Twinning Behavior, Microstructure Evolution and Mechanical Property of Random-Orientated ZK60 Mg Alloy Compressed at Room Temperature
Previous Article in Journal
Strength Prediction of Ball-Milling-Modified Phosphorus Building Gypsum Based on NSGM (1,4) Model
Previous Article in Special Issue
Microstructures and Properties of Al-Mg Alloys Manufactured by WAAM-CMT
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Establishment of Constitutive Model and Analysis of Dynamic Recrystallization Kinetics of Mg-Bi-Ca Alloy during Hot Deformation

1
School of Mechanical Engineering, Yangzhou University, Yangzhou 225127, China
2
School of Materials Science and Engineering, Hebei University of Technology, Tianjin 300130, China
3
School of Materials and Energy, Yunnan University, Kunming 650599, China
*
Author to whom correspondence should be addressed.
Materials 2022, 15(22), 7986; https://doi.org/10.3390/ma15227986
Submission received: 10 October 2022 / Revised: 31 October 2022 / Accepted: 1 November 2022 / Published: 11 November 2022

Abstract

:
The flow behavior of the solution-treated Mg-3.2Bi-0.8Ca (BX31, wt.%) alloy was systematically investigated during hot compression at different deformation conditions. In the present study, the strain-related Arrhenius constitutive model and dynamic recrystallization (DRX) kinetic model were established, and the results showed that both two models had high predictability for the flow curves and the DRX behavior during hot compression. In addition, the hot processing maps were also made to confirm a suitable hot working range. Under the assistance of a hot processing map, the extrusion parameters were selected as 573 K and 0.5 mm/s. After extrusion, the as-extruded alloy exhibited a smooth surface, a fine DRX structure with weak off-basal texture and good strength–ductility synergy. The newly developed strong and ductile BX31 alloy will be helpful for enriching low-cost, high-performance wrought Mg alloy series for extensive applications in industries.

1. Introduction

Magnesium and its alloys, as one of the green materials, have shown wide application prospects in transportation, electronics and military industry due to its excellent characteristics, i.e., low density, high specific strength/stiffness, good vibration-reducing performance, etc. [1]. In recent years, Mg alloys have also made new breakthroughs in the field of hydrogen storage [2,3]. However, some bottleneck problems still exist, such as bad corrosion resistance, poor formability and strength–ductility trade of dilemma, to a large extent restricting commercial applications. In the past decade, some researchers have tried their best to overcome the imbalance of strength and ductility using rare-earth (RE) elements [4,5] and severe plastic deformation techniques [6]. Nevertheless, the high cost and the complex processing vastly limit the applications of Mg alloys. Thus, the development of low RE-containing, even RE-free Mg alloys, is an imminent requirement.
Up to now, some new Mg alloys, such as Mg-Sm- [7,8], Mg-Ca- [9,10], Mg-Al- [11], Mg-Sn- [12], Mg-Mn- [13,14] and Mg-Zn-based [15] alloys, have been fabricated successfully to achieve this goal. In order to further enrich the existing low-cost, high-performance Mg alloy systems, Mg-Bi-based series alloys have been exploited in recent years, and they have great potential in developing RE-free materials with outstanding comprehensive mechanical properties. Al, Zn, Ca, Mn and Sn elements have been attempted to add into Mg-Bi-based alloys to ameliorate their mechanical properties [16,17,18,19,20,21,22,23]. Among them, interestingly, wrought Mg-Bi-Ca series alloys exhibit unique mechanical properties, which are dependent on hot deformation parameters. For instance, Meng et al. [17,18,19] pointed out that Ca addition could trigger the texture change in as-extruded Mg-Bi-Ca alloys. As extrusion temperature or die-exit speed increased, an off-basal texture feature formed, inducing a high tensile ductility (~40%) in Mg-1.3Bi-0.9Ca (wt.%) alloy [17,18]. In contrast, under the conditions of a low extrusion temperature of 280 °C and die-exit speed of 4 mm/s, a strong basal texture occurred in Mg-1.5Bi-0.8Ca (wt.%) alloy leading to a high tensile yield strength (~394 MPa) [19]. In order to obtain the strength–ductility synergic Mg-Bi-Ca series alloys, a two-step deformed Mg-1.3Bi-0.7Ca (wt.%) alloy, with a tensile yield strength of ~351 MPa and elongation-to-failure of ~13.2%, was successfully prepared by extrusion and subsequent caliber rolling [20]. In summary, such a new highly strong and ductile RE-free Mg-Bi-Ca alloy will be helpful for enriching low-cost and high-performance wrought Mg alloy series to achieve extensive applications in industries.
However, until now, the flow behavior, constitutive model, dynamic recrystallization (DRX) kinetic model and hot processing map of Mg-Bi-Ca series alloys during hot deformation are rarely reported systematically. It is important to understand the hot flow behavior of Mg-Bi-Ca series alloys to obtain the desired microstructure and to achieve excellent mechanical properties. The Arrhenius-type constitutive model is commonly used to describe the hot flow behavior, predicting the hot-deformed microstructure and optimizing the hot processing parameters of Mg alloys [24,25]. In Mg alloys, the chemical composition is a key factor in influencing the DRX kinetic. When the added alloying elements are soluble in a substrate, non-basal slip may be activated easily during hot deformation since these elements (i.e., RE, Ca and Li) obviously change the stacking fault energy for non-basal slip reducing the ratio of critical resolved shear stresses, (CRSSs) between non-basal and basal slips [26,27,28]. Within grains, the activation of massive slip systems accelerates the dislocation rearrangement to form low-angle grain boundaries (LAGBs), which provide a precursor for the generation of large-angle grain boundaries (HAGBs). For example, Li et al. [29] pointed out that Ce addition into AZ80 alloy presented a lower activation energy than that in without Ce. In addition to non-basal slip, contraction twinning and/or double twinning also could occur in the early stage of hot deformation in Y-containing Mg-Sn-Zn alloy, as reported by Wang et al. [30]. These twins offer the DRX nucleation sites, also promoting the DRX process. On the other hand, as alloying elements are presented as compounds, two cases exist. In general, large-sized phases (>1 μm) play a role in increasing the DRX nucleation sites, known as particles stimulate nucleation (PSN). While the phase size is below 1 μm, they tend to delay the motion of grain boundaries inhibiting the DRX process. However, on the DRX mechanism of Mg-Bi-Ca series alloys, it is still unknown.
Therefore, in order to investigate the hot deformation behavior of Mg-Bi-Ca series alloys, in this work, taking a new RE-free Mg-Bi-Ca alloy as an example, hot compressive tests were performed at different conditions. The Arrhenius constitutive model and the DRX kinetics of this alloy were established. Based on the data of hot compressive flow curves, the suitable hot processing range was measured. Finally, the extrusion parameter was selected to gain the fine complete DRX structure with weak off-texture and obtain the strength–ductility balance in an as-extruded Mg-Bi-Ca alloy.

