Next Article in Journal
Improving the Anti-Corrosion and Anti-Wear Performance of Anodic Coating on the Surface of AA 5052 via Hydro-Thermal Treatment
Next Article in Special Issue
Research on Vibration Control Technology of Robot Motion Based on Magnetorheological Elastomer
Previous Article in Journal
Evaluating the X-ray-Shielding Performance of Graphene-Oxide-Coated Nanocomposite Fabric
Previous Article in Special Issue
Improving Aeroelastic Stability of Bladed Disks with Topologically Optimized Piezoelectric Materials and Intentionally Mistuned Shunt Capacitance
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Microstructure and Mechanical Properties of Co32Cr28Ni32.94Al4.06Ti3 High-Entropy Alloy

1
School of Mechanical Engineering and Automation, Fuzhou University, Fuzhou 350108, China
2
Fujian Key Laboratory of Force Measurement, Fujian Metrology Institute, Fuzhou 350108, China
3
Sino-French Institute of Nuclear Engineering and Technology, Sun Yat-sen University, Guangzhou 510275, China
*
Author to whom correspondence should be addressed.
Materials 2022, 15(4), 1444; https://doi.org/10.3390/ma15041444
Submission received: 22 December 2021 / Revised: 29 January 2022 / Accepted: 2 February 2022 / Published: 15 February 2022
(This article belongs to the Special Issue Advances in Smart Materials and Structures)

Abstract

:
High-entropy alloys have good application prospects in nuclear power plants due to their excellent mechanical properties and radiation resistance. In this paper, the microstructure of the Co32Cr28Ni32.94Al4.06Ti3 high-entropy alloy was researched using metallurgical microscopy, X-ray diffraction, and scanning electron microscopy. The mechanical properties were tested using a Vickers microhardness tester and a tensile testing machine, respectively. The results showed that Co32Cr28Ni32.94Al4.06Ti3 had a single-phase, disordered, face-centered, cubic solid-solution structure and was strengthened by solid solution. The alloy lattice parameter and density were estimated as 0.304 nm and 7.89 g/cm3, respectively. The test results indicated that the alloy had satisfactory mechanical properties with yield stress and tensile strength of about 530 MPa and 985 MPa, respectively.

1. Introduction

High-entropy alloys (HEAs) are a type of alloys which contain five or more principle alloying elements to stabilize solid solution phases by maximizing configurational entropy. HEAs have been extensively studied since they were first reported in 2004 [1]. The novel design idea underlying HEAs has greatly expanded the composition range and research areas of metallic materials. Owing to the high entropy effect, the alloys tend to form simple microstructures, such as body-centered cubic (BCC), face-centered cubic (FCC), and densely packed hexagonal (HCP) [2,3]. It has been found that some HEAs not only have excellent mechanical properties [4,5], but also excellent thermal stability [5], wear resistance [4,5,6,7], and irradiation resistance. Therefore, HEAs are promising materials for application in nuclear power plants.
The phase composition and mechanical properties of HEAs are determined by the element types and their atomic ratios in the alloy [8]. For transition HEAs, AlCoCrFeNiZrx is known to possess a BCC structure when x = 0 [9]; with an increase in the Zr content, the mechanical properties are significantly improved, because the phase composition of the alloy changes from an ordered BCC solid-solution phase to an ordered Laves + BCC phase. The phase composition of the AlCoCrFeNiBx alloy changes from a BCC phase to BCC + FCC two-phase solid solution with an increase in the B content; meanwhile, the hardness and fracture strength increase first and then decrease [10]. CoCrFeNiWx is known to possess a single-phase structure for x = 0.2 [11]; the phase composition of the alloy changes from a single-phase to a hypoeutectic phase, and the mechanical properties are significantly improved when the W content is increased. The phase composition of AlxCoCrFeNiTi changes from α + Al grains to fine equiaxed crystals when the Al content is increased; in this way, the yield stress is increased, but the elongation is decreased [12]. AlFeCrCoNi only exhibits an FCC structure for a low ratio of Al/Ni. However, for a large ratio of Al/Ni, the alloy exhibits a BCC structure. The hardness increases with the increase in the ratio of Al/Ni [13].
The three-component alloy of CoCrNi has a single FCC structure. Its mechanical properties are better than other alloys in the alloy system, especially at liquid nitrogen temperature [14,15,16], but the strength is relatively low at chamber temperature [16]. The alloy used in this study is a new, unreported alloy with Al and Ti elements added. Therefore, in this paper, the microstructure and tensile properties of Co32Cr28Ni32.94Al4.06Ti3 were researched in order to better understand the microstructure and mechanical properties of CoCrNi HEAs.

2. Experimental Materials and Methods

A Co32Cr28Ni32.94Al4.06Ti3 plate with dimensions of 90 mm × 80 mm × 20 mm was prepared using vacuum arc melting equipment with pure metal Co, Cr, Ni, Al, and Ti with purities greater than 99.9 wt%. In order to ensure that the material was not oxidized in the melting process, pure metal Ti was melted firstly to absorb the residual gas of the electric arc furnace. The composition (atomic fraction and weight ratio, %) of the Co32Cr28Ni32.94Al4.06Ti3 used in this study is shown in Table 1. The crystal structure was identified using a DY1602/Empyrean multifunctional X-ray polycrystalline diffractometer (PAnalytical, Alemlo, Holland) with Cu target radiation scanning in the range from 20° to 90° at a rate of 2°/min in a working voltage of 40 kV, a working current of 100 mA, and a characteristic wavelength of 1.5406 Å. The angle measurement accuracy was 0.02°. The HEA density was measured using a drainage method. In the drainage method, the mass of the HEA was measured by a scale; a measuring cylinder was used to measure the volume of water, and the volume of the HEA was the changed volume of the water in the cylinder before and after the HEA was put into the cylinder. The metallography of the HEA was characterized using a MV5000 metallographic microscope (Nanjing Lianchuang Analytical Instrument Manufacturing, Nanjing, China). The Vickers hardness of the HEA was measured using a THV-1MD microhardness tester (Teshi Detection Technology, Shanghai, China) under a load of 200 gf applied for 15 s. The tensile specimens with dimensions of 51.83 mm × 14 mm × 2.5 mm were used, as shown in Figure 1. Three tensile tests were carried out at air room temperature with a strain rate of 1 × 10−3 mm/s. The fracture morphology of the tensile specimen was analyzed using a Mira3 ultra-high-resolution field emission scanning electron microscope (FE-SEM) (TESCAN, Shanghai, China).

3. Results and Discussion

Figure 2 shows the X-ray diffraction (XRD) pattern of Co32Cr28Ni32.94Al4.06Ti3, wherein three diffraction peaks corresponding to the (111), (200), and (220) peaks of the FCC structure were observed. There were no diffraction peaks corresponding to other structures. The result implies that the HEA was only composed of FCC solid solution.
Generally, Ω > 1.1 and δ < 6.5% are the criteria for determining whether a solid solution phase can be formed [13]. Furthermore, when valence electron concentration (VEC) ≥ 8, the FCC solid solution is considered to be relatively stable [17]. The relevant parameters are calculated as follows:
Δ H mix = i = 1 , i j n Δ H ij mix c i c j
δ = i = 1 n c i 1 r i / i = 1 n c i r i 2
VEC = i = 1 n c i VEC i
Ω = T m Δ S mix Δ H mix
T m = i = 1 n c i T m i
Δ S mix = R i = 1 n c i ln c i
where Δ H mix is the total enthalpy of mixing for the system, Δ H i j mix is the mixing enthalpy of the atomic pair of the ith and jth atoms, c i   and   c j are the atomic percentages of elements i and j, respectively, δ is the difference in atomic radius between the two atoms, r i is the atomic radius of the ith element, VEC is the total VEC of the system, VEC i is the VEC of the ith element, Ω is the disorder of the system, T m is the mixed melting point of the system, Δ S mix is the mixing entropy of the system, T m i is the metal melting point of element i, and R is the gas constant.
Table 2 lists the characteristic parameters of the elements of Co32Cr28Ni32.94Al4.06Ti3, and Table 3 lists the mixing enthalpy values of the atom pairs of the HEA elements [18]. According to the calculations, the difference in the atomic size (δ) of the HEA was 4.26%. The disorder of the system (Ω) of the HEA was 3.91, and the VEC of the HEA was 8.1. Therefore, the HEA considered here should be an FCC solid-solution structure in theory.
The lattice constants of the five elements are listed in Table 4. The lattice constants of alloys can be calculated using the disorder principle [21]:
a mix = i = 1 n c i a i
where c i is the atomic percentage of element i, and a i is the lattice constants of element i. According to the calculations, the lattice constant of Co32Cr28Ni32.94Al4.06Ti3 was 0.304 nm, which was consistent with the lattice constant obtained as per XRD analysis (Table 4).
The theoretical density of the alloy was calculated using the following formula [22]:
ρ mix = i = 1 n c i A i i = 1 n c i A i / ρ i
where c i is the atomic percentage of element i, A i is the atomic weight of element i, and ρ i is the density of element i. From the calculation results, we noted that the theoretical density ( 7.85   g / cm 3 ) of the HEA was almost identical to the measured value ( 7.84   g / cm 3 ). It was also found that the HEA results were consistent with the rule of mixtures upon comparing the lattice constant and theoretical density of the alloy, which was a disordered FCC solid-solution structure.
Figure 3 shows a light microscopy image of the metallographic structure of Co32Cr28Ni32.94Al4.06Ti3. As shown in Figure 3, the alloy had a uniform, single-phase, equiaxial crystal structure, and the grain size was about 163 μ m as measured using the transection method.
Figure 4 shows the tensile stress–strain curve of Co32Cr28Ni32.94Al4.06Ti3. As shown in Figure 4, the yield strength was 530 ± 6 MPa, the tensile strength was 985 ± 7 MPa, and the elongation was 37.16 ± 0.17%. Compared with the CoCrNi alloy, the yield strength and the tensile strength increased by 103% and 14%, while the elongation decreased by 7%. Obviously, the increase in Al and Ti elements improved the tensile properties of the CoCrNi baselime alloy. Moreover, from Table 5, which compares the uniaxial tensile test results of similar alloys, it can be seen that the alloy affords better strength and plasticity. Moreover, the microhardness of the alloy was 313 HV. Therefore, Co32Cr28Ni32.94Al4.06Ti3 exhibits satisfactory tensile mechanical properties and hardness.
The tensile properties of the Co32Cr28Ni32.94Al4.06Ti3 studied in this paper are obviously improved compared with N18 and N36 Zircaloy currently used in the nuclear industry, as shown in Table 5. Therefore, the alloy studied in this paper is could be used in the nuclear industry.
Generally, the main strengthening mechanism of a single disordered FCC solid-solution structure is solid-solution strengthening, which mainly originates from the interaction between solute atoms [26].
Figure 5 shows an SEM micrograph of the fractured tensile specimen of Co32Cr28Ni32.94Al4.06Ti3. A large number of dimples and holes were observed in the fracture. The observed dimples were the traces left on the fracture after micropore nucleation and aggregation, which was the characteristic of micropore aggregation fractures.
The results provide a reference for the study of microstructure and properties of CoCrNi HEAs. In order to fully explain the comprehensive mechanical properties of the HEA, further studies on CoCrNiAlTi HEAs are being carried out, such as the effects of different atomic ratios of major elements on the creep, fatigue properties, and irradiation resistance of CoCrNiAlTi HEAs.

4. Conclusions

In this paper, the microstructure and tensile-fracture characteristics of Co32Cr28Ni32.94Al4.06Ti3 were researched. The following conclusions can be drawn:
(1)
The Co32Cr28Ni32.94Al4.06Ti3 exhibits a single disordered FCC solid-solution structure with a density of 7.89   g / cm 3 .
(2)
The microstructure of Co32Cr28Ni32.94Al4.06Ti3 is equiaxed, with a grain size about 163 μ m .
(3)
The yield strength, tensile strength, and elongation of the Co32Cr28Ni32.94Al4.06Ti3 are about 530 MPa, 985 Mpa, and 37.2%, respectively. The microhardness of the alloy is 313 HV.

Author Contributions

Conceptualization, J.G. and H.S.L.; methodology, J.G. and C.T.; experiment, C.T.; writing—original draft preparation, C.T.; writing—review and editing, J.G. and H.S.L. All authors listed have made a substantial, direct, and intellectual contribution to the work. All authors have read and agreed to the published version of the manuscript.

Funding

The authors are grateful to the National Natural Science Foundation of China (No. 11972005 and No. 51675103), the 2021 Independent Innovation Fund of Tianjin University-Fuzhou University (Grant Number TF2021-5), and the Open Fund of Fujian Key Laboratory of Force Measurement (Fujian Metrology Institute) (FJLZSYS202102) for the financial support to this study.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

No potential conflict of interest was reported by the authors.

References

  1. Yeh, J.W.; Chen, S.K.; Lin, S.J.; Gan, J.Y.; Chin, T.S.; Shun, T.T.; Tsau, C.H.; Chang, S.Y. Nanostructured high-entropy alloys with multiple principal elements: Novel alloy design concepts and outcomes. Adv. Eng. Mater. 2004, 6, 299–303. [Google Scholar] [CrossRef]
  2. Schuh, B.; Mendez-Martin, F.; Völker, B.; George, E.P.; Clemens, H.; Pippan, R.; Hohenwarter, A. Mechanical properties, microstructure and thermal stability of a nanocrystalline CoCrFeMnNi high-entropy alloy after severe plastic deformation. Acta Mater. 2015, 96, 258–268. [Google Scholar] [CrossRef] [Green Version]
  3. Lu, Y.P.; Gao, X.Z.; Jiang, L.; Zhen, Z.; Tang, T.; Jie, J.; Kang, H.; Zhang, Y.; Guo, S.; Ruan, H. Directly cast bulk eutectic and near-eutectic high entropy alloys with balanced strength and ductility in a wide temperature range. Acta Mater. 2017, 124, 143–150. [Google Scholar] [CrossRef] [Green Version]
  4. Chou, Y.L.; Wang, Y.C.; Yeh, J.W.; Shih, H.C. Pitting corrosion of the high-entropy alloy Co1.5CrFeNi1.5Ti0.5Mo0.1 in chloride-containing sulphate solutions. Corros. Sci. 2010, 52, 3481–3491. [Google Scholar] [CrossRef]
  5. Varalakshmi, S.; Kamaraj, M.; Murty, B.S. Processing and properties of nanocrystalline CuNiCoZnAlTi high entropy alloys by mechanical alloying. Mater. Sci. Eng. A 2010, 527, 1027–1030. [Google Scholar] [CrossRef]
  6. Senkov, O.N.; Woodward, C.F. Microstructure and properties of a refractory NbCrMo0.5Ta0.5TiZr alloy. Mater. Sci. Eng. A 2011, 529, 311–320. [Google Scholar] [CrossRef]
  7. Varalakshmi, S.; Appa Rao, G.; Kamaraj, M.; Murty, B.S. Hot consolidation and mechanical properties of nanocrystalline equiatomic AlFeTiCrZnCu high entropy alloy after mechanical alloying. J. Mater. Sci. 2010, 45, 5158–5163. [Google Scholar] [CrossRef]
  8. Guo, S.; Liu, C.T. Phase stability in high entropy alloys: Formation of solid-solution phase or amorphous phase. Prog. Nat. Sci. Mater. 2011, 21, 433–446. [Google Scholar] [CrossRef] [Green Version]
  9. Chen, J.; Niu, P.Y.; Liu, Y.Z.; Lu, Y.K.; Wang, X.H.; Peng, Y.L.; Liu, J.N. Effect of Zr content on microstructure and mechanical properties of AlCoCrFeNi high entropy alloy. Mater. Design 2016, 94, 39–44. [Google Scholar] [CrossRef]
  10. Chen, Q.S.; Lu, Y.P.; Dong, Y.; Wang, T.M.; Li, T.J. Effect of minor B addition on microstructure and properties of AlCoCrFeNi multi-compenent alloy. Trans. Nonferr. Met. Soc. 2015, 25, 2958–2964. [Google Scholar] [CrossRef]
  11. Wang, L.; Wang, L.; Tang, Y.C.; Luo, L.; Luo, L.S.; Su, Y.Q.; Guo, J.J.; Fu, H.Z. Microstructure and mechanical properties of CoCrFeNiWx high entropy alloys reinforced by µ phase particles. J. Alloys Compd. 2020, 845, 155997. [Google Scholar] [CrossRef]
  12. Li, Q.L.; Zhao, S.; Bao, X.P.; Zhang, Y.S.; Zhu, Y.Q.; Wang, C.Z.; Lan, Y.F.; Zhang, Y.X.; Xia, T.D. Effects of AlCoCrFeNiTi high-entropy alloy on microstructure and mechanical properties of pure aluminum. J. Mater. Sci. Technol. 2020, 52, 1–11. [Google Scholar] [CrossRef]
  13. Harihar, S.; Joseph, W.N.; Frank, L.F. Microstructural characterization and mechanical properties of laser deposited high entropy alloys. Mater. Sci. Forum. 2014, 3129, 2370–2375. [Google Scholar]
  14. Gludovatz, B.; Hohenwarter, A.; Thurston KV, S.; Bei, H.B.; Wu, Z.G.; George, E.P.; Ritchie, R.O. Exceptional damage-tolerance of a medium-entropy alloy CrCoNi at cryogenic temperatures. Nat. Commun. 2016, 7, 10602. [Google Scholar] [CrossRef]
  15. Wu, Z.; Bei, H.; Pharr, G.M.; George, E.P. Temperature dependence of the mechanical properties of equiatomic solid solution alloys with face-centered cubic crystal structures. Acta Mater. 2014, 81, 428–441. [Google Scholar] [CrossRef]
  16. Wu, Z.; Bei, H.; Otto, F.; Pharr, G.M.; George, E.P. Recovery, recrystallization, grain growth and phase stability of a family of FCC-structured multi-component equiatomic solid solution alloys. Intermetallics 2014, 46, 131–140. [Google Scholar] [CrossRef]
  17. Guo, S.; Ng, C.; Lu, J.; Liu, C.T. Effect of valence electron concentration on stability of bcc or fcc phase in high entropy alloys. J. Appl. Phys. 2011, 109, 103505. [Google Scholar] [CrossRef] [Green Version]
  18. Takeuchi, A.; Inoue, A. Classification of bulk metallic glasses by atomic size difference, heat of mixing and period of constituent elements and its application to characterization of the main alloying element. Mater. Trans. 2005, 46, 2817–2829. [Google Scholar] [CrossRef] [Green Version]
  19. Pauling, L. Atomic Radii and Interatomic Distances in Metal. J. Am. Chem. Soc. 1947, 69, 542–553. [Google Scholar] [CrossRef]
  20. Petrucci, R.H.; Harwood, W.S.; Geoffery, F.H.; Jeffry, D. Madura. In General Chemistry, 9th ed.; Pearsin Prentice Hall: Hoboken, NJ, USA, 2007. [Google Scholar]
  21. Juan, C.C.; Tsai, M.H.; Tsai, C.W.; Lin, C.M.; Wang, W.R.; Yang, C.C.; Chen, S.K.; Liu, S.J.; Yeh, J.W. Enhanced mechanical properties of HfMoTaTiZr and HfMoNbTaTiZr refractory high-entropy alloys. Intermetallics 2015, 62, 76–83. [Google Scholar] [CrossRef]
  22. Huang, H.; Wu, Y.; He, J.; Wang, H.; Liu, X.; An, K.; Wu, W.; Lu, Z. Phase-transformation ductilization of brittle high-entropy alloys via metastability engineering. Adv. Mater. 2017, 29, 1701678. [Google Scholar] [CrossRef] [PubMed]
  23. Liu, X.L.; Zhao, X.R.; Chen, J.; Lv, Y.K.; Wang, X.H.; Liu, B.; Liu, Y. Effect of C addition on microstructure and mechanical properties of as-cast HEAs (Fe50Mn30Co10Cr10)100-xCx. Mater. Chem. Phys. 2020, 254, 123501. [Google Scholar] [CrossRef]
  24. Listyawan, T.A.; Lee, H.; Park, N.; Lee, U. Microstructure and mechanical properties of CoCrFeMnNi high entropy alloy with ultrasonic nanocrystal surface modification process. J. Mater. Sci. Technol. 2020, 57, 123–130. [Google Scholar] [CrossRef]
  25. Nikulina, A.V. Zirconium alloy in nuclear power engineering. Met. Sci. Heat Treat. 2004, 46, 458–462. [Google Scholar] [CrossRef]
  26. Tian, F.Y.; Varga, L.K.; Chen, N.X.; Shen, J.; Vitos, L. Empirical design of single phase high-entropy alloys with high hardness. Intermetallics 2015, 58, 1–6. [Google Scholar] [CrossRef]
Figure 1. Dimensions of the tensile specimen (mm).
Figure 1. Dimensions of the tensile specimen (mm).
Materials 15 01444 g001
Figure 2. X-ray diffraction (XRD) results of Co32Cr28Ni32.94Al4.06Ti3.
Figure 2. X-ray diffraction (XRD) results of Co32Cr28Ni32.94Al4.06Ti3.
Materials 15 01444 g002
Figure 3. Microstructure of Co32Cr28Ni32.94Al4.06Ti3.
Figure 3. Microstructure of Co32Cr28Ni32.94Al4.06Ti3.
Materials 15 01444 g003
Figure 4. Stress–strain curve of Co32Cr28Ni32.94Al4.06Ti3.
Figure 4. Stress–strain curve of Co32Cr28Ni32.94Al4.06Ti3.
Materials 15 01444 g004
Figure 5. Scanning electron microscopy (SEM) images of the fracture surface of Co32Cr28Ni32.94Al4.06Ti3. (a) magnification of 300 times; (b) magnification of 1000 times.
Figure 5. Scanning electron microscopy (SEM) images of the fracture surface of Co32Cr28Ni32.94Al4.06Ti3. (a) magnification of 300 times; (b) magnification of 1000 times.
Materials 15 01444 g005
Table 1. Atomic and weight ratios of the principal elements of Co32Cr28Ni32.94Al4.06Ti3.
Table 1. Atomic and weight ratios of the principal elements of Co32Cr28Ni32.94Al4.06Ti3.
MetalCoCrNiAlTi
Atomic ratio (%)322832.944.063
Weight ratio (%)34.1126.3434.971.982.60
Table 2. Characteristic parameters of the principal elements of Co32Cr28Ni32.94Al4.06Ti3.
Table 2. Characteristic parameters of the principal elements of Co32Cr28Ni32.94Al4.06Ti3.
MetalCoCrNiAlTi
Melting point
(K)
1768.152132.151728.15933.151941.15
Atomic radius [19,20]
(nm)
0.1250.1280.1230.1430.147
VEC961034
Table 3. Mixed enthalpies among the principal elements of Co32Cr28Ni32.94Al4.06Ti3 (kJ/mol).
Table 3. Mixed enthalpies among the principal elements of Co32Cr28Ni32.94Al4.06Ti3 (kJ/mol).
MetalCoCrNiAlTi
Co/−40−19−28
Cr−4/−7−10−7
Ni0−7/−22−35
Al−19−10−22/−30
Ti−28−7−35−30/
Table 4. Densities and lattice constants of the component metals of Co32Cr28Ni32.94Al4.06Ti3.
Table 4. Densities and lattice constants of the component metals of Co32Cr28Ni32.94Al4.06Ti3.
MetalCoCrNiAlTiAlloy
(Calculated)
Alloy
(Measured)
Lattice constant (nm)0.250.290.350.410.350.300.31
Density
(g/cm3)
8.907.198.902.704.547.857.84
Table 5. Comparison of the tensile mechanical properties.
Table 5. Comparison of the tensile mechanical properties.
AlloyYield Strength (MPa)Tensile Strength (MPa)Elongation to Failure
(%)
Co32Cr28Ni32.94Al4.06Ti3530 ± 6985 ± 737.2 ± 0.17
CoCrNi [15]26087040
(Fe50Mn30Co10Cr10)94C6 [23]45070018
CoCrFeNiW0.4 [10]52597011
Al3CoCrFeNiTi [11]11515226
CoCrFeMnNi [24]46859030
N18 Zircaloy [25]39042038
N36 Zircaloy [25]31052027
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Guo, J.; Tang, C.; Lai, H.S. Microstructure and Mechanical Properties of Co32Cr28Ni32.94Al4.06Ti3 High-Entropy Alloy. Materials 2022, 15, 1444. https://doi.org/10.3390/ma15041444

AMA Style

Guo J, Tang C, Lai HS. Microstructure and Mechanical Properties of Co32Cr28Ni32.94Al4.06Ti3 High-Entropy Alloy. Materials. 2022; 15(4):1444. https://doi.org/10.3390/ma15041444

Chicago/Turabian Style

Guo, Jinquan, Chaozhongzheng Tang, and Huan Sheng Lai. 2022. "Microstructure and Mechanical Properties of Co32Cr28Ni32.94Al4.06Ti3 High-Entropy Alloy" Materials 15, no. 4: 1444. https://doi.org/10.3390/ma15041444

APA Style

Guo, J., Tang, C., & Lai, H. S. (2022). Microstructure and Mechanical Properties of Co32Cr28Ni32.94Al4.06Ti3 High-Entropy Alloy. Materials, 15(4), 1444. https://doi.org/10.3390/ma15041444

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop