Next Article in Journal
Functionalization of Cellulose Nanocrystals in Choline Lactate Ionic Liquid
Next Article in Special Issue
Mechanical Properties and Atomic Explanation of Plastic Deformation for Diamond-Like BC2
Previous Article in Journal
Incorporation of Rutin in Electrospun Pullulan/PVA Nanofibers for Novel UV-Resistant Properties
Previous Article in Special Issue
A Reinvestigation of a Superhard Tetragonal sp3 Carbon Allotrope
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

A Stress-Induced Martensitic Transformation in Aged Ti49Ni51 Alloy after High-Velocity Impact

Science and Technology on Materials Performance Evaluation in Space Environment Laboratory, School of Materials Science and Engineering, Harbin Institute of Technology, Harbin 150001, China
*
Author to whom correspondence should be addressed.
Materials 2016, 9(7), 500; https://doi.org/10.3390/ma9070500
Submission received: 4 May 2016 / Revised: 3 June 2016 / Accepted: 16 June 2016 / Published: 23 June 2016
(This article belongs to the Special Issue Computational Multiscale Modeling and Simulation in Materials Science)

Abstract

:
The effects of a high-velocity impact on the microstructure, phase transformation and mechanical property of aged Ti49Ni51 alloy are investigated. The transformation behavior and microstructure along the impact direction after impact emerge with regionalization characteristics, including a deformed region near the crater (0–4 mm) and an un-deformed region of the distal crater (5–6 mm). Stress-induced martensite is the main deformation mechanism in the deforming region of aged Ti49Ni51 alloy under high-velocity impact.

1. Introduction

TiNi shape memory alloys (SMA) have many current and potential engineering applications since their shape memory and superelasticity properties relate to the martensitic transformation induced by thermal or stress [1,2,3]. In aeronautics and astronautics applications, SMA devices would suffer a high-velocity impact from space debris, which often results in a change in the transformation behavior and microstructures [4,5].
As we know, aging treatment is an effective technology to adjust a material’s performance [6]. The aging of Ni-rich TiNi alloy can lead to the precipitation of Ti3Ni4, Ti2Ni3 and TiNi3 precipitates. Ti3Ni4 is coherent with the matrix B2 and is the most influential in affecting the transformation behavior. Unlike fully annealed and quenched near-equiatomic TiNi alloys, which transform from B2 to B19’ directly, aged Ni-rich TiNi alloys normally transform in two stages (B2-R-B19’) [7,8,9].
Liu investigated the shock-induced transformation behavior in NiTi SMA, and a three-step reverse phase transformation was observed [10]. Kurita et al. studied the transformation behavior of shock-compressed Ni48Ti52; a one-step transformation was observed before the shock treatment, and a three-step transformation was also found after annealing at an appropriate temperature on the shock-treated Ni48Ti52 [11]. The appearance of a three-step phase transformation may be because the shock wave makes the energy difference between the grain interior and grain boundary increase, and this results in the desynchronization of the phase transformation process.
The above research is conducted on the transformation behavior and microstructures of solution-treated TiNi alloys. So far, the research of high-velocity impact on aged Ti49Ni51 alloy is still in blank. In this paper, the transformation behavior and deformed microstructures in aged Ti49Ni51 alloys under high-velocity impact are characterized to investigate the deformed microstructure evolution from the crater rim to the matrix.

2. Materials and Methods

Ti49Ni51 shape memory alloy rod was hot-forged at 1173 K by Beijing Shape Memory Company (Beijing, China). Specimens with 17.5 mm diameter and 12 mm thickness were cut from the rod using a spark-erosion cutting machine. All the sealed samples were solution treated at 1173 K for 2 h and water-quenched to obtain a supersaturated homogeneous solid solution, and then aged at 773 K for 1 h.
Impact experiments were carried out on a powder gun, with a schematic diagram of the powder gun equipment shown in Figure 1a. A GCr15 steel ball with a 3 mm diameter was used as a projectile with the distance between the target and gun barrel being ~10 cm. The impact velocity was measured using a magnetic instrument [12] and a muzzle velocity of ~1.03 km·s−1 was obtained.
After impact, aged Ti49Ni51 alloy specimens were cut in a longitudinal direction using a spark-erosion cutting machine and polished mechanically. As shown in Figure 1b, thin sheets (represented by white lines) on the edge of the crate along the impact direction were cut and examined by differential scanning calorimetry (DSC, Perkin Elmer Diamond, New York, NY, USA) at 20 K·min−1 from 373 K to 193 K, the sample was heated from room temperature to 373 K, kept for 1 min, then cooled to 193 K, kept 1 min, and then heated to 373 K. Transmission electron microscopy (TEM) studies were carried out using a Philips CM-12 microscope (FEI, Rotterdam, The Netherlands) at 120 kV to observe the sample microstructure. Vickers hardness measurements were conducted using 300 g loads for a loading time of 15 s using a MMT-3 microhardness tester (Matsuzawa, Tokyo, Japan). Samples used for hardness measurement were ground and polished.

3. Results and Discussion

3.1. Transformation Behavior

Figure 2 shows the DSC curves of aged Ti49Ni51 alloy specimens after impact during two thermal cycles with different distances (0–6 mm) from the bottom of the crater. A one-step phase transformation occurs corresponding to B2↔B19’ for solution-treated Ti49Ni51 alloy in Figure 2a. The DSC curves of the aged Ti49Ni51 sample before impact are shown in Figure 2b, and it can be seen that multi-step phase transformation occurs compared with the solution-treated Ti49Ni51 alloy. This clearly shows that peak 5 and peak 1 are a pair of phase transformation. They may show a B19’↔B2 transformation in the grain interior, where Ti3Ni4 particles are essentially free. The cooling peak 4 corresponds to its reverse transformation peak 2, which occurs in the grain boundary region. As this pair of peaks has only a narrow hysteresis of 2 K, we can deduce that it may be a B2→R transformation and its reverse transformation. From the microstructure of this sample, as shown in Figure 3a, which shows a segregation of Ti3Ni4 particles around the grain boundaries, we can identify that peak 4 and peak 2 correspond, respectively, to the R phase transformation and its reverse transformation of the grain boundary regions. In addition, peak 6 and peak 3 are a pair of phase transformation, and they may show a R↔B19’ transformation at the grain boundary region, as the R phase transformation occurs only in the presence of Ti3Ni4 particles [14]. As Fan et al. pointed out, the occurrence of a three-step martensitic transformation for aged TiNi alloy depends on the distribution of Ti3Ni4 particles between the grain interior and grain boundary [15].
The DSC curves of impacted Ti49Ni51 alloy are presented in Figure 2c–i. On the bottom of the crater (0 mm), the exothermic and endothermic peaks are too wide to be observed in the range of from 193 K to 373 K. As the distance is 1 mm, two endothermic peaks (peak 2 and peak 3) before impact partially overlap after impact, and this may be because the stress concentrated in the grain boundary during the high-velocity impact, and the stress-induced martensite phase transformation happens while, at the same time, the uneven distribution of stress leads to the width and overlap of peak 2 and peak 3 [16]. The exothermic and endothermic peaks become sharper gradually with the increasing distance (2–4 mm), as shown in Figure 2d–g; meanwhile, peak 3 and peak 2 separated gradually due to less deformation. As the distance is 5–6 mm, the exothermic and endothermic peaks in Figure 2h,i are quite similar to the transformation behavior before impact treatment (Figure 2b).

3.2. Deformed Microstructure

Figure 3 shows the TEM micrographs and the selected area electron diffraction (SAED) pattern of aged Ti49Ni51 alloy. Aged Ti49Ni51 alloy exhibits finely dispersed Ti3Ni4 particles embedded in the grain interior (Figure 3a). The SAED pattern is shown Figure 3b, and it should be noticed that the microstructures are B2 austenite, R phase corresponding to 1/3 <110> B2 super-lattice spots marked with some white circles, and Ti3Ni4 particles corresponding to 1/7 <213> B2 super-lattice spots marked with some white arrows [17]. The corresponding schematic representation is shown in Figure 3c (blue circles represent the R phase, green circles represent Ti3Ni4 particles). Moreover, the dislocation density is approximately calculated to be 8.90 × 1011 cm−2 according to the high-resolution TEM image in Figure 3d,e.
The TEM and SAED patterns of Ti49Ni51 alloys on the bottom (0 mm) of the crater after impact are shown in Figure 4a–c; a lot of plates appear in Figure 4a, and from the SAED pattern in Figure 4b, the structure of the martensite plates is B19’. Meanwhile, the parent phase, R phase, and Ti3Ni4 particles were found in Figure 4c. According to the high-resolution TEM image in Figure 4d,e, the dislocation density is approximately calculated to be 1.40 × 1012 cm−2, which is no significant increase compared with of the density before impact.
From Figure 4a, the martensite plate begins to nucleate in the grain boundary region, and this may be because the shock treatment increases the non-chemical free energy such as the strain energy and interfacial energy of the grain boundary, which provide part of the driving force for nucleation and the growth of martensite; as a result, a martensite plate grows from the grain boundary to the grain interior. Partial Ti3Ni4 particles exist in the interior of the martensite plate.
In conclusion, we can deduce that the deformation mechanism of aged Ti49Ni51 alloy under high-velocity impact is stress-induced martensite rather than a mixture of stress-induced martensite and dislocation generation. This is different from our previous study of high-velocity impacted Ti50Ni50 alloy [18]. It may be because the Ti3Ni4 dispersed uniformly in the matrix and enhanced the strength of the matrix that dislocation is difficult to introduce.
As the distance increases from the crater, the volume fraction of the martensite plates reduces due to the decrease in the material stress, strain, strain rate and degree of deformation, as shown in Figure 5a–f. When the distance from the crater is 5–6 mm, the microstructure is similar to that of non-impact. In short, the transformation behavior and microstructure along the impact direction after high-velocity impact emerge with regionalization characteristics; the bottom of the crater was classified into a deformed region near the crater (0–4 mm) and an un-deformed region of the distal crater (5–6 mm).
Figure 6 shows the microhardness of aged Ti49Ni51 alloy before and after impact. The microhardness for solution-treated Ti49Ni51 alloy is ~240 under 300 g for 15 s, and the microhardness for aged Ti49Ni51 alloy before impact is ~300. While the microhardness near the crater increased to ~380, this may be because the material was subjected to the most severe plastic deformation during impact. Moreover, the microhardness decreased with the increasing distance from the crater due to the decrease in the material stress and degree of deformation. The microhardness of 4–6 mm from the crater approximates that of non-impact. Therefore, impact can achieve a gradient variation in the deformation degree from the bottom of the crater to the deep matrix.

4. Conclusions

The transformation behavior, microstructure and mechanical property of aged Ti49Ni51 alloy can achieve a regionalized variation from the bottom of the crater to the deep matrix. The generation of stress-induced martensitic transformation is due to the concentration of stress in the grain boundary, under the shock waves. The small change of dislocation density is because of the enhanced matrix strength due to Ti3Ni4 particles. The number of martensite plates and the microhardness reduce with the increasing distance from the crater.

Acknowledgments

This work is supported by Natural Science Foundation of China (No. 51571074, 51271066 and 51371069).

Author Contributions

Yingying Zhu conceived and designed the experiments; Yingying Zhu, Haizhen Wang performed the experiments; Yingying Zhu, Haizhen Wang, Zhiyong Gao analyzed the data; Yingying Zhu, Haizhen Wang, Zhiyong Gao and Wei Cai wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Takeda, K.; Matsui, R.; Tobushi, H. Transformation-induced relaxation and stress recovery of TiNi shape memory alloy. Materials 2014, 7, 1912–1926. [Google Scholar] [CrossRef]
  2. Kim, J.I.; Liu, Y.N.; Miyazaki, S. Aging-induced two-stage R-phase transformation in Ti-50.9 at % Ni. Acta Mater. 2004, 52, 487–499. [Google Scholar] [CrossRef]
  3. Kim, J.I.; Miyazaki, S. Effect of nano-scaled precipitates on shape memory behavior of Ti-50.9 at % Ni alloy. Acta Mater. 2005, 53, 4545–4554. [Google Scholar] [CrossRef]
  4. Chang, S.H.; Wu, S.K.; Chang, G.H. Grain size effect on multiple-stage transformations of a cold-rolled and annealed equiatomic TiNi alloy. Scr. Mater. 2005, 52, 1341–1346. [Google Scholar] [CrossRef]
  5. Nazarenko, A.I. Technique and some results of space debris penetration probability estimate for Russian modules of ISS. In Proceedings of the 17th IADC Meeting, Darmstadt, Germany, 11–13 October 1999.
  6. Filip, P.; Mazanec, K. On precipitation kinetics in TiNi shape memory alloys. Scr. Mater. 2001, 45, 701–707. [Google Scholar] [CrossRef]
  7. Jafar, K.A.; Antonin, D.; Gunther, E. Ni4Ti3-precipitation during aging of NiTi shape memory alloys and its influence on martensitic phase transformations. Acta Mater. 2002, 50, 4255–4274. [Google Scholar]
  8. Fatemeh, K.; Jafar, K.A.; Vahid, A.C. Effect of short-time annealing treatment on the superelastic behavior of cold drawn Ni-rich NiTi shape memory wires. Alloys Compd. 2013, 554, 32–38. [Google Scholar]
  9. Zhou, Y.; Fan, G.; Zhang, J.; Ding, X.; Ren, X.; Sun, J.; Otsuka, K. Understanding of multi-stage R-phase transformation in aged Ni-rich Ti-Ni shape memory alloys. Mater. Sci. Eng. A 2006, 438–440, 602–607. [Google Scholar] [CrossRef]
  10. Liu, H.T.; Sun, G.A.; Wang, Y.D. Shock-induced transformation behavior in NiTi shape memory alloy. Acta Phys. Sin. 2013, 62, 018103. [Google Scholar]
  11. Kurita, T.; Matsumoto, H.; Sakamoto, K. Transformation behavior of shock-compressed Ni48Ti52. Alloys Compd. 2005, 400, 92–95. [Google Scholar] [CrossRef]
  12. Gao, C.; Dong, S.L. Damage Behaviors of AZ31 Magnesium Alloy and Zirconium 702 Induced by Hypervelocity Impact. Master’s Thesis, Harbin Institute of Technology, Harbin, China, July 2013. [Google Scholar]
  13. Zou, D.L.; Zhen, L.; Xu, C.Y. Characterization of adiabatic shear bands in AM60B magnesium alloy under ballistic impact. Mater Charact. 2011, 62, 496–502. [Google Scholar] [CrossRef]
  14. Zhou, Y.M.; Zhang, J.; Fan, G.L.; Ding, X.D.; Sun, J.; Ren, X.B.; Otsuka, K. Origin of 2-stage R-phase transformation in low-temperature aged Ni-rich Ti-Ni alloys. Acta Mater. 2005, 53, 5365–5377. [Google Scholar] [CrossRef]
  15. Fan, G.L.; Chen, W.; Yang, S.; Zhu, J.H.; Ren, X.B.; Otsuka, K. Origin of abnormal multi-stage martensitic transformation behavior in aged Ni-rich Ti-Ni shape memory alloys. Acta Mater. 2004, 61, 4351–4362. [Google Scholar] [CrossRef]
  16. Xu, G.L.; Wang, C.Y.; Beltrán, J.I.; LLorca, J.; Cui, Y.W. Landau modeling of dynamical nucleation of martensite at grain boundaries under local stress. Comput. Mater. Sci. 2016, 118, 103–111. [Google Scholar] [CrossRef]
  17. Zhang, X.N.; Xia, B.Y.; Chen, J.; Song, B.; Tian, X.L.; Hao, Y.M.; Xie, C.Y. Effects of equal channel angular extrusion and aging treatment on R phase transformation behaviors and Ti3Ni4 precipitates of Ni-rich TiNi alloys. Alloys Compd. 2011, 509, 6296–6301. [Google Scholar] [CrossRef]
  18. Zhu, Y.Y.; Wang, H.Z.; Gao, Z.Y.; Cai, W. Phase transformation and mechanical properties of Ti50Ni50 alloy after high-velocity impact. Alloys Compd. 2016, 664, 223–228. [Google Scholar] [CrossRef]