2. Materials and Methods

Commercial pure Mg ingot (≥99.99%), Mg-10Bi (wt.%) and Mg-25Ca (wt.%) master alloys were melted at 720 °C in an electric resistance furnace (Shanghai Yuzhi Technology Co., Ltd, China) under a protective atmosphere (SF6:CO2 = 1:99). After a series of sitting and slagging, the melt was poured into a steel mold with Φ 80 (in diameter) × 200 (in height) mm preheated to 350 °C. The chemical composition of the as-cast alloy was detected by an X-ray fluorescence spectrometer (XRF, LAB CENTER XRF-1800) (Shimadzu, Kyoto, Japan), and the real chemical composition is 96.0 wt.% Mg, 3.2 wt.% Bi, and 0.8 wt.% Ca. It can be labeled as BX31. Before hot compression, the solid solution of the as-cast BX31 alloy was treated at 773 K for 24 h. Subsequently, hot compression tests for samples with a size of Φ 8 × 12 mm (diameter × height) were operated on a Gleeble-3500 thermo-mechanical simulator (DSI North America Corp, Marlton, Evesham, United States) at different conditions (temperatures: 573, 623 and 673 K; strain rates: 0.01, 0.1 and 1 s−1). In addition, the solution-treated BX31 alloy was also extruded into the bar with Φ 22 mm in diameter at 573 K using an extrusion ratio of 21:1 and a die-exit speed of 0.5 mm/s by XJ-500 horizontal extruder (WuxiYuanchang Machine Manufacture Co., Wuxi, China). The room-temperature (RT) tensile properties of the as-extruded sample with 25 mm in gauge length and Φ 5 mm in gauge diameter were machined from the as-extruded bar along extrusion direction (ED) and measured using CMT6305-300 kN universal tensile testing machine (MTS Systems Co Ltd, Shanghai, China) at a strain rate of 1 × 10−3 s−1.
The microstructure could be observed by scanning electron microscopy (SEM, Gemini SEM 300) (Carl Zeiss, Oberkochen, Germany) equipped with an energy dispersive spectrometer (EDS) (Carl Zeiss, Oberkochen, Germany) and electron backscattered diffraction (EBSD, JEOL JSM-7800F) device (Japan Electronics Corporation, Tokyo, Japan). The phase constitutions were identified by X-ray diffraction (XRD, Rigaku D/Max 2500) (Bruker AXS, Karlsruhe, Germany). The preparation of EBSD samples was composed of grinding, washing, blow-drying and electro-polishing at 20 V and 0.03 A for 90 s at 298 K using AC2. The scanning step size was set as 0.5 μm. All EBSD data were analyzed using ATEX software v2.01.3 (ATEX, Metz, France).

3. Results and Discussion

3.1. Microstructure of the Solution-Treated BX31 Alloy

Figure 1a shows the SEM image of the solution-treated BX31 alloy with a few bright granular-shaped second phases. The average phase size is about 5 μm. Based on the SEM-EDS mapping scanning results, as shown in Figure 1b–d, these granular-shaped phases mainly consist of Mg, Bi and Ca elements possibly deemed as Mg-Bi-Ca ternary phases. Moreover, by combining the SEM-EDS point scanning result from phase 1 marked by the red arrow in Figure 1a, these ternary phases can be regarded as Mg2Bi2Ca ones, as displayed in Figure 1e. The reports of Remennik et al. [31], Meng et al. [17,18,19,20] and Liu et al. [32] are consistent with this result. In addition, Mg3Bi2 phases, even Mg2Ca ones, also could be found in wrought Mg-Bi-Ca series alloys [17,18,19,20]. However, the mentioned these two kinds of phases are almost undetectable in the solution-treated BX31 alloy. We argue that these dynamically precipitated fine Mg3Bi2 and Mg2Ca particles are the products of a combined effect from deformation force and temperature. On the other hand, the thermal stability of Mg2Bi2Ca phases is superior to Mg3Bi2 and Mg2Ca ones, based on the thermodynamics of phase formation [32]. Therefore, in this work, the main phase constitution in the solution-treated BX31 alloy is Mg2Bi2Ca. In order to further verify this statement, an XRD test was carried out, and the result is shown in Figure 2. We can see that two kinds of characteristic diffraction peaks of phases exist: α-Mg and Mg2Bi2Ca, which is in accordance with the SEM observation.

3.2. Flow Behavior during Hot Compression

Figure 3 shows the compressive flow curves of the solution-treated BX31 alloy at different deformation conditions. We can see the flow curves contain three stages: (1) Rapid ascent stage. Dislocations accumulate sharply, giving rise to remarkable work hardening; (2) Slow descent stage. The flow stress reaches the peak as the strain increases, and subsequently, dislocations annihilate, giving rise to the decline of the flow stress. This is mainly attributed to the DRX triggering the dynamic softening [24,25,33]; (3) Steady-state flow stage. In this stage, the work hardening and the dynamic softening reach a balance, thereby making the flow stress tend to accord. Figure 4 shows the peak stresses and the corresponding peak strains at different deformation conditions. There exists an obvious tendency for the peak stress increment by decreasing the temperature and increasing the strain rate (see Figure 4a), but the peak strain tends to be decreased (see Figure 4b). This phenomenon is closely associated with the acceleration of the DRX process.

3.3. Constitutive Model during Hot Compression

The Arrhenius constitutive models are given [34]:
ε ˙ = A 1 σ n 1 e x p ( Q R T )
ε ˙ = A 2 e x p ( β σ ) e x p ( Q R T )
ε ˙ = A [ s i n h ( α σ ) ] n e x p ( Q R T )
where ε ˙ is the strain rate; σ is the flow stress; T is the temperature; A 1 , n 1 , A 2 , β, A, α and n are material constants; Q is the activation energy; and R is the mole gas constant (8.314 J/mol K). The n 1 , β and α can be described as follows [35]:
α = β n 1
Zener–Hollomon (Z) parameter is introduced to construct the relationship among the Z, ε ˙ and T. It can be shown as follows [36]:
Z = ε ˙ e x p ( Q R T )
For Equation (3) with Equation (5) together, the σ as a function of the Z is expressed as follows [37]:
σ = 1 α l n { ( Z A ) 1 n + [ ( Z A ) 2 n + 1 ] 1 2 }
Under the peak stress condition, these material constants of α , Q, n and A are calculated by Equations (7)–(11).
Both sides of Equations (1) and (2) are taken natural logarithms as follows:
l n ε ˙ = n 1 l n σ + l n A 1 Q R T
l n ε ˙ = β σ + l n A 2 Q R T
Figure 5a,b show the linear relationships of l n ε   ˙   l n σ and l n ε   ˙   σ , respectively. The slopes of these two functions are considered the average n 1 and β values (~7.317 and ~0.089, respectively). According to Equation (4), the α is estimated by ~0.012.
Both sides of Equation (3) are taken natural logarithms as follows:
l n ε ˙ = n l n [ s i n   h ( α σ ) ] + l n A Q R T
Figure 5c plots the functional relation between l n ε ˙ and l n [ s i n h ( α σ ) ] , and the slope can be regarded as the average n value (~5.390).
Both sides of Equation (9) are taken partial derivatives as follows:
Q = R ( l n ε ˙ l n [ s i n   h ( α σ ) ] | T ) ( l n [ sin   h ( α σ ) ] ( 1 / T ) | ε ˙ ) = R n S
Figure 5d shows the functional relation of l n [ s i n   h ( α σ ) ] 1 / T , and the average S value is the slope of this linear relationship, ~3.390. Therefore, the Q value at the peak stress condition is about 151.9 kJ/mol, slightly larger than that of pure Mg (~135 kJ/mol [38]). Fine precipitates could effectively inhibit dislocation movement during deformation, which led to an increase in the activation energy during deformation [39]. According to the reports from the literature [17,18,19,20], fine Mg3Bi2 and Mg2Ca particles may be dynamically precipitated from the Mg matrix in Mg-Bi-Ca series alloys, and a part of them was found to distribute at grain boundaries. Such a grain boundary pinning effect further enhances the resistance of grain boundary motion, giving rise to the increment of the activation energy during hot compression. In addition, recently, the Q value has been successfully related to the atomistic mechanisms for different engineering materials. Savaedi et al. [40] pointed out that the average Q value was close to the weighted self-diffusion activation energy for each element in CoCrFeMnNi alloy. Relevant research was also presented in the report of Jeong et al. [41]. This kind of analysis, considering the atomistic mechanisms, needs more attention in future work.
Combining Equation (3) with Equation (5), the following relationship is shown:
l n Z = n l n [ s i n   h ( α σ ) ] + l n A
The values of Z can be calculated at different deformation conditions by taking into the Q value. Figure 5e matches the linear function of l n Z     l n [ s i n   h ( α σ ) ] , and the lnA is ~26.430 as the intercept of this function. As mentioned above, the Arrhenius constitutive model at the peak stress condition can be established as follows:
ε ˙ = 3.008 × 10 11 [ s i n   h ( 0.012 σ ) ] 5.390 e x p ( 1.827 × 10 4 T )
Under the case of the strain-related Arrhenius constitutive model, the material constants of α , Q, n and A are closely associated with the strain. By using 6-order polynomial equations expresses their relations as follows:
α ( ε ) = α 6 ε 6 + α 5 ε 5 + α 4 ε 4 + α 3 ε 3 + α 2 ε 2 + α 1 ε + α 0
Q ( ε ) = Q 6 ε 6 + Q 5 ε 5 + Q 4 ε 4 + Q 3 ε 3 + Q 2 ε 2 + Q 1 ε + Q 0
n ( ε ) = n 6 ε 6 + n 5 ε 5 + n 4 ε 4 + n 3 ε 3 + n 2 ε 2 + n 1 ε + n 0
A ( ε ) = e x p [ l n A ( ε ) ] = e x p ( A 6 ε 6 + A 5 ε 5 + A 4 ε 4 + A 3 ε 3 + A 2 ε 2 + A 1 ε + A 0 )
where ε is the strain. The coefficients α 0 α 6 ,   Q 0 Q 6 ,   n 0 n 6 and l n A 0 l n A 6 are listed in Table 1. Figure 6 shows these material parameters as functions of the strain. Based on the strain-related Arrhenius constitutive model, the predicted flow stress values at different strains for each deformation condition can be calculated, and Figure 7 compares the experiment flow stresses and the predicted values at different deformation conditions. It can be seen that the strain-related Arrhenius constitutive model is suitable for the flow curves of the solution-treated BX31 alloy during hot compression. The predictability of this model can be evaluated by the correlation coefficient (R) and the average absolute relative error (AARE), and the relative error (δ) as follows [37,42]:
R = i = 1 n ( E I E ¯ ) ( P i P ¯ ) i = 1 n ( E i E ¯ ) 2 i = 1 n ( P i P ¯ ) 2
A A R E ( % ) = 1 n i = 1 n | E i P i E i | × 100 %
δ ( % ) = ( E i P i E i ) × 100 %
where n is the size of flow stress set. E i and P i are the values of experiment flow stress and predicted one, respectively. E ¯ and P ¯ are the mean values of E i and P i , respectively. The calculated result shows the R is ~0.9919 and the AARE is ~4.28%, as shown in Figure 8a. Additionally, the δ is deviated at a low range of ~−1.147%, as shown in Figure 8b. It further suggests that this model works well.

3.4. DRX Kinetics during Hot Compression

In order to describe the DRX kinetics model, in general, the following equation can be used and expressed [43,44]:
X D R X = 1 e x p [ k D ( ε ε c ε 0.5 ) n D ]
where X D R X is the DRX area fraction, ε c is the DRX critical strain, ε 0.5 is the strain for the formation of 50% DRX, k D and n D are the material constants. ε c and ε 0.5 can be as a function of the Z parameter given as follows [44]:
ε c = B 1 Z m 1
ε 0.5 = B 2 Z m 2
where B 1 , B 2 , m 1 and m 2 are material constants. The corresponding ε c and ε 0.5 values are obtained by calculating the σ c and σ 0.5 ones that represent the stress values, and the corresponding initial DRX and 50% DRX occur, respectively. According to the θ-σ relationship (θ represents the work hardening rate), the σ c can be gained. By taking a special case (573 K and 0.01 s−1) as an example in Figure 9a, the key flow stresses, i.e., σ c , peak stress ( σ p ), saturated stress ( σ s a t ) and steady stress ( σ s s ), can be measured. In addition, the σ 0.5 can be calculated as follows [44]:
X D R X ( 50 % ) = σ p σ 0.5 σ p σ s s
According to the calculation o θ-σ curve and Equation (23), Table 2 lists the σ c , σ 0.5 , ε c and ε 0.5 values at different deformation conditions. Figure 9b,c match the linear functions from l n ε c   l n Z and, l n ε 0.5   l n Z respectively. Finally, the ε c and ε 0.5 can be expressed:
ε c = 0.0116 Z 0.0823
ε 0.5 = 0.0073 Z 0.1067
Figure 9d shows the linear relationship between l n ( l n ( 1 σ p σ σ p σ s s ) ) and l n ( ε ε c ε 0.5 ) at different deformation conditions, and the average k D (~0.015) and n D (~3.781) can be determined by the intercept and slope of this function, respectively. Therefore, the DRX kinetics model of the solution-treated BX31 alloy can be expressed as follows:
X D R X = 1 e x p [ 0.015 ( ε 0.0116 Z 0.0823 0.0073 Z 0.1067 ) 3.781 ]
Figure 10 shows the X D R X as a function of the ε at different deformation conditions. As for each curve, as it increased the ε, the X D R X gradually increases along an S shape. At the same temperature, the X D R X descends with the strain rate. At a low strain rate of 0.01 s−1, the X D R X can reach 100% at each temperature when the ε is up to 0.7. As the strain rate enlarges, low temperature obviously declines the DRX degree, especially for the deformation condition of 573 K and 1 s−1 (only ~40% at the 0.7 strain).
In order to verify the accuracy of the DRX kinetics model, the hot compressive samples at 623 K and 0.01 s−1 are selected to observe the DRX area fractions at different strains of 0.3 and 0.5. The result is demonstrated in Figure 11. At 0.3 strain, the DRX and the deformed regions obviously exist (see Figure 11a), and the DRX area fraction is about 36%, as shown in Figure 11c. As the strain increases to 0.5, the DRX region gradually occupies the deformed one (see Figure 11b), and at this moment, the DRX area fraction can reach about 89% shown in Figure 11d. These experiment values are almost accordant with the predicted ones (~30 and ~92%, respectively) using the DRX kinetics model. Therefore, we believe the DRX behavior of the solution-treated BX31 alloy can be forecasted by the DRX kinetics model during hot compression.
Furthermore, we also observed that the DRX nucleation preferentially appears at the original grain boundaries. At a high temperature, the CRSSs of non-basal slips may decline, likely activating the non-basal slips within grains that easily induce the obvious orientation gradient. It is also a type of important DRX mechanism (known as continuous DRX) to promote the formation of the DRXed grains, together with the discontinuous DRX mechanisms (i.e., twinning nucleation, PSN, etc.). As the strain increases, the DRXed grains grow, and its average grain size gradually increases from ~10.6 to 13.9 μm, as seen in Figure 11e,f. Generally, the DRX process plays a key role in refining the grains and weakening the basal texture [43,45]. The DRX area shows a lower basal pole intensity than the whole one in the (0001) pole figures for the 0.3 and 0.5 strains (see Figure 11g,h). Interestingly, the subsequent grain growth induces a weaker basal texture. The related literature has stated that the solute segregation (i.e., Ca) into the boundaries of the basal-oriented grains promoted the preferred growth of the non-basal-oriented ones, which might be a crucial factor in weakening the basal texture [33,46].

3.5. Hot Processing Map during Hot Compression

A dynamic material model is valid to describe the hot processing map. In this model, an equation is given [47]:
P = G + J = σ ε ˙ = 0 ε ˙ σ d ε ˙ + 0 σ ε ˙ d σ
where P, G and J represent the power dissipated by the workpiece, plastic deformation and microstructural evolution, respectively. The σ as a function of the ε ˙ is given [48]:
σ = K ε ˙ m
where K and m are a material constant and the strain rate sensitivity coefficient, respectively. Together Equation (27) with Equation (28), J is expressed as follows:
J = σ ε ˙ 0 ε ˙ K ε ˙ m = m m + 1 σ ε ˙
The efficiency of power dissipation ( η ) is described as follows [35]:
η = J J m a x = m σ ε ˙ / ( m + 1 ) σ ε ˙ / 2 = 2 m m + 1
Based on the extreme principle, the instability criterion is proposed as follows [27]:
ξ ( ε ˙ ) = l n ( m m + 1 ) l n ε ˙ + m < 0
Figure 12 shows the hot processing maps at the 0.3, 0.5 and 0.7 strains. Note that the shaded regions represent the flow instability ones. At 0.3 strain, the flow instability region locates at 573~590 K and 0.1~1 s−1, as shown in the top left corner of Figure 12a. When the strain is up to 0.5, two flow instability regions exist. As for the first region, the temperature and strain rate expand to ~630 K and ~0.5 s−1 (shown in the top left corner of Figure 12b), and the new-formed second one is between 650~673 K and 0.2~0.6 s−1 (seen in the bottom right corner of Figure 12b). As the strain increases to 0.7, the flow instability area at the top left corner almost never changes, while the second one at the bottom right corner gradually enlarges to 630~673 K and 0.2~0.7 s−1 in Figure 12c. Based on the stress–strain curves in Figure 3, the solution-treated BX31 alloy lies in a steady-state flow stage after the 0.7 strain, and thus an appropriate hot processing range can be made up by using the result of Figure 12c.

3.6. Analysis of the as-Extruded BX31 Alloy

According to the hot processing range, we can select a suitable extrusion parameter. It has been widely reported that reducing the extrusion temperature or die-exit speed could effectively obtain fine grains to improve the mechanical properties of Mg alloys [15,21,49]. Therefore, 573 K and 0.1 s−1 are selected as the deformation parameters within the range for hot processing to perform the extrusion process. The average strain rate ( ε ˙ ¯ ) is a function of die-exit speed ( V R ) at a given extrusion ratio ( E R ), billet diameter ( D B ) and extrudate diameter ( D E ) as follows: [50]:
ε ˙ ¯ = 6 D B 2 V R l n E R D B 3 D E 3
In this work, E R , D B and D E were set as 21:1, 85 and 22 mm, respectively. Thus, the corresponding extrusion parameters contain the extrusion temperature of 573 K and the die-exit speed of 0.5 mm/s.
The solution-treated BX31 alloy is perfectly extruded into a bar at a given deformation condition. Figure 13a shows the macroscopic morphology of the as-extruded BX31 alloy. It can be seen that its surface is very smooth by the observation of high magnification. Obviously, the selected extrusion condition is fitted for the forming of the solution-treated BX31 alloy. Furthermore, the grain structure and micro-texture feature of the as-extruded BX31 alloy are measured, as shown in Figure 13b–d. According to the EBSD result from the longitudinal section, the as-extruded BX31 alloy exhibits a relatively homogeneous and complete DRX characteristic, and its average grain size is ~4.56 μm. In terms of micro-texture, a typical RE texture orientation of [2-1-11]//ED is found on the inverse pole figure, accompanied by the maximum pole intensity of ~2.39. Such a texture was also obtained in other wrought Ca-containing Mg alloys [17,18,51,52]. Ca is considered a special element, such as RE ones, being added into Mg alloys to change the stacking fault energies of non-basal slips, thereby to some extent promoting the activation of non-basal dislocations during extrusion. This may be a crucial factor for a typical RE texture formation in the as-extruded BX31 alloy. The detailed DRX mechanism for this alloy during extrusion can be revealed in future work.
Additionally, the SEM analysis of the as-extruded BX31 alloy is shown in Figure 14. There exist some granular-shaped phases distributed along ED, and their average sizes are ~2 μm (see Figure 14a,b). Based on the SEM-EDS mapping scanning results shown in Figure 14c–e, these phases mainly also consist of Mg, Bi and Ca elements. Combined with the SEM-EDS point scanning result from phase 1 marked by red arrow in Figure 14b, these phases also can be considered as Mg2Bi2Ca ternary phases. It indicates that they belong to the broken remains from the second phase in the solution-treated BX31 alloy after extrusion. These fine second phases accelerate the DRX nucleation, known as the PSN effect.
Figure 15a shows the RT tensile engineering stress–strain curve and the corresponding tensile data of the as-extruded BX31 alloy. It exhibits a relatively high yield strength of ~192 MPa, excellent ultimate strength of ~230 MPa and the desired elongation-to-failure of ~22%. Figure 15b plots the relationship between the yield strength and the elongation-to-failure for this work and the reported other Mg-Bi-Ca series alloys [17,18,19,20]. They are divided into three groups: (1) high strength but low ductility, (2) strength–ductility synergy and (3) high ductility but low strength. Obviously, the reported other Mg-Bi-Ca series alloys have a strength–ductility trade-off dilemma. In comparison, the as-extruded BX31 alloy provides a good balance. Such excellent mechanical performance is mainly attributed to three aspects: (1) Fine grain size. According to the Hall–Petch law [15,21,49], fine grains can offer a considerable number of grain boundaries, effectively hindering the dislocation motions, thereby enhancing the strength of this alloy; (2) Homogeneous complete DRX structure. On the one hand, the high homogeneity of microstructure to some extent reduces the degree of stress concentration, and on the other hand, the low residual dislocation density is beneficial for uniform plastic deformation; (3) The formation of off-basal texture. Generally, weakening basal texture benefits the improvement of the ductility in Mg alloys [17,18,52,53]. In this work, the off-basal orientation of [2-1-11]//ED in the as-extruded BX31 alloy induces a high Schmid factor for basal slip (~0.37 from the calculation of EBSD data) during tension. The activation of more basal slips accommodates the larger strains, which is a key factor in increasing the work-hardening capacity and the ductility of this alloy.

4. Conclusions

In this work, the hot deformation behavior of the solution-treated BX31 alloy was systematically studied. The strain-related Arrhenius constitutive model presented a high predictability for the flow curves during hot compression. The flow curves followed the DRX-dominated softening mechanism. The DRX nucleation preferentially appears at the original grain boundaries, and subsequently, non-basal slips might be activated to promote the continuous DRX at a high deformation temperature. For a given deformation condition, the DRX benefited from the texture weakening, and interestingly, with increasing the strain, the DRX growth further reduced the basal texture intensity. This result might be attributed to the preferred growth of non-basal-oriented grains due to the solute segregation. According to the hot processing map, a suitable extrusion parameter could be selected, and the as-extruded BX31 alloy showed a balance of strength and ductility. Such good comprehensive tensile properties were mainly attributed to the following three aspects: (i) fine grain size, (ii) homogeneous complete DRX structure and (iii) the formation of off-basal texture. The newly developed strong and ductile BX31 alloy will be helpful for enriching low-cost, high-performance wrought Mg alloy series for extensive applications in industries.

Author Contributions

Conceptualization, Q.W. and L.W.; methodology, Q.W., L.W. and H.Z.; software, H.Z. and Y.C.; validation, Q.W. and L.W.; formal analysis, Q.W., L.W. and H.Z.; investigation, L.W., H.Z., Y.C. and S.C.; resources, Q.W.; data curation, L.W. and H.Z.; writing—original draft preparation, Q.W.; writing—review and editing, L.W., H.Z., Y.C. and S.C.; visualization, Q.W.; supervision, Q.W.; project administration, Q.W.; funding acquisition, Q.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China (No. 52204407), Natural Science Foundation of Jiangsu Province (No. BK20220595), the Postgraduate Research & Practice Innovation Program of Jiangsu Province (No. SJCX22_1720), and the Innovative Science and Technology Platform Project of Cooperation between Yangzhou City and Yangzhou University, China (No. YZ2020266). The APC was funded by the National Natural Science Foundation of China (No. 52204407).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data available on request.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Jiang, B.; Dong, Z.; Zhang, A.; Song, J.; Pan, F. Recent advances in micro-alloyed wrought magnesium alloys: Theory and design. Trans. Nonferrous Met. Soc. China 2022, 32, 1741–1780. [Google Scholar] [CrossRef]
  2. Feng, X.Y.; Jiang, L.J.; Li, Z.N.; Wang, S.M.; Ye, J.H.; Wu, Y.F.; Yuan, B.L. Boosting the hydrogenation activity of dibenzyltoluene catalyzed by Mg-based metal hydrides. Int. J. Hydrogen Energy 2022, 47, 23994–24003. [Google Scholar] [CrossRef]
  3. Pluengphon, P.; Tsuppayakorn-aek, P.; Tubtimtae, A.; Inceesungvorn, B.; Bovornratanaraks, T. Lightweight alkali-induced lattice-dynamical stability and energy storage mechanism of quaternary Mg-based hydrides under pressure effect. Int. J. Hydrogen Energy 2022, 47, 30592–30601. [Google Scholar] [CrossRef]
  4. Tong, L.B.; Chu, J.H.; Sun, W.T.; Xu, C.; Zou, D.N.; Wang, K.S.; Kamado, S.; Zheng, M.Y. Achieving an ultra-high strength and moderate ductility in Mg–Gd–Y–Zn–Zr alloy via a decreased-temperature multi-directional forging. Mater. Charact. 2021, 171, 110804. [Google Scholar] [CrossRef]
  5. Zhang, D.; Yang, Q.; Li, B.; Guan, K.; Wang, N.; Jiang, B.; Sun, C.; Zhang, D.; Li, X.; Cao, Z.; et al. Improvement on both strength and ductility of Mg−Sm−Zn−Zr casting alloy via Yb addition. J. Alloys Compd. 2019, 805, 811–821. [Google Scholar] [CrossRef]
  6. Rakshith, M.; Seenuvasaperumal, P. Review on the effect of different processing techniques on the microstructure and mechanical behaviour of AZ31 Magnesium alloy. J. Magnes. Alloy. 2021, 9, 1692–1714. [Google Scholar] [CrossRef]
  7. Zhang, Z.; Zhang, J.; Xie, J.; Liu, S.; He, Y.; Guan, K.; Wu, R. Developing a low-alloyed fine-grained Mg alloy with high strength-ductility based on dislocation evolution and grain boundary segregation. Scr. Mater. 2022, 209, 114414. [Google Scholar] [CrossRef]
  8. Zhang, D.; Pan, H.; Li, J.; Xie, D.; Zhang, D.; Che, C.; Meng, J.; Qin, G. Fabrication of exceptionally high-strength Mg-4Sm-0.6Zn-0.4Zr alloy via low-temperature extrusion. Mater. Sci. Eng. A 2022, 833, 142565. [Google Scholar] [CrossRef]
  9. Pan, H.; Kang, R.; Li, J.; Xie, H.; Zeng, Z.; Huang, Q.; Yang, C.; Ren, Y.; Qin, G. Mechanistic investigation of a low-alloy Mg–Ca-based extrusion alloy with high strength–ductility synergy. Acta Mater. 2020, 186, 278–290. [Google Scholar] [CrossRef]
  10. Xie, D.; Pan, H.; Li, M.; Li, J.; Ren, Y.; Huang, Q.; Yang, C.; Ma, L.; Qin, G. Role of Al addition in modifying microstructure and me-chanical properties of Mg-1.0 wt% Ca based alloys. Mater Charact. 2020, 169, 110608. [Google Scholar] [CrossRef]
  11. Zeng, Z.R.; Zhu, Y.M.; Nie, J.F.; Xu, S.W.; Davies, C.H.J.; Birbilis, N. Effects of Calcium on Strength and Microstructural Evolution of Extruded Alloys Based on Mg-3Al-1Zn-0.3Mn. Metall. Mater. Trans. A 2019, 50, 4344–4363. [Google Scholar] [CrossRef]
  12. Zhang, A.; Kang, R.; Wu, L.; Pan, H.; Xie, H.; Huang, Q.; Liu, Y.; Ai, Z.; Ma, L.; Ren, Y.; et al. A new rare-earth-free Mg-Sn-Ca-Mn wrought alloy with ultra-high strength and good ductility. Mater. Sci. Eng. A 2019, 754, 269–274. [Google Scholar] [CrossRef]
  13. Peng, P.; Tang, A.; Wang, B.; Zhou, S.; She, J.; Zhang, J.; Pan, F. Achieving superior combination of yield strength and ductility in Mg–Mn–Al alloys via ultrafine grain structure. J. Mater. Res. Technol. 2021, 15, 1252–1265. [Google Scholar] [CrossRef]
  14. Shao, L.; Zhang, C.; Li, C.; Tang, A.; Liu, J.; Yu, Z.; Pan, F. Mechanistic study of Mg-Mn-Al extrusion alloy with superior ductility and high strength. Mater. Charact. 2022, 183, 111651. [Google Scholar] [CrossRef]
  15. Wang, H.; Zhang, D.T.; Qiu, C.; Zhang, W.W.; Chen, D.L. Achieving superior mechanical properties in a low-alloyed magnesium alloy via low-temperature extrusion. Mater. Sci. Eng. A 2022, 851, 143611. [Google Scholar] [CrossRef]
  16. Meng, S.; Xiao, H.; Luo, Z.; Zhang, M.; Jiang, R.; Cheng, X.; Yu, H. Anew extruded Mg-6Bi-3Al-1Zn alloy with excellent tensile properties. Metals 2022, 12, 1159. [Google Scholar] [CrossRef]
  17. Meng, S.; Yu, H.; Fan, S.; Kim, Y.; Park, S.; Zhao, W.; You, B.; Shin, K. Ahigh-ductility extruded Mg-Bi-Ca alloy. Mater. Lett. 2020, 261, 127066. [Google Scholar] [CrossRef]
  18. Meng, S.; Yu, H.; Li, L.; Qin, J.; Woo, S.K.; Go, Y.; Kim, Y.M.; Park, S.H.; Zhao, W.; Yin, F.; et al. Effects of Ca addition on the microstructures and mechanical properties of as-extruded Mg–Bi alloys. J. Alloys Compd. 2020, 834, 155216. [Google Scholar] [CrossRef]
  19. Meng, S.; Zhang, M.; Xiao, H.; Luo, Z.; Yu, W.; Jiang, R.; Cheng, X.; Wang, L. A superior high-strength dilute Mg-Bi-Ca extrusion alloy with a bimodal microstructure. Metals 2022, 12, 1162. [Google Scholar] [CrossRef]
  20. Meng, S.; Yu, H.; Han, H.; Feng, J.; Huang, L.; Dong, L.; Nan, X.; Li, Z.; Park, S.H.; Zhao, W. Effect of multi-pass caliber rolling on dilute extruded Mg-Bi-Ca alloy. Metals 2020, 10, 332. [Google Scholar] [CrossRef] [Green Version]
  21. Wang, Q.; Zhai, H.; Liu, L.; Xia, H.; Jiang, B.; Zhao, J.; Chen, D.; Pan, F. Novel Mg-Bi-Mn wrought alloys: The effects of extrusion temperature and Mn addition on their microstructures and mechanical properties. J. Magnes. Alloy. 2022, 10, 2588–2606. [Google Scholar] [CrossRef]
  22. Wang, Q.; Zhai, H.; Liu, L.; Jin, Z.; Zhao, L.; He, J.; Jiang, B. Exploiting an as-extruded fine-grained Mg-Bi-Mn alloy with strength-ductility synergy via dilute Zn addition. J. Alloys Compd. 2022, 924, 166337. [Google Scholar] [CrossRef]
  23. Luo, Y.h.; Cheng, W.l.; Li, H.; Yu, H.; Wang, H.X.; Niu, X.F.; Wang, L.F.; You, Z.Y.; Hou, H. Achieving high strength-ductility synergy in a novel Mg–Bi–Sn–Mn alloy with bimodal microstructure by hot extrusion. Mater. Sci. Eng. A 2022, 834, 142623. [Google Scholar] [CrossRef]
  24. Hao, J.; Zhang, J.; Xu, C.; Nie, K. Optimum parameters and kinetic analysis for hot working of a solution-treated Mg-Zn-Y-Mn magnesium alloy. J. Alloys Compd. 2018, 754, 283–296. [Google Scholar] [CrossRef]
  25. Wang, C.; Liu, Y.; Lin, T.; Luo, T.; Zhao, Y.; Hou, H.; Yang, Y. Hot compression deformation behavior of Mg-5Zn-3.5Sn-1Mn-0.5Ca-0.5Cu alloy. Mater. Charact. 2019, 157, 109896. [Google Scholar] [CrossRef]
  26. Sabat, R.K.; Brahme, A.P.; Mishra, R.K.; Inal, K.; Suwas, S. Ductility enhancement in Mg-0.2%Ce alloys. Acta Mater. 2018, 161, 246–257. [Google Scholar] [CrossRef]
  27. Zhu, G.M.; Wang, L.Y.; Zhou, H.; Wang, J.H.; Shen, Y.; Tu, P.; Zhu, H.; Liu, W.; Jin, P.P.; Zeng, X.Q. Improving ductility of a Mg alloy via non-basal <a> slip induced by Ca addition. Int. J. Plast. 2019, 120, 164–179. [Google Scholar] [CrossRef]
  28. Zhao, J.; Jiang, B.; Wang, Q.; Yuan, M.; Chai, Y.; Huang, G.; Pan, F. Effects of Li addition on the microstructure and tensile properties of the extruded Mg-1Zn-xLi alloy. Int. J. Miner. Metall. Mater. 2022, 29, 1380–1387. [Google Scholar] [CrossRef]
  29. Li, Z.J.; Wang, J.G.; Yan, R.F.; Chen, Z.Y.; Ni, T.Y.; Dong, Z.Q.; Lu, T.S. Effect of Ce addition on hot deformation behavior and microstructure evolution of AZ80 magnesium alloy. J. Mater. Res. Technol. 2022, 16, 1339–1352. [Google Scholar] [CrossRef]
  30. Wang, Q.; Jiang, B.; Tang, A.; He, C.; Zhang, D.; Song, J.; Yang, T.; Huang, G.; Pan, F. Formation of the elliptical texture and its effect on the mechanical properties and stretch formability of dilute Mg-Sn-Y sheet by Zn addition. Mater. Sci. Eng. A 2019, 746, 259–275. [Google Scholar] [CrossRef]
  31. Remennik, S.; Bartsch, I.; Willbold, E.; Witte, F.; Shechtman, D. New, fast corroding high ductility Mg–Bi–Ca and Mg–Bi–Si alloys, with no clinically observable gas formation in bone implants. Mater. Sci. Eng. B 2011, 176, 1653–1659. [Google Scholar] [CrossRef]
  32. Liu, Y.H.; Cheng, W.L.; Zhang, Y.; Niu, X.F.; Wang, H.X.; Wang, L.F. Microstructure, tensile properties, and corrosion resistance of extruded Mg-1Bi-1Zn alloy: The influence of minor Ca addition. J. Alloys Compd. 2020, 815, 152414. [Google Scholar] [CrossRef]
  33. Zhao, D.; Zhao, C.; Chen, X.; Huang, Y.; Hort, N.; Gavras, S.; Pan, F. Compressive deformation of as-extruded LPSO-containing Mg alloys at different temperatures. J. Mater. Res. Technol. 2022, 16, 944–959. [Google Scholar] [CrossRef]
  34. Ma, Z.; Li, G.; Su, Z.; Wei, G.; Huang, Y.; Hort, N.; Hadadzadeh, A.; Wells, M.A. Hot deformation behavior and microstructural evolution for dual-phase Mg–9Li–3Al alloys. J. Mater. Res. Technol. 2022, 19, 3536–3545. [Google Scholar] [CrossRef]
  35. Qiao, L.; Zhu, J. Constitutive modeling of hot deformation behavior of AlCrFeNi multi-component alloy. Vacuum 2022, 201, 111059. [Google Scholar] [CrossRef]
  36. Du, Y.Z.; Liu, D.J.; Ge, Y.F.; Jiang, B.L. Effects of deformation parameters on microstructure and texture of Mg–Zn–Ce alloy. Trans. Nonferrous Met. Soc. China 2020, 30, 2658–2668. [Google Scholar] [CrossRef]
  37. Wang, T.; Chen, Y.; Ouyang, B.; Zhou, X.; Hu, J.; Le, Q. Artificial neural network modified constitutive descriptions for hot de-formation and kinetic models for dynamic recrystallization of novel AZE311 and AZX311 alloys. Mater. Sci. Eng. A 2021, 816, 141259. [Google Scholar] [CrossRef]
  38. Park, S.S.; You, B.S.; Yoon, D.J. Effect of the extrusion conditions on the texture and mechanical properties of indirect-extruded Mg–3Al–1Zn alloy. J. Mater. Process Technol. 2009, 209, 5940–5943. [Google Scholar] [CrossRef]
  39. Du, Y.; Jiang, B.; Ge, Y. Effects of precipitates on microstructure evolution and texture in Mg-Zn alloy during hot deformation. Vacuum 2018, 148, 27–32. [Google Scholar] [CrossRef]
  40. Savaedi, Z.; Motallebi, R.; Mirzadeh, H. A review of hot deformation behavior and constitutive models to predict flow stress of high-entropy alloys. J. Alloys Compd. 2022, 903, 163964. [Google Scholar] [CrossRef]
  41. Jeong, H.T.; Park, H.K.; Park, K.; Na, T.W.; Kim, W.J. High-temperature deformation mechanisms and processing maps of equiatomic CoCrFeMnNi high-entropy alloy. Mater. Sci. Eng. A. 2019, 756, 528–537. [Google Scholar] [CrossRef]
  42. Ge, G.; Wang, Z.; Zhang, L.; Lin, J. Hot deformation behavior and artificial neural network modeling of β-γ TiAl alloy containing high content of Nb. Mater. Today Commun. 2021, 27, 102405. [Google Scholar] [CrossRef]
  43. Pang, H.; Li, Q.; Chen, X.; Chen, P.; Li, X.; Tan, J. Hot deformation behavior and microstructure evolution of Mg-Gd-Y(-Sm)-Zr alloys. J. Alloys Compd. 2022, 920, 165937. [Google Scholar] [CrossRef]
  44. Li, L.; Wang, Y.; Li, H.; Jiang, W.; Wang, T.; Zhang, C.-C.; Wang, F.; Garmestani, H. Effect of the Zener-Hollomon parameter on the dynamic recrystallization kinetics of Mg–Zn–Zr–Yb magnesium alloy. Comput. Mater. Sci. 2019, 166, 221–229. [Google Scholar] [CrossRef]
  45. Zhang, Q.; Li, Q.; Chen, X.; Bao, J.; Chen, Z. Effect of Sn addition on the deformation behavior and microstructural evolution of Mg-Gd-Y-Zr alloy during hot compression. Mater. Sci. Eng. A 2021, 826, 142026. [Google Scholar] [CrossRef]
  46. Kaur, N.; Deng, C.; Ojo, O.A. Effect of solute segregation on diffusion induced grain boundary migration studied by molecular dynamics simulations. Comput. Mater. Sci. 2020, 179, 109685. [Google Scholar] [CrossRef]
  47. Prasad, Y.V.R.K.; Gegel, H.L.; Doraivelu, S.M.; Malas, J.C.; Morgan, J.T.; Lark, K.A.; Barker, D.R. Modeling of dynamic material behavior in hot deformation: Forging of Ti-6242. Metall. Trans. A 1984, 15, 1883–1892. [Google Scholar] [CrossRef]
  48. Cheng, W.; Bai, Y.; Ma, S.; Wang, L.; Wang, H.; Yu, H. Hot deformation behavior and workability characteristic of a fine-grained Mg–8Sn–2Zn–2Al alloy with processing map. J. Mater. Sci. Technol. 2019, 35, 1198–1209. [Google Scholar] [CrossRef]
  49. Du, S.; Yang, K.; Li, M.; Li, J.; Ren, Y.; Huang, Q.; Pan, H.; Qin, G. Achieving high strength above 400 MPa in conventionally ex-truded Mg-Ca-Zn ternary alloys. Sci. China Technol. Sci. 2022, 65, 519–528. [Google Scholar] [CrossRef]
  50. Lu, X.; Zhao, G.; Zhou, J.; Zhang, C.; Chen, L.; Tang, S. Microstructure and mechanical properties of Mg-3.0Zn-1.0Sn-0.3Mn-0.3Ca alloy extruded at different temperatures. J. Alloys Compd. 2018, 732, 257–269. [Google Scholar] [CrossRef]
  51. Chai, Y.; Shan, L.; Jiang, B.; Yang, H.; He, C.; Hao, W.; He, J.; Yang, Q.; Yuan, M.; Pan, F. Ameliorating mechanical properties and reducing anisotropy of as-extruded Mg-1.0Sn-0.5Ca alloy via Al addition. Prog. Nat. Sci. 2021, 31, 722–730. [Google Scholar] [CrossRef]
  52. Zhou, N.; Zhang, Z.; Dong, J.; Jin, L.; Ding, W. High ductility of a Mg–Y–Ca alloy via extrusion. Mater. Sci. Eng. A 2013, 560, 103–110. [Google Scholar] [CrossRef]
  53. Wang, Q.; Jiang, B.; Chen, D.; Jin, Z.; Zhao, L.; Yang, Q.; Huang, G.; Pan, F. Strategies for enhancing the room-temperature stretch formability of magnesium alloy sheets: A review. J. Mater. Sci. 2021, 56, 12965–12998. [Google Scholar] [CrossRef]
Figure 1. (a) SEM image; (bd) SEM-EDS mapping scanning results from (a); (e) SEM-EDS point scanning result from phase 1 marked by red arrow in (a).
Figure 1. (a) SEM image; (bd) SEM-EDS mapping scanning results from (a); (e) SEM-EDS point scanning result from phase 1 marked by red arrow in (a).
Materials 15 07986 g001
Figure 2. XRD result of the solution-treated BX31 alloy.
Figure 2. XRD result of the solution-treated BX31 alloy.
Materials 15 07986 g002
Figure 3. True compressive stress–strain curves at strain rates: (a) 0.01 s−1; (b) 0.1 s−1; (c) 1 s−1.
Figure 3. True compressive stress–strain curves at strain rates: (a) 0.01 s−1; (b) 0.1 s−1; (c) 1 s−1.
Materials 15 07986 g003
Figure 4. (a) Peak stresses and (b) peak strains at different deformation conditions. Note that the color difference is to better distinguish the size of the value.
Figure 4. (a) Peak stresses and (b) peak strains at different deformation conditions. Note that the color difference is to better distinguish the size of the value.
Materials 15 07986 g004
Figure 5. Linear relations of (a) l n ε ˙ l n σ p ; (b) l n ε ˙ σ p ; (c) l n ε ˙ l n [ s i n   h ( α σ p ) ] ; (d) l n [ s i n   h ( α σ ) ] 1 / T and (e) l n Z l n [ s i n   h ( α σ p ) ] under the peak stress condition of the solution-treated BX31 alloy.
Figure 5. Linear relations of (a) l n ε ˙ l n σ p ; (b) l n ε ˙ σ p ; (c) l n ε ˙ l n [ s i n   h ( α σ p ) ] ; (d) l n [ s i n   h ( α σ ) ] 1 / T and (e) l n Z l n [ s i n   h ( α σ p ) ] under the peak stress condition of the solution-treated BX31 alloy.
Materials 15 07986 g005
Figure 6. (a) α, (b) Q, (c) n and (d) lnA as functions of the true strain ε.
Figure 6. (a) α, (b) Q, (c) n and (d) lnA as functions of the true strain ε.
Materials 15 07986 g006
Figure 7. Comparison of experiment flow curves and predicted results of the strain-related Arrhenius constitutive model at different strain rates: (a) 0.01 s−1; (b) 0.1 s−1; (c) 1 s−1.
Figure 7. Comparison of experiment flow curves and predicted results of the strain-related Arrhenius constitutive model at different strain rates: (a) 0.01 s−1; (b) 0.1 s−1; (c) 1 s−1.
Materials 15 07986 g007
Figure 8. Correlation (a) and the relative error (b) between experiment and predicted flow stresses by the strain-related Arrhenius constitutive model.
Figure 8. Correlation (a) and the relative error (b) between experiment and predicted flow stresses by the strain-related Arrhenius constitutive model.
Materials 15 07986 g008
Figure 9. (a) θ-σ curve at 573 K and 0.01 s−1. Note that it is divided into three stages marked by I, II and III, respectively; (b) relationship between ln ε c and ln Z; (c) relationship between ln ε 0.5 and ln Z; (d) ln (−ln (( 1 ( σ p σ ) / ( σ p σ s s ) ) ) ) as a function of ln ( ( ε ε c ) / ε 0.5 ) .
Figure 9. (a) θ-σ curve at 573 K and 0.01 s−1. Note that it is divided into three stages marked by I, II and III, respectively; (b) relationship between ln ε c and ln Z; (c) relationship between ln ε 0.5 and ln Z; (d) ln (−ln (( 1 ( σ p σ ) / ( σ p σ s s ) ) ) ) as a function of ln ( ( ε ε c ) / ε 0.5 ) .
Materials 15 07986 g009
Figure 10. XDRX-ε curves at (a) 573 K; (b) 623 K; (c) 673 K for 0.01, 0.1 and 1 s−1.
Figure 10. XDRX-ε curves at (a) 573 K; (b) 623 K; (c) 673 K for 0.01, 0.1 and 1 s−1.
Materials 15 07986 g010
Figure 11. (a,b) EBSD images of the solution-treated BX31 alloy during the hot compressive strains of 0.3 and 0.5 at 623 K and 0.01 s−1, respectively. CD represents the compressive direction; (c,d) DRX regions selected from (a) and (b), respectively; (e,f) grain size distribution maps of DRX regions from (c) and (d), respectively; (g,h) (0001) pole figures containing the whole and DRX areas of the samples with 0.3 and 0.5 strains, respectively.
Figure 11. (a,b) EBSD images of the solution-treated BX31 alloy during the hot compressive strains of 0.3 and 0.5 at 623 K and 0.01 s−1, respectively. CD represents the compressive direction; (c,d) DRX regions selected from (a) and (b), respectively; (e,f) grain size distribution maps of DRX regions from (c) and (d), respectively; (g,h) (0001) pole figures containing the whole and DRX areas of the samples with 0.3 and 0.5 strains, respectively.
Materials 15 07986 g011
Figure 12. Hot processing maps at different strains: (a) 0.3; (b) 0.5; (c) 0.7.
Figure 12. Hot processing maps at different strains: (a) 0.3; (b) 0.5; (c) 0.7.
Materials 15 07986 g012
Figure 13. Microstructure analysis of the as-extruded BX31 alloy from longitudinal section (ED-RD plane, RD represents radial direction): (a) macroscopic morphology; (b) EBSD map; (c) grain size distribution map; (d) inverse pole figure.
Figure 13. Microstructure analysis of the as-extruded BX31 alloy from longitudinal section (ED-RD plane, RD represents radial direction): (a) macroscopic morphology; (b) EBSD map; (c) grain size distribution map; (d) inverse pole figure.
Materials 15 07986 g013
Figure 14. SEM analysis of the as-extruded BX31 alloy from longitudinal section: (a) SEM image; (b) high magnified view from red frame in (a); (ce) SEM-EDS mapping scanning results containing Mg, Bi and Ca elements from (b); (f) SEM-EDS point scanning result from phase 1 marked by red arrow in (b).
Figure 14. SEM analysis of the as-extruded BX31 alloy from longitudinal section: (a) SEM image; (b) high magnified view from red frame in (a); (ce) SEM-EDS mapping scanning results containing Mg, Bi and Ca elements from (b); (f) SEM-EDS point scanning result from phase 1 marked by red arrow in (b).
Materials 15 07986 g014
Figure 15. (a) Tensile engineering stress–strain curve of the as-extruded BX31 alloy; (b) relationship between the ultimate strength and the elongation-to-failure for this work (marked by red star) and the reported other Mg-Bi-Ca series alloys (labeled by different symbols). Note that orange and gray circles represent “high strength but low ductility” and “high ductility but low strength” regions, respectively. Reproduced with permission from Refs. [17,18,19,20]. Copyright 2020, 2022, Elsevier, MDPI.
Figure 15. (a) Tensile engineering stress–strain curve of the as-extruded BX31 alloy; (b) relationship between the ultimate strength and the elongation-to-failure for this work (marked by red star) and the reported other Mg-Bi-Ca series alloys (labeled by different symbols). Note that orange and gray circles represent “high strength but low ductility” and “high ductility but low strength” regions, respectively. Reproduced with permission from Refs. [17,18,19,20]. Copyright 2020, 2022, Elsevier, MDPI.
Materials 15 07986 g015
Table 1. Coefficients in the polynomial fitting of α, Q, n and lnA.
Table 1. Coefficients in the polynomial fitting of α, Q, n and lnA.
αQnlnA
α0 = 0.0343Q0 = 138.6302n0 = 5.6236InA0 = 22.9529
α1 = −0.5172Q1 = −1049.6868n1 = −22.5556InA1 = −181.8720
α2 = 5.1075Q2 = 18,785.7115n2 = 432.5720InA2 = 3422.1192
α3 = −25.5741Q3 = −110,944.6683n3 = −2667.7302InA3 = −20,427.6000
α4 = 67.i.e60Q4 = 303,759.5483n4 = 7324.5991InA4 = 56,149.0301
α5 = −88.9583Q5 = −398,898.1624n5 = −9495.3504InA5 = −73,886.5001
α6 = 46.1098Q6 = 203,225.5371n6 = 4756.1032InA6 = 37,684.4203
Table 2. σc, σ0.5, εc and ε0.5 values at different deformation conditions.
Table 2. σc, σ0.5, εc and ε0.5 values at different deformation conditions.
Strain Rate (s−1)Deformation Temperature (K)
573623673
σc (MPa)0.0167.542.931.9
0.193.956.450.3
1125.878.472.8
σ0.5 (MPa)0.0169.147.232.0
0.1102.867.551.2
1130.788.874.8
εc0.010.1030.0860.070
0.10.1290.1190.096
10.1520.1380.111
ε0.50.010.1230.1010.085
0.10.1550.1370.107
10.2370.1810.121
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Wang, Q.; Wang, L.; Zhai, H.; Chen, Y.; Chen, S. Establishment of Constitutive Model and Analysis of Dynamic Recrystallization Kinetics of Mg-Bi-Ca Alloy during Hot Deformation. Materials 2022, 15, 7986. https://doi.org/10.3390/ma15227986

AMA Style

Wang Q, Wang L, Zhai H, Chen Y, Chen S. Establishment of Constitutive Model and Analysis of Dynamic Recrystallization Kinetics of Mg-Bi-Ca Alloy during Hot Deformation. Materials. 2022; 15(22):7986. https://doi.org/10.3390/ma15227986

Chicago/Turabian Style

Wang, Qinghang, Li Wang, Haowei Zhai, Yang Chen, and Shuai Chen. 2022. "Establishment of Constitutive Model and Analysis of Dynamic Recrystallization Kinetics of Mg-Bi-Ca Alloy during Hot Deformation" Materials 15, no. 22: 7986. https://doi.org/10.3390/ma15227986

APA Style

Wang, Q., Wang, L., Zhai, H., Chen, Y., & Chen, S. (2022). Establishment of Constitutive Model and Analysis of Dynamic Recrystallization Kinetics of Mg-Bi-Ca Alloy during Hot Deformation. Materials, 15(22), 7986. https://doi.org/10.3390/ma15227986

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop