Next Article in Journal
A Prototype Sensor System Using Fabricated Piezoelectric Braided Cord for Work-Environment Measurement during Work from Home
Next Article in Special Issue
Enhanced Red Emission from Amorphous Silicon Carbide Films via Nitrogen Doping
Previous Article in Journal
Detection of Electrical Circuit in a Thin-Film-Transistor Liquid-Crystal Display Using a Hybrid Optoelectronic Apparatus: An Array Tester and Automatic Optical Inspection
Previous Article in Special Issue
The Effect of Nitrogen Incorporation on the Optical Properties of Si-Rich a-SiCx Films Deposited by VHF PECVD
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Improving Color Quality of Nanowire White Light-Emitting Diodes with Mn4+ Doped Fluoride Nanosheets

by
Thi Hong Quan Vu
1,2,
Thi Tuyet Doan
1,3,
Barsha Jain
2,
Ravi Teja Velpula
2,
Tung Cao Thanh Pham
1,
Hieu Pham Trung Nguyen
2,* and
Hoang-Duy Nguyen
1,*
1
Institute of Chemical Technology, Vietnam Academy of Science and Technology, Ho Chi Minh City 700000, Vietnam
2
Helen and John C. Hartmann Department of Electrical and Computer Engineering, New Jersey Institute of Technology, Newark, NJ 07102, USA
3
Faculty of Materials Science, University of Science, Vietnam National University, Ho Chi Minh City 700000, Vietnam
*
Authors to whom correspondence should be addressed.
Micromachines 2021, 12(8), 965; https://doi.org/10.3390/mi12080965
Submission received: 30 June 2021 / Revised: 9 August 2021 / Accepted: 13 August 2021 / Published: 15 August 2021
(This article belongs to the Special Issue Nanostructured Light-Emitters, Volume II)

Abstract

:
A two-dimensional nanostructured fluoride red-emitting phosphor with an excellent quantum yield of ~91% is studied for cost-effective and high-color quality nanowire white light-emitting diodes (WLEDs). K2TiF6:Mn4+ phosphors are synthesized via an emulsification method using surfactants as sodium dodecyl sulphonate and oleic acid. The K2TiF6:Mn4+ phosphors in ultra-thin and nanosheet crystals are observed via scanning electron microscopy and high-resolution transmission electron microscopy. The surfactants are found to play a key role in inhibition of KTFM crystal growth process and stabilization of Mn4+ ions doping into the K2TiF6 host. The prepared phosphors exhibited intensive red emission at approximately 632 nm and excellent thermal stability in the range of 300–500 K upon 460 nm light excitation. Moreover, the K2TiF6:Mn4+ nanosheets were integrated on InGaN/AlGaN nanowire WLEDs for color quality study. The results show that the nanowire WLEDs with red-emitting phosphor exhibit unprecedentedly high color rendering index ~96.4, and correlated color temperature ~4450 K.

1. Introduction

White light-emitting diodes (WLED), composed of yellow phosphor and blue-light LED, have been replacing traditional lights such as incandescent and fluorescent lamps for general lighting because of their highlight efficiency, long lifetime and energy saving [1,2,3]. In order to improve the color rendering index (CRI) of WLED, red-emitting fluoride materials with high quantum yield area promising candidate, which is considered as a phosphor converted WLED or pc-WLED approach [4,5,6]. Alternatively, nanowire structures have been intensively studied for WLEDs [4,5,6,7,8,9,10]. In these nanowire WLEDs, intrinsic white-light emissions are generated by integrating full-color emission in a single nanowire. Nanowire WLEDs exhibit high quantum efficiency due to the reduced dislocation densities, the resultant polarization fields [5,6] and the absence of phosphor converter. However, the development of high-power red emission in LEDs still remains challenging due to the immature growth condition and large lattice mismatch resulted from high indium composition in the InGaN layers. Therefore, the utilization of red-emitting fluoride materials in nanowire LEDs offers a promising solution for achieving high power and high color quality nanowire WLEDs.
Manganese (IV) doped fluoride phosphor materials such as A2MF6:Mn4+ (with A = Na, K, Rb, Cs; B = Si, Ge, Ti), A3BF6:Mn4+ (B = Al, Ga) and BaMF6:Mn4+ (B = Si, Ti) [11] exhibit a sharp photoluminescence (PL) band, intensive red emission and low thermal quenching compared to those of rare-earth phosphor. Among the fluoride phosphors, K2TiF6:Mn4+ (KTFM) is noticed with dramatically strong red emission at 630 nm and high quantum yield up to 98% under UV or blue-light excitation [11,12,13,14]. Additionally, the synthesis of fluoride phosphors at room temperature is not complex, which is suitable for industry production. Owing to their special structural, electronic and optical properties, nanocrystals offer new possibilities for applications in lighting, display, energy and environmental technologies [15]. It is known that sub-micrometer-sized phosphors can facilitate a decrease in their consumption and improved resolution of phosphor screens. When the particle size becomes comparable to wavelengths of light, the optical properties of phosphor powders undergo remarkable qualitative changes [16,17,18]. Nanophosphors can be defined as nanoparticles of transparent dielectrics (hosts) doped with optically active ions (activators), so that the emission of light happens due to the electronic transitions between the levels of the impurity ions inside the bandgap of the host (characteristic luminescence) [17]. Currently, thin-KTFM red-emitting phosphor with 30–100 μm size and 3–5 μm thickness synthesized via an alcohol-assisted co-precipitation method showed a reduction of light-scattering loss. The luminous efficacy and color rendering index (CRI) of white-light emitting diodes (LEDs) using thin-KTFM has been improved remarkably [19]. In this study, we prepared K2TiF6:Mn4+ ultrathin and nanosheet crystals through the emulsification method using surfactants to control the thickness and size of phosphors. The effect of the surfactants on luminescent properties of KTFM phosphor is studied in detail. Moreover, a significant improvement in color quality of nanowire WLEDs integrated with KTFM nanosheets is also studied and reported.

2. Experimental Section

2.1. Chemicals

Sodium dodecyl sulphonate (SDS), oleic acid (OA), potassium permanganate (KMnO4 99%), potassium fluoride (KF.2H2O 99%), hydrofluoric acid (HF 40%), titanium(IV) isopropoxide (Ti-iso 97%), isopropanol (99%), acetone (98%) and hydrogen peroxide solution (H2O2 30%): All chemicals were of standard grade and used as received without further purification.

2.2. Synthesis of K2TiF6:Mn4+

The K2TiF6:Mn4+(KTFM) nanoparticles were synthesized by an emulsification method. A mixture of 0.13 g KMnO4, 3.2 g KF.2H2O and 0.05 g SDS surfactant was dissolved in 20 mL HF 40% solution (Solution A). Solution B composed of 5 mL isopropanol, 0.5 mL Ti-iso and OA (with various weight ratios of OA/SDS ~ 0.0, 2.0, 6.0 and 10.0). A solution of 10 μL H2O2 and 5 mL isopropanol was dropped into a mixture of A and B solutions under vigorous stirring at 3 °C until the violet solution turned to deep yellow. The yellow precipitates were isolated and washed with HF acid 20% and then with acetone for several times. Finally, the sample was dried at 50 °C for 2 h in oven vacuum.

2.3. Fabrication of K2TiF6:Mn4+ on Nanowire WLED

The InGaN/AlGaN nanowire WLED heterostructures were grown by a Veeco GEN II molecular beam epitaxy (MBE) system under nitrogen-rich condition. The device structure consists of ten couples of 3 nm InGaN/3 nm AlGaN quantum dot (QD) active region sandwiched in between a ~200 nm GaN:Si template and ~200 nm GaN:Mg layer. The emission spectrum of the nanowire WLEDs is optimized so that red/green/blue emissions are generated from a single nanowire. The color emission of the nanowire WLEDs can be optimized by controlling the indium composition in the InGaN active region. The nanowire LED devices are then fabricated from nanowire LEDs on Si wafer using the following procedure. The nanowires are coated with polyimide by spin-coating, then oxygen-plasma dry etching to expose the nanowires’ tips. Anode electrode (p-contact) is fabricated by evaporating thin nickel (Ni), gold (Au) and indium tin oxide (ITO) layers on top of the nanowires, respectively. Subsequently, thick Ni and Au layers are covered on the top of the ITO layer. The back side of the silicon wafer is deposited with titanium (Ti) and then Au layers for cathode electrode (n-contact). The epitaxial growth and device fabrication of such nanowire WLED structures are reported elsewhere [6,7,20,21]. An isopropanol suspension of 6.0wt% K2TiF6:Mn4+ was then coated onto the surface of the 100×100 µm2 nanowire WLED via a spin coating method.