Figure 1. Schematic diagram of the powder gun equipment (a) and sampling modes of DSC and TEM specimens (b) [13].
Figure 1. Schematic diagram of the powder gun equipment (a) and sampling modes of DSC and TEM specimens (b) [13].
Materials 09 00500 g001
Figure 2. DSC curves for aged Ti49Ni51 alloy with different distances (0–6 mm) from the crater before and after impact: (a) solution-treated; (b) non-impact; (c) 0 mm; (d) 1 mm; (e) 2 mm; (f) 3 mm; (g) 4 mm; (h) 5 mm; (i) 6 mm.
Figure 2. DSC curves for aged Ti49Ni51 alloy with different distances (0–6 mm) from the crater before and after impact: (a) solution-treated; (b) non-impact; (c) 0 mm; (d) 1 mm; (e) 2 mm; (f) 3 mm; (g) 4 mm; (h) 5 mm; (i) 6 mm.
Materials 09 00500 g002
Figure 3. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy before impact: (a) Bright-field image; (b) SAED pattern; (c) Corresponding schematic representation of (b); (d) High-resolution TEM image of (a); (e) Inverse Fourier filtered image of the area indicated by a dotted square in (d).
Figure 3. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy before impact: (a) Bright-field image; (b) SAED pattern; (c) Corresponding schematic representation of (b); (d) High-resolution TEM image of (a); (e) Inverse Fourier filtered image of the area indicated by a dotted square in (d).
Materials 09 00500 g003
Figure 4. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy after impact: (a) Bright-field image of the bottom of crater (0 mm); (b) SAED pattern of area A in (a); (c) SAED pattern of area B in (a); (d) High-resolution TEM image of (a); (e) Inverse Fourier filtered image of the area indicated by a dotted square in (d).
Figure 4. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy after impact: (a) Bright-field image of the bottom of crater (0 mm); (b) SAED pattern of area A in (a); (c) SAED pattern of area B in (a); (d) High-resolution TEM image of (a); (e) Inverse Fourier filtered image of the area indicated by a dotted square in (d).
Materials 09 00500 g004
Figure 5. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy after impact: (a) Bright-field image of 1 mm; (b) SAED pattern of area A in (a); (c) SAED pattern of area B in (a); (d) Bright-field image of 2–4 mm; (e) SAED pattern of area A in (d); (f) SAED pattern of area B in (d); (g) Bright-field image of 5–6 mm; (h) Magnified microstructures of area B in (g); (i) SAED pattern of area B in (g).
Figure 5. TEM micrographs and SAED patterns of aged Ti49Ni51 alloy after impact: (a) Bright-field image of 1 mm; (b) SAED pattern of area A in (a); (c) SAED pattern of area B in (a); (d) Bright-field image of 2–4 mm; (e) SAED pattern of area A in (d); (f) SAED pattern of area B in (d); (g) Bright-field image of 5–6 mm; (h) Magnified microstructures of area B in (g); (i) SAED pattern of area B in (g).
Materials 09 00500 g005
Figure 6. Microhardness distribution along crater in aged Ti49Ni51 alloy before and after impact.
Figure 6. Microhardness distribution along crater in aged Ti49Ni51 alloy before and after impact.
Materials 09 00500 g006

Share and Cite

MDPI and ACS Style

Zhu, Y.; Wang, H.; Gao, Z.; Cai, W. A Stress-Induced Martensitic Transformation in Aged Ti49Ni51 Alloy after High-Velocity Impact. Materials 2016, 9, 500. https://doi.org/10.3390/ma9070500

AMA Style

Zhu Y, Wang H, Gao Z, Cai W. A Stress-Induced Martensitic Transformation in Aged Ti49Ni51 Alloy after High-Velocity Impact. Materials. 2016; 9(7):500. https://doi.org/10.3390/ma9070500

Chicago/Turabian Style

Zhu, Yingying, Haizhen Wang, Zhiyong Gao, and Wei Cai. 2016. "A Stress-Induced Martensitic Transformation in Aged Ti49Ni51 Alloy after High-Velocity Impact" Materials 9, no. 7: 500. https://doi.org/10.3390/ma9070500

APA Style

Zhu, Y., Wang, H., Gao, Z., & Cai, W. (2016). A Stress-Induced Martensitic Transformation in Aged Ti49Ni51 Alloy after High-Velocity Impact. Materials, 9(7), 500. https://doi.org/10.3390/ma9070500

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.