1. Introduction
The electrochemical capacitor (ECC) is an energy storage device, which is also called supercapacitor or ultracapacitor [
1,
2]. The energy storage devices with a high power and energy density are in high demand for versatile applications, such as industrial equipment, modern electric vehicles, and other small devices [
3,
4,
5]. Basically, supercapacitor can be divided by two types. One is an electric double layer capacitor (EDLC) and the other is a pseudocapacitor. Here, the difference between EDLC and pseudocapacitors is that the former stores energy at the interface between electrolyte and electrode, whereas the latter utilizes additional faradaic reactions at the surface of electrodes in addition to the intrinsic EDLC capacitance [
6,
7,
8].
Numerous studies have focused on creating the most effective electronic gadgets in the smallest possible sizes as a result of the science and technology sector’s ongoing advancement. The interdigital structured micro-supercapacitor is one example. Due to its excellent power density, this tiny supercapacitor is gradually replacing micro-batteries [
9]. Micro-batteries have a limited lifespan and must be replaced frequently, which is a hassle when doing an analysis. Due to their superior charge and discharge rates, as well as their longer life term, micro-supercapacitors are mostly used as energy storage devices in the biomedical industry. Paper supercapacitors are another type of supercapacitor that has been of interest lately. They are thin and flexible since they are constructed from paper-based substrates. These characteristics enable their use on walls or billboards without adding bulk to the space. A high operational voltage can be obtained by connecting them in series [
10]. Due to their high voltage window, asymmetric supercapacitors have also attracted attention [
11,
12], EDLC and pseudo-capacitive cathode types in particular. Metal oxides or conducting polymers like polyaniline or polypyrrole can be used as cathode materials. The EDLC//battery-type hybrid supercapacitor is another type [
13], which uses metal oxides and hydroxides as the cathode materials and carbon materials as an anode.
As an electrode material for supercapacitors, semiconducting and metallic polymers (i.e., -conjugated materials) have been employed. Among these, polypyrrole (PPy) has become the industry standard material for energy storage due to its numerous benefits, including eco-friendliness, low cost, simple handling, and high capacity [
14,
15,
16,
17,
18]. Its pyrrole monomer does, however, have significant downsides, such as a low conductivity of 10
−11–10
−10 S/cm. Prior to doping with halogens like iodine, bromine, and chlorine, PPy functions as an insulator in its natural condition. The conductivity range of un-doped PPy is 10
−6 to 10
−3 S/cm [
19,
20,
21]. Its mechanical performance has various flaws, according to Du et al., and this has a detrimental impact on its electrochemical performance since capacitance degrades [
19]. To make up for these drawbacks, carbon-based compounds like graphene and carbon nanotubes (CNT) were developed as structural fillers. Algae, fungi, viruses, and prokaryotic bacteria are examples of adaptable biomaterials that have been employed as a bio-template to enhance the performance of composite materials [
11]. Because they are among these microorganisms that are not only plentiful but also mass-producible and renewable, bacteria, in particular, are a focus of attention. As a result, these bacteria have been employed as a model for composite electrodes, providing thin sheets with a clearly defined shape. The interlocking pore networks, heteroatom moiety, and a sizable surface area in composite electrodes may all be directly related to the structure of bacteria [
12].
In earlier investigations, Catauro et al. used a sol-gel synthesis process to create antimicrobial biomedical implants. This was accomplished by first embedding various ratios of poly(e-caprolactone) and polyethylene glycol in the silica matrix. Then, substantial quantities of chlorogenic acid were added to each SiO
2/PEG and SiO
2/PCL solution. Cell adhesion and growth were boosted by polyethylene glycol polymer. When
E. coli bacteria were tested for resistance, the materials’ antibacterial activity responded favorably [
22].
The electrochemical behavior of carbon nanohorns/polyaniline (PANI)/PPy composites was examined by Chang et al. [
13,
23], who found that they had outstanding cycling stability after 5000 cycles and a specific capacitance of 762 F∙g
−1 at 5 m∙Vs
−1. For the PPy materials, Jiang et al. employed CNT as a reinforcing component to lessen swelling and shrinkage throughout the doping and dedoping procedures. This CNT/PPy composite has a specific capacitance of 154.5 F∙g
−1, compared to only 25 F∙g
−1 for a single PPy, showing a six-fold difference between the two [
14]. Canobre et al. also investigated CNT/PPy composites, which had a coulombic efficiency of 99.2% and a specific capacitance of 530 F∙g
−1 [
15,
24]. In order to manufacture the PPy/CNT composite on ceramic fabrics, Lee et al. used chemical vapor deposition (CVD) to grow the CNT on the fabrics and then chemical polymerization to coat the surface of the CNT with PPy. This PPy/CNT/ceramic fabric demonstrated a specific capacitance of 152.7 F∙g
−1 at 1 mA/cm
−2 and showed exceptional stability even after 5000 cycles) [
16,
25]. However, there have been no reports of the use of bacteria with PPy/CNT complexes as supercapacitor electrodes.
The creation of a nanostructural composite electrode for use in supercapacitor applications was the study’s main goal. As a bio-template for this, we created active electrodes made of PPy, CNT, and
E. coli (gram-negative bacteria). Here, it was intended to increase the porosity and surface area of the composite electrode because these microstructures are directly related to the electrochemical performance of composite electrodes. It is well known that the heteroatom nitrogen, which is a component of
E. coli bacteria, contributes to the increase in capacitance when the bacteria are present. In a study by Kwang et al., it was found that the bacterium
E. coli improved the electrochemical performance of electrodes in the composite [
1]. As a result, when compared to CNT and PPy/CNT composite electrodes, the PPy/CNT–
E. coli composite electrodes showed better electrochemical performance.
3. Results and Discussion
The chemical species in the electrode materials, CNT, PPy/CNT, and PPy/CNT–
E. coli composite, are represented by FT-IR spectra in
Figure 1. The stretching vibrations of the pyrrole rings, which are associated with two observed peaks at 1537 and 1454 cm
−1, are symmetric and asymmetric, respectively. At roughly 1301 cm
−1, the C-N stretching in the pyrrole rings is visible. While the peaks at 991 cm and 920 cm
−1 are attributed to C-H in-plane and C-H out-of-plane deformation, respectively, the peak at 1160 cm
−1 reflects the C-H stretching vibration of pyrrole rings. The peaks at 1402 (1454) and 964 (960) cm
−1 are attributable to the symmetric stretching vibration of phosphoryl groups and the C-O of carboxylic groups, respectively. Furthermore, the P=O vibration in phosphodiesters of nucleic acids, phosphorylated proteins, and polyphosphate products is connected to the bands at 1225 (1238) and 1085 cm
−1Figure 2 displays the XRD patterns for the following samples: pure CNT (c), PPy/CNT nano-composites (a), and PPy/CNT–
E. coli nano-composites (b).
Figure 2c demonstrates that the pure CNT’s two XRD peaks were found at 25.78° and 42.84°, respectively, which translate into d-spacings of 0.34 and 0.21 nm. Here, the former is associated with the crystallographic plane (002), while the latter is associated with the plane (100). Notably, Braggs’ law is λ = 2
d sin 𝜃, where
d is the interplanar distance, 𝜃 is the diffraction angle, and (λ) is the x-ray wavelength, respectively. On the other hand, it is known that PPy has a large peak at 2 = 20.5° [
26], indicating that this polymer is almost amorphous and has disordered π-π stacking. The (002) peak at 2 = 25.78° is, in fact, significantly widened by the presence of PPy, as seen in
Figure 2b, and the same is true for the PPy/CNT–
E. coli sample in
Figure 2a. Here, it is noteworthy that although the presence of both Ppy and CNT was justified through XRD, it is not possible to identify the presence of
E. coli bacteria because these bacteria are amorphous materials.
This section may be divided by subheadings. It should provide a concise and precise description of the experimental results, their interpretation, as well as the experimental conclusions that can be drawn.
The nitrogen-adsorption isotherm was examined using a BET analyzer to look at the porosity of nano-microstructural PPy/CNT and PPy/CNT–
E. coli samples (
Table 1). Because it can both improve capacitance and make electrolyte ions more mobile, a porous structure with large surface areas is crucial for the supercapacitor electrodes in this case. The pore volume of PPy/CNT–
E. coli is 0.34 cm
3g
−1, PPy/CNT has 0.28 cm
3g
−1, and pure CNT has 0.16 cm
3g
−1, indicating the advantage of the full composite material (PPy/CNT–
E. coli). Here, the inclusion of PPy ought to improve the redox-active sites, allowing for more effective electron transport. The energy density of energy storage devices is directly influenced by the kinetics and electrochemical activity of electrode materials. Therefore, for good electrochemical performances, the diffusion of charged ions across the interface between the electrolyte and electrode should be sufficiently smooth. The PPy/CNT-
E. coli has a surface area of 85.93 m
2g
−1, which enables electro-active species to participate in the Faradaic redox processes. The meso/macro porous structure could be seen in the morphology of the PPy/CNT–
E. coli composite. It is known that this type of microstructure is related to the open space between the nearby PPy/CNT–
E. coli superstructures [
27].
When pyrrole monomers were mixed with CNT dispersion, the monomers adhered easily to the CNT surface and then chemically polymerized. The attractive interactions between CNT and pyrrole molecules, as demonstrated by the SEM images in
Figure 3, may be the cause of this simple adhesion. According to
Figure 3a,b, the diameter of the pure CNT fibers is around 25 nm. However, as shown in
Figure 3c,d, the diameter of the CNT fibers expanded up to around 50 nm after pyrrole was polymerized on their surface, providing unmistakable proof that PPy had grown on the surface of the CNT. This PPy coverage on the CNT seems to be all over the CNT fibers/particles, and eventually, PPy encapsulated them. Interestingly, the
E. coli bacteria template has a tendency to create irregular bumps on the fibril morphologies of the PPy/CNT–
E. coli composite electrode as shown in
Figure 3e,f [
12]. Both intracellular and extracellular membrane features in
E. coli cells are known to have an impact on the final composite electrode. [
28]. When the PPy/CNT–
E. coli composite electrode was made, these
E. coli qualities led to a wide surface area with rich porosity, which was better than the outcome of the PPy/CNT composite alone. We anticipate that these characteristics, along with structural regularity, should result in the expected capacitance output from the PPy/CNT–
E. coli electrodes. These structural characteristics encourage charged ion migration (diffusion and drift) into the majority of accessible areas of the composite electrodes.
Cyclic voltammetry was used to assess the CNT, PPy/CNT, and PPy/CNT–
E. coli at varied scan rates of 5–200 m∙Vs
−1. The conducing PPy coating on the surface of CNT fibers allows a quick diffusion of charged ions, enhancing the performance of the supercapacitor incorporating this composite electrode [
29]. PPy content can be associated with pseudo capacitance contribution because the PPy is able to promote rapid pseudo-Faradaic reactions. The reversible doping/undoping process of anions (D
− = I
−, SO
42-−) in PPy is inferred to be the key driver of the charge storage of PPy.
Comparing the CV voltammograms obtained for CNT and PPy/CNT composite, the PPy/CNT–
E. coli composite showed the highest total charge. These voltammograms show that the pseudo-capacitance is mostly responsible for the electrochemical capacitance of the PPy/CNT-
E. coli. The redox current increases with increasing scan rate, which suggests good reversibility of the fast charge-discharge response. The bacteria
E. coli acts positively as an additional template material to completely use the electroactivity of PPy/CNT. Indeed, the addition of the bacteria in the composite increased the surface area (85.93 m
2∙g
–1) of the PPy/CNT–
E. coli composite when compared with PPy/CNT and CNT.
Figure 4 demonstrates that the capacitance of the PPy/CNT-
E. coli composite electrode originates from both the pseudocapacitance from PPy fibers and the EDLC capacitive behavior from the CNT-
E. coli-based composite electrode [
28]. This finding shows how much better the PPy/CNT–
E. coli composite electrode performs than either PPy/CNT or CNT materials. The heteroatom moiety from the bacteria is introduced due to the presence of
E. coli. The presence of the E-coli introduces the heteroatom moiety from the bacteria. The heteroatoms functionalities have a faradaic nature, which induces pseudocapacitance. On the other hand, the small specific capacitance (37 F∙g
–1) of CNT indicates that the morphology of this CNT electrode is not much optimized, i.e., a very limited surface area and pores.
Figure 5 shows the galvanostatic charge/discharge curves for the CNT, PPy/CNT, and PPy/CNT–
E. coli systems. Galvanostatic charge/discharge curves were used to calculate the electrodes’ precise capacitance values (
Table 2). A high specific capacitance of 173 F∙g
−1 at 0.2 Ag
−1 was displayed by PPy/CNT–
E. coli (
Figure 5d). The specific capacitance of the PPy/CNT and CNT materials was 150 F∙g
−1 and 37 F∙g
−1, respectively, at the same current density (0.2 Ag
−1). The symmetrical properties of the charge/discharge curves show that the composite electrodes made of PPy/CNT–
E. coli have good capacitive performance with reversible redox processes [
17].
The cycle test for the PPy/CNT–
E. coli electrodes is depicted in
Figure 6. The specific capacitance retention below 0.2 Ag
−1 was excellent for the PPy/CNT–
E. coli electrodes. For instance, the PPy/CNT–
E. coli electrodes showed a nearly constant specific capacitance even after 1000 cycles, demonstrating the device is electrochemically stable. Importantly, 1000 charge/discharge cycles showed that PPy/CNT–
E. coli electrodes maintained a 95.95% capacity, demonstrating long-term cycling stability. According to this stability, the PPy fraction of a composite electrode’s volume change did not impact its electrochemical characteristics, resulting in good capacity retention [
30].
4. Conclusions
In this study, the chemical oxidative polymerization approach was used to create the PPy/CNT–
E. coli composite. The resulting PPy/CNT–
E. coli superstructures had a hierarchical structure and were made of phase-pure porous PPy/CNT with a flower-like morphology. In addition to having an astonishingly huge BET surface area (85 m
2∙g
−1), they also have meso-/macroporous characteristics brought on by the open space between the nearby individual PPy/CNT–
E. coli superstructures. These were combined with the mesoporosity present in the nanotubes composed of small nanoparticles. Based on this, the as-prepared materials were used as electrode materials for a supercapacitor. The PPy/CNT–
E. coli redox reactions were made possible by the numerous electro-active sites that these favorable features supplied. These characteristics ensured a sufficient electrochemical utilization of the proposed composite electrode. PPy/CNT–
E. coli composite exhibited higher specific capacitance than some of the previously reported PPy/CNT composites at the same current density, as well as large power density, and good stability after 1000 charge/discharge cycles. An important study that successfully demonstrates how PPy/CNT–
E. coli materials can be used as active materials for supercapacitor electrodes is the measurement of the electrochemical characteristics of PPy/CNT–
E. coli. The electrochemical activity and electrode kinetics have a significant impact on a supercapacitor’s performance. Therefore, it is essential to improve the kinetics of ion and electron transport in the electrodes and at the electrode/electrolyte interface in order to increase the energy density in supercapacitors at high rates. For the Faradaic redox reactions, it is essential to also engage enough electro-active species that are exposed on the surface. The
E. coli bacteria was added to the PPy/CNT composite to improve the overall electrode performance. In comparison to the CNT and the PPy/CNT, the specific capacitance of the PPy/CNT–
E. coli composite electrode was 173 F∙g
−1 at 0.2 A∙g
−1. The PPy/CNT–
E. coli electrode was fully exploited in terms of specific capacitance, as shown by the acquired specific capacitance and the aforementioned features, making it superior to the other samples. The nitrogen species in the
E. coli bacteria, XPS data (
Figure S1) displayed quaternary N(401.1 eV), pyridinic N(398.1 eV), and pyrrolic N(399.4 eV). This gives evidence of the heteroatom contribution from the
E-coli bacteria incorporated in the PPY/CNT-
E coli composite. The foreign atoms in bacteria play a superior role in the electrochemical performance of the supercapacitor electrode through faradaic reactions. Since the use of PPy/CNT–
E. coli composite as supercapacitor electrodes has not yet been published, our preliminary study requires additional research in order to be applied in the future to energy storage devices, such as lithium-ion batteries and supercapacitors.