2.4. Characterization of Materials

The solid products were characterized by using X-ray powder diffraction (X’Pert Pro Panalytical X-ray using Cu-Kα radiation, λ = 1.54056 Å and a graphite monochromator operating at 40 kV and 30 mA between 10° and 70° at a scanning rate of 0.026 °/s). The morphologies of phosphors are observed through a scanning electron microscope (SEM, JEOL, JSM-6700F) and high-resolution transmission electron microscopy (HRTEM, JEOL, JEM-2100). The photoluminescence excitation (PLE) and photoluminescence (PL) spectra were measured using an F-7000 FL spectrophotometer equipped with a 150-W xenon lamp at room temperature. Steady-state luminescence spectra were excited with the wavelength of 460 nm. For the temperature-dependent measurements, the samples were placed in a small platinum hold with its temperature controlled by a Linkam THMS600 heating/freezing stage (Linkam Scientific Instruments Ltd., Tadworth, UK). Light was radiated by a Hamamatsu R928 photo-multiplier tube. The quantum yield was measured using the Hamamatsu PMA-12 spectrophotometer equipped with an integrating sphere. The electroluminescence (EL) of the LED devices was collected by an optical fiber and analyzed using an USB2000 Ocean Optics spectrometer at room temperature.

3. Results and Discussion

X-ray diffraction patterns of the prepared KTFM samples are shown in Figure 1a. All diffracted peaks can be indexed to the space group D 3 d 3 -P-3m1 of the hexagonal structure K2TiF6 (JCPDS No. 08-0488). The characteristic diffraction peaks of manganese oxide were no observed in the XRD of KTFM samples. Crystal structure of KTFM is depicted in Figure 1b. Each Ti4+ ion is surrounded by 6 F ions, resulting in formation of [TiF6]2– octahedral. K+ ions were coordinated by 12 F ions to form [KF12]11− polyhedron and located among octahedral to balance the structure.
The SEM images of the KTFM samples are shown in Figure 2. In the absence of surfactant, the KTFM sample exhibited a hexagonal shape with average size and thickness of ~35 μm and ~3 μm, respectively (Figure 2a). A remarkable decrease in size of ~15 μm and thickness of ~500 nm is observed for KTFM samples prepared using OA and SDS with the weight ratio ~2.0 and ~6.0 (Figure 2b,c).The KTFM nanosheets with size in the range of 200–300 nm and thickness of 70–90 nm were obtained as increasing the OA/SDS ratio up to ~10.0 (Figure 2d). It is suggested that the SDS reduced interface surface tension of the mixture solutions in synthesis process and OA was active as ligands covering onto KTFM nuclei surface and inhibited further crystal growth [22]. The crystal passivation effect was not obvious using only OA or SDS. The TEM image and the selected area electron diffraction (SAED) pattern indicate that the KTFM nanosheets are single crystals (Figure 2e and the inserted picture). The high-resolution TEM (HRTEM) image with the interplanar spacing of 0.28 nm corresponding to the (110) crystal planes of hexagonal K2TiF6, presented in Figure 2f, reflects the crystalline nature of the KTFM nanosheets.
Figure 3a,b presents the top-view and 45° tilted angle SEM images of a typical InGaN/AlGaN nanowire WLED sample grown by MBE. The nanowires exhibit quite uniform wire diameters and lengths. Figure 3c illustrates the schematic structure of a single nanowire WLED that includes GaN:Si, InGaN/AlGaN active region and GaN:Mg layers. The fabricated nanowire LED device is illustrated in Figure 3c showing a schematic structure nanowire-LED device with anode and cathode electrodes and can be found in our previous publication [9]. The SEM images of the coated nanowire LEDs with KTFM red nanophosphor are shown in Figure 3d. The top electrode, nanowire LED on Si, and KTFM are clearly presented. The thickness of the KTFM layer on the LED is estimated to be ~2 µm. The p-contact electrode layer with thickness ~350 nm, which includes Ni/Au and ITO, is shown in inserted picture of Figure 3d.
Figure 4a illustrates the photoluminescence excitation (PLE) spectra of prepared K2TiF6:Mn4+ samples at room temperature. The excitation bands of the Mn4+ doped K2TiF6 nanocrystals assigned to the 4A24T1 and 4A24T2 transitions are located at the 330–400 nm and 430–500 nm regions with the maxima at 350 nm and 460 nm, respectively. The emission at 632 nm (λem = 632 nm) was monitored. The sharp red emissions in the range of 600–680 nm, originated from the spin-forbidden 2Eg4A2g transitions of Mn4+ in octahedral crystal-field, are presented in photoluminescence (PL) spectra (Figure 4b). The peaks at ~601, 610, 615, 622, 632, 636 and 648 nm are due to transitions of the ν3(t1u), ν4(t1u), ν6(t2u), zero phonon line (ZPL), ν6(t2u), ν4(t1u) and v3(t1u) vibronic modes, respectively, under blue-light excitation (λex = 460 nm). The shape of the spectrum is characteristic of Mn4+ doped A2XF6 materials [23]. The emission intensity of KTFM samples increased gradually following the weight ratios of OA/SDS ~0.0, 2.0, 6.0 and 10.0. The KTFM nanosheet exhibited an excellent quantum yield (QY) of ~91.1%, which is much higher than that of KTFM without using surfactants ~63.1% and close to that of the KTFM micro-phosphor prepared via the cation exchange method ~93% [12,24].
