ion transport mechanism in polymerized ionic liquids. Macromolecules 2016, 49, 4557–4570. [Google Scholar] [CrossRef]
  120. Kuray, P.; Noda, T.; Matsumoto, A.; Iacob, C.; Inoue, T.; Hickner, M.A.; Runt, J. Ion transport in pendant and backbone polymerized ionic liquids. Macromolecules 2019, 52, 6438–6448. [Google Scholar] [CrossRef]
  121. Delhorbe, V.; Bresser, D.; Mendil-Jakani, H.; Rannou, P.; Bernard, L.; Gutel, T.; Lyonnard, S.; Picard, L. Unveiling the ion conduction mechanism in imidazolium-based poly(ionic liquids): A comprehensive investigation of the structure-to-transport interplay. Macromolecules 2017, 50, 4309–4321. [Google Scholar] [CrossRef]
  122. Yin, K.; Zhang, Z.; Yang, L.; Hirano, S.-I. An imidazolium-based polymerized ionic liquid via novel synthetic strategy as polymer electrolytes for lithium ion batteries. J. Power Sources 2014, 258, 150–154. [Google Scholar] [CrossRef]
  123. Zhang, P.; Li, M.; Yang, B.; Fang, Y.; Jiang, X.; Veith, G.M.; Sun, X.-G.; Dai, S. Polymerized ionic networks with high charge density: Quasi-solid electrolytes in lithium-metal batteries. Adv. Mater. 2015, 27, 8088–8094. [Google Scholar] [CrossRef]
  124. Tian, X.; Yi, Y.; Yang, P.; Liu, P.; Qu, L.; Li, M.; Hu, Y.-S.; Yang, B. High-charge density polymerized ionic networks boosting high ionic conductivity as quasi-solid electrolytes for high-voltage batteries. ACS Appl. Mater. Interfaces 2019, 11, 4001–4010. [Google Scholar] [CrossRef]
  125. Zhou, D.; Liu, R.; Zhang, J.; Qi, X.; He, Y.-B.; Li, B.; Yang, Q.-H.; Hu, Y.-S.; Kang, F. In situ synthesis of hierarchical poly(ionic liquid)-based solid electrolytes for high-safety lithium-ion and sodium-ion batteries. Nano Energy 2017, 33, 45–54. [Google Scholar] [CrossRef]
Figure 1. Ragone plot of some energy storage devices.
Figure 1. Ragone plot of some energy storage devices.
Materials 13 02488 g001
Figure 2. Illustration of all solid-state lithium polymer batteries (ASSLPB) composition.
Figure 2. Illustration of all solid-state lithium polymer batteries (ASSLPB) composition.
Materials 13 02488 g002
Figure 3. Ion transport mechanism in non-ionic polymer.
Figure 3. Ion transport mechanism in non-ionic polymer.
Materials 13 02488 g003
Figure 4. Synthesis of oxyethylene-grafted polyphosphazenes (MEEPs).
Figure 4. Synthesis of oxyethylene-grafted polyphosphazenes (MEEPs).
Materials 13 02488 g004
Figure 5. Temperature dependence of ionic conductivity of (a) LiTFSI/PEO polymer electrolytes with a molar ratio EO/Li+ = 20 [66]; (b) LiTFSI/poly-PEGMEM with a molar ratio EO/Li+ = 18 [65]; (c) LiTFSI/polymethacrylate-graft-poly(ethylene glycol) monomethyl ether (Poly(MA)-g-PEGME) with a molar ratio EO/Li+ = 16 [67]. Reproduced with permission from [65]. Copyright 2019, The Chinese Ceramic Society; [66]. Copyright 2014, Elsevier E. V.; [67]. Copyright 2019, American Chemical Society.
Figure 5. Temperature dependence of ionic conductivity of (a) LiTFSI/PEO polymer electrolytes with a molar ratio EO/Li+ = 20 [66]; (b) LiTFSI/poly-PEGMEM with a molar ratio EO/Li+ = 18 [65]; (c) LiTFSI/polymethacrylate-graft-poly(ethylene glycol) monomethyl ether (Poly(MA)-g-PEGME) with a molar ratio EO/Li+ = 16 [67]. Reproduced with permission from [65]. Copyright 2019, The Chinese Ceramic Society; [66]. Copyright 2014, Elsevier E. V.; [67]. Copyright 2019, American Chemical Society.
Materials 13 02488 g005
Figure 6. Structure of hyper-branched star polymer HBPS-(PMMA- b-PPEGMA)x (a) and photograph of HBPS-(PMMA- b-PPEGMA)46/LiTFSI electrolyte film (b) [83]. Reproduced with permission from [83]. Copyright 2016, Elsevier E. V.
Figure 6. Structure of hyper-branched star polymer HBPS-(PMMA- b-PPEGMA)x (a) and photograph of HBPS-(PMMA- b-PPEGMA)46/LiTFSI electrolyte film (b) [83]. Reproduced with permission from [83]. Copyright 2016, Elsevier E. V.
Materials 13 02488 g006
Figure 7. Synthesis of hbPPEGMAm-s-PSn hyperstar polymers; (a) synthetic route; (b) schematic of hyper-branched hbPPEGMAm and hbPPEGMAm-s-PSn polymers with different average chain lengths of branched PEO (m) and linear PS (n); (c) digital photograph of hbPPEGMA50-s-PS299 SPE membrane [85]. Reproduced with permission from [85]. Copyright 2019, American Chemical Society.
Figure 7. Synthesis of hbPPEGMAm-s-PSn hyperstar polymers; (a) synthetic route; (b) schematic of hyper-branched hbPPEGMAm and hbPPEGMAm-s-PSn polymers with different average chain lengths of branched PEO (m) and linear PS (n); (c) digital photograph of hbPPEGMA50-s-PS299 SPE membrane [85]. Reproduced with permission from [85]. Copyright 2019, American Chemical Society.
Materials 13 02488 g007
Figure 8. Dependence of ideal morphology factor (fideal) on morphology. The blue and red regions represent conducting and non-conducting micro-phases, respectively [93]. Reproduced with permission from [93]. Copyright 2015, American Chemical Society.
Figure 8. Dependence of ideal morphology factor (fideal) on morphology. The blue and red regions represent conducting and non-conducting micro-phases, respectively [93]. Reproduced with permission from [93]. Copyright 2015, American Chemical Society.
Materials 13 02488 g008
Figure 9. Synthesis route of polymer electrolyte membrane (a) and ionic conductivity of membranes with varying LiTFSI contents (b) [95]. Reproduced with permission from [95]. Copyright 2017, Elsevier B.V.
Figure 9. Synthesis route of polymer electrolyte membrane (a) and ionic conductivity of membranes with varying LiTFSI contents (b) [95]. Reproduced with permission from [95]. Copyright 2017, Elsevier B.V.
Materials 13 02488 g009
Figure 10. (a) Diagram of PTT–SPE inter-crosslinking structure; (b,c) SEM images of PTT–SPE membrane; (d,e) Photographs of PTT–SPE (2:1:2) film in stretching mode [97]. Reproduced with permission from [97]. Copyright 2019, Elsevier B.V.
Figure 10. (a) Diagram of PTT–SPE inter-crosslinking structure; (b,c) SEM images of PTT–SPE membrane; (d,e) Photographs of PTT–SPE (2:1:2) film in stretching mode [97]. Reproduced with permission from [97]. Copyright 2019, Elsevier B.V.
Materials 13 02488 g010
Figure 11. (a) Glass transition temperature as a function of poly(ethylene glycol) dimethacrylate (PEGDMA) fraction (Φ) in the membranes. The red line is the Gordon-Taylor fit to the experimental results; (b) Tensile analysis of the crosslinked membrane at various PEGDMA content. The oscillatory tensile measurement was done on thin films at a low strain rate of 0.1% in the frequency range of 100–10 Hz. The plateau modulus is plotted as a function of PEGDMA content in the inset [98]. Reproduced with permission from [98]. Copyright 2019, Springer Nature Limited.
Figure 11. (a) Glass transition temperature as a function of poly(ethylene glycol) dimethacrylate (PEGDMA) fraction (Φ) in the membranes. The red line is the Gordon-Taylor fit to the experimental results; (b) Tensile analysis of the crosslinked membrane at various PEGDMA content. The oscillatory tensile measurement was done on thin films at a low strain rate of 0.1% in the frequency range of 100–10 Hz. The plateau modulus is plotted as a function of PEGDMA content in the inset [98]. Reproduced with permission from [98]. Copyright 2019, Springer Nature Limited.
Materials 13 02488 g011
Figure 12. Preparation schemes of comb-like network polymer electrolyte [106]. Reproduced with permission from [103]. Copyright 2005, Elsevier B.V.
Figure 12. Preparation schemes of comb-like network polymer electrolyte [106]. Reproduced with permission from [103]. Copyright 2005, Elsevier B.V.
Materials 13 02488 g012
Figure 13. Effect of polymer architecture on electrolyte properties.
Figure 13. Effect of polymer architecture on electrolyte properties.
Materials 13 02488 g013
Figure 14. (Top) Chemical structures of aliphatic imidazolium-based backbone and pendant PILs and varying counter anions; (Bottom) (a) conductivity profiles of B-PILs and P-PILs from DRS shown as a function of temperature (TFSI = bis(trifluoromethane)sulfonimide anion; NfO = nonafluorobutanesulfonate anion; CPFSI = 1,1,2,2,3,3-hexafluoropropane-1,2-disulfonimide anion) and (b) scaled to each material’s corresponding glass transition temperature [120]. Reproduced with permission from [120]. Copyright 2019, American Chemical Society.
Figure 14. (Top) Chemical structures of aliphatic imidazolium-based backbone and pendant PILs and varying counter anions; (Bottom) (a) conductivity profiles of B-PILs and P-PILs from DRS shown as a function of temperature (TFSI = bis(trifluoromethane)sulfonimide anion; NfO = nonafluorobutanesulfonate anion; CPFSI = 1,1,2,2,3,3-hexafluoropropane-1,2-disulfonimide anion) and (b) scaled to each material’s corresponding glass transition temperature [120]. Reproduced with permission from [120]. Copyright 2019, American Chemical Society.
Materials 13 02488 g014
Table 1. Backbone structure and electrochemical properties of comb-like polymers.
Table 1. Backbone structure and electrochemical properties of comb-like polymers.
BackboneChemical StructureSaltConductivity
(S∙cm−1)
Potential Window (V)Ref.
Poly(epoxide ether) Materials 13 02488 i001LiTFSI3.2 × 10−4
(60 °C)
ND[75]
Polysiloxane Materials 13 02488 i002LiTFSI>10−4
(25 °C)
4.5[63]
Polyphosphazene Materials 13 02488 i003lithium triflate (LiSO3CF3)~ 3 × 10−5
(25 °C)
ND[61]
Polymethacrylate Materials 13 02488 i004LiTFSI1.44 × 10−4
(30 °C)
7.26 × 10−4
(60 °C)
> 5[65]
Poly(acrylonitrile-butadiene) Materials 13 02488 i005LiSO3CF3~3 × 10−5
(25 °C)
ND[68]
Polynorbornene Materials 13 02488 i006LiTFSI>3 × 10−5
(25 °C)
>7 × 10−4
(80 °C)
~ 3.5[67]
Poly(hydroxyl styrene) Materials 13 02488 i007LiSO3CF3∼6 × 10−5
(60 °C)
ND[71]
Polyether ether ketone Materials 13 02488 i008LiClO4> 10−5
(room temperature)
ND[70]
Polypeptoid Materials 13 02488 i009LiTFSI~10−5
(50 °C)
2.6 × 10−4
(100 °C)
ND[69]
Poly(ethylene-co-maleic anhydride) Materials 13 02488 i010LiTFSI4.5 × 10−5
(room temperature)
5.3 × 10−4
(70 °C)
>4
(stainless steel electrode)
>3
(aluminum electrode)
[72]
ND = No data

Share and Cite

MDPI and ACS Style

Zhang, X.; Daigle, J.-C.; Zaghib, K. Comprehensive Review of Polymer Architecture for All-Solid-State Lithium Rechargeable Batteries. Materials 2020, 13, 2488. https://doi.org/10.3390/ma13112488

AMA Style

Zhang X, Daigle J-C, Zaghib K. Comprehensive Review of Polymer Architecture for All-Solid-State Lithium Rechargeable Batteries. Materials. 2020; 13(11):2488. https://doi.org/10.3390/ma13112488

Chicago/Turabian Style

Zhang, Xuewei, Jean-Christophe Daigle, and Karim Zaghib. 2020. "Comprehensive Review of Polymer Architecture for All-Solid-State Lithium Rechargeable Batteries" Materials 13, no. 11: 2488. https://doi.org/10.3390/ma13112488

APA Style

Zhang, X., Daigle, J. -C., & Zaghib, K. (2020). Comprehensive Review of Polymer Architecture for All-Solid-State Lithium Rechargeable Batteries. Materials, 13(11), 2488. https://doi.org/10.3390/ma13112488

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop