1. Introduction
GaN/AlGaN ultraviolet (UV) photodetectors are highly regarded for their outstanding potential, characterized by their low dark current density and heightened sensitivity. Their capability has spurred extensive research into their applications, notably in missile detection, flame monitoring, and space communications [
1,
2,
3]. Historically, research has predominantly focused on photodetectors without internal gain, such as p-i-n, Schottky, and metal–semiconductor–metal (MSM) photodiodes [
4,
5,
6]. In contrast, although avalanche photodiodes (APDs) offer high quantum efficiency and inherent gain, they require high-voltage biases and are prone to noise due to avalanching [
7,
8,
9,
10].
Heterojunction phototransistors (HPTs) present a viable alternative, capable of achieving high current gain with substantially reduced noise compared to APDs, making them suitable candidates for sensitive GaN-based UV detection applications [
11]. Achieving high internal gain is critical for advanced UV photodetectors designed to detect low-intensity UV light signals. Consequently, precise engineering of the HPT base’s structural parameters is essential. While previous research has led to advancements in GaN/AlGaN-based HPTs, these studies often overlooked the optimization of the HPT base design [
12,
13,
14,
15]. Although L. Sun et al. reported improved performance of an AlGaN HPT with a polarization-doped p-base structure, the underlying mechanism remains unclear, necessitating further systematic research [
16].
This paper addresses this research gap by exploring the fabrication and performance analysis of GaN/AlGaN HPTs featuring both a compositionally graded base and a doping-graded base, comparing their efficacy to conventional GaN bases. Both grading approaches are theorized to create a built-in electric field, which facilitates electron transport across the base, thereby reducing base recombination current and significantly boosting common emitter current gain. These modifications are anticipated to substantially enhance the performance of GaN/AlGaN HPTs. Through detailed theoretical analysis and experimental validations, this study aims to elucidate the beneficial impacts of graded base designs, thereby advancing our understanding and application of these devices in high-sensitivity UV detection scenarios.
3. Materials and Methods
Based on the theoretical calculations presented above, GaN/AlGaN visible-blind heterojunction phototransistors (HPTs) were fabricated and characterized, featuring a compositionally graded base (Structure A) and a doping-graded base (Structure B). A third structure (Structure C) with a normal base was also fabricated for comparative analysis. The samples utilized in this study were grown on
c-plane sapphire substrates using a low-pressure metal–organic chemical vapor deposition (MOCVD) system. Precursors included trimethyl-gallium (TMGa), trimethyl-aluminum (TMAl), trimethyl-indium (TMIn), and ammonia (NH
3), while bis-cyclopentadienyl-magnesium (Cp
2Mg) and silane (SiH
4) served as p- and n-type doping sources, respectively. General structural layouts for all samples are provided in
Table 1.
For each sample, a 25 nm thick low-temperature GaN nucleation layer was initially deposited, followed by the high-temperature growth of a 1.5 μm thick unintentionally doped (uid) GaN buffer layer. Subsequently, a 1 μm thick n-type GaN layer (with an electron concentration of approximately 3.5 × 10
18 cm
−3) was grown as the sub-collector and ohmic-contact layer, followed by a 200 nm thick uid GaN layer (
n ≈ 8 × 10
16 cm
−3) as the collector layer. For Structure A, a 100 nm thick p-type Mg:Al
xGa
1−xN layer (x = 0–0.15,
p ≈ 3.8 × 10
17 cm
−3) was subsequently deposited as the base. The reactor was then cooled to 550 °C in an NH
3 atmosphere for 30 min to reduce Mg atoms adhering to the chamber wall [
13]. A 50 nm thick uid Al
0.15Ga
0.85N layer (
n ≈ 8 × 10
16 cm
−3) was grown as the absorbing layer, followed by a 250 nm thick n-type Al
0.25Ga
0.75N layer (
n ≈ 2 × 10
18 cm
−3) as the collector contact/window layer. For Structure B, a 100 nm thick p-type Mg:GaN layer was deposited as the base, with the doping concentration gradually increasing and the hole concentration approximating 3.8 × 10
16–3.8 × 10
17 cm
−3. For Structure C, a 100 nm thick p-type Mg:GaN layer (
p ≈ 3.8 × 10
17 cm
−3) was subsequently deposited as the base. The reactor was then cooled to 550 °C in an NH
3 atmosphere for 30 min to minimize the Mg atoms’ memory effect. A 50 nm thick uid GaN layer (
n ≈ 8 × 10
16 cm
−3) was grown as the absorbing layer, followed by a 250 nm thick n-type Al
0.1Ga
0.9N layer (
n ≈ 2 × 10
18 cm
−3) as the collector contact/window layer. Although the device can be scaled to higher voltages by applying a thicker graded structure, this may introduce other issues, such as increased carrier recombination and electrical field non-uniformity, which can lower response speed and optical gain. Details of the layer structures for the three samples are also provided in
Table 1.
The uid GaN layer between the emitter and the base serves the purpose of preventing Mg atoms from compensating the emitter layer. This approach aims to enhance Mg redistribution at the base–emitter (B–E) junction, thereby improving the emitter injection efficiency. Simultaneously, the heterojunction formed as the emitter–base junction contributes to a larger built-in potential, facilitating higher injection efficiency and greater gain. It is noteworthy that the heterojunction in all three samples features an energy gap with a 0.1 difference in Al composition. Furthermore, two-dimensional electron gas (2DEG) may be generated in Structures B and C at the GaN/AlGaN interfaces. The lateral 2DEG can impact vertical current transport by enhancing electron mobility, forming high electron concentration channels, reducing interface scattering, and lowering noise levels. The high electron mobility of the 2DEG improves overall device conductivity, while the high-concentration electron channel leads to a more uniform and stable vertical current distribution.
The device fabrication commenced with mesa definition achieved through an inductively coupled plasma (ICP) etching process down to the sub-emitter layer, utilizing BCl
3/Cl
2 as gas sources. For the contact electrodes of the emitter and the collector, a Ti/Al/Ni/Au multilayer was formed via electron-beam evaporation. Subsequently, a rapid thermal annealing process was conducted at 830 °C for 30 s in a N
2 ambient environment, resulting in the formation of ring-shaped ohmic contacts. The fabricated HPTs are two-terminal devices with a floating base, featuring an active area diameter of 150 μm. A schematic diagram illustrating the complete device structure is presented in
Figure 1.
The carrier concentrations of the underlayers were determined using Hall measurements conducted on additional samples, where the growth process was interrupted after the underlayers. The structural properties of the as-grown Structures A, B, and C were investigated through high-resolution X-ray diffraction (HRXRD) measurements. Surface morphologies were characterized using a Bruker Dimension Edge atomic force microscope (AFM). Current–voltage (I–V) measurements, both with and without UV illumination, were conducted on the fabricated GaN/Al0.1Ga0.9N HPTs using a Keithley 4200-SCS semiconductor parameter analyzer. UV illumination was applied from the front side of the device, utilizing an UV lamp with a center wavelength of 357 nm. A UV-enhanced, calibrated Si detector was employed to measure the power density of the incident light. Each I–V curve was recorded after applying a reverse bias of 5 V to eliminate accumulated holes in the base region, which could otherwise lower the quasi-Fermi level and introduce additional gains during testing.
4. Results and Discussion
The full-widths at half-maximum (FWHMs) of the HRXRD (002)/(102) plane rocking curves of the GaN epilayers are 246.5/298.2, 230.1/280.4, and 228.2/280.5 arcsecs for Structures A, B, and C, respectively. These values correspond to a total threading dislocation density (TDD) of 4.72 × 10
8 cm
−2, 4.18 × 10
8 cm
−2, and 4.18 × 10
8 cm
−2, respectively [
17], indicating a high crystalline quality for all three samples. The crystal quality is comparable to those grown on patterned sapphire substrates (PSSs) [
18,
19,
20]. The TDDs are nearly identical for Structures B and C, while they are slightly larger in Structure A. This difference is attributed to newly generated dislocations caused by lattice mismatches, resulting from the higher Al composition in the base of Structure A.
Figure 2 depicts the surface morphology of the three samples measured by an AFM. Smooth surfaces with distinct atomic steps are evident in all samples. The root mean square (RMS) roughness, defined as the root mean square height difference of peaks and valleys on the surfaces, was measured to be 0.685 nm, 0.629 nm, and 0.522 nm, respectively. These values signify the high crystalline quality of the top AlGaN epilayers. Although the RMS values are similar, the morphological characteristics differ noticeably. Local clusters due to insufficient diffusion of Al adatoms were observed in
Figure 2a, indicating degraded crystalline quality due to higher Al mole fractions in Structure A. The mono-atomic steps tend to bunch, and the step edges become blurry in
Figure 2b, probably due to flow fluctuations during the growth of the graded layer. Consequently, shifting from a uniform GaN layer to graded structures in the base may slightly degrade the surface morphology. However, whether this trade-off is worthwhile depends on the device’s performance.
Figure 3 displays the dark current and photocurrent versus the collector–emitter voltage (V
CE) for the three samples, while
Figure 4 provides a comparison of the dark and illuminated current in these samples. In
Figure 4a, all samples exhibit typical output characteristics of a bipolar transistor under dark conditions, with an offset voltage ranging from 1.8 to 2.0 V. For V
CE values below 2 V, the measured dark collector current (I
Cdark) remains less than 10 pA. As the V
CE increases, the I
Cdark exhibits a linear and rapid rise, reaching 0.6 μA, 0.5 μA, and 0.4 μA for Structures A, B, and C, respectively. Subsequently, it approaches saturation more gradually after the V
CE exceeds 4.5 V, attributed to the reduction in neutral base width and the subsequent increase in static common emitter current gain with the V
CE. It is evident that Structure A exhibits a higher dark current, possibly stemming from the compositionally graded base and high TDDs caused by lattice mismatches. Notably, the dark current of Structure C is at least an order of magnitude lower than that of the other two structures.
Figure 4b highlights noticeable differences in illuminated current among the three samples. With an increase in the V
CE, the illuminated current rises rapidly up to 4.71 × 10
−7 A, 7.08 × 10
−5 A, and 5.77 × 10
−4 A at V
CE = 1.2 V for Structures A, B, and C, respectively. Subsequently, it approaches saturation more gradually after the V
CE exceeds 2.0 V, attributed to the decrease in neutral base width and the subsequent increase in static common emitter current gain with the V
CE, which is consistent with the behavior observed in the dark current. Structure A, featuring an Al compositionally graded base, exhibits a more rapid increase and provides the highest illuminated current compared to Structure B with a doping-graded base. Conversely, Structure C, with a conventional base, displays the lowest illuminated current, aligning with the theoretical calculations.
With the assumption of 100% internal quantum efficiency, the current gain is defined as the ratio of charge carriers to the photon flux:
where
q is the electronic charge; Δ
IC (=
ICph −
ICdark) is the net collector photocurrent induced by current injection;
hv is the incident photon energy; and
Pin is the total incident current power [
21,
22]. The intensity of the input current power for all samples was consistent. Therefore, the gain varies directly with the Δ
IC:
While V
CE = 10 V, for a compositionally graded base, the current gain is improved compared to a GaN base by a factor of:
The experimental current gains of the HPTs with a compositionally graded base are observed to be higher than the theoretical calculations, primarily due to the following factors: In HPTs, incident photons are absorbed, generating electron–hole pairs. These charge carriers are separated by the electric field, drifting towards opposite sides of the junction. Photogenerated holes accumulate in the floating base region, leading to a reduction in the B–E built-in barrier. This barrier lowering facilitates a significant diffusion of electrons across the base to the collector, amplifying the primary photocurrent. For Structure A, under UV illumination with a dominant wavelength of 357 nm, most incident photons traverse the n-Al0.25Ga0.75N emitter–contact/window layer and p-AlxGa1−xN (x = 0–0.15) base layer. They are effectively absorbed in the depletion region of the reverse-biased base–collector junction, generating electron–hole pairs. The photogenerated electrons are efficiently swept to the collector by the strong electric field in the base–collector junction. Conversely, for Structure C, UV light is predominantly absorbed in the GaN layer before reaching the base–collector junction. The photogenerated holes and electrons are separated by the electric field in the emitter–base junction. However, the electric field in the forward-biased emitter–base junction is relatively weak, leading to the possible recombination of photogenerated holes and electrons before separation. This significantly decreases the quantum efficiency. The theoretical bandgap variation (ΔEg) of the base can theoretically range from 0 to 0.5 eV. However, an increase in the Al mole fraction of the AlxGa1−xN epilayers poses challenges in growing high-crystalline-quality epilayers due to the easier formation of dislocations and uncontrollable doping. Therefore, a tradeoff is necessary between the advantages of an increased built-in electrical field and the disadvantages of increased misfit and threading dislocations. ΔEg should be controlled within a reasonable range, and the recommended value of ΔEg in the HPT with a compositionally graded base is between 0.1 and 0.25 eV.
For a doping-graded base, while V
CE = 10 V, the current gain is improved compared to a GaN base by a factor of:
The experimental results for a doping-graded base surpass the theoretical calculations, possibly attributed to a reduced Mg memory effect in Structure B. The phenomenon where Cp
2Mg tends to be absorbed onto the reactor liners and walls after sources turn off results in the redistribution of Mg atoms in the emitter layer. The comparatively lower Mg concentration in the base of Structure B mitigates the Mg redistribution issue, enhancing emitter injection and consequently increasing the current gain [
13]. In a typical bipolar transistor, maintaining a high current gain necessitates the doping concentration in the base to be substantially lower than that in the emitter and higher than that in the collector. Consequently, the factor
in Equation (10) remains relatively unchanged, primarily limiting the effectiveness of a doping-graded base in enhancing current gain.
5. Conclusions
This investigation has focused on GaN/AlxGa1−xN-based HPTs featuring both a compositionally graded base and a doping-graded base. Theoretical analyses and empirical fabrications were conducted to evaluate the performance enhancements afforded by these designs. Relative to conventional GaN base structures, HPTs with a compositionally graded base exhibited substantial improvements in current gain, with theoretical predictions and experimental outcomes showing increases by factors of 12 and 27.9, respectively. The observed enhancement correlates with a controlled bandgap variation (ΔEg) of 0.15 eV within the graded Al composition of the base.
Additionally, HPTs with a doping-graded base demonstrated significant current gain enhancements, with theoretical and experimental increases by factors of 2 and 6.1, respectively. This improvement is directly linked to the variation in hole concentration, which spans from 3.8 × 1016 cm−3 at the base–emitter junction to 3.8 × 1017 cm−3 at the base–collector junction.
Collectively, the results affirm that both doping and compositional gradations within the base structure substantially elevate current gain, with the effects being more pronounced in the compositionally graded bases. These enhancements are principally attributed to the inherent built-in electric fields created by the graded structures. This study not only underscores the efficacy of graded base designs in boosting the performance of GaN/AlxGa1−xN HPTs but also contributes valuable insights into optimizing phototransistor designs for enhanced sensitivity and efficiency in UV detection applications.