Figure 5a shows the emission spectra of K2TiF6:Mn4+ nanosheets in the temperature range of 77 K–573 K upon 460 nm excitation. The emission peaks became broader and a slight red shift occurred within creasing temperature. The integrated intensity of anti-Stokes emission lines (Ia) gradually increased in temperature range of 77–450 K, whereas that of Stokes emission lines (IS) slight decreased. Subsequently, both emission lines degraded with further increasing temperature (>450 K), which demonstrated a good color quality of KTFM nanosheets at high temperature. The ratio of Ia/Is, increasing from ~0.09 at 77 K to ~0.578 at 523 K, shows a linear temperature dependence of red emission, as depicted in Figure 5b. The temperature-dependent performance of the integrated PL intensity presented in Figure 5c denotes considerable stability of KTFM nanosheets within the temperature range of 273–573 K. The integrated PL intensity of the sample started to drop at 423 K, and the quenching temperature T1/2 reached 500 K; this thermal stability is as good as that of the KTFM thin phosphor [19]. The decrease in the integrated PL intensity is attributed to the temperature-induced carriers escaping from the emission centers leading to a nonradiative recombination. Non-radiative transition probability increased with temperature, and the integrated PL intensity exhibited thermal quenching, which can be described by using the follow in gequation:
I ( T ) = I 0 1 + A . e E a k B T  
where I0 is the initial intensity at 298 K, I(T) is the emission intensity at temperature T, A is a constant, k is the Boltzmann constant and Ea is the thermal activation energy. The Ea value obtained for KTFM nanosheets ~1.09 eV is considerably higher than that of the KTFM micro-phosphor (~0.34 eV) [25]. Figure 5d presents the changes in the International Commission on Illumination (CIE) chromaticity coordinates of the KTFM nanosheets at different temperatures. At 298 K, the CIE coordinates of KTFM nanosheets was (0.7140, 0.2836) showing a deep-red emission compared to the currently reported Mn4+ doped fluorides with chromaticity coordinate (0.660–0.688, 0.305–0.337) [26]. When temperature increased from 298 K to 523 K, the CIE coordinates slightly shifted in the red region from (0.7140, 0.2836) to (0.6690, 0.3248).
The EL spectra of the nanowire WLED without using nanosheet KTFM red phosphor and the nanowire pc-WLEDs with KTFM red phosphor are presented in Figure 6. As illustrated in Figure 6a, three dominant peaks at ~440 nm, 525 nm and 610 nm are clearly presented corresponding to the blue, green and red emissions from the InGaN/AlGaN active regions. The nanowire WLED exhibits strong white-light emission with CRI of ~85. The inset figure shows the optical image of the nanowire WLED under 20 mA injection current. Figure 6b reveals the EL spectrum of the nanowire pc-WLED with a driving current of 20 mA. The sharp emission lines of Mn4+ in the K2TiF6 lattice were observed in the EL spectrum. The excellent CRI values, i.e., Ra ~96.4 and the corresponding corelated color temperature (CCT) ~4450 K were recorded. The bright warm white-light emissions of nanowire pc-WLEDs are shown in the inserted picture of Figure 6b. Moreover, the nanowire pc-WLED exhibits superior color quality with strong and stable white-light emission, which was recorded for injection current in the range of 20–100 mA, as shown in Figure 6c. The chromaticity coordinates are almost invariant, which are x ~ 0.3476–0.3481 and y ~ 0.2778–0.2782, as illustrated in Figure 6d. The related CCT shows a negligible variation which is in the range of 4249–4450 K. The stable white-light emission from the nanowire pc-WLEDs is attributed to the reduced quantum confined Stark effect in the high quality InGaN/AlGaN nanowire heterostructure combining with the high efficiency and thermal stability nanosheet KTFM red phosphor. The results suggest that KTFM nanosheet is a promising candidate for improving the color reproducibility of micro-WLEDs and current commercial WLEDs.

4. Conclusions

In summary, high efficiency K2TiF6:Mn4+ nanosheets were synthesized via the emulsification method using sodium dodecyl sulphonate and oleic acid surfactants. The prepared K2TiF6:Mn4+ exhibited strong and stable red emission with high quantum yield ~91%. Moreover, the K2TiF6:Mn4+ nanosheets shows a high color quality and low thermal quenching with the relative luminescent intensity of ~100% at 423 K. We further demonstrated that, with an integration of such a KTFM nanosheet, the InGaN/AlGaN nanowire WLEDs could achieve an unprecedentedly high CRI ~96.4 and CCT ~4450 K, as recorded. The present study demonstrates that KTFM nanosheet is a promising red component for mini/micro display technologies.

Author Contributions

Conceptualization, H.-D.N.; methodology, H.P.T.N. and H.-D.N.; software, T.H.Q.V. and H.-D.N.; validation, H.P.T.N., T.C.T.P. and H.-D.N.; formal analysis, T.H.Q.V., T.T.D., B.J., R.T.V. and H.-D.N.; investigation, T.H.Q.V., T.T.D., B.J. and R.T.V.; resources, H.P.T.N. and H.-D.N.; data curation, T.H.Q.V., T.T.D., H.P.T.N. and H.-D.N.; writing—original draft preparation, H.P.T.N. and H.-D.N.; writing—review and editing, T.H.Q.V., T.T.D., B.J., R.T.V., T.C.T.P., H.P.T.N. and H.-D.N.; visualization, H.P.T.N. and H.-D.N.; supervision, H.P.T.N. and H.-D.N.; project administration, H.-D.N.; funding acquisition, H.-D.N. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Ho Chi Minh City Department of Science and Technology (HCMC DOST), grant number 113/2019/HĐ-QPTKHCN.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Smet, P.F.; Parmentier, A.B.; Poelman, D. Selecting conversion phosphors for white light-emitting diodes. J. Electrochem. Soc. 2011, 158, R37–R54. [Google Scholar] [CrossRef] [Green Version]
  2. Jiang, S.; Yamamoto, H.; Digonnet, M.J.F.; Glesener, J.W.; Dries, J.C. White LED Phosphors: The Next Step. In Optical Components and Materials VII, Proceedings of the SPIE OPTO, San Francisco, CA, USA, 23–28 January 2010; SPIE: Bellingham, WA, USA, 2010; Volume 7598, pp. 759808–759817. [Google Scholar]
  3. Schubert, E.F.; Kim, J.K. Solid-state light sources getting smart. Science 2005, 308, 1274–1278. [Google Scholar] [CrossRef] [PubMed]
  4. Guo, W.; Banerjee, A.; Bhattacharya, P.; Ooi, B.S. InGaN/GaN disk-in-nanowire white light emitting diodes on (001) silicon. Appl. Phys. Lett. 2011, 98, 193102. [Google Scholar] [CrossRef] [Green Version]
  5. Guo, W.; Zhang, M.; Banerjee, A.; Bhattacharya, P. Catalyst-Free InGaN/GaN Nanowire Light Emitting Diodes Grown on (001) Silicon by Molecular Beam Epitaxy. Nano Lett. 2010, 10, 3355–3359. [Google Scholar] [CrossRef] [PubMed]
  6. Nguyen, H.P.T.; Zhang, S.; Cui, K.; Han, X.; Fathololoumi, S.; Couillard, M.; Botton, G.A.; Mi, Z. p-Type modulation doped InGaN/GaN dot-in-a-wire white-light-emitting diodes monolithically grown on Si (111). Nano Lett. 2011, 11, 1919–1924. [Google Scholar] [CrossRef] [PubMed]
  7. Nguyen, H.P.T.; Zhang, S.; Connie, A.T.; Kibria, M.G.; Wang, Q.; Shih, I.; Mi, Z. Breaking the carrier injection bottleneck of phosphor-free nanowire white light-emitting diodes. Nano Lett. 2013, 13, 5437–5442. [Google Scholar] [CrossRef]
  8. Zhao, C.; Ng, T.K.; Prabaswara, A.; Conroy, M.; Jahangir, S.; Frost, T.; O’Connell, J.; Holmes, J.D.; Parbrook, P.J.; Bhattacharya, P.; et al. An enhanced surface passivation effect in InGaN/GaN disk-in-nanowire light emitting diodes for mitigating Shockley–Read–Hall recombination. Nanoscale 2015, 7, 16658–16665. [Google Scholar] [CrossRef] [Green Version]
  9. Philip, M.R.; Choudhary, D.D.; Djavid, M.; Bhuyian, M.N.; Piao, J.; Pham, T.T.; Misra, D.; Nguyen, H.P. Controlling color emission of InGaN/AlGaN nanowire light-emitting diodes grown by molecular beam epitaxy. J. Vac. Sci. Technol. B 2017, 35, 02B108. [Google Scholar] [CrossRef]
  10. Philip, M.R.; Choudhary, D.D.; Djavid, M.; Bhuyian, M.N.; Bui, T.H.Q.; Misra, D.; Khreishah, A.; Piao, J.; Nguyen, H.D.; Le, K.Q.; et al. Fabrication of phosphor-free III-nitride nanowire light-emitting diodes on metal substrates for flexible photonics. ACS Omega 2017, 2, 5708–5714. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  11. Nguyen, H.-D.; Liu, R.-S. Narrow-band red-emitting Mn4+-doped hexafluoride phosphors: Synthesis, optoelectronic properties, and applications in white light-emitting diodes. J. Mater. Chem. C 2016, 4, 10759–10775. [Google Scholar] [CrossRef]
  12. Zhu, H.; Lin, C.C.; Luo, W.; Shu, S.; Liu, Z.; Liu, Y.; Kong, J.; Ma, E.; Cao, Y.; Liu, R.S.; et al. Highly efficient non-rare-earth red emitting phosphor for warm white light-emitting diodes. Nat. Commun. 2014, 5, 1–10. [Google Scholar] [CrossRef] [Green Version]
  13. Fang, M.-H.; Hsu, C.-S.; Su, C.; Liu, W.; Wang, Y.-H.; Liu, R.-S. Integrated surface modification to enhance the luminescence properties of K2TiF6: Mn4+ phosphor and its application in white-light-emitting diodes. ACS Appl. Mater. Interfaces 2018, 10, 29233–29237. [Google Scholar] [CrossRef]
  14. Zhou, Y.-Y.; Song, E.-H.; Deng, T.-T.; Zhang, Q.-Y. Waterproof narrow-band fluoride red phosphor K2TiF6: Mn4+ via facile superhydrophobic surface modification. ACS Appl. Mater. Interfaces 2018, 10, 880–889. [Google Scholar] [CrossRef]
  15. Khan, I.; Saeed, K.; Khan, I. Nanoparticles: Properties, applications and toxicities. Arabian J. Chem. 2019, 12, 908–931. [Google Scholar] [CrossRef]
  16. Malkiel, I.; Mrejen, M.; Nagler, A.; Arieli, U.; Wolf, L.; Suchowski, H. Plasmonic nanostructure design and characterization via deep learning. Light Sci. Appl. 2018, 7, 1–8. [Google Scholar] [CrossRef]
  17. Flory, F.; Escoubas, L.; Berginc, G. Optical properties of nanostructured materials: A review. J. Nanophotonics 2011, 5, 052502. [Google Scholar] [CrossRef] [Green Version]
  18. Tuyet, D.T.; Quan, V.T.H.; Bondzior, B.; Dereń, P.J.; Velpula, R.T.; Nguyen, H.P.T.; Tuyen, L.A.; Hung, N.Q.; Nguyen, H.D. Deep red fluoride dots-in-nanoparticles for high color quality micro white light-emitting diodes. Opt. Express 2020, 28, 26189–26199. [Google Scholar] [CrossRef] [PubMed]
  19. Zhou, W.; Wang, R.H.; Yin, L.; Chen, J.; Su, C.; Xing, X.; Liu, R.S. Alcohol-guided growth of two-dimensional narrow-band red-emitting K2TiF6: Mn4+ for white-light-emitting diodes. ACS Appl. Mater. Interfaces 2019, 11, 20143–20149. [Google Scholar] [CrossRef]
  20. Nguyen, H.P.T.; Cui, K.; Zhang, S.; Fathololoumi, S.; Mi, Z. Full-color InGaN/GaN dot-in-a-wire light emitting diodes on silicon. Nanotechnology 2011, 22, 445202. [Google Scholar] [CrossRef]
  21. Philip, M.R.; Choudhary, D.D.; Djavid, M.; Le, K.Q.; Piao, J.; Nguyen, H.P.T. High efficiency green/yellow and red InGaN/AlGaN nanowire light-emitting diodes grown by molecular beam epitaxy. J. Sci. Adv. Mater. Devices 2017, 2, 150–155. [Google Scholar] [CrossRef]
  22. Wu, S.; Liu, Y.; Chang, J.; Zhang, S. Ligand dynamic effect on phase and morphology control of hexagonal NaYF4. CrystEngComm 2014, 16, 4472–4477. [Google Scholar] [CrossRef]
  23. Chen, D.; Zhou, Y.; Zhong, J. A review on Mn4+ activators in solids for warm white light-emitting diodes. RSC Adv. 2016, 6, 86285–86296. [Google Scholar] [CrossRef]
  24. Wang, T.; Gao, Y.; Chen, Z.; Huang, Q.; Song, B.; Huang, Y.; Liao, S.; Zhang, H. Cation exchange synthesis and cations doped effects of red-emitting phosphors K2TiF6: Mn4+, M2+ (M= Mg, Ca, Sr, Ba, and Zn). J. Mater. Sci. Mater. Electron. 2017, 28, 11878–11885. [Google Scholar] [CrossRef]
  25. Han, T.; Lang, T.; Wang, J.; Tu, M.; Peng, L. Large micro-sized K2TiF6: Mn4+ red phosphors synthesised by a simple reduction reaction for high colour-rendering white light-emitting diodes. RSC Adv. 2015, 5, 100054–100059. [Google Scholar] [CrossRef]
  26. Lin, C.C.; Meijerink, A.; Liu, R.-S. Critical red components for next-generation white LEDs. J. Phys. Chem. Lett. 2016, 7, 495–503. [Google Scholar] [CrossRef] [PubMed]
Figure 1. (a) XRD patterns of KTFM prepared with various OA/SDS weight ratios of (α) 0.0, (β) 2.0, (γ) 6.0 and (δ) 10.0. (b) Picture of K2TiF6 structure viewed along the [100] direction.
Figure 1. (a) XRD patterns of KTFM prepared with various OA/SDS weight ratios of (α) 0.0, (β) 2.0, (γ) 6.0 and (δ) 10.0. (b) Picture of K2TiF6 structure viewed along the [100] direction.
Micromachines 12 00965 g001
Figure 2. SEM images of KTFM prepared with different OA/SDS weight ratios of (a) 0.0, (b) 2.0, (c) 6.0 and (d) ~10.0. (e) TEM image and (f) HRTEM image of KTFM nanosheets. Inserted picture shows SAED pattern of KTFM nanosheets.
Figure 2. SEM images of KTFM prepared with different OA/SDS weight ratios of (a) 0.0, (b) 2.0, (c) 6.0 and (d) ~10.0. (e) TEM image and (f) HRTEM image of KTFM nanosheets. Inserted picture shows SAED pattern of KTFM nanosheets.
Micromachines 12 00965 g002
Figure 3. SEM images of the (a) top-view and (b) 45° tilted angle of a typical InGaN/AlGaN nanowire WLED. (c) Schematic illustration of the nanowire-WLED device with anode and cathode electrodes. The schematic structure of a single nanowire WLED is also presented. (d) SEM images of the nanowire WLEDs with KTFM nanophosphor layer. The inserted picture shows the electrode layer on the top of the nanowire WLED.
Figure 3. SEM images of the (a) top-view and (b) 45° tilted angle of a typical InGaN/AlGaN nanowire WLED. (c) Schematic illustration of the nanowire-WLED device with anode and cathode electrodes. The schematic structure of a single nanowire WLED is also presented. (d) SEM images of the nanowire WLEDs with KTFM nanophosphor layer. The inserted picture shows the electrode layer on the top of the nanowire WLED.
Micromachines 12 00965 g003
Figure 4. (a) PLE spectra and (b) PL spectra of KTFM prepared with various OA/SDS ratios of (α) 0.0, (β) 2.0, (γ) 6.0 and (δ) 10.0.
Figure 4. (a) PLE spectra and (b) PL spectra of KTFM prepared with various OA/SDS ratios of (α) 0.0, (β) 2.0, (γ) 6.0 and (δ) 10.0.
Micromachines 12 00965 g004
Figure 5. (a) Temperature-dependent PL spectra of the KTFM nanosheets in the range of 77 K–523K. (b)The integrated intensity of anti-Stokes and Stokes emission lines. (c) The relative red PL intensity as a function of temperature (273 K–573 K). The solid line represents the fitting result with the expression IT/I0 = [1 + D exp(−Ea/kBT)]−1. (d) CIE chromaticity coordinates (x, y) shift from 298 K to 523 K of KTFM nanosheets.
Figure 5. (a) Temperature-dependent PL spectra of the KTFM nanosheets in the range of 77 K–523K. (b)The integrated intensity of anti-Stokes and Stokes emission lines. (c) The relative red PL intensity as a function of temperature (273 K–573 K). The solid line represents the fitting result with the expression IT/I0 = [1 + D exp(−Ea/kBT)]−1. (d) CIE chromaticity coordinates (x, y) shift from 298 K to 523 K of KTFM nanosheets.
Micromachines 12 00965 g005
Figure 6. (a) Electroluminescence spectrum of the nanowire WLED without nanosheet KTFM red phosphor. The inset is the optical image of white-light emission from the nanowire WLED. (b) Electroluminescence spectrum of the nanowire pc-WLED showing clear red emission from the KTFM nanosheets. The inserted pictures show bright warm-white light emissions of the nanowire pc-WLEDs. (c) Electroluminescence spectra of the nanowire pc-WLED under injection current from 20–100 mA. (d) The chromaticity coordinate in Commission Internationale de IʹÉclairage (CIE) 1931 color spaces of the nanowire pc-WLED.
Figure 6. (a) Electroluminescence spectrum of the nanowire WLED without nanosheet KTFM red phosphor. The inset is the optical image of white-light emission from the nanowire WLED. (b) Electroluminescence spectrum of the nanowire pc-WLED showing clear red emission from the KTFM nanosheets. The inserted pictures show bright warm-white light emissions of the nanowire pc-WLEDs. (c) Electroluminescence spectra of the nanowire pc-WLED under injection current from 20–100 mA. (d) The chromaticity coordinate in Commission Internationale de IʹÉclairage (CIE) 1931 color spaces of the nanowire pc-WLED.
Micromachines 12 00965 g006
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Vu, T.H.Q.; Doan, T.T.; Jain, B.; Velpula, R.T.; Pham, T.C.T.; Nguyen, H.P.T.; Nguyen, H.-D. Improving Color Quality of Nanowire White Light-Emitting Diodes with Mn4+ Doped Fluoride Nanosheets. Micromachines 2021, 12, 965. https://doi.org/10.3390/mi12080965

AMA Style

Vu THQ, Doan TT, Jain B, Velpula RT, Pham TCT, Nguyen HPT, Nguyen H-D. Improving Color Quality of Nanowire White Light-Emitting Diodes with Mn4+ Doped Fluoride Nanosheets. Micromachines. 2021; 12(8):965. https://doi.org/10.3390/mi12080965

Chicago/Turabian Style

Vu, Thi Hong Quan, Thi Tuyet Doan, Barsha Jain, Ravi Teja Velpula, Tung Cao Thanh Pham, Hieu Pham Trung Nguyen, and Hoang-Duy Nguyen. 2021. "Improving Color Quality of Nanowire White Light-Emitting Diodes with Mn4+ Doped Fluoride Nanosheets" Micromachines 12, no. 8: 965. https://doi.org/10.3390/mi12080965

APA Style

Vu, T. H. Q., Doan, T. T., Jain, B., Velpula, R. T., Pham, T. C. T., Nguyen, H. P. T., & Nguyen, H. -D. (2021). Improving Color Quality of Nanowire White Light-Emitting Diodes with Mn4+ Doped Fluoride Nanosheets. Micromachines, 12(8), 965. https://doi.org/10.3390/mi12080965

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop