BiOCOOH Microflowers Decorated with Ag/Ag2CrO4 Nanoparticles as Highly Efficient Photocatalyst for the Treatment of Toxic Wastewater
Next Article in Special Issue
The Catalytic Performance of Ni-Co/Beta Zeolite Catalysts in Fischer-Tropsch Synthesis
Previous Article in Journal
Promotional Effect of Cu, Fe and Pt on the Performance of Ni/Al2O3 in the Deoxygenation of Used Cooking Oil to Fuel-Like Hydrocarbons
Previous Article in Special Issue
Advanced Ga2O3/Lignin and ZrO2/Lignin Hybrid Microplatforms for Glucose Oxidase Immobilization: Evaluation of Biosensing Properties by Catalytic Glucose Oxidation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Active IrO2 and NiO Thin Films Prepared by Atomic Layer Deposition for Oxygen Evolution Reaction

1
Basic Research and Scanning, Research and Development Division, Industrie De Nora S.p.A., 20134 Milan, Italy
2
Department of Inorganic Technology, University of Chemistry and Technology, Technická 5, 166 28, Prague 6, Czech Republic
3
Department of Chemistry and Materials Science, School of Chemical Engineering, Aalto University, 02150 Espoo, Finland
*
Author to whom correspondence should be addressed.
Catalysts 2020, 10(1), 92; https://doi.org/10.3390/catal10010092
Submission received: 14 December 2019 / Revised: 3 January 2020 / Accepted: 6 January 2020 / Published: 8 January 2020

Abstract

:
Atomic layer deposition (ALD) is a special type of chemical vapor deposition (CVD) technique that can grow uniformed thin films on a substrate through alternate self-limiting surface reactions. Recently, the application of these thin film materials to catalytic systems has begun to attract much attention, and the capacity to deposit these catalytic films in a highly controlled manner continues to gain importance. In this study, IrO2 and NiO thin films (approximately 25 to 60 nm) were deposited on industrial Ni expanded mesh as an anode for alkaline water electrolysis. Different ALD operating parameters such as the total number of deposition cycles, sublimation and deposition temperatures, and precursors pulse and purge lengths were varied to determine their effects on the structure and the electrochemical performance of the thin film materials. Results from the electrochemical tests (6 M KOH, 80 °C, up to 10 kA/m2) showed the catalytic activity of the samples. Oxygen overpotential values (ηO2) were 20 to 60 mV lower than the bare Ni expanded mesh. In summary, the study has demonstrated the feasibility of using the ALD technique to deposit uniformed and electroactive thin films on industrial metallic substrates as anodes for alkaline water electrolysis.

1. Introduction

Current research trends focus on developing thin film materials, especially semi-conducting oxides, due to their wide number of technological applications such as in the field of optics, sensors, microelectronics, electrocatalysis, and energy production [1,2,3,4]. In addition, the rapid growth of industrial demand on reducing the materials’ cost leads to downscaling the amount of materials in terms of film thickness. Moreover, the application of these conformal thin film materials to catalytic systems has begun to attract much attention, and the capacity to deposit these thin catalytic films in a highly controlled manner continues to gain importance [5]. Atomic layer deposition (ALD), a special type of chemical vapor deposition (CVD) technique, is considered as one of the most attractive thin film deposition techniques where the conformality, uniformity, and thickness controllability of the films are crucial [6]. This technique relies on the successive, separated, and self-terminating gas–solid reactions of typical two gaseous reactants [7]. During the past decades, hundreds of materials have been explored and have been developed using this technique, and it has successfully demonstrated its importance in the thin film electroluminescent display production. However, the industrial use of this technique remained marginal for more than two decades [8].
In the industry, roll-to-roll and continuous ALD coating technology has been developed where the typical process conditions applied are 0.1 to 10 mbar or atmospheric pressure and a temperature range of 50 to 500 °C. Additionally, ALD is not limited to film deposition but can also be applied on particles and powders. Currently, the ALD process can be used to deposit a wide range of binary oxides, nitrides, carbides, metals, sulfides, fluorides, polymers, and mixed structures [9].
Looking at the side of energy production, hydrogen is one of the promising sustainable solutions for the energy problem. One of the most efficient ways of producing H2 at low cost and high purity is the electrochemical water splitting into hydrogen and oxygen. However, this process is still not optimal because of the sluggish kinetics of the anodic oxygen evolution reaction (OER) subsequently due to the well-known scaling relation restriction [10]. This eventually leads to the increase in the operating cell voltage for the electrolysis and to the challenges faced for the large-scale commercialization of the technology. A number of metal oxides have been tested as electrocatalysts, and nickel and noble metal oxides have shown suitable qualities as anode materials both in acidic and alkaline media [11]. Numerous studies [11,12,13] have already discussed the use of transition metal oxides as the most suitable OER electrode material. Furthermore, industries have strict requirements for an electrode material such as high surface area, high electrical conductivity, good weldability, good electrochemical activity (measured through the oxygen overpotential values) and stability over several years, low cost, and safe in terms of the environment, health, and safety (EHS).
In this work, iridium dioxide (IrO2) and nickel oxide (NiO) thin films were deposited on Ni expanded mesh suitable for industrial applications and on an Si (100) substrate, which served as a reference material. Then, thin films deposited on Ni-expanded meshes were applied as anodes for alkaline water electrolysis. The choice of these two materials comes from the need to demonstrate the electrochemical activity of thin films for what are known to be particularly active noble and non-noble metal oxides for oxygen evolution reaction. ALD operating parameters such as the total number of deposition cycles, deposition and sublimation temperatures, precursors pulse, and purge lengths were varied to determine their effect on the structure and electrochemical performance of the synthesized (thin film) material. The electrochemical tests done in this study are pushing the boundaries of the single electrode potential at the highest values of current densities so far reported in the literature. In addition, these tests were done to demonstrate the functionality of the anodes suitable to the industrial needs for the deployment of the next generation of alkaline water electrolysis for the stationary energy storage application. The samples were characterized using various structural and morphological characterization techniques: XRR (X-ray reflectivity), GIXRD (grazing-incidence X-ray diffraction), XRF (X-ray fluorescence), and SEM (scanning electron microscopy). The electrochemical activity, in terms of oxygen overpotential value, was measured using iR-SEP (iR-corrected single electrode potential) tests, where resistance measurements were done using EIS (electrochemical impedance spectroscopy).

2. Results

In the proceeding sections, synthesized thin film metal oxides are referred to as Samples A to D (for NiO samples) and Samples E to H (for IrO2 samples). The number that follows the letter refers to the pre-treatment method performed on the Ni expanded mesh substrates: 1—for sandblasted and acid etched; and 2—for not sandblasted but acid etched; otherwise stated, the substrate used is Si (100). All the Ni expanded meshes are proprietary of Industrie De Nora S.p.A. (Milan, Italy). For other details of the substrate pre-treatment, see Section 4.

2.1. Film Thickness and Catalyst Loading

The thickness of the films was measured, and the total catalyst loading was estimated by the change in the mass of the samples before and after the deposition. The film thickness of NiO was measured using XRR on the samples deposited on the Si (100) substrate. Moreover, for the more accurate film thickness of IrO2 samples, EDX results analyzed using a GMR electron probe thin film microanalysis program was used. This is also done to integrate various characterization techniques.
As discussed by Miikkulainen V. et al. [7], one deposition cycle consists typically of four steps: (1) Step 1a: gas–solid reaction (chemisorption reaction) of the first reactant (Reactant A), typically of a metal reactant; (2) Step 1b: purge or evacuation to remove the unreacted precursor and gaseous by-products; (3) Step 2a: second gas–solid reaction (chemisorption reaction) of the second reactant (Reactant B), typically of a non-metal reactant; and (4) Step 2b: purge or evacuation to remove the unreacted precursor and gaseous by-products.
Table 1 shows the calculated film thickness and metal loading of the samples at a different total number of deposition cycles (sum of cycles for the ‘front’ and ‘back’ side of the electrode). The ‘front’ side of the electrode is the side facing the top, while the ‘back’ is facing the bottom during the first half of the deposition cycle. For the second half of the deposition cycle, the electrode was turned over, making the ‘front’ side facing the bottom. NiO samples have approximately 26 to 59 nm thickness, while IrO2 samples have 49 to 59 nm film thickness.
It can be noted that for the IrO2 samples, only one deposition cycle set (2000 cycles) was performed in this work, which was based on the previously reported study [6]. However, for the NiO samples, a different total number of deposition cycles was studied, and Figure 1 shows the linear relation of the total number of deposition cycles on the film thickness and metal loading, as also observed by Hämäläinen J. et al. [6].
As mentioned earlier, one feature of the ALD technique is the uniformity of the films deposited. To verify this, SEM images on the IrO2 thin films on the sandblasted substrate are shown in Figure 2. It can be observed from these images that the deposited thin films appear to be uniformed over the whole surface irrespective of the substrate surface roughness or defects. This uniformed deposition offers more advantage than other deposition methods (i.e., evaporation) that usually leads to reduced coating thickness on the edges or other parts of the substrate and sometimes no coating at all.
Figure 3 shows the XRF results (in terms of iridium counts) on the IrO2 samples. This analysis was not possible for the NiO samples due to the limitation of the technique regarding distinguishing the Ni content from the coating itself and from the substrate. XRF analysis in this case was done as a rapid screening (semi-quantitative analysis) to determine if there is uniformity of the metal loading across the surface of the electrode. It can be observed that the samples with the not sandblasted Ni substrate have relatively lower (darker) iridium content than the samples with the sandblasted Ni substrate. These results illustrate the uniformity of the coating and are well in agreement with the SEM observations (Figure 2). In addition, the electrode has a front and back side, and both the sides are ALD-coated. Additionally, it can be noted that the amount of iridium is relatively the same for both the sides.

2.2. Sublimation and Deposition Temperature

Table 2 summarizes the different sublimation (Tsub) and deposition (Tdep) temperatures studied in this work. For the NiO samples, Tsub was varied from 110 to 120 °C, and Tdep was maintained the same at 200 °C. Hagen et al. [14] reported that this deposition temperature is well above the vaporization temperatures and below the decomposition temperatures of the precursors. While for the IrO2 samples, Tsub was varied from 150 to 155 °C and Tdep was varied from 205 to 210 °C. The sublimation and deposition temperatures were chosen as low as reasonably possible to study the low-temperature growth of the films required. The nickel substrates have a maximum temperature limit of 500 °C (atmospheric conditions) in which nickel starts to be oxidized, thus changing its properties and especially mechanical properties.
It can be seen from the GIXRD patterns in Figure 4 that all of the as-deposited thin films were crystalline. Cubic NiO (JCPDS No. 01-073-1519) is the crystalline species detected from the NiO samples, while tetragonal IrO2 (JCPDS No. 01-088-0288) and cubic Ir (JCPDS No. 03-065-1686) are the crystalline species detected on the IrO2 samples. Generally, from the GIXRD patterns, the crystallinity of the materials was not significantly affected by the change in the sublimation and deposition temperature. In particular, IrO2-F shows an increased intensity of metallic Ir (111) on the GIXRD patterns compared to the other samples.
The growth rates per cycle of the films (Å/cycle) are calculated from the film thickness and presented in Table 2. The growth rate of the NiO films deposited at 200 °C is 0.2 Å/cycle, which is similar to the results reported by Hagen et al. [14]. Meanwhile, it can be noted that the IrO2 growth rate increases with increasing deposition temperature up to 0.6 Å/cycle at 210 °C.

2.3. Precursors Pulse and Purge Length

The precursors (Reactant A) used in this study were Ni-bis-2,2,6,6-tetramethyl-heptane-3,5-dionate (Ni(tmhd)2) for NiO and iridium (III) acetylacetonate (Ir(acac)3) for IrO2. These precursors were placed in open glass boats within the reactor, and N2 was used as a carrier and purging gas. Ozone (O3) was used as the oxygen source (Reactant B), which was supplied by the ozone generator near the ALD reactor (see more details in the Materials and Methods section). As mentioned in the previous section, one ALD reaction cycle consists of four steps that involve Reactant A and B pulse and purging.
The length for the precursor pulses and the inert gas purges needs to be optimized to avoid either too long processes or uneven films. Table 3 summarizes the pulse and purge rates of Reactant A and Reactant B used in this study.
The growth behavior can be analyzed from the relationship of the pulse length versus growth per cycle (GPC). For the NiO samples, the same precursor pulse and purge rates were applied according to the study previously reported by Hagen et al. [14]. When NiO films were grown using a precursor pulse length of 2.5 s, a similar GPC value of about 0.2 Å per cycle (Table 2) was measured. Therefore, these conditions were chosen for this study. While for IrO2 films, Hämäläinen et al. [6] reported that a constant growth rate of about 0.4 Å/cycle is achieved with 0.5 s and longer Ir(acac)3 pulse lengths. The effect of ozone pulse length on the growth rate is that the growth rate saturates to 0.4 Å/cycle when 0.5 s and longer pulses of ozone are used. Therefore, good saturation with respect to both the precursors has been obtained as a characteristic of ALD for all the depositions of this study.

2.4. Electrochemical Characterization

In order to evaluate the electrochemical activity of the synthesized thin film electrodes, chronopotentiometry steps (1 to 10 kA/m2) in a three-electrode glass electrochemical cell were performed, and the iR-corrected single electrode potential (iR-SEP) was measured. All the measurements were done in 6 M KOH, 80 °C, and continuous agitation. The polarization curves shown in Figure 5 and Figure 6 were iR-corrected and calibrated against a reversible hydrogen electrode (RHE).
The polarization curve of the uncoated Ni expanded mesh (black square) is also included in Figure 5 and Figure 6 to determine the voltage advantage in terms of mV-gain for all the thin film electrodes synthesized. Since for the industrial application, it is necessary to run the electrolysis system at the lowest power consumption as possible and given that the next generation alkaline water electrolysis will operate at current loads around 1000 mA/cm2 (10 kA/m2), the focus of this study is to compare the oxygen overvoltage (ηO2) at such high current density. From the graphs, it can be seen that for the NiO samples, the oxygen overpotential (ηO2) values at 10 kA/m2 are approximately 10 to 50 mV lower than those of the bare Ni substrate. While for the IrO2 samples, ηO2 values at 10 kA/m2 are approximately 25 to 55 mV lower than those of the bare Ni substrate. Table 4 and Figure 7 summarize the ηO2 values at 10 kA/m2 for each thin film electrode. The Tafel slope of the thin film electrodes ranges from 42 to 70 mV/dec for the NiO samples and 45 to 60 mV/dec for the IrO2 samples (see Section 3 for more details).
For NiO thin film electrodes, it can be observed from Figure 7 that samples with not sandblasted but acid etched Ni substrate have lower ηO2 values than those of the samples with the sandblasted and acid etched Ni substrate. However, the opposite trend can be observed from the IrO2 samples. Table 4 summarizes the oxygen overpotential values at 10 kA/m2 and the Tafel slope of each electrode material.

3. Discussion

As can be noted from the presented results, this study did not focus on the optimization of the ALD parameters, since these were already presented by Hagen et al. [14] for NiO thin films and by Hämäläinen et al. [6] for IrO2 thin films. However, both the previous and current studies were able to show that thermal ALD can be employed for NiO and IrO2 thin film deposition between the temperature range of 200 and 210 °C. These deposition temperatures were chosen to allow future studies where the co-deposition of IrO2 and NiO can be done simultaneously, leading to a mixed oxide structure.
The film thickness depended linearly on the number of deposition cycles applied (shown in Figure 1). Additionally, this study was able to show the uniformity of the thin films deposited based on different characterization techniques (SEM and XRF). From the XRF results, the front and back side of the electrode has relatively the same amount of iridium, which signifies the uniformity of the coating. Moreover, based on the GIXRD analysis, all the as-deposited thin films were crystalline. Other important ALD parameters are the pulse and purge rates of the precursors. It can be seen from the results that full saturation was achieved because of the application of the same operating conditions from the previous study and the use of small substrates. However, for an industrial-scale setup, this would not be the same case. The larger surface area of the substrates would require longer pulse and purge times to achieve full saturation. The problem can also be addressed through the application of batch processes where multiple batches of the substrates will be deposited simultaneously [15]. In addition to the industrial scale-up of the process, there are some severe drawbacks of the technique, such as (a) the need of high-purity precursors that are not always commercially available; (b) the slow deposition rate, which is approximately 24 h total deposition time for the film described in this study; (c) the precursors are often sensitive to air/oxygen; and (d) expensive instruments. Nevertheless, a current industrial ALD instrument can treat substrates with a maximum dimension of 1 m2. Finding the most suitable vacuum chamber for the deposition would be the major challenge to demonstrate the possible industrialization of the technique.
The focus of the study is the electrochemical application of these thin films as electrodes. Depositing uniformly such a small amount of materials (less than 1 g/m2 of metal) is a huge advantage for industrial scale electrochemistry, especially when a noble metal will be employed. Moreover, it has been proven that the small amount of materials deposited on the substrate resulted in electrochemically active materials for OER at strict industrial conditions (6 M KOH, 80 °C, up to 10 kA/m2). Oxygen overpotential (ηO2) values at 10 kA/m2 are approximately 10 to 50 mV lower than the bare Ni substrate for the NiO thin films, while they are 25 to 55 mV lower than the bare Ni substrate for the IrO2 thin films. These values correspond to energy savings in the industry especially when compared to the cost of materials employed. Comparing the ηO2 values of the NiO and IrO2 thin film electrodes, it can be seen that the IrO2 samples offered relatively higher mV saving than the NiO samples. For further study, the stability and lifetime of these electrodes should be explored.
One of the key points in this study that was not previously discussed deeply is the substrate pre-treatment. Two types of pre-treatment are applied on the Ni expanded meshes; one involves both sandblasting and acid etching, while the other involves only acid etching. Although both types of the pre-treatment method aim to increase the substrate surface roughness that subsequently improves the adhesion of the film, there are some differences in the characteristics of the materials. First, from the XRF analysis of the IrO2 samples (Figure 3), it can be observed that thin films deposited on the not sandblasted Ni substrate have relatively lower (darker) iridium content compared to the thin films deposited on the sandblasted Ni substrate. Then, this observation translates to the lower electrochemical performance of the samples with the not sandblasted Ni substrate (Figure 7) compared to the ones with the sandblasted Ni substrate. However, the trend is the opposite for the NiO thin films, but these results agree with those previously reported study by Bocca et al. [16]. Due to the limitations of the characterization techniques available, it is not possible to quantify the actual amount of Ni deposited on the substrate, but this could be more explored for further study.
Another observation is the relatively lower ηO2 value of IrO2-F among the set of IrO2 thin films. This could be due to the presence of more crystalline metallic Ir, as can be seen from the GIXRD patterns (Figure 4b). The XRF results also agree with this observation, as IrO2-F has relatively more Ir content among all the IrO2 samples. In addition to this, among the set of samples, NiO-A exhibits the highest ηO2 value due to the low metal loading as well as low film thickness. Moreover, only one side of the substrate has been coated for these samples, which corresponds to approximately half of the total thickness of the other samples.
Figure 5 and Figure 6 shows the polarization curves (Tafel plots) of the thin film electrodes, and Table 4 summarizes the values of the Tafel slope. All the polarization curves of NiO and IrO2 are shifted toward lower potentials compared to those of the bare Ni substrate, which leads to the lower ηO2 values at 10 kA/m2. Additionally, the polarization curves display steeper slopes (lower Tafel slope—except NiO-A) than that of the bare Ni substrate. The Tafel slope values are relatively similar ranging between 42 and 60 mV/dec, suggesting that the OER that takes place has the same reaction mechanism and fast reaction kinetics during the OER.
In summary, the study has demonstrated the feasibility of using the ALD technique to deposit conformal, uniform, and electroactive thin films on an industrially relevant metallic substrate as an anode for alkaline water electrolysis, which could be a source of hydrogen and is one of the promising sustainable solutions for the energy problem.

4. Materials and Methods

4.1. Materials Synthesis and ALD Coating Technique

Iridium and nickel oxide thin films were deposited in an ASM-Microchemistry F-120 flow-type reactor, which was operated under a moderate vacuum of 1 to 3 mbar. The precursors, iridium (III) acetylacetonate (Ir(acac)3) and Ni-bis-2,2,6,6-tetramethyl-heptane-3,5-dionate (Ni(tmhd)2), were synthesized according to previously reported methods [17] and were purified by sublimation under vacuum before use. This type of precursor was used for the ALD process due to its relatively simplicity to synthesize, stability in air, and volatility at reasonable temperatures.
The precursors were placed in open glass boats within the reactor, and N2 was used as a carrier and purging gas. The sublimation temperature for Ir(acac)3 is 155 °C, and that for Ni(tmhd)2 is 115 °C. Ozone was used as the oxygen source and supplied from a Fischer Model 502 generator. In this work, the term “number of cycles” refers to the total number of deposition cycles (front and back side of the electrode), which varied from 1500 to 3000 cycles. Thin films were grown on 2.5 × 5 cm Ni expanded mesh (pre-treated) and Si (100), which served as the reference material. The Ni expanded mesh substrates used are proprietary of Industrie De Nora S.p.A. (Milan, Italy), and the pre-treatment procedure details are not deeply discussed here. However, the pre-treatment involves increasing the substrate surface roughness (sandblasting and acid etching), which subsequently improves the adhesion of the film. Sandblasting was performed using the abrasive properties of silica sand. Acid etching was done at least 24 h before the deposition to avoid the passivation of nickel. The sublimation (Tsub) and deposition temperature (Tdep) range studied was the following: (a) IrO2: Tsub = 150 to 155 °C; Tdep = 205 to 210 °C; and (b) NiO: Tsub = 110 to 120 °C; Tdep = 220 °C. Pulses for both metal precursors were varied from 1 to 2.5 s. Each precursor pulse was then followed by a 1 to 4 s N2 purge, while O3 pulses were varied from 1 to 3 s and purge rates varied from 1 to 5 s.

4.2. Structural Characterization

The thickness of the films was determined by X-ray reflectivity (XRR) measurements using a Panalytical X’Pert Pro MPD diffractometer with Cu Kα radiation. The same instrument was also used for grazing-incidence X-ray diffraction (GIXRD) with an incidence angle of ω = 0.5°, a step size of 0.025°, and a time per step of 10 s for the identification of crystalline phases. Film morphology was studied with scanning electron microscopy (SEM, FEI Quanta 400 ESEM) and energy-dispersive X-ray spectroscopy (EDX). Then, the EDX results were analyzed using a GMR electron probe thin film microanalysis program [18] to estimate the film thickness for the IrO2 samples. The content of noble metals is determined using X-ray fluorescence (XRF) using a Niton Xlt 898 portable gun.

4.3. Electrochemical Characterization

To study the electrochemical activities of the thin film electrodes, the samples were characterized using chronopotentiometry steps (1 to 10 kA/m2) in a three-electrode glass electrochemical cell, and the iR-corrected single electrode potential (iR-SEP) was measured. The potential was controlled using Parstat 4000A and Versastat 3 potentiostats. Measurements were done in 6 M KOH, 80 °C, and continuous agitation.
All polarization curves were iR-corrected and were calibrated against a reversible hydrogen electrode (RHE). The current density was normalized to the geometrical surface area of the substrate. Measured potentials versus saturated calomel electrode (SCE) were converted to a reversible hydrogen electrode (RHE) scale by using the Nernst equation:
ERHE = ESCE + 0.0591 × pH + 0.241 − iR.
The resistance was determined through an electrochemical impedance spectroscopy (EIS) test and measurements were iR compensated by subtracting off the resistance multiplied by the current being drawn at each point.

5. Conclusions

Thin films (approximately 25 to 60 nm) of nickel and iridium oxide were deposited on industrial metallic (Ni) substrates using the atomic layer deposition technique. Characterization of the NiO and IrO2 thin films showed the formation of a uniform coating. The as-deposited crystalline thin films showed good activity for OER especially at strict industrial conditions (high temperature, high pH, and high current density). Further study could be focused on the determination of the electrochemical stability of the materials, since this is one of the major requirements for industrial electrodes. Additionally, examining the adhesion of the coating could be a good measure of the lifetime of these electrodes. Furthermore, creating mixed oxide thin film electrodes could also be explored, as this will reduce the amount of noble metals that will be used.
Thus, ALD can produce active NiO and IrO2 catalysts that can be deposited as uniformed thin film coatings over industrially relevant metallic substrates. This offers a lot of advantages in terms of less usage of noble metals due to the nanometer-range film thickness. Similarly, ALD may be explored to produce other active and catalytic materials, and this work suggests that the ALD-deposited materials will have similar activity to films produced through other techniques. Hence, from this work, a promising route to manufacture an active thin film for sustainable H2 production was reported.

Author Contributions

D.D.M. data curation, formal analysis, methodology, investigation, writing—original draft preparation, and conceptualization. D.S. methodology, investigation, writing—review and editing. E.I. and T.K. project administration, conceptualization, supervision, resources, writing—review and editing, funding acquisition. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded the European Commission within the framework of the Innovative Training Network Elcorel (Contract 722614).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Yu, X.; Marks, T.J.; Facchetti, A. Metal oxides for optoelectronic applications. Nat. Mater. 2016, 15, 383. [Google Scholar] [CrossRef] [PubMed]
  2. Ellmer, K. Past achievements and future challenges in the development of optically transparent electrodes. Nat. Photonics 2012, 6, 809. [Google Scholar] [CrossRef]
  3. Stadler, A. Transparent conducting oxides—An up-to-date overview. Materials 2012, 5, 661–683. [Google Scholar] [CrossRef] [PubMed]
  4. Mattinen, M.; Hämäläinen, J.; Gao, F.; Jalkanen, P.; Mizohata, K.; Raisanen, J.; Puurunen, R.L.; Ritala, M.; Leskelä, M. Nucleation and conformality of iridium and iridium oxide thin films grown by atomic layer deposition. Langmuir 2016, 32, 10559–10569. [Google Scholar] [CrossRef] [PubMed]
  5. Pickrahn, K.L.; Park, S.W.; Gorlin, Y.; Lee, H.B.R.; Jaramillo, T.F.; Bent, S.F. Active MnOx electrocatalysts prepared by atomic layer deposition for oxygen evolution and oxygen reduction reactions. Adv. Energy Mater. 2012, 2, 1269–1277. [Google Scholar] [CrossRef]
  6. Hämäläinen, J.; Kemell, M.; Munnik, F.; Kreissig, U.; Ritala, M.; Leskelä, M. Atomic layer deposition of iridium oxide thin films from Ir (acac) 3 and ozone. Chem. Mater. 2008, 20, 2903–2907. [Google Scholar] [CrossRef]
  7. Miikkulainen, V.; Leskelä, M.; Ritala, M.; Puurunen, R.L. Crystallinity of inorganic films grown by atomic layer deposition: Overview and general trends. J. Appl. Phys. 2013, 113, 2. [Google Scholar] [CrossRef]
  8. Ritala, M.; Niinistö, J. Industrial applications of atomic layer deposition. Ecs Trans. 2009, 25, 641–652. [Google Scholar]
  9. Atomic Layer Deposition. n.d. Available online: https://beneq.com/en/thin-films/technology/atomic-layer-deposition (accessed on 28 November 2019).
  10. Man, I.C.; Su, H.Y.; Calle-Vallejo, F.; Hansen, H.A.; Martínez, J.I.; Inoglu, N.G.; Kitchin, J.; Jaramillo, T.F.; Nørskov, J.K.; Rossmeisl, J. Universality in oxygen evolution electrocatalysis on oxide surfaces. ChemCatChem 2011, 3, 1159–1165. [Google Scholar] [CrossRef]
  11. Matsumoto, Y.; Sato, E. Electrocatalytic properties of transition metal oxides for oxygen evolution reaction. Mater. Chem. Phys. 1986, 14, 397–426. [Google Scholar] [CrossRef]
  12. Hong, W.T.; Risch, M.; Stoerzinger, K.A.; Grimaud, A.; Suntivich, J.; Shao-Horn, Y. Toward the rational design of non-precious transition metal oxides for oxygen electrocatalysis. Energy Environ. Sci. 2015, 8, 1404–1427. [Google Scholar] [CrossRef] [Green Version]
  13. Burke, M.S.; Enman, L.J.; Batchellor, A.S.; Zou, S.; Boettcher, S.W. Oxygen evolution reaction electrocatalysis on transition metal oxides and (oxy) hydroxides: Activity trends and design principles. Chem. Mater. 2015, 27, 7549–7558. [Google Scholar] [CrossRef]
  14. Hagen, D.J.; Tripathi, T.S.; Karppinen, M. Atomic layer deposition of nickel-cobalt spinel thin films. Dalton Trans. 2017, 46, 4796–4805. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  15. Ahvenniemi, E. Atomic Layer Deposition of Complex Thin Films. Ph.D. Thesis, Aalto University School of Chemical Technology, Helsinki, Finland, 2016. [Google Scholar]
  16. Bocca, C.; Barbucci, A.; Cerisola, G. The influence of surface finishing on the electrocatalytic properties of nickel for the oxygen evolution reaction (OER) in alkaline solution. Int. J. Hydrogen Energy 1998, 23, 247–252. [Google Scholar] [CrossRef]
  17. Hammond, G.S.; Nonhebel, D.C.; Wu, C.-H.S. Chelates of β-Diketones. V. Preparation and Properties of Chelates Containing Sterieally Hindered Ligands. Inorg. Chem. 1963, 2, 73–76. [Google Scholar] [CrossRef]
  18. Waldo, R.A. An iteration procedure to calculate film compositions and thicknesses in electron-probe microanalysis. In Proceedings of the 23rd Annual Conference of the Microbeam Analysis Society, Milwaukee, WI, USA, 8–12 August 1988; pp. 310–314. [Google Scholar]
Figure 1. Thickness of NiO on the Si (100) substrate as a function of the number of the deposition cycles. The precursors’ pulse and purge rates are the same. The film thickness was calculated using the X-ray reflectivity (XRR) technique. The Ni loading was calculated from the mass difference of the sample before and after the deposition.
Figure 1. Thickness of NiO on the Si (100) substrate as a function of the number of the deposition cycles. The precursors’ pulse and purge rates are the same. The film thickness was calculated using the X-ray reflectivity (XRR) technique. The Ni loading was calculated from the mass difference of the sample before and after the deposition.
Catalysts 10 00092 g001
Figure 2. SEM images (at 6000× magnification) of (a) the bare sandblasted Ni expanded mesh; (b) IrO2-E1; (c) IrO2-F1; (d) IrO2-G1; and (e) IrO2-H1.
Figure 2. SEM images (at 6000× magnification) of (a) the bare sandblasted Ni expanded mesh; (b) IrO2-E1; (c) IrO2-F1; (d) IrO2-G1; and (e) IrO2-H1.
Catalysts 10 00092 g002
Figure 3. X-ray fluorescence (XRF) mapping of the IrO2 samples in terms of iridium counts. Iridium counts range from 3 to 7. Darker shade means less iridium content.
Figure 3. X-ray fluorescence (XRF) mapping of the IrO2 samples in terms of iridium counts. Iridium counts range from 3 to 7. Darker shade means less iridium content.
Catalysts 10 00092 g003
Figure 4. GIXRD patterns of the NiO (Samples A to D) and IrO2 (Samples E to H) thin films on Si (100) substrate () with the following JCPDS No.: (a) ▼ cubic NiO (01-073-1519); and (b) ■ tetragonal IrO2 (01-088-0288) and ✕ cubic Ir (03-065-1686).
Figure 4. GIXRD patterns of the NiO (Samples A to D) and IrO2 (Samples E to H) thin films on Si (100) substrate () with the following JCPDS No.: (a) ▼ cubic NiO (01-073-1519); and (b) ■ tetragonal IrO2 (01-088-0288) and ✕ cubic Ir (03-065-1686).
Catalysts 10 00092 g004
Figure 5. Electrochemical oxygen evolution reaction (OER) polarization curves of the NiO thin film electrodes (Tafel plots). The number after the letter corresponds to the pre-treatment of the Ni expanded mesh substrates: 1—sandblasted and acid etched; 2—not sandblasted but acid etched. The symbol ■ corresponds to the bare/uncoated Ni expanded mesh.
Figure 5. Electrochemical oxygen evolution reaction (OER) polarization curves of the NiO thin film electrodes (Tafel plots). The number after the letter corresponds to the pre-treatment of the Ni expanded mesh substrates: 1—sandblasted and acid etched; 2—not sandblasted but acid etched. The symbol ■ corresponds to the bare/uncoated Ni expanded mesh.
Catalysts 10 00092 g005
Figure 6. Electrochemical oxygen evolution reaction (OER) polarization curves of the IrO2 thin film electrodes (Tafel plots). Number after the letter corresponds to the pre-treatment of the Ni expanded mesh substrates: 1—sandblasted and acid etched; 2—not sandblasted but acid etched. The symbol ■ corresponds to the bare/uncoated Ni expanded mesh.
Figure 6. Electrochemical oxygen evolution reaction (OER) polarization curves of the IrO2 thin film electrodes (Tafel plots). Number after the letter corresponds to the pre-treatment of the Ni expanded mesh substrates: 1—sandblasted and acid etched; 2—not sandblasted but acid etched. The symbol ■ corresponds to the bare/uncoated Ni expanded mesh.
Catalysts 10 00092 g006
Figure 7. Oxygen overpotential values (at 10 kA/m2) of the thin film electrodes. Left—sandblasted and acid etched; Right—not sandblasted but the acid etched Ni substrate.
Figure 7. Oxygen overpotential values (at 10 kA/m2) of the thin film electrodes. Left—sandblasted and acid etched; Right—not sandblasted but the acid etched Ni substrate.
Catalysts 10 00092 g007
Table 1. Film thickness and metal loading of the electrode materials.
Table 1. Film thickness and metal loading of the electrode materials.
Sample Total Number of Deposition CyclesFilm Thickness (nm)Metal Loading (g Ni or Ir/m2)
NiO-A1500260.14
NiO-B2400520.27
NiO-C3000550.27
NiO-D3000590.31
IrO2-E2000490.21
IrO2-F2000530.16
IrO2-G2000580.26
IrO2-H2000590.27
Table 2. Sublimation, deposition temperature, and growth rate of the electrode materials.
Table 2. Sublimation, deposition temperature, and growth rate of the electrode materials.
SampleSublimation Temperature (°C)Deposition Temperature (°C)Growth Rate (Å/Cycle)
NiO-A1102000.18
NiO-B1152000.22
NiO-C1102000.17
NiO-D1202000.20
IrO2-E1502050.49
IrO2-F1552050.53
IrO2-G1552100.57
IrO2-H1552100.59
Table 3. Precursors pulse and purge length of the electrode materials.
Table 3. Precursors pulse and purge length of the electrode materials.
SampleReactant A
Ni(tmhd)2 or Ir(acac)3
Reactant B
O3
Pulse Length (s)Purge Length (s)Pulse Length (s)Purge Length (s)
NiO-A2.53.03.05.0
NiO-B2.53.03.05.0
NiO-C2.53.03.05.0
NiO-D2.53.03.05.0
IrO2-E1.02.01.02.0
IrO2-F2.04.01.02.0
IrO2-G1.01.01.01.0
IrO2-H2.01.01.01.0
Table 4. Summary of the OER catalytic activity (ηO2 at 10 kA/m2 and Tafel slope) of the NiO and IrO2 thin films.
Table 4. Summary of the OER catalytic activity (ηO2 at 10 kA/m2 and Tafel slope) of the NiO and IrO2 thin films.
SampleηO2 at 10 kA/m2
(mV)
Tafel Slope
(mV/dec)
Bare Ni34064
NiO-A1331 ± 1070
NiO-A2315 ± 2058
NiO-B1316 ± 958
NiO-B2294 ± 442
NiO-C1321 ± 458
NiO-C2316 ± 1158
NiO-D1311 ± 954
NiO-D2314 ± 357
IrO2-E1311 ± 157
IrO2-E2316 ± 1460
IrO2-F1298 ± 648
IrO2-F2285 ± 754
IrO2-G1296 ± 045
IrO2-G2300 ± 847
IrO2-H1298 ± 852
IrO2-H2301 ± 1454

Share and Cite

MDPI and ACS Style

Matienzo, D.D.; Settipani, D.; Instuli, E.; Kallio, T. Active IrO2 and NiO Thin Films Prepared by Atomic Layer Deposition for Oxygen Evolution Reaction. Catalysts 2020, 10, 92. https://doi.org/10.3390/catal10010092

AMA Style

Matienzo DD, Settipani D, Instuli E, Kallio T. Active IrO2 and NiO Thin Films Prepared by Atomic Layer Deposition for Oxygen Evolution Reaction. Catalysts. 2020; 10(1):92. https://doi.org/10.3390/catal10010092

Chicago/Turabian Style

Matienzo, DJ Donn, Daniel Settipani, Emanuele Instuli, and Tanja Kallio. 2020. "Active IrO2 and NiO Thin Films Prepared by Atomic Layer Deposition for Oxygen Evolution Reaction" Catalysts 10, no. 1: 92. https://doi.org/10.3390/catal10010092

APA Style

Matienzo, D. D., Settipani, D., Instuli, E., & Kallio, T. (2020). Active IrO2 and NiO Thin Films Prepared by Atomic Layer Deposition for Oxygen Evolution Reaction. Catalysts, 10(1), 92. https://doi.org/10.3390/catal10010092

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.