Next Article in Journal
Lean-Green Manufacturing Practices and Their Link with Sustainability: A Critical Review
Next Article in Special Issue
Predicting Unconfined Compressive Strength Decrease of Carbonate Building Materials against Frost Attack Using Nondestructive Physical Tests
Previous Article in Journal
The Use of Big Data and Its Effects in a Diffusion Forecasting Model for Korean Reverse Mortgage Subscribers
Previous Article in Special Issue
Influence of Partial Coarse Fraction Substitution of Natural Aggregate by Recycled Concrete Aggregate in Hot Asphalt Mixtures
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Experimental Study to Design Warm Mix Asphalts and Recycled Warm Mix Asphalts Using Natural Zeolite as Additive for Sustainable Pavements

by
Elsa Sanchez-Alonso
*,
Gonzalo Valdes-Vidal
and
Alejandra Calabi-Floody
Department of Civil Engineering, Universidad de La Frontera, Francisco Salazar street 01145, Temuco 4811230, Chile
*
Author to whom correspondence should be addressed.
Sustainability 2020, 12(3), 980; https://doi.org/10.3390/su12030980
Submission received: 20 November 2019 / Revised: 17 January 2020 / Accepted: 19 January 2020 / Published: 29 January 2020
(This article belongs to the Special Issue Sustainable Construction and Building Materials for Environment)

Abstract

:
There are currently various technologies for the manufacture of warm mix asphalts (WMA). This paper presents the possibility of using a natural zeolite to manufacture WMA as an alternative to existing synthetic products for the manufacture of this type of mixture. Moreover, the possibility of manufacturing WMA with the addition of recycled asphalt pavement (RAP) using natural zeolite as the basis of a warm mix technology was evaluated. Firstly, asphalt mixtures were manufactured at three different temperatures (145 °C, 135 °C, and 125 °C) with different percentages of natural zeolite to determine the temperature and the optimum content for the manufacture of WMA. Then, the zeolite moisture content and its release over time were determined at different temperatures, and its distribution in the binder was checked at different concentrations by scanning electron microscopy and fluorescence. Next, with the optimum zeolite content, the addition of RAP between 10–30% in the WMA at the same three manufacturing temperatures was evaluated. Two types of compaction were used: the impact and gyratory compactions. The Marshall parameters were evaluated for all the designed mixtures. The results indicated that the manufacture of WMA with the addition of natural zeolite is feasible, and depending on the required mixing temperature, recycled WMA with different percentages of RAP can be obtained.

1. Introduction

The pavement industry currently faces a double dilemma: on the one hand, the demand for environmentally friendly asphalt materials has increased, and on the other hand, the cost of raw materials has risen [1]. Therefore, the industry has worked on the drop-in manufacturing temperatures through different technologies that have emerged since 1996, when the European Union (EU) began to legislate with respect to emissions produced by in the asphalt industry [2]. France is the only EU country where the production of warm mix asphalts (WMA) is above 10% of its production. However, in other European countries, its use is limited to laboratory tests and test sections [2]. By contrast, these technologies were used to manufacture 32% of the total mixes manufactured in the US in 2014 [3].
There are several studies on the use of different techniques to manufacture WMA. For example, Sengoz et al. [4] evaluated different WMA technologies (zeolites, an organic additive and another chemical), to determine the stability in storage, the mixing and compaction temperatures in terms of the optimum of additive, as well as the rheological properties to check their performance. According to the results obtained, the mixing temperatures were reduced between 6 °C to 13 °C and the compaction between 6 °C to 10 °C depending on the type of additives used, being 3% s/b the optimum for the organic and chemical additives and between 5–6% s/b for zeolites to be able to use them in conditions of heavy traffic and high temperatures.
Sanchez-Alonso et al. [5] evaluated the ease of compaction, water sensitivity and stiffness of WMA with waxes, zeolites and tensoactives at different manufacturing temperatures. The results showed that all additives improved the workability of the asphalt mixtures manufactured compared to the reference hot asphalt mixture (HMA). The additivated asphalt mixtures had better water sensitivity results compared than the reference mixture at the same manufacture temperature. In all the asphalt mixtures manufactured (reference and modified), the stiffness moduli were reduced, but this reduction was less in the case of warm asphalt mixtures. In 2013, Sanchez-Alonso et al. [6] continued their study of WMA behavior, evaluating the rutting and fatigue behavior of the same WMA. All the WMA studied were more deformable than HMA, but the asphalt mixtures with waxes and zeolite additives manufactured at 140 °C showed similar fatigue life to HMA.
Woszuk and Franus [7] evaluated the mechanical properties of two different zeolites: a synthetic and a natural one, which had 28% and 17% water in their structure, respectively. Three compaction temperatures in the design of the mixtures (145 °C, 130 °C, and 115 °C) were used, obtaining a natural zeolite optimum of 1% w/m and 0.5% w/m for the synthetic zeolite. The results of water sensitivity and plastic deformations showed a good performance with both zeolites according to Polish specifications. Topal et al. [8] evaluated the Marshall stability properties, stiffness modulus, and indirect tensile fatigue of asphalt mixtures made with natural and synthetic zeolites. According to the data shown by the authors, a slight decrease in the amount of binder is required compared to the conventional asphalt mixtures, which would mean an initial cost saving. The use of both zeolites increased the stiffness of the mixture. However, comparing the results of fatigue resistance and permanent deformation, the results were slightly better with the synthetic zeolite. Wu and Li [9] evaluated the effect of the curing time (two weeks, one and two months) for WMA manufactured with synthetic zeolite. The properties evaluated were dynamic modulus, rutting, resistance to moisture damage, and fatigue behavior. The results showed that the WMA properties improved with the curing time, probably due to losing of water contained in the mixture, unlike the HMA, the properties of which were not affected and remaining practically constant over the time.
On the other hand, the use of different materials that were previously thrown away makes it possible to reduce the demand of raw materials by reducing the environmental impact generated by their production and the associated energy saving [10], resulting in lower costs for companies. These materials include steel slag, shingles, coal ash, and recycled asphalt pavement (RAP) [11]. The use of RAP offers a second life to the aggregates and binder that they have in their composition, decreasing the high costs associated with oil and the extraction of raw materials [12]. When combining RAP technology with WMA techniques in addition to saving on raw materials, there would be a decrease in CO2 emissions, which results in a more environmentally friendly mixture [13,14], obtaining mechanical properties of WMA with RAP similar to the conventional HMA [15].
Using Superpave® methodology, Xiao et al. [16] presented a study on the volumetric properties of asphalt mixtures manufactured with two different technologies (Evotherm® and foamed bitumen), with three different types of binders (two PG64-22 and one PG58-28) and, two RAP of different origin, using them in four different percentages varying between 20% and 50%. According to the results, the increase of RAP content increased the binder viscosity regardless of the type of binder, origin of the RAP or test temperature. The increase of %RAP did not affect the optimum binder content regardless of the origin and type of binder used. The percentage of air voids was affected by the type of binder and the WMA technology used. The mineral aggregate voids in WMA were reduced by increasing the %RAP regardless of the binder origin. The filler-bitumen relationship was affected by the RAP content and not by the WMA technology used.
Zhao et al. [17] evaluated the properties of water sensitivity, resistance to plastic deformation, and fatigue of two different WMA technologies (Evotherm® additive and foaming technique) using several percentages of RAP, between 15 and 40%. The WMAs showed lower resistance to plastic deformations than their HMA counterparts, regardless of the WMA technology used, %RAP or pavement layer evaluated. The addition of RAP improved the results of WMAs and HMAs, regardless of the WMA technology or the pavement layer. WMAs with lower RAP contents presented better results than WMAs with high %RAP. The addition of RAP increased the fatigue resistance of WMAs and decreased it in HMAs by up to 30% RAP. The addition of RAP to a maximum of 30% can be an alternative to reduce the moisture susceptibility of the WMAs without taking into account the WMA technology used or the pavement layer.
Oner and Sengoz [18] evaluated the use of different WMA technologies with the addition of RAP, at a manufacturing (147–152 °C) and compaction (135–140 °C) temperatures, and presented a cost-benefit evaluation of these techniques. To carry out the study, they used an organic additive, a chemical additive, and a last one containing water in the proportions recommended by the manufacturers. According to the results, the RAP optimum obtained for each technique was 30%, 10%, and 20%, respectively. With respect to the cost-benefit analysis that they carried out, it was concluded that a cost saving to WMA compared with the conventional mixture was obtained using both WMA and WMA + RAP technologies. According to the data shown, the greatest saving occurred using WMA + RAP, between 8–25% compared with respect to HMA, depending on the chosen technique.
As noted above, there are many WMA techniques that have been developed in recent times. They are based on the use of emulsifying chemical additives, organic additives to lower the viscosity of asphalt binders, or the use of synthetic additives that generates foaming processes. However, the study of WMA with the use of natural additives, such as natural zeolite, has not been sufficiently addressed both in its design phase and its mechanical properties, as well as the influence of the compaction process. Therefore, this paper presents the possibility of using a natural zeolite to produce WMA mixtures as an alternative to existing synthetic products for the manufacture of this these types of mixtures. In turn, the possibility of manufacturing WMA mixtures with the addition of RAP using natural zeolite as the basis of WMA technology is evaluated.

2. Materials and Methods

2.1. Materials

A conventional asphalt binder is used in this research. Its characterization according to Chilean specifications is shown in Table 1.
The fluvial aggregates composed mainly of dolomite, basalt, dacite, andesite, rhyolite, sandstone, quartz, and quartzite were characterized for their use in asphalt mixtures according to the Chilean standards (Table 2).
The natural zeolite used in this research is a clinoptilolite and was acquired from the Maule Region in Chile. Due to its open and porous structure, this material could maintain water or other type of chemical elements inside of its structure. This natural zeolite contains water, which will be released if it is heated at temperatures beyond 100 °C, provoking a micro-foaming into the asphalt binder. Therefore, this natural additive could be used to manufacture warm asphalt mixtures. The characterization of the natural zeolite is shown in Table 3.
The RAP used came from milling works on Route 5, in La Araucania Region (Chile). RAP was separated in two fractions: 0/5 mm and 5/20 mm. It was characterized to know its gradation and bitumen content (Table 4) as well as and the properties of bitumen recovered (Table 5).

2.2. Mix Design

A semi-dense type IV-A-12 gradation with a maximum aggregate size of 12.5 mm was selected. The IV-A-12 particles were classified by size and adjusted to the grading envelope as shown in Figure 1.
The optimum asphalt binder content was obtained by the Marshall method and the analysis of air voids in a reference mix (R mix) manufactured at 155 °C, leading to 5.4% weight of aggregates. This optimal optimum binder content was used in the manufacture of all the mixtures included in this paper.
Three manufacturing temperatures were studied: 145 °C, 135 °C, and 125 °C. Four percentages of natural zeolite were evaluated (0.3, 0.6, 0.9, and 1.2%) to obtain the optimum amount of additive to achieve the lowest manufacturing temperature of asphalt mixtures.
With the optimum content of natural zeolite, three percentages of RAP were analyzed (10%, 20%, and 30%) to obtain recycled warm mixtures asphalts (RWMA). The content of raw binder for each RAP mixture was calculated, considering that 50% of the RAP binder contributes to the mixture and using the Federal Highway Administration method [19]. To obtain the manufactured temperatures in RWMA, the raw aggregates were overheated, taking into account the moisture content of RAP [20]. In Table 6, the characteristics of the RWMA studied are shown.

2.3. Methodology

First, the moisture content of the natural zeolite was determined. For this, the samples were dried in an oven at 110 ± 5 °C until constant mass, obtaining the moisture content of the zeolite by means of the loss of mass of the sample. In addition, a test was carried out to determine the process of releasing the water contained in its structure over time, and compared with a commercial synthetic zeolite used for the manufacture of WMA. This test was made at temperatures of 155 °C, 145 °C, and 135 °C, and were measured every 5 min up to 90 min, the average period of time estimated for the manufacture and the laying process of an asphalt mixture. On the other hand, the dispersion of the natural zeolite in the asphalt binder was verified by scanning electron microscopy (SEM) and fluorescence images, using different amounts of natural zeolite, 1%, 5%, and 10%, by weight of the binder.
For the compaction of the different asphalt mixtures manufactured, the impact and gyratory compactions were used. In the case of impact compaction, the specimens were compacted to 75 blows per face. In the case of the gyratory compactor, a vertical pressure of 600 kPa was applied with a compaction angle of 1.16° and a speed of 30 rpm. The number of cycles was 100 for each mixture and the diameter of the mold used was 100 mm. To the impact and gyratory specimens, the Marshall parameters such as density, stability, flow, and the air and mineral aggregate voids were determined. Chile only has mix design specifications for asphalt mixtures compacted by impact, but these values were used as a guide to analyze the results obtained with the gyratory compactor.

3. Analysis of Results

The moisture content was calculated for both zeolites. The average of moisture content obtained in the natural zeolite was 12.6% in mass, a percentage lower than the water content of synthetic zeolite, which was around 20% in mass. However, as shown in Figure 2, the water release curves at the different temperatures evaluated indicate that the natural zeolite released higher water content during the time of manufacturing and laying of the asphalt mixtures, unlike the synthetic zeolite, which did it for a longer time. This could be due to the difference of chemical elements that the zeolites may have in their structure. The composition of synthetic zeolite is purer (less variability) than natural zeolite (generated by different geological processes). However, the compounds used in its synthesis could have more polar elements than natural zeolite, generating more polar structure and therefore greater attraction to water (formation of chemical bonds like Van der Waals or hydrogen bonds), requiring more time applying heat to release all the water contained. According to the results shown, the use of natural zeolite as substitute for synthetic zeolites seems feasible.
The analysis of the natural zeolite dispersion in the binder shown in Figure 3 demonstrated a good dispersion within the binder at the three proportions studied, which would help to achieve a greater optimization of the foaming effect in the asphalt mixtures. However, at the 10% concentration of natural zeolite on binder, zeolite clusters began to appear, so higher concentrations of this additive would not be recommended since the distribution of the additive would not be homogeneous and could affect the quality of the mixture.
The results of the Marshall parameters of the WMA are presented in Figure 4 and Figure 5. According to the results shown, when the manufacturing temperature is reduced, there was a decrease in the density of the asphalt mixtures, although the addition of zeolite seemed to mitigate this decrease in density, as can be seen with the results obtained at 135 °C (Figure 4A left). On the other hand, the density values obtained with the gyratory specimens did not present significant differences in the density regardless of the manufacturing temperature and the amount of zeolite used, although higher densities were obtained compared to the impact specimens (Figure 4A right).
All WMA fulfilled the stability specifications required by Chilean standards (9000 N), regardless of manufacturing temperature and the amount of natural zeolites used (Figure 4B). The mixtures manufactured at 135 °C and 125 °C obtained stability values similar to the reference mixture. If it compares a reference mixture manufactured at 135 °C against the WMA with the different percentages of additives, it can see the influence of the addition of natural zeolite, improving the stability values obtained. On the other hand, although the gyratory specimens complied with the minimum value required by the standards, they obtained lower values than the impact specimens (Figure 4B right). This may be due to the kneading effect produced by the gyratory compaction which causes the aggregates to settle within the structure in a more efficiently way.
Regarding the flow results, all WMA compacted by impact obtained values within the requirements by the Chilean standards (9–16 in 0.25 mm units). However, the gyratory specimens obtained values higher than the upper limit indicated in the standards and no significant trend was observed with the reduction of the temperature or the variation of the additive content (Figure 4C).
All WMA compacted by impact complied with the values established in the Chilean standards, both in percentage of air and mineral aggregate voids (Figure 5A,B left). On the other hand, the gyratory WMA did not show a clear tendency in the variation of the percentage of air and mineral aggregate voids due to the increased of the percentage of natural zeolite used or by the manufacturing temperature (Figure 4A,B right). Although most of the mixtures were below the limit of the percentage of air and mineral aggregate voids allowed, this may be due to the over-compacting of the asphalt mixtures by an excess of the number of cycles during compaction.
Although all the WMA complied with the Marshall parameters indicated in the standards, not all the asphalt mixtures achieved a good coating of the aggregates. The 30 °C reduction in the manufacture of the asphalt mixtures caused a lack of aggregates’ coating with any of the proportions of natural zeolite (Figure 6A). So, this could cause problems with the water, which could significantly affect the structure of the pavement and/or lead to significant deteriorations. The WMA at 145 °C and 135 °C and all the amounts of natural zeolite used were possible to achieve a good aggregate coating (Figure 6B,C). Based on these results and in the search for a greater reduction in costs and energy, the optimum WMA would be manufactured at 135 °C with 0.3% and 0.6% of zeolite.
In the case of recycled WMAs (RWMA), they were manufactured using 0.6% zeolite in the asphalt mixture to facilitate the foaming of the binder provided by the RAP. In Figure 7 and Figure 8, the results of the Marshall parameters are shown. The density results obtained showed that as the RAP content in the mixture increased, the mixtures became denser for the same manufacturing temperature (Figure 7A left). Similarly to what occurred with the WMAs, the density of the gyratory specimens was higher than the impact ones (Figure 7A right), probably due to the kneading effect produced by this type of compaction.
Concerning the stability of the recycled warm asphalt mixtures, for both compact and gyratory specimens, they complied with the minimum established in the Chilean standards (Figure 7B). With the results of gyratory specimens, for the same temperature, the stability increased with the RAP content in the asphalt mixture. However, for the same amount of RAP, the stability remained almost constant when the manufacturing temperature was changed.
In the case of flow, the asphalt mixtures compacted by impact complied with Chilean requirements. However, the gyratory asphalt mixtures exceeded the upper limit (Figure 7C). With both types of compaction, the influence of the manufacturing temperature or the RAP content had not clear trend in the results. With respect to the content of air and mineral aggregate voids obtained in the impact compactor, all the mixtures complied with the requirements of the standard, except for mixtures with 20% and 30% RAP at 125 °C and 30% RAP at 135 °C (Figure 8A,B left). However, analogous to the results of WMAs, the gyratory compaction of the RWMA produced values of both types of voids quite below that required by the standard (Figure 8A,B right).
According to the results obtained and seeking to optimize the different variables evaluated, three types of RWMA could be obtained: one where the decrease in temperature was maximized to the detriment of RAP (manufacturing temperature at 125 °C and 10% RAP), another one in which the amount of RAP is was maximized without lowering the temperature much (manufacturing temperature at 145 °C and 30% RAP), and a third mixture where both variables were optimized (manufacturing temperature at 135 °C and 20% RAP).

4. Conclusions

The addition of the natural zeolite to the asphalt mixture generates a micro-foaming when it comes into contact with the asphalt binder, which allows for a better coating of the aggregates in the mixture when the temperature is reduced.
Although all WMAs at the three temperatures and the four natural zeolite contents complied with the parameters of the Marshall design, the WMAs manufactured at 125 °C had difficulties in the process of coating the aggregates because the workability of the asphalt mixture decreased with respect to the manufacture process at 145 °C and 135 °C. Therefore, it is not recommended that the manufacturing and compaction temperatures be reduced below 20 °C compared to the HMA.
According to the results obtained, optimizing the Marshall properties and taking into account the coating of aggregates, the amount of natural zeolite recommended to use in WMA is between 0.3% and 0.6% by weight of the aggregates.
The addition of natural zeolite in recycled asphalt mixtures makes it possible to reduce the manufacturing temperature compared to a conventional HMA up to 30 °C, complying with the Marshall parameters.
Recycled WMA mixtures can be manufactured with the addition of natural zeolite at different temperatures, one maximizing the amount of RAP (30% RAP at 145 °C), another maximizing the decrease in manufacturing temperature (125 °C and 10% RAP), and a mixture where both variables are optimized (135 °C and 20% RAP).
Therefore, it is feasible to manufacture WMA with the addition of natural zeolite and WMA with the addition of RAP, according to the Chilean standards for pavements. It is recommended to evaluate mechanical properties such as water sensitivity or rutting to extend the scope of knowledge in the performance of these types of asphalt mixtures. It is also recommended to carry out a study of the costs, reduction of energy consumption, and the emission of gases from this type of asphalt mixtures.

Author Contributions

Conceptualization, E.S.-A., G.V.-V. and A.C.-F.; Funding acquisition, G.V.-V.; Investigation, E.S.-A., G.V.-V. and A.C.-F.; Methodology, E.S.-A., G.V.-V. and A.C.-F.; Writing—original draft, E.S.-A.; Writing—review & editing, G.V.-V. and A.C.-F. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by CONICYT program (a FONDEF IDea Project), grant number ID15I10235.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Farooq, M.A.; Mir, M.S. Use of reclaimed asphalt pavement (RAP) in warm mix asphalt (WMA) pavements: A review. Innov. Infrastruct. Solut. 2017, 2, 10. [Google Scholar] [CrossRef] [Green Version]
  2. Woszuk, A.; Franus, W. A Review of the Application of Zeolite Materials in Warm Mix Asphalt Technologies. Appl. Sci. 2017, 7, 293. [Google Scholar] [CrossRef] [Green Version]
  3. Hansen, K.R.; Copeland, A. Asphalt Pavement Industry Survey on Recycled Materials and Warm Mix Asphalt Usage: 2014; Information Series 138; NAPA: Lanham, MD, USA, 2015; p. 28. [Google Scholar]
  4. Sengoz, B.; Topal, A.; Gorkem, C. Evaluation of natural zeolite as warm mix asphalt additive and its comparison with other warm mix additives. Constr. Build. Mater. 2013, 43, 242–252. [Google Scholar] [CrossRef]
  5. Sanchez-Alonso, E.; Vega-Zamanillo, A.; Castro-Fresno, D.; DelRio-Prat, M. Evaluation of compactability and mechanical properties of bituminous mixes with warm additives. Constr. Build. Mater. 2011, 25, 2304–2311. [Google Scholar] [CrossRef]
  6. Sanchez-Alonso, E.; Vega-Zamanillo, A.; Calzada-Perez, M.A.; Castro-Fresno, D. Effect of warm additives on rutting and fatigue behaviour of asphalt mixtures. Constr. Build. Mater. 2013, 47, 240–244. [Google Scholar] [CrossRef]
  7. Woszuk, A.; Franus, W. Properties of the warm mix asphalt involving clinoptilolite and Na-P1 zeolite additives. Constr. Build. Mater. 2016, 114, 556–563. [Google Scholar] [CrossRef]
  8. Topal, A.; Sengoz, B.; Kok, B.V.; Yilmah, M.; Agazadeh Dokhandari, P.; Oner, J.; Kaya, D. Evaluation of mixture characteristics of warm mix asphalt involving natural and synthetic zeolite additives. Constr. Build. Mater. 2014, 57, 38–44. [Google Scholar] [CrossRef]
  9. Wu, S.; Li, X. Evaluation of effect of curing time on mixture performance of Advera warm mix asphalt. Constr. Build. Mater. 2017, 145, 62–67. [Google Scholar] [CrossRef]
  10. Chang, C.-J.; Tseng, L.; Lin, T.-S.; Wang, W.-J.; Lee, T.-C. Recycling of modified MSWI ash-mix slag and CMP sludge as a cement substitute and its optimal composition. Indian J. Eng. Mater. Sci. 2012, 19, 31–40. [Google Scholar]
  11. Xu, S.; Xiao, F.; Amirkhaniana, S.; Singh, D. Moisture characteristics of mixtures with warm mix asphalt technologies—A review. Constr. Build. Mater. 2017, 142, 148–161. [Google Scholar] [CrossRef]
  12. Sengoz, B.; Topal, A.; Oner, J.; Yilmaz, M.; Aghazadeh Dokandari, P.; Kok, B.V. Performance evaluation of warm mix asphalt mixtures with recycled asphalt pavement. Period. Polytech. Civil. Eng. 2017, 61, 117–127. [Google Scholar] [CrossRef] [Green Version]
  13. Mallick, R.; Kandhal, P.; Bradbury, R. Using warm mix asphalt technology to incorporate high percentage of reclaimed asphalt pavement material in asphalt mixtures. J. Transp. Res. Board 2008, 2051, 71–79. [Google Scholar] [CrossRef]
  14. O’Sullivan, K.; Wall, P. The Effects of Warm Mix Asphalt Additives on Recycled Asphalt Pavement. Bachelor of Science Thesis, Worcester Polytech Inst., Worcester, MA, USA, 2009. [Google Scholar]
  15. Mallick, R.; Bradley, J.; Bradbury, R. Evaluation of heated reclaimed asphalt pavement material and wax-modified asphalt for use in recycled hot-mix asphalt. Transp. Res. Rec. J. Transp. Res. Board 2007, 1998, 112–122. [Google Scholar] [CrossRef]
  16. Xiao, F.; Hou, X.; Amirkhanian, S.; Kim, K.W. Superpave evaluation of higher RAP contents using WMA technologies. Constr. Build. Mater. 2016, 112, 1080–1087. [Google Scholar] [CrossRef]
  17. Zhao, S.; Huang, B.; Shu, X.; Woods, M. Comparative evaluation of warm mix asphalt containing high percentages of reclaimed asphalt pavement. Constr. Build. Mater. 2013, 44, 92–100. [Google Scholar] [CrossRef]
  18. Oner, J.; Sengoz, B. Utilization of Recycled Asphalt Concrete with Warm Mix Asphalt and Cost-Benefit Analysis. PLoS ONE 2015, 10, e116180. [Google Scholar] [CrossRef] [PubMed]
  19. Kandhal, P.S.; Mallick, R.B. Pavement Recycling Guidelines for State and Local Governments; Report No. FHWA-SA-98-042; US Department of Transportation, Federal Highway Administration: Washington, DC, USA, 1997. [Google Scholar]
  20. Don Brock, J.; Richmond, J.L. Technical Paper T-127: Milling and Recycling; ASTEC INC.: Chatanooga, TN, USA, 2007; p. 36. [Google Scholar]
Figure 1. IV-A-12 aggregate gradation.
Figure 1. IV-A-12 aggregate gradation.
Sustainability 12 00980 g001
Figure 2. Water release of the natural zeolite vs. synthetic zeolite at different temperatures.
Figure 2. Water release of the natural zeolite vs. synthetic zeolite at different temperatures.
Sustainability 12 00980 g002
Figure 3. Dispersion of natural zeolite in asphalt binder.
Figure 3. Dispersion of natural zeolite in asphalt binder.
Sustainability 12 00980 g003
Figure 4. Results of Marshall parameters for WMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Density, (B) Stability, (C) Flow.
Figure 4. Results of Marshall parameters for WMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Density, (B) Stability, (C) Flow.
Sustainability 12 00980 g004aSustainability 12 00980 g004b
Figure 5. Results of Marshall parameters for WMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Air voids, (B) VAM.
Figure 5. Results of Marshall parameters for WMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Air voids, (B) VAM.
Sustainability 12 00980 g005
Figure 6. Coating of aggregates of WMA with 0.3% of natural zeolite at: (A) 125 °C, (B) 135 °C, (C) 145 °C.
Figure 6. Coating of aggregates of WMA with 0.3% of natural zeolite at: (A) 125 °C, (B) 135 °C, (C) 145 °C.
Sustainability 12 00980 g006
Figure 7. Results of Marshall parameters for RWMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Density, (B) Stability, (C) Flow.
Figure 7. Results of Marshall parameters for RWMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Density, (B) Stability, (C) Flow.
Sustainability 12 00980 g007aSustainability 12 00980 g007b
Figure 8. Results of Marshall parameters for RWMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Air voids, (B) VAM.
Figure 8. Results of Marshall parameters for RWMA specimens compacted by impact (left) and by gyratory compactor (right): (A) Air voids, (B) VAM.
Sustainability 12 00980 g008aSustainability 12 00980 g008b
Table 1. Properties of conventional asphalt binder.
Table 1. Properties of conventional asphalt binder.
TestsCA-24Criteria
Absolute Viscosity at 60 °C, 300 mm Hg (P)3077(*)
Ductility at 25 °C, (cm)>150Min 100
Oliensis Spot Test, (% xylene)<25Max 25
Cleveland Open Cup Flash Point, (°C)332Min 232
Softening Point R&B, (°C)51To be reported
Penetration Index−0.7−1.5a + 1.0
RTFOT
Mass Loss, (%).0.0Max 0.8
Absolute Viscosity at 60 °C, 300 mm Hg (P)7475To be reported
Ductility at 25 °C, 5 cm/min>150Min 100
Durability Index2.4Max 3.5
(*): Min 2400 for CA-24.
Table 2. Properties of aggregates.
Table 2. Properties of aggregates.
Type of AggregateTestsResultsCriteria
CoarseLos Angeles Abrasion Loss(%)18.4<25(*)–35%
Crushed Particles(%)97.3>90(*)–70%
Flakiness Index(%)0.1<10(*)–15%
Specific Gravity(kg/m3)2661-
Absorption(%)1.54-
FinePlasticity indexNon plasticNon plastic
Riedel-Weber adhesion0–9Min. 0–5
Specific gravity(kg/m3)2629-
Absorption(%)1.09-
(*) Surface layer.
Table 3. Properties of the natural zeolite.
Table 3. Properties of the natural zeolite.
Identification of Mineral
DescriptionClinoptilolite—natural zeolite
Chemical nameCalcium magnesium aluminosilicates hydrated
Grain size0–0.173 mm
Mineralogical Characteristics
Main zeolitic componentClinoptilolite
Other componentsPlagioclase, Smectite and Quartz
ColorIvory
Physicochemical Characteristics
Chemical composition (%)SiO2: 64.19; TiO2: 0.51; Al2O3: 11.65; Fe2O3: 2.53; MnO: 0.03; MgO: 0.66; CaO: 3.42; Na2O: 0.75; K2O: 1.60; P2O5: 0.03; PxC: 14.64
Cation exchange capacity (cec)86.82 a 112.88 cmol/kg
Specific surface (Bet method)446 a 480 m2/g
Thermal stability<450 °C
Chemical stability8.9
Density0.661 g/cm3
Table 4. RAP gradation and bitumen content (after extraction).
Table 4. RAP gradation and bitumen content (after extraction).
RAP Fraction (mm)0/55/20
Bitumen Content (% by Weight of Mix)7.53.3
Sieve Size (mm)Gradation (% Passing)Gradation (% Passing)
20100100
12.510073
1010056
510029
2.57018
0.633511
0.315258
0.16195
0.08154
Table 5. Characteristics of binder recovered from the RAP.
Table 5. Characteristics of binder recovered from the RAP.
TestsResults
Penetration at 25 °C, 100 g. 5 s. (0.1 mm)10
Fraas Breaking Point (°C)+3
Softening Point R&B (°C)55.6
Brookfield Viscosity at 60 °C (Pa s)30.883
Table 6. Characteristics of Recycled Warm Mixture Asphalt studied.
Table 6. Characteristics of Recycled Warm Mixture Asphalt studied.
MixtureBinder Content (%)Temperatures (°C)
Raw AggregateRAPCA-24RAP ContributionRaw AggregatesRAPMixture
100-5.4-155-155
90105.190.2116215145
90105.190.2115215135
90105.190.2114215125
80204.980.4318015145
80204.980.4316915135
80204.980.4315715125
70304.770.5420215145
70304.770.5419015135
70304.770.5417815125

Share and Cite

MDPI and ACS Style

Sanchez-Alonso, E.; Valdes-Vidal, G.; Calabi-Floody, A. Experimental Study to Design Warm Mix Asphalts and Recycled Warm Mix Asphalts Using Natural Zeolite as Additive for Sustainable Pavements. Sustainability 2020, 12, 980. https://doi.org/10.3390/su12030980

AMA Style

Sanchez-Alonso E, Valdes-Vidal G, Calabi-Floody A. Experimental Study to Design Warm Mix Asphalts and Recycled Warm Mix Asphalts Using Natural Zeolite as Additive for Sustainable Pavements. Sustainability. 2020; 12(3):980. https://doi.org/10.3390/su12030980

Chicago/Turabian Style

Sanchez-Alonso, Elsa, Gonzalo Valdes-Vidal, and Alejandra Calabi-Floody. 2020. "Experimental Study to Design Warm Mix Asphalts and Recycled Warm Mix Asphalts Using Natural Zeolite as Additive for Sustainable Pavements" Sustainability 12, no. 3: 980. https://doi.org/10.3390/su12030980

APA Style

Sanchez-Alonso, E., Valdes-Vidal, G., & Calabi-Floody, A. (2020). Experimental Study to Design Warm Mix Asphalts and Recycled Warm Mix Asphalts Using Natural Zeolite as Additive for Sustainable Pavements. Sustainability, 12(3), 980. https://doi.org/10.3390/su12030980

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.