Next Article in Journal
Materials AIILnInO4 with Ruddlesden-Popper Structure for Electrochemical Applications: Relationship between Ion (Oxygen-Ion, Proton) Conductivity, Water Uptake, and Structural Changes
Next Article in Special Issue
An Effective Strategy to Maintain the CALPHAD Atomic Mobility Database of Multicomponent Systems and Its Application to Hcp Mg–Al–Zn–Sn Alloys
Previous Article in Journal
C-A-S-H Gel and Pore Structure Characteristics of Alkali-Activated Red Mud–Iron Tailings Cementitious Mortar
Previous Article in Special Issue
A First-Principles Study of the Cu-Containing β″ Precipitates in Al-Mg-Si-Cu Alloy
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Nb/Sn Liquid-Solid Reactive Diffusion Couples and Their Application to Determination of Phase Equilibria and Interdiffusion Coefficients of Nb-Sn Binary System

State Key Lab of Powder Metallurgy, Central South University, Changsha 410083, China
*
Authors to whom correspondence should be addressed.
Materials 2022, 15(1), 113; https://doi.org/10.3390/ma15010113
Submission received: 29 November 2021 / Revised: 16 December 2021 / Accepted: 20 December 2021 / Published: 24 December 2021
(This article belongs to the Special Issue Light Alloys and High-Temperature Alloys)

Abstract

:
Nb3Sn plays an irreplaceable role in superconducting parts due to its stable performance under high field conditions. Accurate phase equilibria and interdiffusion coefficients are of great significance for designing novel Nb3Sn superconductors. However, the related experimental information is still in a state of scarcity because of the difficulty in fabrication of Nb-Sn alloys caused by the large difference in melting points of Nb and Sn. In this paper, a simple but pragmatic approach was first proposed to prepare the Nb/Sn liquid-solid reactive diffusion couples (LSDCs) at 1100 °C and 1200 °C, of which the phase identification of the formed layer and the measurement of composition-distance profiles were conducted. The formed layer in Nb/Sn LSDCs was confirmed to be Nb3Sn compound. While the measured composition profiles were employed to determine the phase equilibria according to the local equilibrium hypothesis and the interdiffusion coefficients with an aid of the latest version of HitDIC software. The determined phase equilibria of Nb3Sn, (Nb) and liquid show good agreement with the assessed phase diagram. While the calculated interdiffusion coefficients and activation energy for diffusion in Nb3Sn are consistent with both experimental and theoretical data in the literature. Moreover, the growth of the formed Nb3Sn layer in Nb/Sn LSDCs was also found to be diffusion controlled. All the obtained phase equilibria and interdiffusion coefficients are of great value for further thermodynamic and kinetic modeling of the Nb-Sn system. Furthermore, it is anticipated that the presently proposed approach of fabricating liquid-solid reactive diffusion couple should serve as a general one for various alloy systems with large differences in melting points.

1. Introduction

Due to its high superconducting critical temperature Tc = 18 K, high superconducting critical magnetic field Hc = 27T (4 K) and stable performance [1], Nb3Sn superconductor has been of great importance in high field working environments since the 1960s [2]. Tokamak device, used in nuclear-fusion research for magnetic confinement of plasma, is the core unit of both the International Thermonuclear Experimental Reactor (ITER) project and the China Fusion Engineering Test Reactor (CFETR) project. Nb3Sn acts as the vital toroidal field coil in Tokamak devices [3]. However, as one of A15 type intermetallic compounds in the cubic lattice system [4], Nb3Sn owns the poor plasticity and toughness, and can be easily damaged, resulting in destruction of superconductivity. In order to improve the properties/performance of Nb3Sn-based parts and even explore novel Nb3Sn-based alloys, accurate phase equilibria and diffusion coefficients [5,6] are the prerequisites for understanding the Nb-Sn and its related systems. Unfortunately, a very large difference in melting points between Nb (2468 °C) and Sn (231.89 °C) makes it extremely difficult to fabricate the Nb-Sn alloys. To overcome this problem, researchers have made many attempts, and developed several techniques for preparing Nb-Sn alloys, including the powder-in-tube process [7], the bronze process [8], the internal tin process [9], the restacked rod process [10], the powder metallurgy method [11], and so on. Even so, the experimental data on phase equilibria and diffusion coefficients of the Nb-Sn binary system are still in a state of scarcity.
Up to now, only about 10 groups of researchers have performed experimental measurement of phase equilibria of the binary Nb-Sn system [12,13,14,15,16,17,18,19,20]. Based on the limited experimental phase equilibrium information, Toffolon [18] performed a CALPHAD (CALculation of PHAse Diagram) [21] thermodynamic assessment of Nb-Sn system in 1998. During the assessment, Toffolon [18] adopted the conclusion of Massalski [17] and Shunk [22] that Nb3Sn would not be stable below 796 °C. However, on account of the enthalpy of formation of Nb3Sn determined by drop calorimetry and other new literature data [13,14,15], it was believed that Nb3Sn can exist stably down to the room temperature. Then in 2002, Toffolon [19] updated the thermodynamic assessment of binary Nb-Sn system accordingly. Although the calculated phase equilibria of binary Nb-Sn system according to the thermodynamic descriptions by Toffolon [19] are in general agreement with the limited experimental data [12,13,14,15,16,20], it is still necessary to provide more accurate experimental phase equilibrium data for further validation. While for the diffusion coefficients in Nb-Sn binary, there is only one report from Wallach [23], who obtained the interdiffusion coefficients of Nb3Sn from the ternary Cu-Nb-Sn system measured by two different methods, i.e., the Nb-bronze multi-layered thin-film composites and the multi-filamentary composites. Moreover, the data from Wallach [23] only cover the low-temperature range between 350 °C and 800 °C. Again, accurate experimental diffusion coefficients of the binary Nb-Sn system, especially at high temperatures, are in urgent need.
Consequently, the major objectives of this paper are: (i) to fabricate the Nb/Sn liquid-solid reactive diffusion couples (LSDCs) at 1100 °C and 1200 °C. Here, a simple but pragmatic approach is to be proposed for preparing the Nb/Sn LSDCs, of which the melting points of two end-members show a large difference; and (ii) to apply the prepared Nb/Sn LSDCs to determine the accurate phase equilibria and interdiffusion coefficients of the binary Nb-Sn system at the corresponding temperatures. The phase equilibria are to be measured based on the classic local equilibrium hypothesis, while the interdiffusion coefficients of the compound Nb3Sn will be evaluated by using the HitDIC (High-throughput Determination of Interdiffusion Coefficients) software [24,25,26,27], based on the measured composition-distance profiles over the interdiffusion zones in Nb/Sn LSDCs.

2. Materials and Methods

The raw materials for preparing Nb/Sn LSDCs were Nb blocks (25 × 15 × 14 mm) with a purity of 99.99% (wt.%) and Sn particles (1~2 mm in diameter) with a purity of 99.99% (wt.%). The Nb block was fixed on the leveling workbench for blind hole processing. An Nb cap (25 × 15 × 3 mm) was first cut from the Nb block by means of the wire-electrode technique, and then a blind hole (17 × 9 × 6 mm) was dug by the drill bit in the center of the remaining Nb block. Considering that the high-speed rotation of the drill bit may generate a large amount of heat, causing the slight oxidation on the surface of the Nb block, it is thus necessary to polish the inner surface of the blind hole after machining to remove the oxide layer and level the inner surface. After that, Sn particles were filled into the hole, and the Nb block was welded and sealed with the Nb cap. The assembled Nb/Sn LSDC is schematically shown in Figure 1a.
Two identical Nb/Sn diffusion couples were put into the corundum boats equipped with quartz cotton. The corundum boats containing the samples were preheated for a few minutes at the furnace port and then subjected to annealing at 1100 °C for 2.33 h and 1200 °C for 2 h in a high-temperature vacuum tube furnace (GSL1700X, Hefei Kejing Materials Technology Co., Ltd., Hefei, China), respectively. There are three reasons for choosing the annealing temperatures as 1100 °C and 1200 °C. First, according to the assessed phase diagram [19], only three stable phases (bcc, liquid and Nb3Sn) exist in the Nb-Sn binary system between 911 °C~2152 °C. Such simple phase equilibria are beneficial for the study on thermodynamic and diffusion properties related to the Nb3Sn phase. Second, no experimental studies on the phase equilibria in Nb-Sn binary system around 1100 °C. Third, the reported interdiffusion coefficients of Nb3Sn phase only cover the low-temperature range (350 °C~800 °C), and more information on interdiffusion coefficients of Nb3Sn phase at higher temperatures is highly needed. Moreover, the formation of Nb3Sn phase was clearly observed in Nb-bronze multi-filamentary composites after annealing at 700 °C for only 1 h in the work of Ref. [28]. Therefore, the annealing time at 1100 °C and 1200 °C was chosen to be around 2 h for the formation of Nb3Sn phase with sufficient thickness in Nb/Sn LSDCs. At both 1100 °C and 1200 °C, the Nb block keeps the solid state, while the Sn particles are melted into the liquid state. The schematic diagrams for top view and side view of Nb/Sn LSDC are displayed in Figure 1b,c. After annealing, the Nb/Sn LSDCs were quickly quenched in liquid nitrogen. Subsequently, each Nb/Sn LSDC was cut into five pieces, and metallographically polished for the subsequent analysis of interdiffusion zones over the Nb/Sn interface. The photos of the physical samples of the Nb/Sn LSDCs after quenching are presented in Figure 1d,e. The optical microscopy (OM), scanning electron microscope (SEM), electron probe micro-analysis (EPMA), and electron backscattered diffraction (EBSD) techniques were used to analyze the microstructure and composition of the Nb/Sn LSDCs.

3. Results and Discussion

3.1. Phase Equilibria

According to the Nb-Sn binary phase diagram assessed by Toffolon [19], three phases are stable over the temperature range of 911~2152 °C, i.e., bcc, Nb3Sn and liquid. The microstructure of the Nb/Sn LSDCs annealed at 1100 °C and 1200 °C taken from the position of the red circle in Figure 1e are respectively shown in Figure 2a,b. As can be observed in the figures, one apparent layer formed over the interdiffusion zone across the Nb/Sn interface at both 1100 and 1200 °C. The composition of the formed layer was measured by means of the EPMA technique, while its crystal structure (at point 1 in Figure 2b) was characterized by using the EBSD technique, as shown in Figure 3. Both EPMA and EBSD results indicated that the layer formed over interdiffusion zone is the Nb3Sn phase, which corresponds well with the Nb-Sn phase diagram assessed by Toffolon [19]. Moreover, the average size of Nb3Sn grains annealed at 1200 °C for 2 h was measured to be 4.36 ± 0.85 μm.
As also indicated in Figure 2, the EPMA scans of the compositions in Nb/Sn LSDCs across the entire diffusion zone perpendicularly to the diffusion interface were performed, and the obtained composition-distance profiles are displayed as scattered points in Figure 4a,b. Here, it should be noted that two EPMA runs were conducted for Nb/Sn LSDC at each temperature. Based on the measured composition-distance profiles, the average thickness of the Nb3Sn phase layer can be evaluated to be 6.63 ± 1.86 μm at 1200 °C for 2 h and 3.43 ± 0.62 μm at 1100 °C for 2.33 h.
The measured concentration profiles of Nb/Sn LSDCs at two temperatures were then superimposed on the Nb-Sn binary phase diagram from Toffolon [19], as presented in Figure 5. It is worth mentioning that there should be no two-phase mixture regions in binary diffusion couples because they are thermodynamically forbidden. Thus, based on the local equilibrium hypothesis at the phase interfaces, the equilibrium compositions of phases could be obtained by extrapolating the measured concentration profiles to the phase interfaces. The concentration profiles of Nb3Sn and liquid phases can be clearly seen in Figure 5, and their equilibrium compositions at 1100 and 1200 °C were determined and marked by solid circles in Figure 5 and summarized in Table 1. As can be clearly seen in the figure, the determined homogeneity range of Nb3Sn compound at both 1100 °C and 1200 °C are in good agreement with the assessed phase equilibria by [19]. Moreover, it is astonishing to see a general agreement between the determined solubility limits of Nb in liquid (Sn) at both 1100 °C and 1200 °C and the assessed ones [19] exist, though there should be some further phase transformations from the remaining liquid to solids during quenching of LSDCs. For the solubility of Sn in (Nb) phase, the determined value at 1200 °C is in good consistency with the assessed one [19], as displayed in Figure 5. However, the solubility of Sn in (Nb) phase at 1100 °C cannot be accurately determined due to the relatively scattered composition profile of Nb/Sn LSDC at 1100 °C. Instead, a rough value between 3.1 at.% and 7.1 at.% was proposed for the solubility of Sn in (Nb) phase at 1100 °C, which is still close to the assessed one by [19]. Based on Figure 5 and the above analysis, the phase equilibria in binary Nb-Sn system at both 1100 °C and 1200 °C determined by the present LSDCs and predicted by thermodynamic assessment [19] should be reliable.

3.2. Interdiffusion Coefficients

Based on the experimental composition-distance profiles yielded in the interdiffusion zones of Nb/Sn LSDCs, the interdiffusion coefficients were extracted using the latest version of HitDIC software [24,25,26] originally developed under the framework of pragmatic numerical inverse approach [29,30]. By simplifying the diffusion processes in reactive diffusion couple to be a one-dimensional moving boundary problem, the evolution of composition cn for the n-th phase and interface position sn between the n-th phase and the (n + 1)-th phase described as
c n t = r ( D n c n r )
D n 1 c n 1 r | r = s n ( t ) D n c n r | r = s n + ( t ) = ( c n + 1 c n ) d s n d t     at   r = s n ( t )
where D n are the interdiffusion coefficients to be recovered by means of the numerical inverse method. That is, with the setting of a diffusion couple, i.e., initial compositions of terminal alloys, diffusion time, and component-distance profile, an inverse routine based on optimization is used to iteratively evaluate a suggested set of interdiffusion coefficients for all the solution phases and intermetallic compounds. At each iteration, deviation between the prediction and experimental observations can be evaluated, while suggestions for an alternative set of interdiffusion coefficients may be provided according to the employed optimization methods, i.e., the genetic algorithm. The optimization processes can be terminated once the satisfactory prediction result towards the experimental observation is obtained, and the related set of interdiffusion coefficients can therefore be taken as the determined results. Among the calculation processes, the local equilibrium assumption is applied for adjacent phases in the reactive diffusion couple.
The measured composition-distance profiles were used to evaluate the interdiffusion coefficients for the Nb-Sn system at 1100 °C and 1200 °C, respectively. The predicted composition-distance profiles using HitDIC are also displayed as the solid lines in Figure 5. As can be seen in the plots, good consistency between the predicted composition-distance profiles and the experimental data exists for the two investigated temperatures. Here, only the interdiffusion coefficients of Nb3Sn compound are to be evaluated. That is because (i) during the quenching, the liquid Sn near the interdiffusion zone and diffused Nb may form the NbSn2 phase, resulting in the Sn content in the diffusion zone near the liquid side lower than the theoretical value, and (ii) the spatial resolution of EPMA makes the measured composition points close to (Nb) side insufficient for evaluating the interdiffusion coefficient of bcc phase especially at 1100 °C.
Figure 6a shows the presently extracted interdiffusion coefficients of Nb3Sn from Nb/Sn LSDCs at 1100 °C and 1200 °C (i.e., 4.66 × 10−15 m2∙s−1 and 1.85 × 10−14 m2∙s−1), which generally follow the same trend as the low-temperature data from multi-layered thin-film composites and multi-filamentary composites [23]. Based on presently extracted interdiffusion coefficients at 1100 °C and 1200 °C, the pre-exponential factor and the activation energy for diffusion in Nb3Sn compound can be obtained by fitting to the Arrhenius equation:
D = D 0 exp ( Q R T ) .
The obtained pre-exponential factor of the Nb3Sn phase D0 in Equation (4) is 1.80 × 10−6 m2∙s−1, while the activation energy Q is 232.04 kJ∙mol−1. The presently evaluated activation energy for Nb3Sn compound shows very good agreement with the data from the kinetics measurements (i.e., 248.71 kJ∙mol−1) by [31] and ab initio density functional theory calculations (i.e., 269.79 kJ∙mol−1) by [32], validating the reliability of the presently obtained interdiffusion coefficients of Nb3Sn compound.
Moreover, with interdiffusion coefficients calculated by HitDIC and the simultaneous diffusional growth of Nb3Sn layer [33], the average thickness of the Nb3Sn phase layer was determined as a function of the annealing time, which can be expressed as the following equation,
l = k ( t t 0 ) n ,
where l is the average thickness of the Nb3Sn phase layer, t is the annealing time, and t0 is the unit time. As shown in Figure 6b, we obtained k = 2.28 μm and n = 0.51 for the Nb/Sn LSDC annealed at 1100 °C, and k = 4.69 μm and n = 0.51 for the Nb/Sn LSDC annealed at 1200 °C, with the experimental thickness data locating precisely on the predicted profile. Such a fact indicates that the growth of the Nb3Sn phase layer is controlled by diffusion.
It should be noted in Figure 6a that the interdiffusion coefficients of Nb3Sn obtained in this work are a bit lower than the values extrapolated from low temperature data [23]. To explore the probable reasons for this case, the interface of the Nb/Sn liquid-solid reactive diffusion couple was further characterized by experiments. The element mapping characteristics over the diffusion zone were analyzed using the EPMA map analysis, as shown in Figure 7. The result shows that the Nb3Sn phase layer formed across the Nb/Sn interface, while some free Nb3Sn particles existed in the (Sn) region. The reason is considered that the Nb element diffused into melted Sn during the annealing process, and some Nb3Sn particles formed and remained in the solidified Sn region after the quench. There are also some lath-like microstructures distributing in the solidified (Sn) region, and that might be due to the composition segregation in solidified liquid that resulted in the formation of the NbSn2 phase. Because of the peritectic reactions, L + Nb3Sn→NbSn2 and L + NbSn2→(Sn), a fraction of generated Nb3Sn phase reacted with the remained liquid, which can make the measured thickness of the Nb3Sn phase layer smaller than the actual one, thus lowering the interdiffusion coefficients of the Nb3Sn phase.

4. Conclusions

A simple but pragmatic approach was proposed to fabricate the Nb/Sn LSDCs, which were subjected to annealing at 1100 °C and 1200 °C for 2.33 h and 2 h, respectively. It was found that apparent interdiffusion zones formed across the Nb/Sn interface in both LSDCs. The interdiffusion zone was then comprehensively characterized by EPMA and EBSD techniques. Both composition and crystal structure results confirm that the formed layer at the Nb/Sn interface is the Nb3Sn phase.
The equilibrium homogeneity range of Nb3Sn, solubility limits of (Nb) and liquid phases at 1100 °C and 1200 °C were determined, and the results are in general agreement with the Nb-Sn binary phase diagram assessed by [19].
The interdiffusion coefficients of the Nb3Sn phase at 1100 °C and 1200 °C were evaluated by HitDIC software to be 3.22 × 10−15 m2∙s−1 and 1.73 × 10−14 m2∙s−1, respectively. The evaluated diffusion properties of compound Nb3Sn, including the interdiffusion coefficients and activation energy, are consistent with the corresponding experimental and theoretical values in the literature. Moreover, the relation between the model-predicted thickness of the Nb3Sn layer and the annealing time of Nb/Sn LSDCs was also observed to be in good agreement with the experimental data, indicating the growth of Nb3Sn layer in Nb/Sn LSDCs is diffusion controlled.
The presently proposed approach for preparing Nb/Sn LSDCs is anticipated to be a universal one for various alloy systems with large differences in melting points. Furthermore, combined with the local equilibrium hypothesis and HitDIC software, the corresponding phase equilibria and diffusion coefficients can be accurately determined simultaneously.

Author Contributions

Conceptualization, L.Z.; methodology, L.Z., Q.L.; investigation, J.Z. (Jiali Zhang) and J.Z. (Jing Zhong); data curation, J.Z. (Jiali Zhang); Writing—original draft preparation, J.Z. (Jiali Zhang); Writing—review and editing, J.Z. (Jing Zhong), L.Z. and Q.L.; visualization, J.Z. (Jiali Zhang); supervision, L.Z.; project administration, L.Z. All authors have read and agreed to the published version of the manuscript.

Funding

This work was financially supported by Natural Science Foundation of Hunan Province (Grant No.: 2021JJ10062), China. Jiali Zhang acknowledges the financial support by the Fundamental Research Funds for the Central Universities of Central South University (Fund No. 2021ZZTS0583), China.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data sharing not applicable.

Acknowledgments

The authors would like to thank Jianbao Gao, Wang Yi, and Guangchen Liu from Central South University for their kind help on fixing the problems during the experimental tests.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Larbalestier, D.; Gurevich, A.; Feldmann, D.M.; Polyanskii, A. High-Tc superconducting materials for electric power applications. Nature 2001, 414, 368–377. [Google Scholar] [CrossRef] [PubMed]
  2. Foner, S. High-field magnets and high-field superconductors. IEEE Trans. Appl. Supercond. 1995, 5, 121–140. [Google Scholar] [CrossRef]
  3. Shikov, A.K.; Panstsyrnyi, V.I.; Vorob’Eva, A.; Dergunova, E.A.; Sud’Ev, S.; Mareev, K.A.; Belyakov, N.A.; Abdyukhanov, I.M.; Sergeev, V.V. Microstructure and properties of Nb3Sn superconductors for the magnet system of the international thermonuclear experimental reactor. Met. Sci. Heat Treat. 2004, 46, 504–513. [Google Scholar] [CrossRef]
  4. Wang, R.; Luo, Q. A15 structure. Cryog. Supercond. 1986, 14, 57–65. [Google Scholar]
  5. Lu, Z.; Zhang, L. Thermodynamic description of the quaternary Al-Si-Mg-Sc system and its application to the design of novel Sc-additional A356 alloys. Mater. Des. 2017, 116, 427–437. [Google Scholar] [CrossRef]
  6. Zhong, J.; Chen, L.; Zhang, L. High-throughput determination of high-quality interdiffusion coefficients in metallic solids: A review. J. Mater. Sci. 2020, 55, 10303–10338. [Google Scholar] [CrossRef] [PubMed]
  7. Barsoum, M.W.; Ganguly, A.; Seifert, H.J.; Aldinger, F. The 1300 °C isothermal section in the Nb–Sn–C ternary phase diagram. J. Alloy. Compd. 2002, 337, 202–207. [Google Scholar] [CrossRef]
  8. Adam, E.; Beischer, P.; Marancik, W.; Young, M. Fabrication and properties of niobium-tin (Nb3Sn) tapes by the ”bronze process”: Application to superconducting power transmission lines. IEEE Trans. Magn. 1977, 13, 425–428. [Google Scholar] [CrossRef]
  9. Gregory, E.; Gulko, E.; Pyon, T. Development of Nb3Sn wires made by the Internal-Tin Process. In Advances in Cryogenic Engineering Materials; Balachandran, U.B., Gubser, D.G., Hartwig, K.T., Reed, R.P., Warnes, W.H., Bardos, V.A., Eds.; Springer: Boston, MA, USA, 1998; Volume 44, pp. 903–909. [Google Scholar]
  10. Ghosh, A.K.; Cooley, L.D.; Moodenbaugh, A.R.; Parrell, J.A.; Field, M.B.; Zhang, Y.; Hong, S. Magnetization studies of high Jc Nb3Sn strands. IEEE Trans. Appl. Supercond. 2005, 15, 3494–3497. [Google Scholar] [CrossRef]
  11. Qiu, Q.; Suo, H.; Cheng, J.; Zhang, Z.; Ji, Y.; Wang, Q. Fabrication and superconducting properties of Nb3Sn superconducting bulks. Chin. J. Rare Met. 2020, 44, 57–62. [Google Scholar]
  12. Ellis, T.G.; Wilhelm, H.A. Phase equilibria and crystallography for the niobium-tin system. J. Less-Common Met. 1964, 7, 67–83. [Google Scholar] [CrossRef]
  13. van Vucht, J.H.N.; van Ooijen, D.J.; Bruning, H.A.C.M. Some investigations of the niobium-tin phase diagram. Philips Res. Rep. 1965, 20, 136–161. [Google Scholar]
  14. Charlesworth, J.P.; Macphail, I.; Madsen, P.E. Experimental work on the niobium-tin constitution diagram and related studies. J. Mater. Sci. 1970, 5, 580–603. [Google Scholar] [CrossRef]
  15. Matstakova, A.; Lazarev, B. Peculiarities of the constitution phase diagram of the system niobium-tin. Phys. Met. Metallogr. 1973, 35, 133–141. [Google Scholar]
  16. Schiffman, R.A.; Bailey, D.M. Thermodynamics of the incongruently subliming niobium-tin system. High Temp. Sci. 1982, 15, 165–177. [Google Scholar]
  17. Massalski, T.B.; Murray, J.L.; Bennett, L.H.; Baker, H. Binary Alloy Phase Diagrams, 2nd ed.; American Society for Metals Research: Geauga, OH, USA, 1986. [Google Scholar]
  18. Toffolon, C.; Servant, C.; Sundman, B. Thermodynamic assessment of the Nb-Sn system. J. Phase Equilib. 1998, 19, 479. [Google Scholar] [CrossRef]
  19. Toffolon, C.; Servant, C.; Gachon, J.; Sundman, B. Reassessment of the Nb-Sn system. J. Phase Equilib. 2002, 23, 134. [Google Scholar] [CrossRef]
  20. Vieland, L.J. High-temperature phase equilibrium and superconductivity in the system niobium-tin. RCA Rev. 1964, 25, 366–378. [Google Scholar]
  21. Gao, J.; Zhong, J.; Liu, G.; Yang, S.; Song, B.; Zhang, L.; Liu, Z. A Machine Learning Accelerated Distributed Task Management System (Malac-Distmas) and Its Application in High-Throughput CALPHAD Computations Aiming at Efficient Alloy Design. Adv. Powder Mater. 2021, in press. [CrossRef]
  22. Hansen, M.; Shunk, F.A. Constitution of Binary Alloys, 2nd ed.; McGraw-Hill Book Company: New York, NY, USA, 1969. [Google Scholar]
  23. Wallach, E.; Evetts, J. The development of microstructure in multifilamentary bronze route A15 composites. In Advances in Cryogenic Engineering Materials; Gubser, D.G., Hartwig, K.T., Reed, R.P., Warnes, W.H., Bardos, V.A., Balachandran, B., Eds.; Springer: Berlin/Heidelberg, Germany, 1986; pp. 911–923. [Google Scholar]
  24. Zhong, J.; Chen, W.; Zhang, L. HitDIC: A free-accessible code for high-throughput determination of interdiffusion coefficients in single solution phase. Calphad 2018, 60, 177–190. [Google Scholar] [CrossRef]
  25. Zhong, J.; Zhang, L.; Wu, X.; Chen, L.; Deng, C. A novel computational framework for establishment of atomic mobility database directly from composition profiles and its uncertainty quantification. J. Mater. Sci. Technol. 2020, 48, 163–174. [Google Scholar] [CrossRef]
  26. Zhong, J.; Chen, L.; Zhang, L. Automation of diffusion database development in multicomponent alloys from large number of experimental composition profiles. npj Comput. Mater. 2021, 7, 35–47. [Google Scholar] [CrossRef]
  27. HitDIC: HIgh-Throughput Determination of Interdiffusion Coefficients. Available online: https://hitdic.com/ (accessed on 16 December 2021).
  28. Shi, F. Calculation formula of multi-core Nb3Sn layer thickness. Min. Metall. Eng. 1981, 4, 66–68. [Google Scholar]
  29. Chen, W.; Zhang, L.; Du, Y.; Tang, C.; Huang, B. A pragmatic method to determine the composition-dependent interdiffusivities in ternary systems by using a single diffusion couple. Scr. Mater. 2014, 90–91, 53–56. [Google Scholar] [CrossRef]
  30. Chen, W.; Zhong, J.; Zhang, L. An augmented numerical inverse method for determining the composition-dependent interdiffusivities in alloy systems by using a single diffusion couple. MRS Commun. 2016, 6, 295–300. [Google Scholar] [CrossRef]
  31. Agarwal, S.; Narlikar, A. Ordering of Nb3Sn layer formed in the bronze process-I. Solid State Commun. 1985, 55, 563–566. [Google Scholar] [CrossRef]
  32. Besson, R.; Guyot, S.; Legris, A. Atomic-scale study of diffusion in A15 Nb3Sn. Phys. Rev. B Condens. Matter Mater. Phys. 2007, 75, 1–7. [Google Scholar] [CrossRef]
  33. Ma, S.; Xing, F.; Zhang, L. A novel analytical approach to describe the simultaneous diffusional growth of multilayer stoichiometric compounds in binary reactive diffusion couples. Scr. Mater. 2020, 191, 111–115. [Google Scholar] [CrossRef]
Figure 1. Geometry of Nb/Sn LSDC: (a) Schematic diagram for the assembled Nb/Sn LSDC; (b) top view and (c) side view of Nb/Sn LSDC during the heat treatment. Typical photos of physical sample for the Nb/Sn LSDC after annealing at 1200 °C for 2 h: (d) top view and (e) side view.
Figure 1. Geometry of Nb/Sn LSDC: (a) Schematic diagram for the assembled Nb/Sn LSDC; (b) top view and (c) side view of Nb/Sn LSDC during the heat treatment. Typical photos of physical sample for the Nb/Sn LSDC after annealing at 1200 °C for 2 h: (d) top view and (e) side view.
Materials 15 00113 g001
Figure 2. BSE images of Nb/Sn LSDCs annealed (a) at 1100 °C for 2.33 h, and (b) at 1200 °C for 2 h.
Figure 2. BSE images of Nb/Sn LSDCs annealed (a) at 1100 °C for 2.33 h, and (b) at 1200 °C for 2 h.
Materials 15 00113 g002
Figure 3. (a) EBSD pattern of Nb3Sn phase and (b) its index calibration in Nb/Sn LSDC annealed at 1200 °C for 2 h. The pattern was acquired with the voltage of 20 kV, and the specimen tilting angle was set to 70°.
Figure 3. (a) EBSD pattern of Nb3Sn phase and (b) its index calibration in Nb/Sn LSDC annealed at 1200 °C for 2 h. The pattern was acquired with the voltage of 20 kV, and the specimen tilting angle was set to 70°.
Materials 15 00113 g003
Figure 4. Experimental composition-distance profiles in the Nb/Sn LSDCs annealed (a) at 1100 °C for 2.33 h, (b) at 1200 °C for 2 h, compared with the corresponding model-predicted composition-distance profiles by HitDIC. Note that the caption “Experiment 1, 2 and 3” in the figures denotes the three separate measurements of composition profiles for each annealed Nb/Sn sample.
Figure 4. Experimental composition-distance profiles in the Nb/Sn LSDCs annealed (a) at 1100 °C for 2.33 h, (b) at 1200 °C for 2 h, compared with the corresponding model-predicted composition-distance profiles by HitDIC. Note that the caption “Experiment 1, 2 and 3” in the figures denotes the three separate measurements of composition profiles for each annealed Nb/Sn sample.
Materials 15 00113 g004
Figure 5. Comparison between the experimental composition profiles measured in this study and the Nb-Sn binary phase diagram calculated according to the thermodynamic parameters assessed by Toffolon [19].
Figure 5. Comparison between the experimental composition profiles measured in this study and the Nb-Sn binary phase diagram calculated according to the thermodynamic parameters assessed by Toffolon [19].
Materials 15 00113 g005
Figure 6. (a) Comparison between the presently evaluated interdiffusion coefficients of Nb3Sn at 1100 °C and 1200 °C and the low-temperature data from Wallach [23]; (b) Model-predicted thickness of the Nb3Sn layer as function of annealing time for the Nb/Sn LSDCs, compared with the experimental data in the present work.
Figure 6. (a) Comparison between the presently evaluated interdiffusion coefficients of Nb3Sn at 1100 °C and 1200 °C and the low-temperature data from Wallach [23]; (b) Model-predicted thickness of the Nb3Sn layer as function of annealing time for the Nb/Sn LSDCs, compared with the experimental data in the present work.
Materials 15 00113 g006
Figure 7. (a) BSE image, (b) mapping distribution of Sn, and (c) mapping distribution of Nb of Nb/Sn LSDC annealed at 1200 °C for 2 h.
Figure 7. (a) BSE image, (b) mapping distribution of Sn, and (c) mapping distribution of Nb of Nb/Sn LSDC annealed at 1200 °C for 2 h.
Materials 15 00113 g007
Table 1. Equilibrium compositions for different phases measured from the Nb/Sn LSDCs.
Table 1. Equilibrium compositions for different phases measured from the Nb/Sn LSDCs.
Temperature (°C)Equilibrium PhasesEquilibrium Compositions
(at.% Sn)
Phase 1Phase 2Phase 1Phase 2
1100bccNb3Sn3.1~7.124.6
Nb3Snliquid27.699.4
1200bccNb3Sn5.724.4
Nb3Snliquid27.699.1
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zhang, J.; Zhong, J.; Li, Q.; Zhang, L. Nb/Sn Liquid-Solid Reactive Diffusion Couples and Their Application to Determination of Phase Equilibria and Interdiffusion Coefficients of Nb-Sn Binary System. Materials 2022, 15, 113. https://doi.org/10.3390/ma15010113

AMA Style

Zhang J, Zhong J, Li Q, Zhang L. Nb/Sn Liquid-Solid Reactive Diffusion Couples and Their Application to Determination of Phase Equilibria and Interdiffusion Coefficients of Nb-Sn Binary System. Materials. 2022; 15(1):113. https://doi.org/10.3390/ma15010113

Chicago/Turabian Style

Zhang, Jiali, Jing Zhong, Qin Li, and Lijun Zhang. 2022. "Nb/Sn Liquid-Solid Reactive Diffusion Couples and Their Application to Determination of Phase Equilibria and Interdiffusion Coefficients of Nb-Sn Binary System" Materials 15, no. 1: 113. https://doi.org/10.3390/ma15010113

APA Style

Zhang, J., Zhong, J., Li, Q., & Zhang, L. (2022). Nb/Sn Liquid-Solid Reactive Diffusion Couples and Their Application to Determination of Phase Equilibria and Interdiffusion Coefficients of Nb-Sn Binary System. Materials, 15(1), 113. https://doi.org/10.3390/ma15010113

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop