Next Article in Journal
Highly Efficient Photo-Degradation of Gaseous Organic Pollutants Catalyzed by Diatomite-Supported Titanium Dioxide
Next Article in Special Issue
Acetonitrile’s Effect on the Efficiency of Ethanol Electrooxidation at a Polycrystalline Pt Electrode in Relation to pH-Dependent Fuel Cell Applications
Previous Article in Journal
Self-Nitrogen-Doped Carbon Nanosheets Modification of Anodes for Improving Microbial Fuel Cells’ Performance
Previous Article in Special Issue
The Relationship between Reaction Temperature and Carbon Deposition on Nickel Catalysts Based on Al2O3, ZrO2 or SiO2 Supports during the Biogas Dry Reforming Reaction
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of Pressure on Na0.5La0.5Ni0.3Al0.7O2.5 Perovskite Catalyst for Dry Reforming of CH4

by
Anis Hamza Fakeeha
1,2,
Ahmed Sadeq Al-Fatesh
1,*,
Jehad K. Abu-Dahrieh
3,
Ahmed Aidid Ibrahim
1,
Samsudeen Olajide Kasim
1 and
Ahmed Elhag Abasaeed
1
1
Chemical Engineering Department, College of Engineering, King Saud University, P.O. Box 800, Riyadh 11421, Saudi Arabia
2
King Abdullah City for Atomic and Renewable Energy, (K.A.CARE) Energy Research and Innovation Center, 11421 Riyadh, Saudi Arabia
3
School of Chemistry and Chemical Engineering, Queen’s University Belfast, Belfast BT9 5AG, Northern Ireland
*
Author to whom correspondence should be addressed.
Catalysts 2020, 10(4), 379; https://doi.org/10.3390/catal10040379
Submission received: 29 January 2020 / Revised: 11 March 2020 / Accepted: 29 March 2020 / Published: 1 April 2020
(This article belongs to the Special Issue Catalyst Deactivation in Hydrocarbon Processing)

Abstract

:
In this paper, a comprehensive study was carried out on the application of perovskite catalyst in dry reforming of CH4. The perovskite catalyst was prepared using a sol–gel method. The prepared samples were characterized by N2 adsorption/desorption, TPR, XRD, CO2-TPD, TGA, TPO, Raman, and SEM techniques. In addition, the effect of operating pressure, namely, 1 bar, 3 bar, 5 bar, and 7 bar, temperature (500–800 °C) was evaluated. The characterization results indicated that catalysts operated at 1 bar, gas hourly space velocity of 84000 (mL/g/h) gave the best catalytic performance. CH4 and CO2 conversions of 77 and 80% were obtained at 1 bar and at 700 °C reaction temperature. The increase of reaction temperatures from 500 °C to 800 °C increased the reaction rate and hence the methane and carbon dioxide conversions were increased. A unity ratio of H2/CO was obtained at 1 bar for temperatures 600 °C and above. Similarly, the time on stream tests, obtained at a 700 °C reaction temperature, showed that the best ratio in terms of the closeness of unity and the stable profile could be attained when the pressure was set to 1 bar. The TGA analysis showed the drop of mass due to oxidation of carbon deposits, which started at 500 °C. The catalyst operated at 1 bar produced the least amount of carbon, equivalent to 35% weight loss, while the 3 and 5 bar operated catalysts generated carbon formation, equivalent to 65% weight loss. However, the 7 bar operated catalyst resulted the highest accumulation of carbon formation, equivalent to 83% weight reduction. Hence, the TGA profile indicated the relative carbon deposition on the catalyst, which was dependent of the operated pressure and hence confirmed the suitability operation pressure of 1 bar. The characterizations of the Raman, EDX, TGA, and TPO all presented the formation of carbon.

1. Introduction

The carbon dioxide, methane reforming universally known as dry reforming (DRM) is a convenient method for producing synthesis gases from two powerful greenhouse gases (CH4 and CO2) [1,2,3,4,5]. Nevertheless, synthesis gas, the product of CH4 dry reforming, is a vital raw material for the production of liquid hydrocarbons [6,7,8]. The utilization of dry reforming is therefore accompanied by two crucial benefits. In the first place, the utilization of carbon dioxide together with methane in DRM permits the conversion of the pair greenhouse gases into components with advanced added merit. Moreover, the syngas attained from DRM gives equimolar amount of H2 and CO which is appropriate for Fischer–Tropsch (FT) synthesis to generate hydrocarbons [9,10]. The choice of proper catalyst plays an essential role in the catalytic activity and stability [11]. Transition metals such as Ni, Co are suitable for catalysing this process [12,13,14]. Ni based catalysts are often used due to their cheap price, abundance, and quick turnover rates [15]. Main difficulties encountered in using Ni-based catalysts come from the sintering which causes the loss of active metal surface areas and the carbon deposition on the surface, which deactivates and reduces the activity by covering the active metal surface and alters product selectivity [16].
Perovskites are used in catalytic and photovoltaic industries for their excellent performance. Perovskite structures containing Ni are employed for CO2 reforming of CH4. It has been depicted that perovskite-type oxides accomplish the need of high thermal stability and metal dispersion [17,18]. The use of perovskite oxides, where the B-site cation is a diluted transition metal such as Ni, has called for more research [19,20]. Ren et al. investigated the unexpected coke-resistant stability in steam-CO2 dual reforming of methane over the robust Mo2C-Ni/ZrO2 catalyst [21]. Their results showed high catalytic activity and unexpected stability in steam-CO2 dual reforming of CH4 for syngas production. Alternatively, Ziaei-Azad et al. studied the influence of Pd on the enhancement of oxidation activity of LaBO3 (B = Mn, Fe, Co, and Ni) perovskite catalysts for pollution abatement from natural gas fueled vehicles [22]. Their results indicated that Pd significantly enhanced the reducibility of B in LaBPd0.05O3 perovskites and improves the mobility of lattice oxygen in the prepared samples, which results in activity enhancement for Pd-containing catalysts. The work of Messaoudi et al. reports the investigation of LaxNiOy and LaxNiOy/MgAl2O4 catalysts in CO2 reforming of methane [23]. The outcome exhibited higher specific surface areas and nickel dispersions of the supported catalysts and thus supported catalysts were found more active and stable with low carbon deposition. Ruocco et al. [24] investigated the influence of preparation techniques, reaction temperature and gas hourly velocity in dry reforming reaction using ternary perovskites-type oxides, AZrRuO3 (A = Ca, Ba, Sr). They found SrZrRuO3 catalyst provided the best results of conversion and stability. Whereas, Wang et al. [25] explored the use of bimetallic Ni-Co catalysts supported on La2O3-LaFeO3 perovskite. The catalytic activity and coking resistance were enhanced by substituting a proper amount of Co. The crystalline structure of the perovskite also played a crucial role.
In this study, we investigated the performance of a typical perovskite catalyst (Na0.5La0.5Ni0.3Al0.7O2.5) obtained using the sol gel technique. The effect of different reaction temperatures and pressures over the efficiency of the process was examined.

2. Results and Discussion

2.1. Catalyst Characterization

The surface texture of the catalyst was evaluated via the nitrogen adsorption–desorption isotherms. Figure 1A demonstrates the nitrogen adsorption isotherms of the unused catalysts calcined at 725 °C with BET surface area of 12.4 m2/g, pore volume of 0.04 cm3/g, pore diameter of 13 nm, according to IUPAC labelling, catalysts showing type IV isotherm with H1 hysteresis loop [26]. While Figure 1B matches the distributions of pore size attained via BJH method. The pore size distribution depicts that most particles possess 140 nm particle diameters, which means macroporous characteristics. The H2-TPR evaluations of the perovskite catalyst were done to disclose the removal of the oxygen behavior of various oxide species of nickel. As shown in Figure 1C, the H2-TPR profile of the catalyst presents three peaks, the first one appeared around 332°C corresponding to the reduction of NiO species that barley interacted with the support. The second peak occurred at 653 °C, where NiO strongly interacted with the alumina support, and the third peak appeared at 744 °C with a maximum consumption of H2 between 500 and 900 °C was ascribed to the reduction of intimately associated surface to nickel deposited on lanthanum and alumina oxides [27]. From the TPR result, it is apparent that the Ni interacts strongly with the support confirming the hydrothermal stability of perovskites. For the generation of CO from the adsorption and activation of CO2, it is essential to perform the basicity of the catalyst. The reactive O2 species produced from CO2 activation can assist the removal of the formed carbon on the catalyst [28]. In this study, CO2-TPD was used to investigate the catalyst’s basicity. As depicted in Figure 1D, two small peaks in low temperature regions (100 °C and 280 °C) and intense peaks in high temperature regions about 760 °C. It is largely considered that the peaks at lower temperature regions can be credited to the weak basic sites resulting from the physical adsorption of CO2 [29]. While the peak appearing at the high temperature relates to the strong basic sites attributed to the chemisorption of CO2. As the result of the number of basic sites, peaks take different sizes [30]. It can be concluded that the catalyst is manifested by strong basic sites which enhances the adsorption of CO2 on the catalyst surface.
The crystalline nature of Na0.5La0.5Ni0.3Al0.7O2.5 catalysts was investigated by XRD, and the results are illustrated in Figure 2. The results revealed that the characteristic Bragg diffraction peaks at 2θ = 23.47, 32.96, 41.5, 48.4, 54.2, 59.5, and 63.3 are correlated well with the Al0.5LaNi0.5O3.054 (Rhombohedral Crystal System, JCPDS NO: 01-083-0757) whereas peaks at 2θ = 37.3, 43.1 are correlating with Na5NiO4 (Orthorhombic Crystal System JCPDS-01-071-1988). The structural characteristic of elements well matched with standard data.

2.2. Catalytic Activity

The perovskite catalyst activated at 750 °C was researched in dry reforming at 700 °C reaction temperature and a gas hourly space velocity (GHSV) of 84,000 mL g−1h−1. Figure 3 shows the time on stream of 8 h versus conversions of methane and CO2 for various pressures (1, 3, 5, 7 bar). The effect of the pressure is well denoted such that both methane and CO2 conversions assumed the highest values of 77% and 80% respectively, with % deactivation factor of 9.3, when 1 bar pressure was used. While the lowest conversions of 45% and 52.5% were recorded, with % deactivation factor of 10.9, when highest pressure of 7 bar was implemented. The stability is also affected by the increase of the pressure. For instance, at 5 bar the CH4 and CO2 conversion decreased from 58% and 55% to 45% and 50% respectively. On the other hand, Figure 4 displays the time on stream of hydrogen and CO ratios for 8 h when different pressures were used. The result indicates that the best ratio in terms to the closeness to unity and the stable value could be attained when the pressure was set to 1 bar. It can be deduced from this section that both stability and activity of the catalyst is significantly affected by the operating pressures.
Table 1 exhibits the CH4 conversion of this work and those in the literature. The achieved result compares well with the literature values, particularly those operated at similar reaction temperatures. The activity per gram obtained shows quite improvement in comparison.
Figure 4B and Figure 5A,B show the effect of reaction temperature on methane and carbon dioxide conversions for pressures (1, 3, 5, and 7 bar). It is evident from the profiles that the conversions grew with the rise of the reaction temperature. This is expected as the DRM process is endothermic. The conversions operated at 1 bar pressure depicted an average improvement of 15% for moderate temperatures less than 750 °C. This means that the conversion values of 1 bar operated catalyst are higher than those operated at other pressures, where their conversion values are at least 15% less than that of 1 bar operated catalyst when the reaction temperature is higher than 650 °C and lower than 750 °C. The result of reaction temperatures displays the effect of operating pressure, where high pressures impedes the activity.
Figure 6 depicts the effect of reaction temperature on hydrogen and CO ratios for pressures (1, 3, 5, and 7 bar). It is evident from the profiles that the ratio increases with the rise of the reaction temperature from 500 °C to 600 °C. This could be related to the endothermicity of the process. The highest value of H2/CO is obtained at 600 °C for all operating pressures. The same effect was observed for dry reforming of methane over alumina-supported nickel catalysts for all Ni Loading [33]. The phenomenon was related to the fact that the highest carbon deposition was recorded at 600 °C. Beyond 600 °C, the ratio is either maintained at an almost constant value as in in the case of 1 bar, or decreased as in the case of 7 bar where the ratio reduced by 26%. The H2/CO ratio obtained at 1 bar pressure depicted a unity ratio for temperatures equal to or greater than 600 °C.
Stability test was performed on the catalyst over 30 h time on stream. The results obtained in Figure 7, shows that there is no significant loss of activity for the period under investigation. The reaction was performed at 1 bar, 700 °C and 84000 mL/g/h space velocity. The steady stability obtained symbolizes the constituents of the perovskite hinders the deactivation commonly seen with Ni based catalysts.
Catalysts’ morphology was examined using SEM as shown in Figure 8. In the fresh catalyst (Figure 8A) individual leaf-blade shapes are in majority but in used catalyst (Figure 8B,C) this identity vanishes. The coke deposition on the used catalyst is verified in EDX as well as in TGA results.
The identification of the types of carbon deposited over used catalysts in DRM is crucial in comprehending its deactivation behaviour. Thus, temperature programming oxidation (TPO) analysis is often carried out. Figure 9 displayed the TPO of the used perovskite in this work for four different pressures (1, 3, 5, and 7 bar). The TPO tests were performed with spent Na0.5La0.5Ni0.3Al0.7O2.5 catalysts operated at 700 °C and lasted for 8 h of reaction. The TPO patterns demonstrated the presence of a single peak for each pressure with maxims at 500–620 °C. This can be assigned to polymeric respectively [34]. The type of coke represented here for high pressure was graphic carbon deposited on the support which metallic centre did not catalyse and removed at T > 650 °C [35] and this type of coke can be totally removed using pure O2 at 700 °C. The TPO analysis discloses the formation of amorphous carbon at 1 bar while high pressure forms graphitic carbon. The shifting of peaks toward high temperature denotes the growth tendency of graphitic carbon. The TPO analysis confirms the TGA analysis showing the increase formation of carbon deposit with the increase of pressure.
Figure 10 presents the output of the thermogravimetric analysis (TGA) of the used catalysts after 8 h on reaction at 700 °C. The measured weight drop denoted the influence of pressure. The catalyst operated at 1 bar gave 33% weight drop, while the catalysts operated at higher pressures (3 and 5 bar) gave a higher weight loss of about 63%. On the hand, the catalyst operated at 7 bar gave the highest weight loss of 83%. This is justified since the tendency of carbon formation increased with the pressure increase. Figure 11 displays the result of the thermogravimetric analysis (TGA) of the used catalysts for two reaction times (8 h and 30 h) operated on 1 bar pressure and at 700 °C. The measured weight drop compared the influence of time on stream. The catalyst operated for 8 h time on stream gave 33% weight drop, while the catalysts operated for 30 h time on stream produced a 47% weight loss. The 14% increase of the weight drop for the longer time on stream is reasonable as the carbon formation increased with the reaction increase.
The TGA investigation exhibits the influence of operation pressure, where high pressure favors the increase of carbon deposition. Figure 12 exhibited the TPO of the used perovskite catalyst for 1 bar pressure at two different reaction durations (8 h and 30). The TPO tests were accomplished with the used Na0.5La0.5Ni0.3Al0.7O2.5 catalysts operated at 700 °C. The TPO patterns showed the presence of a single peak for each reaction time with maxims at 500 °C and 620 °C for 8 h and 30 h respectively. This showed the increase of the reaction time affected the structure of the carbon deposited and its quantity. The higher reaction time favored the formation of graphitic carbon as its peak was shifted to the higher region temperature. It is remarkable that 1 bar operated for 8 h has its peak appeared at relatively lower temperature and hence more resistant to the surface oxidation than 1 bar operated for 30 h.
The carbon deposition is a significant feature, which affects the catalytic performance on methane dry reforming reaction. The different carbon type generates different influence on catalytic performance. Thus, Raman spectroscopic analysis was carried out to study the structure of formed carbon over the used catalysts. The attained Raman spectra are shown in Figure 13. For all the used samples, two main spectra were observed at approximately 1470 cm−1 and 1533 cm−1 corresponding to the D (assigned to sp3 hybridized amorphous carbon) and G band (indicated the presence of graphitized carbon), respectively [36]. The G band can be ascribed to the ideal vibration of the graphite layers as a result of the in-plane carbon-carbon stretching. The D band is credited to the structural defect of graphite [37]. In addition, a small shoulder that appeared at 1582 cm−1 can be associated to disordered carbons at the edge [38]. In general, the ratio of the intensity of D band to G band (ID/IG) delivers a measure of the crystalline order of graphite in carbonaceous materials [39]. This indicates that the degree of graphitization is higher for small values of ID/IG. The ID/IG of all the used catalysts exhibited in Figure 13 denotes that the carbon deposits over the catalysts have almost equal disordered amorphous and graphitic structures. The Raman investigation labels similar degree of graphitization regardless of the operating pressure. However, the intensity of the peaks changes with the operating pressure.

3. Materials

3.1. Catalyst Preparation

The description of the experimental procedure can be partly obtained from our paper [40] and partly from the given support information. Perovskite catalysts have been prepared using a sol–gel technique [41].
The materials used in this work were obtained from Sigma-Aldrich Ltd. with a purity >99%. These include CH3CH2COOH acid and precursor reagents, La(NO3)3∙6H2O, Al(NO3)3·9H2O, Ni(NO3)2·6H2O, and NaNO3. The chemicals of the precursor were individually mixed with a slight volume of a pre-heated CH3CH2COOH at 1 bar and 90 ℃. Subsequent to dissolution, every solution was well stirred at 1 bar at 130 °C for 2 h. Subsequently, a reflux process was used to distil the acid until a gel was seen. The gel was dried at 90 ℃ overnight and then calcined in air at 725 ℃ for 4 h. The formula of the obtained catalyst was Na0.5La0.5Ni0.3Al0.7O2.5 [35,42].

3.2. Catalyst Performance

DRM was accomplished in a tubular, reactor (ID = 0.9 cm) at 1 bar. The reactor was obtained from PID Eng. & Tech. In the event of carrying out the DRM test, a 50 mg catalyst was reduced with 20 mL/min of hydrogen at 750 °C for 1 h. Nitrogen was passed to the reactor for 0.33 h to desorb the attached H2 meanwhile, the reaction temperatures (500–800 °C) move to the desired values. Similarly, the pressure varied from (1–7 bar).
Later on, CO2, CH4, and N2 were introduced at the rates of 1800, 1800, and 60 mL/h, in that order. A GC (GC-2014 SHIMADZU) equipped with a thermal conductivity detector and Porapak Q and Molecular Sieve 5A columns, was linked in bypass/series attachments to get the entire constituents of the effluent gas stream. the reaction outputs. The formulas for conversion and yield are
% CH 4   conversion = CH 4   in CH 4   out CH 4   in × 100 % CO 2   conversion = CO 2   in CO 2   out CO 2   in × 100 H 2 CO = moles   of   H 2   produced moles   of   CO   produced H 2   Yield   ( % ) = moles   of   H 2   produced 2   X   moles   of   CH 4   in   the   feed × 100 CO   Yield   ( % ) = moles   of   CO   produced ( mole   of   CH 4 + moles   of   CO 2 )   in   the   feed × 100 Deactivation   Factor   ( % DF ) = Final   Conversion   of   CH 4 Initial   conversion   of   CH 4 Initial   conversion   of   CH 4 × 100

3.3. Catalyst Characterization

The N2-physisorption was used to compute the specific surface area using a Micromeritics Tristar II (Micromeritics, Atlanta, GA, USA). The analysis was achieved by N2 adsorption-desorption accomplished at −196 °C. Prior to the analysis, each sample was degassed at 200 °C for 3 h. in the flow of nitrogen gas.
The determination of TPR was carried out by means of Micromeritics AutoChem II apparatus (Micromeritics, Atlanta, GA, USA). A 0.7 g catalyst was put in the TPR compartment and flowed with Ar at 150 °C for 0.5 h. After that the temperature was decreased to the ambient temperature. Eventually, at 10 °C/min ramp, the furnace temperature was raised to 1000 °C while the H2/Ar mixture was kept at 0.04 L/min. A thermal conductivity detector (TCD) was employed to monitor the signals denoting the hydrogen utilization.
The (CO2-TPD) measurement was carried out using Micromeritics AutoChem II (Micromeritics, Atlanta, GA, USA). A 0.5 g of catalyst was activated with H2 at 600 °C for 60 min. under He (30 mL/min), after that reduced the temperature to 50 °C. The flow rate of CO2 was maintained for an hour, and He gas was used to expel any physisorbed CO2. The desorption figure outline of the catalysts was registered by raising the temperature up to 800 °C at the rate of 10 °C/min. The CO2 composition in the outflow stream was determined by a thermal conductivity detector. The desorbed CO2 quantities during TPD were calculated from the areas under the peaks.
The (TPO) was done in O2 ambient to find out the type of carbon formed on the surface of the catalyst via Micromeritics AutoChem II (Micromeritics, Atlanta, GA, USA). The analysis was done up to 800 °C under 40 mL/min of 10% O2/He. The used catalyst was pre-treated in the presence of Ar at 150 °C for 30 min. and afterward the temperature is lowered to 25 °C.
TGA was used to determine the carbon formed on the surface of the used catalyst under air by a Shimadzu TGA-15 SHIMADZU analyzer (Shimadzu Corporation, Kyoto, OP, Japan). The temperature of spent catalyst (0.10–0.15 g) was raised to 1000 °C at the rate of 20 °C/min and the weight loss was determined.
XRD was used for phase identification of catalysts, with Cu Kα radiation functioned at 40 kV and 40 mA. A 0.01° scanning step and 10°–85° range of 2θ were adopted.
The scanning electron microscopy (SEM) was used to examine the surface structure of the catalysts. The images of the fresh and used catalysts were provided by JSM-7500F (Rigaku Corporation, Dover, DE, USA).

4. Conclusions

As a summary, perovskite catalyst employed for CO2 reforming of CH4 was examined in this work. The catalytic performance of methane dry reforming could be greatly influenced by the operating pressure and temperature. Catalysts operated at 1 bar pressure gave the best catalytic and stability performance. The rise of reaction temperature from 500 to 800 °C increases the activity. The H2/CO ratio acquired approximately a unity ratio in operating at 1 bar pressure for temperatures at 600 °C and beyond. Correspondingly, the time on stream tests showed that the best ratio close to unity with a stable profile can be achieved operating at 1 bar pressure. The TPO analysis gave single peaks around 600–650 °C symbolizing the graphitic type of coke which can be eliminated using pure O2 and operating at 700 °C. While the TGA analysis indicated that higher pressure operations favor greater amounts of coke formation. The characterizations of the Raman, EDX, TGA, and TPO all presented the formation of carbon.

Author Contributions

A.S.A.-F., A.A.I., and S.O.K. synthesized the catalysts, carried out all the experiments and characterization tests, and wrote the manuscript. J.K.A.-D. prepared the catalyst and contributed in proofreading of the manuscript. A.E.A. and A.H.F. contributed to the analysis of the data and proofread the manuscript. All authors have read and agreed to the published version of the manuscript.

Funding

The authors would like to express their sincere appreciation to the Deanship of Scientific Research at King Saud University for funding this research project (no. RGP-119).

Acknowledgments

The KSU authors would like to extend their sincere appreciation to the Deanship of Scientific Research at the King Saud University for its funding for this research group project (no. RGP-119).

Conflicts of Interest

The authors declare no competing interests.

References

  1. Wang, Y.; Yao, L.; Wang, S.; Mao, D.; Hu, C. Low-temperature catalytic CO2 dry reforming of methane on Ni-based catalysts: A review. Fuel Process. Technol. 2018, 169, 199–206. [Google Scholar] [CrossRef]
  2. Li, H.; He, Y.; Shen, D.; Cheng, S.; Wang, J.; Liu, H.; Xing, C.; Shan, S.; Lu, C.; Yang, R. Design an in-situ reduction of Ni/C-SiO2 catalyst and new insight into pre-treatment effect for CH4-CO2 reforming reaction. Int. J. Hydrog. Energy 2017, 42, 10844–10853. [Google Scholar] [CrossRef]
  3. Al-Fatesh, A.S.; Arafat, Y.; Atia, H.; Ibrahim, A.A.; Ha, Q.L.M.; Schneider, M.; M-Pohl, M.; Fakeeha, A.H. CO2-reforming of methane to produce syngas over Co-Ni/SBA-15 catalyst: Effect of support modifiers (Mg, La and Sc) on catalytic stability. J. CO2 Util. 2017, 21, 395–404. [Google Scholar] [CrossRef]
  4. Ibrahim, A.A.; Fakeeha, A.H.; Al-Fatesh, A.S. Enhancing hydrogen production by dry reforming process with strontium promoter. Int. J. Hydrog. Energy 2014, 39, 1680–1687. [Google Scholar] [CrossRef]
  5. Li, D.; Lu, M.; Xu, S.; Chen, C.; Zhan, Y.; Jiang, L. Preparation of supported Co catalysts from Co-Mg-Al layered double hydroxides for carbon dioxide reforming of methane. Int. J. Hydrog. Energy 2017, 42, 5063–5071. [Google Scholar] [CrossRef]
  6. Al-Fatesh, A.S.; Arafat, Y.; Ibrahim, A.A.; Atia, H.; Fakeeha, A.H.; Armbruster, U.; Abasaeed, A.E.; Frusteri, F. Evaluation of Co-Ni/Sc-SBA–15 as a novel coke resistant catalyst for syngas production via CO2 reforming of methane. Appl. Catal. A Gen. 2018, 567, 102–111. [Google Scholar] [CrossRef]
  7. Djinovic, P.; Batista, J.; Pintar, A. Efficient catalytic abatement of greenhouse gases: Methane reforming with CO2 using a novel and thermally stable Rh-CeO2 catalyst. Int. J. Hydrog. Energy 2012, 37, 2699–2707. [Google Scholar] [CrossRef]
  8. El Hassan, N.; Kaydouh, M.N.; Geagea, H.; El Zein, H.; Jabbour, K.; Casale, S.; El Zakhem, H.; Massiani, P. Low temperature dry reforming of methane on rhodium and cobalt based catalysts: Active phase stabilization by confinement in mesoporous SBA-15. Appl. Catal. A Gen. 2016, 520, 114–121. [Google Scholar] [CrossRef] [Green Version]
  9. Horn, R.; Schlögl, R. Methane Activation by Heterogeneous Catalysis. Catal. Lett. 2015, 45, 23–39. [Google Scholar] [CrossRef] [Green Version]
  10. Rostrup-Nielsen, J.R.; Sehested, J.; Nørskov, J.K. Hydrogen and synthesis gas by steam- and CO2 reforming. Adv. Catal. 2002, 47, 65–139. [Google Scholar] [CrossRef]
  11. Kang, D.; Yu, J.; Ma, W.; Zheng, M.; He, Y.; Li, P. Synthesis of Cu/Ni-La0.7Sr0.3Cr0.5Mn0.5O3–δ and its catalytic performance on dry methane reforming. J. Rare Earth 2019, 37, 585–593. [Google Scholar] [CrossRef]
  12. Chein, R.-Y.; Fung, W.-Y. Syngas production via dry reforming of methane over CeO2 modified Ni/Al2O3 catalysts. Int. J. Hydrog. Energy 2019, 44, 14303–14315. [Google Scholar] [CrossRef]
  13. Ma, Q.; Guo, L.; Fang, Y.; Li, H.; Zhang, J.; Zhao, T.-S.; Yang, G.; Yoneyam, Y.; Tsubaki, N. Combined methane dry reforming and methane partial oxidization for syngas production over high dispersion Ni based mesoporous catalyst. Fuel Process. Technol. 2019, 188, 98–104. [Google Scholar] [CrossRef]
  14. Abdullah, B.; Ghani, N.A.A.; Vo, D.-V.N. Recent advances in dry reforming of methane over Ni-based catalysts. J. Clean Prod. 2017, 162, 170–185. [Google Scholar] [CrossRef] [Green Version]
  15. Ali, S.; Khader, M.M.; Almarri, M.J.; Abdelmoneim, A.G. Ni-based nano-catalysts for the dry reforming of methane. Catal. Today 2019, in press, corrected proof. [Google Scholar] [CrossRef]
  16. Shen, J.; Allen, A.C.; Semagina, N. Ni/MgAl2O4 catalyst for low-temperature oxidative dry methane reforming with CO2. Int. J. Hydrog. Energy 2019, 44, 4616–4629. [Google Scholar] [CrossRef]
  17. Jacobson, A.J. Materials for Solid Oxide Fuel Cells. Chem. Mater. 2010, 22, 660–674. [Google Scholar] [CrossRef]
  18. Kim, W.Y.; Jang, J.S.; Ra, E.C.; Kim, K.Y.; Eun Hyup Kim, E.H.; Lee, J.S. Reduced perovskite LaNiO3 catalysts modified with Co and Mn for low coke formation in dry reforming of methane. Appl. Catal. A Gen. 2019, 575, 198–203. [Google Scholar] [CrossRef]
  19. Khalesi, A.; Arandiyan, H.R.; Parvari, M. Production of Syngas by CO2 Reforming on MxLa1−xNi0.3Al0.7O3−d (M = Li, Na, K). Ind. Eng. Chem. Res. 2008, 47, 5892–5898. [Google Scholar] [CrossRef]
  20. Pérez-Camacho, M.N.; Abu-Dahrieh, J.; Goguet, A.; Sun, K.; Rooney, D. Self-cleaning perovskite-type catalysts for the dry reforming of methane. Chin. J. Catal. 2014, 35, 1337–1346. [Google Scholar] [CrossRef]
  21. Ren, P.; Zhao, Z. Unexpected coke-resistant stability in steam-CO2 dual reforming of methane over the robust Mo2C-Ni/ZrO2 catalyst. Catal. Commun. 2019, 119, 71–75. [Google Scholar] [CrossRef]
  22. Ziaei-Azad, H.; Khodadadi, A.; Esmaeilnejad-Ahranjani, P.; Mortazavi, Y. Effects of Pd on enhancement of oxidation activity of LaBO3 (B = Mn, Fe, Co and Ni) perovskite catalysts for pollution abatement from natural gas fueled vehicles. Appl. Catal. B Environ. 2011, 102, 62–70. [Google Scholar] [CrossRef]
  23. Messaoudi, H.; Thomas, S.; Djaidja, A.; Slyemi, S.; Barama, A. Study of LaxNiOy and LaxNiOy/MgAl2O4 catalysts in dry reforming of methane. J. CO2 Util. 2018, 24, 40–49. [Google Scholar] [CrossRef]
  24. Ruocco, C.; Caprariis, B.D.; Palma, V.; Petrullo, A.; Ricca, A.; Scarsella, M.; Filippis, P.D. Methane dry reforming on Ru perovskites, AZrRuO3: Influence of preparation method and substitution of a cation with alkaline earth metals. J. CO2 Util. 2019, 30, 222–231. [Google Scholar] [CrossRef]
  25. Wang, H.; Dong, X.; Zhao, T.; Yu, H.; Li, M. Dry reforming of methane over bimetallic Ni-Co catalyst prepared from La(CoxNi1-x)0.5Fe0.5O3 perovskite precursor: Catalytic activity and coking resistance. Appl. Catal. B Environ. 2009, 245, 302–313. [Google Scholar] [CrossRef]
  26. Sing, K.S.W. Reporting physisorption data for gas/solid systems with special reference to the determination of surface area and porosity (recommendations 1984). Pure Appl. Chem. 1985, 57, 603–619. [Google Scholar] [CrossRef]
  27. Pecchi, Y.G.; Gilberto, M.G.; Delgado, E.J.; Cadús, L.E.; Fierro, L.G. Effect of B-site cation on the catalytic activity of La1−xCaxBO3 (B = Fe, Ni) perovskite-type oxides for toluene combustion. J. Chem. Technol. Biot. 2011, 86, 1067–1073. [Google Scholar] [CrossRef]
  28. Bhavani, A.G.; Kim, W.Y.; Lee, J.S. Barium substituted lanthanum manganite perovskite for CO2 reforming of methane. ACS Catal. 2013, 3, 1537–1544. [Google Scholar] [CrossRef]
  29. Wierzbickia, D.; Baran, R.; Debek, R.; Motak, M.; Galvez, M.E.; Grzybek, T.; Costa, P.D.; Glatzel, P. Examination of the influence of La promotion on Ni state in hydrotalcite-derived catalysts under CO2 methanation reaction conditions: Operando X-ray absorption and emission spectroscopy investigation. Appl. Catal. B 2018, 232, 409–419. [Google Scholar] [CrossRef]
  30. Li, D.; Li, R.; Lu, M.; Lin, X.; Zhan, Y.; Jiang, L. Carbon dioxide reforming of methane over Ru catalysts supported on Mg-Al oxides: A highly dispersed and stable Ru/Mg (Al)O catalyst. Appl. Catal. B Environ. 2017, 200, 566–577. [Google Scholar] [CrossRef]
  31. Whang, H.S.; Choi, M.S.; Lim, J.; Kim, C.; Heo, I.; Chang, T.-S. Enhanced activity anddurability of Ru catalyst dispersed on zirconia for dry reforming of methane. Catal. Today 2017, 293–294, 122–128. [Google Scholar] [CrossRef]
  32. Nematollahi, B.; Rezaei, M.; Khajenoori, M. Combined dry reforming and partialoxidation of methane to synthesis gas on noble metal catalysts. Int. J. Hydrog. Energy 2011, 36, 2969–2978. [Google Scholar] [CrossRef]
  33. Al-Fatish, A.S.A.; Ibrahim, A.A.; Fakeeha, A.H.; Soliman, M.A.; Siddiqui, M.R.H.; Abasaeed, A.E. Coke formation during CO2 reforming of CH4 over alumina-supported nickel catalysts. Appl. Catals A Gen. 2009, 364, 150–155. [Google Scholar] [CrossRef]
  34. Kumar, N.; Shojaee, M.; Spivey, J.J. Catalytic bi-reforming of methane: From greenhouse gases to syngas. Curr. Opin. Chem. Eng. 2015, 9, 8–15. [Google Scholar] [CrossRef] [Green Version]
  35. Liu, D.; Quek, X.Y.; Cheo, W.N.E.; Lau, R.; Borgna, A.; Yang, Y. MCM-41 supported nickel-based bimetallic catalysts with superior stability during carbon dioxide reforming of methane: Effect of strong metal-support interaction. J. Catal. 2009, 266, 380–390. [Google Scholar] [CrossRef]
  36. Chen, X.; Oh, W.D.; Hu, Z.T.; Sun, Y.M.; Webster, R.D.; Li, S.Z.; Lim, T.T. Enhancing sulfacetamide degradation by peroxymonosulfate activation with N-doped graphene produced through delicately-controlled nitrogen functionalization via tweaking thermal annealing processes. Appl. Catal. B Environ. 2018, 225, 243–257. [Google Scholar] [CrossRef]
  37. Koo, K.Y.; Lee, S.H.; Jung, U.H.; Roh, H.S.; Yoon, W.L. Syngas production via combined steam and carbon dioxide reforming of methane over Ni-Ce/MgAl2O4 catalysts with enhanced coke resistance. Fuel Process. Technol. 2014, 119, 151–157. [Google Scholar] [CrossRef]
  38. Darmstadt, H.; Sümmchen, L.; Ting, J.-M.; Roland, U.; Kaliaguine, S.; Roy, C. Effects of surface treatment on the bulk chemistry and structure of vapor grown carbon fibers. Carbon 1997, 35, 1581–1585. [Google Scholar] [CrossRef]
  39. Donphai, W.; Witoon, T.; Faungnawakij, K.; Metta Chareonpanich, M. Carbon-structure affecting catalytic carbon dioxide reforming of methane reaction over Ni-carbon composites. J. CO2 Util. 2016, 16, 245–256. [Google Scholar] [CrossRef]
  40. Al-Fatesh, A.S.; Ibrahim, A.A.; Fakeeha, A.H.; Singh, S.K.; Labhsetwar, N.K.; Shaikh, H.; Qasim, S.O. CO2 reforming of CH4: Effect of Gd as promoter for Ni supported over MCM-41 as catalyst. Renew. Energy 2019, 140, 658–667. [Google Scholar] [CrossRef]
  41. Zhao, J.; Li, J.; Liu, H.; Zhang, X.; Zheng, K.; Yu, H.; Lian, Q.; Wang, H.; Zhu, Y.; Huo, J. Cesium immobilization in perovskite-type Ba1-x(La, Cs)xZrO3 ceramics by sol-gel method. Ceram. Int. 2020, 46, 9968–9971. [Google Scholar] [CrossRef]
  42. Pérez-Camacho, M.N.; Abu-Dahrieh, J.; Rooney, D.; Sun, K. Biogas reforming using renewable wind energy and induction heating. Catal. Today 2015, 242, 129–138. [Google Scholar] [CrossRef]
Figure 1. (A) N2 adsorption–desorption isotherms, (B) pore size distribution, (C) TPR, and (D) CO2-TPD profile for fresh catalyst calcined at 725 °C.
Figure 1. (A) N2 adsorption–desorption isotherms, (B) pore size distribution, (C) TPR, and (D) CO2-TPD profile for fresh catalyst calcined at 725 °C.
Catalysts 10 00379 g001
Figure 2. XRD profiles of catalyst calcined at 725 °C.
Figure 2. XRD profiles of catalyst calcined at 725 °C.
Catalysts 10 00379 g002
Figure 3. TOS against (A) methane and (B) carbon dioxide conversions, for catalyst at 725 °C, 700 °C calcination and reaction respectively, 0.05g catalyst, CH4 = 30 mL/min, CO2 = 30 mL/min, N2 = 10 mL/min, GHSV = 84000 (mL/g/h).
Figure 3. TOS against (A) methane and (B) carbon dioxide conversions, for catalyst at 725 °C, 700 °C calcination and reaction respectively, 0.05g catalyst, CH4 = 30 mL/min, CO2 = 30 mL/min, N2 = 10 mL/min, GHSV = 84000 (mL/g/h).
Catalysts 10 00379 g003
Figure 4. TOS against hydrogen and carbon monoxide ratios, for catalyst: calcination at 725 °C, activation at 750 °C, reaction at 700 °C, 0.05g catalyst, CH4 = 30 mL/min, CO2 = 30 mL/min, N2 = 10mL/min, GHSV = 84000 (mL/g/h).
Figure 4. TOS against hydrogen and carbon monoxide ratios, for catalyst: calcination at 725 °C, activation at 750 °C, reaction at 700 °C, 0.05g catalyst, CH4 = 30 mL/min, CO2 = 30 mL/min, N2 = 10mL/min, GHSV = 84000 (mL/g/h).
Catalysts 10 00379 g004
Figure 5. Catalytic activities of perovskite catalyst calcined at 725 °C, using 0.05 g of catalyst and CH4: CO2:N2 = 30/30/10 mL/min. at GHSV of 84000 mL/g/h at T = 500–800 °C. (A) CH4 conversion, (B) CO2 conversion.
Figure 5. Catalytic activities of perovskite catalyst calcined at 725 °C, using 0.05 g of catalyst and CH4: CO2:N2 = 30/30/10 mL/min. at GHSV of 84000 mL/g/h at T = 500–800 °C. (A) CH4 conversion, (B) CO2 conversion.
Catalysts 10 00379 g005aCatalysts 10 00379 g005b
Figure 6. Catalytic activities of perovskite catalyst calcined at 725 °C, activated at 750 °C, using 0.05 g of catalyst and CH4: CO2:N2 = 30/30/10 mL/min at GHSV of 84000 mL/g/h at T = 500–800 °C. Effect of hydrogen and carbon monoxide ratios.
Figure 6. Catalytic activities of perovskite catalyst calcined at 725 °C, activated at 750 °C, using 0.05 g of catalyst and CH4: CO2:N2 = 30/30/10 mL/min at GHSV of 84000 mL/g/h at T = 500–800 °C. Effect of hydrogen and carbon monoxide ratios.
Catalysts 10 00379 g006
Figure 7. Long time-on-stream for perovskite catalyst calcined at 725 °C, using 0.05 g of catalyst with GHSV of 84 L/g/h; T = 700 °C.
Figure 7. Long time-on-stream for perovskite catalyst calcined at 725 °C, using 0.05 g of catalyst with GHSV of 84 L/g/h; T = 700 °C.
Catalysts 10 00379 g007
Figure 8. SEM images of (A) fresh catalyst, (B) used catalyst at 1 bar, (C) used catalyst at 7 bar.
Figure 8. SEM images of (A) fresh catalyst, (B) used catalyst at 1 bar, (C) used catalyst at 7 bar.
Catalysts 10 00379 g008aCatalysts 10 00379 g008b
Figure 9. TPO of the used catalyst, calcined at 725 °C, after 8 h reaction time in DRM at 700 °C.
Figure 9. TPO of the used catalyst, calcined at 725 °C, after 8 h reaction time in DRM at 700 °C.
Catalysts 10 00379 g009
Figure 10. TGA patterns for catalyst, calcined at 725 °C, after 8 h reaction time in DRM, operated at 700 °C for pressure (1, 3, 5, 7 bar).; GHSV 84,000 (mL/(g h)).
Figure 10. TGA patterns for catalyst, calcined at 725 °C, after 8 h reaction time in DRM, operated at 700 °C for pressure (1, 3, 5, 7 bar).; GHSV 84,000 (mL/(g h)).
Catalysts 10 00379 g010
Figure 11. TGA patterns for catalysts, calcined at 725 °C, after 8 h and 30 h reaction times in DRM, operated at 700 °C for 1 bar pressure; GHSV 84,000 (mL/(g h)).
Figure 11. TGA patterns for catalysts, calcined at 725 °C, after 8 h and 30 h reaction times in DRM, operated at 700 °C for 1 bar pressure; GHSV 84,000 (mL/(g h)).
Catalysts 10 00379 g011
Figure 12. TPO of the used catalysts, calcined at 725 °C for different reaction time in DRM at 700 °C; 1 bar.
Figure 12. TPO of the used catalysts, calcined at 725 °C for different reaction time in DRM at 700 °C; 1 bar.
Catalysts 10 00379 g012
Figure 13. Room temperature Raman spectra of used catalysts upon 532 nm excitation.
Figure 13. Room temperature Raman spectra of used catalysts upon 532 nm excitation.
Catalysts 10 00379 g013
Table 1. Comparison between the CH4 conversion obtained and those from data available in literature for different catalysts used in dry reforming of CH4
Table 1. Comparison between the CH4 conversion obtained and those from data available in literature for different catalysts used in dry reforming of CH4
CatalystCH4: CO2GHSV (mL/g/h)Catalyst weight (g)T (°C)%CH4References
1%Ru/ZrO2-SiO21:1800000.0337580067[31]
1% Ru-Al2O3-MgO1:1160000.1500070074[32]
CaZrRuO31:1360000.1000070060[24]
La (Co0.1Ni0.9)0.5Fe0.5 O31:1120000.3000075072[25]
Na0.5La0.5Ni0.3Al0.7O31:1840000.0500070077Present work

Share and Cite

MDPI and ACS Style

Fakeeha, A.H.; Al-Fatesh, A.S.; Abu-Dahrieh, J.K.; Ibrahim, A.A.; Kasim, S.O.; Abasaeed, A.E. Effect of Pressure on Na0.5La0.5Ni0.3Al0.7O2.5 Perovskite Catalyst for Dry Reforming of CH4. Catalysts 2020, 10, 379. https://doi.org/10.3390/catal10040379

AMA Style

Fakeeha AH, Al-Fatesh AS, Abu-Dahrieh JK, Ibrahim AA, Kasim SO, Abasaeed AE. Effect of Pressure on Na0.5La0.5Ni0.3Al0.7O2.5 Perovskite Catalyst for Dry Reforming of CH4. Catalysts. 2020; 10(4):379. https://doi.org/10.3390/catal10040379

Chicago/Turabian Style

Fakeeha, Anis Hamza, Ahmed Sadeq Al-Fatesh, Jehad K. Abu-Dahrieh, Ahmed Aidid Ibrahim, Samsudeen Olajide Kasim, and Ahmed Elhag Abasaeed. 2020. "Effect of Pressure on Na0.5La0.5Ni0.3Al0.7O2.5 Perovskite Catalyst for Dry Reforming of CH4" Catalysts 10, no. 4: 379. https://doi.org/10.3390/catal10040379

APA Style

Fakeeha, A. H., Al-Fatesh, A. S., Abu-Dahrieh, J. K., Ibrahim, A. A., Kasim, S. O., & Abasaeed, A. E. (2020). Effect of Pressure on Na0.5La0.5Ni0.3Al0.7O2.5 Perovskite Catalyst for Dry Reforming of CH4. Catalysts, 10(4), 379. https://doi.org/10.3390/catal10040379

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop