Next Article in Journal
Progressive Failure and Energy Absorption of Chopped Bamboo Fiber Reinforced Polybenzoxazine Composite under Impact Loadings
Next Article in Special Issue
Association between Nonionic Amphiphilic Polymer and Ionic Surfactant in Aqueous Solutions: Effect of Polymer Hydrophobicity and Micellization
Previous Article in Journal
One-Pot Polymerization of Dopamine as an Additive to Enhance Permeability and Antifouling Properties of Polyethersulfone Membrane
Previous Article in Special Issue
Water-Soluble and Cytocompatible Phospholipid Polymers for Molecular Complexation to Enhance Biomolecule Transportation to Cells In Vitro
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis of Amphiphilic Statistical Copolymers Bearing Methoxyethyl and Phosphorylcholine Groups and Their Self-Association Behavior in Water

1
Department of Applied Chemistry, Graduate School of Engineering, University of Hyogo, 2167 Shosha, Himeji, Hyogo 671-2280, Japan
2
Department of Materials Engineering, School of Engineering, The University of Tokyo, 7-3-1 Hongo, Bunkyo-ku, Tokyo 113-8656, Japan
*
Author to whom correspondence should be addressed.
Polymers 2020, 12(8), 1808; https://doi.org/10.3390/polym12081808
Submission received: 28 May 2020 / Revised: 7 August 2020 / Accepted: 9 August 2020 / Published: 12 August 2020
(This article belongs to the Special Issue Polymer Micelles II)

Abstract

:
Biocompatible amphiphilic statistical copolymers P(MEA/MPCm) composed of 2-methoxyethyl acrylate (MEA) and 2-methacryloyloxyethyl phosphorylcholine (MPC) were prepared with three different mol% of the hydrophilic unit MPC (m = 6, 12 and 46 mol%). The monomer reactivity ratios of MEA (rMEA) and MPC (rMPC) were 0.53 and 2.21, respectively. The rMEA × rMPC value of 1.17 demonstrated that statistical copolymerization was successful. P(MEA/MPC12) and P(MEA/MPC46) copolymers did not undergo aggregation in water, whereas the P(MEA/MPC6) copolymer formed micelles in water with a hydrodynamic radius (Rh) of 96.9 nm and a critical aggregation concentration, which was determined using pyrene fluorescence, at 0.0082 g/L. The restricted motion of the protons in the hydrophobic MEA units in the micelles’ cores provided additional evidence of self-association in P(MEA/MPC6).

Graphical Abstract

1. Introduction

The self-association of random copolymers has become increasingly important in drug delivery systems [1,2,3], imaging techniques [4,5,6,7] and many other fields [8]. The self-association behavior of amphiphilic random copolymers is more complicated than that of block polymers because of their ill-defined, randomly arranged monomer sequence. As such, the association between the hydrophobic units of a single polymer chain can form unimer micelles, and is independent of the polymer’s concentration or the presence of interpolymer micelles, which are generated via the interaction of multiple polymer chains above the critical aggregation concentration (CAC). Morishima et al. [9] investigated the self-organization of random copolymers of sodium 2-(acrylamido)-2-methylpropanesylfonate (AMPS) and methacrylamides bearing bulky hydrophobic groups, including n-dodecyl (LA), cyclododecyl (CD) and 1-adamantyl (AD) groups. Here, the aggregates formed from these random copolymers in aqueous solutions were due to intra and/or intermolecular self-association. The copolymers of AMPS and CD or AD tended to form unimer micelles up to a concentration limit of ca. 7 wt.%; conversely, the LA-containing copolymers self-associated to form unimers at concentrations below 0.2 wt.% and interpolymer aggregates at higher concentrations. These results showed that the chemical structure of the hydrophobic monomer in random copolymers was a critical factor in the self-association process. Additionally, the self-association of random copolymers depends on other factors, such as the type of solvent, the hydrophobic content in the copolymer [10,11], the distribution of the hydrophobic groups along the polymer chains [12], and the prevailing protocol for micellization [13]. Recently, Terashima et al. [11] reported on amphiphilic random methacrylate copolymers composed of poly(ethylene glycol) methacrylate and alkyl methacrylate (RMA) with linear alkyl chains that were 1–18 carbon units long. Here, copolymers with an RMA content of 20–40% tended to undergo single-chain folding even at polymer concentrations of up to ~6 wt.%. Generally, the copolymers tended to exist as unimer micelles in water when the concentration of dodecyl methacrylate (DMA) was less than 40 mol%, and as multi-chain aggregates when the concentration of DMA was over 50 mol%. Neal et al. [14] showed that the copolymer’s composition was important to the mean nano-object size of the structures formed from random copolymers. Here, a series of poly(n-butyl methacrylate-stat-methacrylic acid) (P(BMA-stat-MAA) statistical copolymers with various BMA/MAA compositions (i.e., from 77:23 to 93:7) was synthesized. It was found that the radii of the nano-objects formed by the self-assembly of the copolymers were independent of the copolymer’s molecular weight, but inversely proportional to the hydrophilic methyl methacrylate (MMA) content. In other words, fewer MAA units in the copolymer chain resulted in the formation of larger nano-objects. Since the polymer’s micelles were formed with a hydrophobic core and a hydrophilic shell, molecules that exhibited poor water solubility, such as pharmaceutical drugs, could be encapsulated, transported, and protected from the surrounding environment. Moreover, this tactic minimized the associated side effects of the drug and extended its circulation time [15].
The formation of micelles in water was investigated for applications in biological environments. Here, the hydrophobic domain of the polymer’s micelles encapsulated the hydrophobic drugs and imaging moieties, while the outer hydrophilic shell exhibited biocompatibility with various biological applications. Hydrophobic poly(2-methoxyethyl acrylate) (PMEA) showed excellent biological and blood compatibility, and inhibited the adsorption of proteins [16,17,18,19]. Hoshiba et al. [16] reported that the surface of PMEA underwent weak interactions with proteins and blood components due to the presence of “intermediate water” molecules in the polymer that crystallized at elevated temperatures. However, very little is known about the mechanism of expression of hemocompatibility in PMEA. Tanaka et al. [18] reported that the MEA content in MEA/2-hydroxyethyl methacrylate copolymers was an important parameter affecting the state of the water molecules in the polymer, ultimately influencing platelet compatibility. The lowest values associated with the adhesion number and the morphological changes in the platelets on the copolymer’s surface were observed in copolymers containing 80–100 mol% MEA. Conversely, the copolymers with less than 60 mol% MEA exhibited poor biocompatibility. Furthermore, PMEA has a glass transition temperature as low as −50 °C, is soluble in organic solvents, and exhibits traits such as hydrophobicity, transparency and adhesiveness, thereby making this compound a good coating material for various substrates. Reports have shown that PMEA is an effective coating agent for artificial heart–lung systems [20,21]. Poly(2-methacryloyloxyethylphosphorylcholine) (PMPC) has pendant phosphorylcholine groups and a structure that is identical to that of cell membrane phospholipids, thereby making it a useful biocompatible material for suppressing protein adsorption [22]. Copolymers containing 2-methacryloyloxyethyl phosphorylcholine (MPC) units with different structures have also been utilized for long-term biomedical applications [23,24,25,26,27,28,29,30,31,32]. Inspired by these results, we theorized that an MEA/MPC copolymer would exhibit excellent biocompatibility and would be useful for numerous biomedical applications.
In this research, biocompatible amphiphilic copolymers like P(MEA/MPCm), which were composed of hydrophobic 2-methoxyethyl acrylate (MEA) and hydrophilic MPC, were prepared via conventional free-radical polymerization. Here, m was equivalent to 6, 12 and 46 mol%, and was indicative of the number of hydrophilic MPC units present within the copolymer, as indicated via 1H NMR. In addition, the self-association behavior of P(MEA/MPCm) was investigated in water. In this case, P(MEA/MPC12) and P(MEA/MPC46) were dissolved in water as unimers, whereas P(MEA/MPC6) formed interpolymer micelles containing a PMEA hydrophobic domain and a PMPC shell (Figure 1).

2. Materials and Methods

2.1. Materials

2-Methoxyethyl acrylate (MEA, >98%), which had been obtained from Wako Pure Chemical (Osaka, Japan), was removed with a Sigma-Aldrich (St. Louis, MI, USA) inhibitor remover column. 2-Methacryloyloxyethyl phosphorylcholine (MPC), which had been obtained from NOF Corp. (Tokyo, Japan), was purified using a previously reported method [33]. 2′-Azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70, >95%), which had been purchased from Wako Pure Chemical (Osaka, Japan), was used as received without any further purification. The pyrene (97%) purchased from Wako Pure Chemical was purified via recrystallization using methanol. Methanol was dried using 4Å molecular sieves and purified via distillation. Water was purified with an ion-exchange column system.

2.2. Monomer Reactivity Ratio and Polymerization Kinetics

The monomer reactivity ratio was determined using the Fineman–Ross method [34]. Here, MEA, MPC and V-70 were dissolved in methanol with feed ratios of MPC ranging from 10% to 90% (([MEA] + [MPC])/[V-70] = 100/0.4). A small amount of methanol-d4 was added to the solution, which was transferred to NMR tubes and purged with argon gas for 30 min. Polymerization was performed in an oil bath at 40 °C. Quenching procedures were conducted via rapid cooling in an ice bath when the monomer conversion, which was monitored via 1H NMR, was less than 20%. The reaction mixture was dialyzed (MWCO:500 ~ 1000) using pure water for one night. Next, the solvent was removed via evaporation, and then the residue obtained was subsequently dissolved in 300 µL of methanol-d4 before 1H NMR analysis was conducted. The MEA and MPC contents in the copolymer were determined by comparing the 1H NMR integral intensities of the peaks attributed to the pendant methylene protons in MEA (3.62 ppm) and MPC (3.72 ppm) (Figure S2 and Table S1).
The ratio (mMEA/mMPC = f) of the MEA and MPC contents in the copolymer was determined using the following equation:
m MEA m MPC = [ M MEA ] 0 [ M MPC ] 0 × r MEA [ M MEA ] 0 + [ M MPC ] 0 r MPC [ M MPC ] 0 + [ M MEA ] 0
where mMEA and mMPC are the molar contents of MEA and MPC in the copolymer, [MMEA]0 and [MMPC]0 are the initial molar concentration of the MEA and MPC monomers before polymerization, and rMEA and rMPC are the monomer reactivity ratios of MEA and MPC. Equation (1) can be rewritten as:
F ( f 1 ) f = r MEA F 2 f r MPC
where F is the ratio of the initial molar concentrations of MEA and MPC (=[MMEA]0/[MMPC]0). A plot of F(f − 1)/f as the ordinate and (F2/f) as the abscissa results in a straight line whose slope is represented by rMEA, and the intercept is the negative rMPC value.
The relationship between the extent of the monomer conversion and the polymerization time was also studied. Here, MEA (65.5 mg, 0.503 mmol), MPC (148.5 mg, 0.503 mmol) and V-70 (1.28 mg, 0.00412 mmol) were dissolved in 0.5 mL of methanol-d4 ([MEA]/[MPC]/[V-70] = 50/50/0.4) before the solution was transferred to an NMR tube and purged with argon gas for 30 min. The polymerization reaction was performed at 40 °C, and NMR analysis was used to monitor the process. The resulting NMR spectra were recorded at different polymerization times to determine the extent of conversion of the MEA and MPC monomers by comparing the integral intensity ratios of the vinyl protons observed at 6.37 and 5.62 ppm, respectively, before and after polymerization.

2.3. Preparation of the MEA Homopolymer

PMEA was synthesized via the conventional free-radical polymerization reaction using the following procedure. First, MEA (0.260 g, 2.0 mmol) and V-70 (2.45 mg, 0.008 mmol) were dissolved in methanol (2.0 mL), and the mixture was purged with Ar gas in 30 min before polymerization was conducted at 40 °C for 18 h. We noted that MEA conversion was 66.7%. After polymerization, the solution was dialyzed using methanol for one day and pure water for an additional 24 h. Mild precipitation was observed after dialysis. The solution was transferred to a 20-mL glass bottle (Figure S3a) and was subjected to dynamic light scattering (DLS) as a means of monitoring the formation of PMEA polymer micelles. After a portion of the aqueous solution was evaporated under vacuum, the residue obtained was dissolved in methanol-d4 or the mobile phase to prepare samples for 1H NMR analysis or size exclusion chromatography (SEC), respectively.

2.4. Preparation of the P(MEA/MPCm) Copolymer

Statistical copolymers (i.e., P(MEA/MPCm)) were synthesized via conventional free-radical polymerization in methanol using three MPC feed mol% values, namely, 5, 10 and 40 mol% (Figure 1). A typical procedure for the synthesis of P(MEA/MPCm), with m in the feed of 10 mol%, was as follows: first, MEA (0.240 g, 1.84 mmol), MPC (0.0594 g, 0.201 mmol) and V-70 (25.2 mg, 0.082 mmol) were dissolved in methanol (2.0 mL). The mixture was then purged with Ar gas for 30 min and subsequently stirred at 40 °C for 18 h. After polymerization, the reaction mixture was dialyzed using methanol for one day and then pure water for an additional 24 h. After dialysis, the P(MEA/MPC6) solution obtained was cloudy, indicating the formation of polymer micelles. Clear liquids were obtained in other cases, i.e., for P(MEA/MPC12) and P(MEA/MPC46) (Figure S3). The polymer solutions after dialysis were used for experiments focused on determining the association behavior of the copolymers in water. 1H NMR spectroscopy was conducted after purification to estimate the MEA and MPC contents of the copolymers obtained. A portion of the solution was freeze-dried, and the residue was dissolved in methanol or methanol-d4 to prepare a solution for further experimentation.

2.5. Measurements

1H NMR spectroscopy was performed on a JNM-ECZ 400 MHz spectrometer (JEOL, Tokyo, Japan) using D2O or methanol-d4 as the deuterated solvents. Spin–spin relaxation times (T2) were measured using the Car–Purcell–Meiboom–Gill method. Echoes were observed at the 180° pulse, and the amplitude of the successive echoes decayed exponentially with a time constant equal to T2 [35]. Array parameters of the delay list, which included 16 points, were set for conducting the measurements. The data were analyzed via the Weight Linear Spin Lock method using Delta v5.3.1 software (JEOL, Tokyo, Japan). SEC was performed using an instrument equipped with a 7.0-μm bead GF-7M HQ column from Shodex (Tokyo, Japan) and a Shodex RI-101 refractive index (RI) detector operating at 40 °C. The elution phase was methanol containing 0.1 M lithium perchlorate at a flow rate of 0.6 mL/min. Poly(ethylene oxide) was used to prepare the universal standard curve to determine the number-average molecular weight (Mn) and the molecular weight distribution (Đ). Sample solutions were filtered using a 0.2-μm pore size membrane conducting the relevant measurements. The hydrodynamic radius (Rh) and light scattering intensity (LSI) of P(MEA/MPCm) in water were obtained using a Malvern (Worcestershire, UK) Zetasizer 7.11 equipped with a 4-mW He–Ne laser at 25 °C. The wavelength of the light source was 632.8 nm. The data obtained were analyzed using a Malvern (Worcestershire, UK) Zetasizer 7.11. The polymer concentration (Cp) of P(MEA/MPCm) in aqueous solution was fixed at 1.0 g/L. The sample solutions were filtered with a 0.45-μm pore size membrane before conducting the analysis. Transmission electron microscopy (TEM) was performed using a JEOL JEM-2100F (Tokyo, Japan) with an acceleration voltage of 160 kV. The samples were prepared by adding the respective aqueous polymer solution dropwise onto a JEOL (Tokyo, Japan) 150-mesh copper TEM grid, and subsequently staining it with 0.1 wt.% phosphotungstic acid aqueous solution. Next, the samples were dried under vacuum conditions at room temperature. Static light scattering (SLS) measurements were conducted using a DLS-7000 Otsuka Electronics PhotalTM (Osaka, Japan) at 25 °C, with a He–Ne laser (10.0 mW at 632.8 nm) as the light source. The weight-average molecular weight (Mw), the radius of gyration (Rg) and the second virial coefficient (A2) of the P(MEA/MPC6) polymer micelles in water were estimated from Zimm plots constructed using data derived from aqueous polymer solutions at two different concentrations (i.e., 0.25 and 0.5 g/L). The Mw and Rg values of all copolymers in methanol in the random-coil state were calculated from the Zimm plot at 10 g/L. The RI increment (dn/dCp) values were determined using a DRM-3000 differential refractometer (Otsuka Electronics Co., Osaka, Japan) at 25 °C. The dn/dCp values were 0.0619, 0.0768 and 0.104 mL/g for P(MEA/MPCm) in methanol, with m values of 5, 10 and 40 mol%, respectively, in the feed. These values were used for conducting SLS analysis of the corresponding samples. The CAC of the polymer aqueous solution was determined using pyrene as the fluorescent probe. The fluorescence spectra of the pyrene/polymer aqueous solutions were recorded with an F-2500 fluorescence spectrophotometer from Hitachi (Tokyo, Japan).

3. Results and Discussion

3.1. Determination of the Monomer Reactivity Ratio

Conventional free-radical polymerizations of equimolar concentrations of MEA and MPC were conducted in the presence of the V-70 initiator at 40 °C. Here, the monomer concentration was estimated based on the observed decrease in the integral intensity of the vinyl protons in the 1H NMR spectra, at 6.37 and 5.62 ppm for MEA and MPC, respectively. The time conversion plots (Figure S1a) indicated that MPC conversion rapidly reached 90% after 120 min and continued to increase to 99% after 300 min. Conversely, the MEA reaction was notably slower, as MEA conversion after 300 min was 82%. These results were consistent with the reported monomer reactivity findings obtained using the Fineman–Ross method (Figure 2b). The first-order kinetic plots showed that both plots were linearly related to the polymerization time during the early stages of the polymerization reaction until the 100-min time mark, indicating that the propagating radical concentration was constant (Figure S1b). The late stages of the polymerization reaction (i.e., after 100 min) produced plots with a downward curvature, suggesting that the propagating radical concentration had decreased. Thus, a straight fitted line was obtained from the Fineman–Ross plots, in which the slope and intercept represented the monomer reactivity ratios of MEA and MPC, respectively. The monomer reactivity ratios of MEA and MPC were 0.53 and 2.21, respectively. Since the reactivity of MPC was almost four times higher than that of MEA, the probability of MPC being incorporated into the copolymer was much higher. Figure 2a also showed that the MPC mol% in the copolymer was always higher than the percentage of MPC in the feed ratio. The reactivity ratios of MEA and MPC were in good agreement with the values observed during the copolymerization of methyl acrylate (MA) and MMA, both of which possessed similar structures. Grassie et al. [36] reported that the reactivity ratios of MA and MMA were 0.35 and 1.8, respectively, during copolymerization at 65 °C. For MA and MMA, these values were 0.47 and 2.3, respectively, during copolymerization at 130 °C, indicating that the reactivity ratio of MMA was almost four to five times higher than MA, and was temperature-independent. From the results, rMEA × rMPC was 1.17, which demonstrated that an almost random monomer sequence was the main feature of the copolymerization process in these compounds. Note, however, that the repeating units in the copolymer were composed of more MPC, since MPC was significantly more active than MEA.

3.2. Preparation of PMEA and P(MEA/MPCm)

PMEA was prepared via conventional free-radical polymerization reactions. The conversion of MEA, which was estimated from the corresponding NMR data, was 66.7%. The Mn and Đ values were 1.32 × 104 g/mol and 2.54, respectively. The P(MEA/MPCm) copolymers were prepared with three different compositions (i.e., m = 6, 12 and 46 mol%) via conventional free-radical polymerization reactions. The conversions of the MEA and MPC monomers were in the ranges of 72–89% and 98–100%, respectively. The MPC content in the copolymer was estimated from 1H NMR spectra obtained in methanol-d4, using the integral intensity ratio of the peaks attributed to the pendant methylene protons in the MEA and MPC units; these peaks were observed at 3.62 and 3.72 ppm for MEA and MPC, respectively (Figure 3 and Table S2). SEC measurements were conducted for all polymers, and unimodal curves were observed for all samples with Đ values between 2.0 and 2.6 (Figure S4). We theorized that this was due to the occurrence of uncontrolled polymerization. The SEC charts indicated that P(MEA/MPC46) had the longest retention time (Figure S4), which was possibly due to unexpected interactions between the SEC column and the copolymer. The Mw values of a single polymer chain were determined using SLS measurements in methanol. Unimodal distribution was observed in the DLS results for the methanolic solutions of the copolymer, with small Rh values between 9 and 10 nm (Figure S5). The Rg and Mw values of the copolymers were estimated via conducting SLS measurements in methanol (Figure S6). Here, we noted that the Rg/Rh values for all the copolymers were less than or equal to 1.6, indicating that the polymers were dissolved in methanol as with a large polydispersity index (PDI) [37]. In particular, the Rg/Rh value for P(MEA/MPC46) was associated with a large degree of error due to the bimodal Rh distribution (Figure S5). These features made it possible to determine the molecular weight of the individual polymer chains using SLS measurements in methanol. The characteristics of all samples are summarized in Table 1.

3.3. Self-Association Behavior of P(MEA/MPCm) in Water

NMR measurements were recorded for all copolymers in D2O (Figure 4). Here, the pendant methylene proton signals of the MEA units were observed at 3.68 ppm in D2O, which was shifted downfield from their position at 3.62 ppm in methanol-d4. As a result, the signals of the MEA and MPC units overlapped at 3.72 ppm.
The dynamic motion of individual molecular segments could be estimated by measuring the 1H NMR spin–spin relaxation time (T2) [38,39]. We noted that when the polymer micelles were formed, the motion of the protons relative to the hydrophobic MEA unit was restricted to the hydrophobic domain of the polymer micelle. As a result, restrictions in the motion of the MEA units decreased the T2 values. Here, the T2 values were estimated for the methyl protons at 3.39 and 3.23 ppm in the MEA and MPC units of the copolymers, respectively, in D2O (Figure 5). We noted that the T2 values of the pendant methyl protons in the MEA units decreased with decreasing m, as exemplified by the smallest value of 332 ms, which was obtained when m was 6 mol%. For P(MEA/MPC12) and P(MEA/MPC46), the T2 values (namely, 528 and 561 ms, respectively) were greater than those observed for P(MEA/MPC6). The T2 values did not significantly change when m increased from 12 to 46 mol%. These observations indicated that the motion of the hydrophobic MEA units in P(MEA/MPC6) was restricted due to the formation of the hydrophobic domain. In contrast, the motion of the MEA units in P(MEA/MPC12) and P(MEA/MPC46) was free, since these copolymers were dissolved as unimers in water. The T2 values of the pendant methyl protons in the MPC units were almost the same, regardless of the m value; for P(MEA/MPC6), P(MEA/MPC12), and P(MEA/MPC46), these values were 393, 414, and 412 ms, respectively. As noted earlier, the hydrophilic MPC units were arranged on the surface of the micelles when P(MEA/MPC6) formed polymer micelles, whereas P(MEA/MPC12) and P(MEA/MPC46) were dissolved as unimers. Since the MPC units were always exposed to water, their motion remained almost the same for all samples. The T2 values of the pendant methyl protons in the MPC units of P(MEA/MPC6) decreased slightly as some of the MPC units may have been incorporated into the hydrophobic domain due to the statistical sequence in the copolymer’s structure. These results provided additional evidence of the formation of polymer micelles of P(MEA/MPC6) in water.
The self-association behavior of P(MEA/MPCm) in water was studied by conducting DLS measurements on the copolymer aqueous solutions at Cp = 1.0 g/L (Figure 6). Here, the Rh distribution values for PMEA were established as a reference sample. Small amounts of precipitate were obtained after the purification of PMEA via dialysis, which contained high molecular weight chains (i.e., large aggregates) that were removed via filtration. The PMEA chains with lower molecular weight values did not precipitate, as they were dispersed in water during dialysis. For the aqueous solution of P(MEA/MPC46), unimodal distribution was observed with a small Rh value of 9.0 nm, suggesting that P(MEA/MPC46) was dissolved in water as the unimer. Interestingly, bimodal distribution was observed in P(MEA/MPC12), which contained one peak with the same Rh value (i.e., 9.0 nm) as P(MEA/MPC46) in water and another peak with a higher Rh (i.e., 222 nm) value. In this case, the formation of interpolymer associates composed of some of the hydrophobic MEA units in the copolymer was identified as the reason for these observations.
Generally, weak hydrophobic interactions were noted when the hydrophobic content in the polymer was insufficient, resulting in the formation of only a few micelles. For PMEA and P(MEA/MPC6), unimodal distribution was noted with Rh values of 290 and 96.9 nm, respectively, indicating that P(MEA/MPC6), with its 94 mol% of the hydrophobic MEA unit, easily formed interpolymer aggregates in water. The radius of the polymer aggregates increased when PMEA was employed, resulting in self-association to generate larger aggregates in water. All of the above mentioned findings were supported by the results obtained via LSI analysis of these samples. Here, the precipitation observed after dialysis using pure water was evidence that PMEA could form very large aggregates. Only the supernatant was used for DLS analysis, and the estimated concentration of the PMEA aqueous solution was believed to be lower than the true value. This was proposed as the possible reason for the lower LSI values observed for PMEA relative to P(MEA/MPC6) in water at the same concentration. By extension, the LSI values of both PMEA and P(MEA/MPC6) were greater than those obtained for P(MEA/MPC12) and P(MEA/MPC46) due to the formation of polymer micelles. Since P(MEA/MPC46) was dissolved as random coils in water, the smallest recorded LSI value in our study was 0.087 Mcps. As noted, the aqueous solution of PMEA became cloudier after a few days, whereas the P(MEA/MPC6) aggregates exhibited increased stability over the same observation time. The stability of the P(MEA/MPC6) aggregates during dilution was confirmed via DLS measurements. Here, the Rh values of P(MEA/MPC6) were nearly constant and independent of Cp in the 0.05–5 g/L region (Figure S7). Note, however, that lower concentrations were difficult to measure due to the low LSI values associated.
On another note, spherical objects were observed for PMEA and P(MEA/MPC6) copolymers using TEM (Figure 7), with average radii of 240 and 103 nm for PMEA and P(MEA/MPC6), respectively. Additional TEM observations for P(MEA/MPC6) are shown in Figure S8.
The characterization of the P(MEA/MPC6) micelles in water was conducted via SLS measurements (Figure 8). Here, the dn/dCp value for P(MEA/MPC6) in water was 0.0651 mL/g, and was subsequently used during SLS analysis to estimate the apparent Mw of the P(MEA/MPC6) micelles. The aggregation number (Nagg), which is the number of individual polymer chains present in one micelle, was calculated from the Mw values of the polymer micelle in water and the individual polymer chain in methanol obtained from SLS measurements. The Nagg of P(MEA/MPC6) micelle was 143 in water, indicating the formation of interpolymer micelles. It was speculated that the hydrophobic interactions between the MEA units in the individual polymer chains were too weak to facilitate the self-folding of a single chain. For P(MEA/MPC6) with 94 mol% of the relatively hydrophobic MEA units in the copolymer’s composition, hydrophobic interactions between multiple chains resulted in interpolymer aggregates. This phenomenon was also seen in the aqueous solution of random copolymers of sodium 2-(acrylamido)-2-methylpropanesulfonate and n-dodecyl methacrylamide, and in the copolymers of poly(ethylene glycol) methacrylate and n-dodecyl methacrylate. Here, interpolymer aggregates were formed when the hydrophobic content of the copolymer exceeded 50 mol% [10,11].
Theoretically, the shape and size distribution of the aggregates can be estimated using Rg/Rh. For instance, a value of 0.778 represents a rigid sphere with a narrow distribution, whereas a value of 1.0 is associated with spherical aggregates, and values higher than 2 are often seen in rodlike structures [37,40]. In our study, the Rg/Rh value for P(MEA/MPC6) in water was 0.95, indicating that the polymer micelles were spherical (Table 2). The A2 value provides information about the affinity of solute molecules with the solvent of interest [41]. For our case, the A2 value obtained from the SLS analysis of P(MEA/MPC6) in water was 2.5 × 10−5 cm3 g−2 mol. This positive value was proof that the hydrophilic MPC unit had completely covered P(MEA/MPC6), thereby facilitating its solubility in water. The A2 value for the MPC homopolymer was reported as 2.5 × 104 cm3 g−2 mol in aqueous solution [42]. The A2 value for P(MEA/MPC6) was 10 times lower than that of the MPC homopolymer, which was attributed to the composition of the copolymer; here, the copolymer consisted of 94 mol% of the hydrophobic MEA unit.
The CAC value of P(MEA/MPC6) was determined via fluorescence spectroscopy using pyrene as the probe molecule. Pyrene is hydrophobic and its fluorescence spectrum is heavily dependent on the polarity of the surrounding environment. The intensity ratio (I3/I1) between the third and the first vibronic peaks in the pyrene emission spectra can be used as a measure of the environmental polarity [43]. Therefore, the fluorescence spectra of pyrene in the presence of P(MEA/MPC6) at varying Cp were recorded at the excitation wavelength of 334 nm (Figure S9). The changes in the I3/I1 ratio in the pyrene emission spectra were plotted as a function of Cp to determine CAC (Figure 9). We noted that the copolymers did not form micelles below the CAC. The solubility of pyrene in water ensured that the resulting fluorescence spectrum remained almost unchanged (I3/I1 ≈ 0.572). This calculated value was nearly the same as that obtained for pyrene in the absence of the copolymer (I3/I1 ≈ 0.562), demonstrating that there was no discernible difference in the polarity of the environment surrounding pyrene as the P(MEA/MPC6) copolymer was locked in random coils at low concentrations in water. However, the formation of copolymer micelles above the CAC meant that the pyrene molecules were entrapped in the hydrophobic domains. As such, the pyrene molecules were surrounded by a non-polar environment. The number of pyrene molecules in the hydrophobic domain increased when Cp rose. Consequently, the I3/I1 value gradually increased to a maximum of 0.602 at Cp = 0.08 g/L. The CAC value of P(MEA/MPC6) in water was determined at the inflection point as 0.0082 g/L. Unlike the formation of unimer micelles independent of Cp, P(MEA/MPC6) was incapable of aggregation in dilute aqueous solutions. Interpolymer association occurred when the P(MEA/MPC6) concentration increased to a certain level. Therefore, the CAC value was determined as the Cp at which the interpolymer micelles started to form.

4. Conclusions

Biocompatible, amphiphilic, statistical copolymers, P(MEA/MPCm), which were composed of hydrophobic MEA and hydrophilic MPC units, were prepared via conventional free-radical polymerization reactions. P(MEA/MPC12) and P(MEA/MPC46) possessed a high MPC content, were dissolved as unimers, and did not aggregate in water. On the other hand, P(MEA/MPC6) formed uniform micelles composed of a PMEA core and a PMPC shell, with Rh and Nagg values of 96.9 nm and 133, respectively, due to the hydrophobic interactions of the MEA units. The mobility of the MEA units in P(MEA/MPC6) was restricted, as confirmed via the observed 1H NMR spin–spin relaxation times. A slight decrease in the motion of the MPC units was also observed and was attributed to the entrapment of some MPC units in the hydrophobic domain; the associated interpolymer aggregates were covered by phosphorylcholine groups. From these results, we concluded that P(MEA/MPCm) copolymers with m ≤ 6 mol% formed micelles, and, as such, were well suited for biomedical applications.

Supplementary Materials

The following are available online at https://www.mdpi.com/2073-4360/12/8/1808/s1: Figure S1. (a) Time-conversion and (b) the pseudo first-order kinetic plots for conventional free-radical polymerization of equimolar concentrations of MEA () and MPC () in methanol at 40 °C. [M]0 and [M] were the monomer concentrations at a polymerization times of 0 and t min, respectively; Figure S2. 1H NMR spectra of P(MEA/MPCm) with various feed mol% of the hydrophilic MPC in methanol-d4 at room temperature; Figure S3. Photographs of (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12) and (d) P(MEA/MPC46) solutions after dialysis using pure water; Figure S4. SEC elution curves for (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12) and (d) P(MEA/MPC46) using methanol containing 0.1 M lithium perchlorate as the eluent at 40 °C; Figure S5. Hydrodynamic radius (Rh) distributions for (a) P(MEA/MPC6), (b) P(MEA/MPC12) and (c) P(MEA/MPC46) in methanol at Cp = 10 g/L at 25 °C; Figure S6. Zimm plots of (a) P(MEA/MPC6), (b) P(MEA/MPC12) and (c) P(MEA/MPC46) in methanol at 25 °C; Figure S7. Hydrodynamic radius (Rh) of P(MEA/MPC6) as a function of polymer concentration (Cp) in water; Figure S8. Transmission electron microscopy (TEM) images for P(MEA/MPC6) at Cp = 1.0 g/L in water with different magnification; Figure S9. Fluorescence spectra of pyrene excited at 334 nm in water in the presence of P(MEA/MPC6) at Cp = 0.08 (solid line) and 0.0012 g/L (dashed line); Table S1. The Fineman–Ross parameters of the copolymers, as determined using 1H NMR measurements in methanol-d4 at room temperature; and Table S2. The composition of the copolymer, as estimated using 1H NMR measurements in methanol-d4 at room temperature.

Author Contributions

Conceptualization, T.L.N. and S.-i.Y.; Methodology, T.L.N., Y.K. and S.-i.Y.; Data curation, T.L.N. and S.-i.Y.; Project administration, S.-i.Y.; Writing—original draft, T.L.N. and S.-i.Y.; Writing—review and editing, S.-i.Y. and K.I. All authors have read and agreed to the published version of the manuscript.

Funding

This work was funded by a Grant-in-Aid for Scientific Research (17H03071) from the Japan Society for the Promotion of Science (JSPS), JSPS Bilateral Joint Research Projects (JPJSBP120203509), and the Cooperative Research Program of “Network Joint Research Center for Materials and Devices (20204034).”

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Geng, Y.; Discher, D.E. Hydrolytic degradation of poly(ethylene oxide)-block-polycaprolactone worm micelles. J. Am. Chem. Soc. 2005, 127, 12780–12781. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  2. Duncan, R. The dawning era of polymer therapeutics. Nat. Rev. Drug Discov. 2003, 2, 347–360. [Google Scholar] [CrossRef] [PubMed]
  3. Tong, R.; Cheng, J. Anticancer polymeric nanomedicines. Polym. Rev. 2007, 47, 345–381. [Google Scholar] [CrossRef]
  4. Choi, K.Y.; Liu, G.; Lee, S.; Chen, X. Theranostic nanoplatforms for simultaneous cancer imaging and therapy: Current approaches and future perspectives. Nanoscale 2012, 4, 330–342. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  5. Cui, S.; Yin, D.; Chen, Y.; Di, Y.; Chen, H.; Ma, Y.; Achilefu, S.; Gu, Y. In vivo targeted deep-tissue photodynamic therapy based on near-infrared light triggered upconversion nanoconstruct. ACS Nano 2013, 7, 676–688. [Google Scholar] [CrossRef]
  6. Lee, S.J.; Koo, H.; Jeong, H.; Huh, M.S.; Choi, Y.; Jeong, S.Y.; Byun, Y.; Choi, K.; Kim, K.; Kwon, I.C. Comparative study of photosensitizer loaded and conjugated glycol chitosan nanoparticles for cancer therapy. J. Control. Release 2011, 152, 21–29. [Google Scholar] [CrossRef]
  7. Williams, R.J.; Dove, A.P.; O’Reilly, R.K. Self-assembly of cyclic polymers. Polym. Chem. 2015, 6, 2998–3008. [Google Scholar] [CrossRef] [Green Version]
  8. Li, L.; Raghupathi, K.; Song, C.; Prasad, P.; Thayumanavan, S. Self-assembly of random copolymers. Chem. Commun. 2014, 50, 13417–13432. [Google Scholar] [CrossRef] [Green Version]
  9. Morishima, Y.; Nomura, S.; Ikeda, T.; Seki, M.; Kamachi, M. Characterization of unimolecular micelles of random copolymers of sodium 2-(acrylamido)-2-methylpropanesulfonate and methacrylamides bearing bulky hydrophobic substituents. Macromolecules 1995, 28, 2874–2881. [Google Scholar] [CrossRef]
  10. Yamamoto, H.; Morishima, Y. Effect of hydrophobe content on intra- and interpolymer self-associations of hydrophobically modified poly(sodium 2-(acrylamido)-2-methylpropanesulfonate) in water. Macromolecules 1999, 32, 7469–7475. [Google Scholar] [CrossRef]
  11. Terashima, T.; Sugita, T.; Fukae, K.; Sawamoto, M. Synthesis and single-chain folding of amphiphilic random copolymers in water. Macromolecules 2014, 47, 589–600. [Google Scholar] [CrossRef]
  12. Chang, Y.; McCormick, C.L. Water-soluble copolymers. 49. Effect of the distribution of the hydrophobic cationic monomer dimethyldodecyl(2-acrylamidoethyl)ammonium bromide on the solution behavior of associating acrylamide copolymers. Macromolecules 1993, 26, 6121–6126. [Google Scholar] [CrossRef]
  13. Yamamoto, H.; Hashidzume, A.; Morishima, Y. Micellization protocols for amphiphilic polyelectrolytes in water. How do polymers undergo intrapolymer associations? Polym. J. 2000, 32, 745–752. [Google Scholar] [CrossRef] [Green Version]
  14. Neal, T.J.; Beattie, D.L.; Byard, S.J.; Smith, G.N.; Murray, M.W.; Williams, N.S.J.; Emmett, S.N.; Armes, S.P.; Spain, S.G.; Mykhaylyk, O.O. Self-assembly of amphiphilic statistical copolymers and their aqueous rheological properties. Macromolecules 2018, 51, 1474–1487. [Google Scholar] [CrossRef] [Green Version]
  15. Movassaghian, S.; Merkel, O.M.; Torchilin, V.P. Applications of polymer micelles for imaging and drug delivery. Wiley Interdiscip. Rev. Nanomed. Nanobiotechnol. 2015, 7, 691–707. [Google Scholar] [CrossRef]
  16. Hoshiba, T.; Otaki, T.; Nemoto, E.; Maruyama, H.; Tanaka, M. Blood-compatible polymer for hepatocyte culture with high hepatocyte-specific functions toward bioartificial liver development. ACS Appl. Mater. Interfaces 2015, 7, 18096–18103. [Google Scholar] [CrossRef]
  17. Murakami, D.; Kobayashi, S.; Tanaka, M. Interfacial structures and fibrinogen adsorption at blood-compatible polymer/water interfaces. ACS Biomater. Sci. Eng. 2016, 2, 2122–2126. [Google Scholar] [CrossRef]
  18. Tanaka, M.; Mochizuki, A.; Ishii, N.; Motomura, T.; Hatakeyama, T. Study of blood compatibility with poly(2-methoxyethyl acrylate). relationship between water structure and platelet compatibility in poly(2-methoxyethylacrylate-co-2-hydroxyethylmethacrylate). Biomacromolecules 2002, 3, 36–41. [Google Scholar] [CrossRef]
  19. Morita, S.; Tanaka, M.; Ozaki, Y. Time-resolved in situ ATR-IR observations of the process of sorption of water into a poly(2-methoxyethyl acrylate) film. Langmuir 2007, 23, 3750–3761. [Google Scholar] [CrossRef]
  20. Kobayashi, S.; Wakui, M.; Iwata, Y.; Tanaka, M. Poly(ω-methoxyalkyl acrylate)s: Nonthrombogenic polymer family with tunable protein adsorption. Biomacromolecules 2017, 18, 4214–4223. [Google Scholar] [CrossRef]
  21. Haraguchi, K.; Takehisa, T.; Mizuno, T.; Kubota, K. Antithrombogenic properties of amphiphilic block copolymer coatings: Evaluation of hemocompatibility using whole blood. ACS Biomater. Sci. Eng. 2015, 1, 352–362. [Google Scholar] [CrossRef]
  22. Kyomoto, M.; Ishihara, K. Self-initiated surface graft polymerization of 2-methacryloyloxyethyl phosphorylcholine on poly(ether ether ketone) by photoirradiation. ACS Appl. Mater. Interfaces 2009, 1, 537–542. [Google Scholar] [CrossRef] [PubMed]
  23. Ishihara, K.; Iwasaki, Y.; Nakabayashi, N. Polymeric lipid nanosphere consisting of water-soluble poly(2-methacryloyloxyethyl phosphorylcholine-co-n-butyl methacrylate). Polym. J. 1999, 31, 1231–1236. [Google Scholar] [CrossRef] [Green Version]
  24. Kojima, R.; Kasuya, M.C.Z.; Ishihara, K.; Hatanaka, K. Synthesis of amphiphilic copolymers by soap-free interface-mediated polymerization. Polym. J. 2009, 41, 370–373. [Google Scholar] [CrossRef]
  25. Kojima, R.; Kasuya, M.C.Z.; Ishihara, K.; Hatanaka, K. Physicochemical delivery of amphiphilic copolymers to specific organelles. Polym. J. 2011, 43, 718–722. [Google Scholar] [CrossRef]
  26. Ma, Y.; Tang, Y.; Billingham, N.C.; Armes, S.P.; Lewis, A.L.; Lloyd, A.W.; Salvage, J.P. Well-defined biocompatible block copolymers via atom transfer radical polymerization of 2-methacryloyloxyethyl phosphorylcholine in protic media. Macromolecules 2003, 36, 3475–3484. [Google Scholar] [CrossRef]
  27. Iwasaki, Y.; Akiyoshi, K. Design of biodegradable amphiphilic polymers:  Well-defined amphiphilic polyphosphates with hydrophilic graft chains via atrp. Macromolecules 2004, 37, 7637–7642. [Google Scholar] [CrossRef]
  28. Ishihara, K. Revolutionary advances in 2-methacryloyloxyethyl phosphorylcholine polymers as biomaterials. J. Biomed. Mater. Res. Part A 2019, 107, 933–943. [Google Scholar] [CrossRef]
  29. Chen, S.-H.; Chang, Y.; Ishihara, K. Reduced blood cell adhesion on polypropylene substrates through a simple surface zwitterionization. Langmuir 2017, 33, 611–621. [Google Scholar] [CrossRef]
  30. Iwasaki, Y.; Ishihara, K. Cell membrane-inspired phospholipid polymers for developing medical devices with excellent biointerfaces. Sci. Technol. Adv. Mater. 2012, 13, 64101. [Google Scholar] [CrossRef]
  31. Sugihara, S.; Blanazs, A.; Armes, S.P.; Ryan, A.J.; Lewis, A.L. Aqueous dispersion polymerization: A new paradigm for in situ block copolymer self-assembly in concentrated solution. J. Am. Chem. Soc. 2011, 133, 15707–15713. [Google Scholar] [CrossRef] [PubMed]
  32. Du, J.; Armes, S.P. Preparation of biocompatible zwitterionic block copolymer vesicles by direct dissolution in water and subsequent silicification within their membranes. Langmuir 2009, 25, 9564–9570. [Google Scholar] [CrossRef] [PubMed]
  33. Ishihara, K.; Ueda, T.; Nakabayashi, N. Preparation of phospholipid polymers and their properties as polymer hydrogel membranes. Polym. J. 1990, 22, 355–360. [Google Scholar] [CrossRef]
  34. Fineman, M.; Ross, S.D. Linear method for determining monomer reactivity ratios in copolymerization. J. Polym. Sci. 1950, 5, 259–262. [Google Scholar] [CrossRef]
  35. Meiboom, S.; Gill, D. Modified spin-echo method for measuring nuclear relaxation times. Rev. Sci. Instrum. 1958, 29, 688–691. [Google Scholar] [CrossRef] [Green Version]
  36. Grassie, N.; Torrance, B.J.D.; Fortune, J.D.; Gemmell, J.D. Reactivity ratios for the copolymerization of acrylates and methacrylates by nuclear magnetic resonance spectroscopy. Polymer 1965, 6, 653–658. [Google Scholar] [CrossRef]
  37. Adolphi, U.; Kulicke, W.-M. Coil dimensions and conformation of macromolecules in aqueous media from flow field-flow fractionation/multi-angle laser light scattering illustrated by studies on pullulan. Polymer 1997, 38, 1513–1519. [Google Scholar] [CrossRef]
  38. Bloembergen, N.; Purcell, E.M.; Pound, R.V. Relaxation effects in nuclear magnetic resonance absorption. Phys. Rev. 1948, 73, 679–712. [Google Scholar] [CrossRef]
  39. Zhao, S.; Yuan, H.-Z.; Yu, J.-Y.; Du, Y.-R. Hydrocarbon chain packing in the micellar core of surfactants studied by 1H NMR relaxation. Colloid Polym. Sci. 1998, 276, 1125–1130. [Google Scholar] [CrossRef]
  40. Akcasu, A.Z.; Han, C.C. Molecular weight and temperature dependence of polymer dimensions in solution. Macromolecules 1979, 12, 276–280. [Google Scholar] [CrossRef]
  41. Bruns, W. The second osmotic virial coefficient of polymer solutions. Macromolecules 1996, 29, 2641–2643. [Google Scholar] [CrossRef]
  42. Matsuda, Y.; Kobayashi, M.; Annaka, M.; Ishihara, K.; Takahara, A. Dimensions of a free linear polymer and polymer immobilized on silica nanoparticles of a zwitterionic polymer in aqueous solutions with various ionic strengths. Langmuir 2008, 24, 8772–8778. [Google Scholar] [CrossRef]
  43. Kalyanasundaram, K.; Thomas, J.K. Environmental effects on vibronic band intensities in pyrene monomer fluorescence and their application in studies of micellar systems. J. Am. Chem. Soc. 1977, 99, 2039–2044. [Google Scholar] [CrossRef]
Figure 1. Synthesis and conceptual illustration of the self-assembly processes of the statistical copolymer, P(MEA/MPCm), in water.
Figure 1. Synthesis and conceptual illustration of the self-assembly processes of the statistical copolymer, P(MEA/MPCm), in water.
Polymers 12 01808 g001
Figure 2. (a) Relationship between the 2-methacryloyloxyethyl phosphorylcholine (MPC) content in the copolymer and the feed. (b) The graphic representation of the Fineman–Ross equation, with F(f-1)/f as a function of (F2/f).
Figure 2. (a) Relationship between the 2-methacryloyloxyethyl phosphorylcholine (MPC) content in the copolymer and the feed. (b) The graphic representation of the Fineman–Ross equation, with F(f-1)/f as a function of (F2/f).
Polymers 12 01808 g002
Figure 3. 1H NMR spectra for (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12), and (d) P(MEA/MPC46) in methanol-d4 at room temperature.
Figure 3. 1H NMR spectra for (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12), and (d) P(MEA/MPC46) in methanol-d4 at room temperature.
Polymers 12 01808 g003
Figure 4. 1H NMR spectra for (a) P(MEA/MPC6), (b) P(MEA/MPC12), and (c) P(MEA/MPC46) in D2O at room temperature.
Figure 4. 1H NMR spectra for (a) P(MEA/MPC6), (b) P(MEA/MPC12), and (c) P(MEA/MPC46) in D2O at room temperature.
Polymers 12 01808 g004
Figure 5. Spin–spin relaxation time (T2) for the pendant methyl protons in the MEA unit at 3.39 ppm () and the MPC unit at 3.23 ppm () as a function of the MPC content (m) in P(MEA/MPCm) in D2O at 25 °C.
Figure 5. Spin–spin relaxation time (T2) for the pendant methyl protons in the MEA unit at 3.39 ppm () and the MPC unit at 3.23 ppm () as a function of the MPC content (m) in P(MEA/MPCm) in D2O at 25 °C.
Polymers 12 01808 g005
Figure 6. Hydrodynamic radius (Rh) distributions for (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12), and (d) P(MEA/MPC46) in pure water at Cp = 1.0 g/L at 25 °C.
Figure 6. Hydrodynamic radius (Rh) distributions for (a) PMEA, (b) P(MEA/MPC6), (c) P(MEA/MPC12), and (d) P(MEA/MPC46) in pure water at Cp = 1.0 g/L at 25 °C.
Polymers 12 01808 g006
Figure 7. Transmission electron microscopy (TEM) images for (a) PMEA and (b) P(MEA/MPC6) at Cp = 1.0 g/L in water.
Figure 7. Transmission electron microscopy (TEM) images for (a) PMEA and (b) P(MEA/MPC6) at Cp = 1.0 g/L in water.
Polymers 12 01808 g007
Figure 8. Zimm plots of P(MEA/MPC6) in water at 25 °C.
Figure 8. Zimm plots of P(MEA/MPC6) in water at 25 °C.
Polymers 12 01808 g008
Figure 9. Fluorescence intensity ratio (I3/I1) of pyrene in the presence of P(MEA/MPC6) plotted against the polymer concentration (Cp). I3 and I1 are the fluorescence intensities of the third and the first vibronic peaks, respectively, in the pyrene emission spectra recorded at the excitation wavelength of 334 nm.
Figure 9. Fluorescence intensity ratio (I3/I1) of pyrene in the presence of P(MEA/MPC6) plotted against the polymer concentration (Cp). I3 and I1 are the fluorescence intensities of the third and the first vibronic peaks, respectively, in the pyrene emission spectra recorded at the excitation wavelength of 334 nm.
Polymers 12 01808 g009
Table 1. Characteristics of the P(MEA/MPCm) copolymers.
Table 1. Characteristics of the P(MEA/MPCm) copolymers.
m aMn(SEC) b × 104 (g/mol)Đ bMw(SLS) c × 105 (g/mol)Rhd (nm)Rgc (nm)Rg/Rh
61.412.612.369.615.51.6
121.462.241.5310.014.81.5
462.692.040.739.212.81.4
a m indicates the MPC content (mol%) in the copolymer, as estimated using NMR data obtained in methanol-d4. b The number-average molecular weight (Mn) and molecular weight distribution (Đ) were estimated via SEC analysis. c The apparent weight-average molecular weight (Mw) and the radius of gyration (Rg) were estimated from SLS measurements in methanol. d The hydrodynamic radius (Rh) was obtained from DLS measurements in the methanolic solutions of the copolymers.
Table 2. The association behavior of P(MEA/MPC6) in water.
Table 2. The association behavior of P(MEA/MPC6) in water.
SampleMw(SLS) a × 10−7 (g/mol)Rhb (nm)Rga (nm)Rg/RhRTEMc (nm)NaggdA2a × 105 (cm3 g−2 mol)CAC e (g/L)
P(MEA/MPC6)3.3796.992.10.951031432.50.0082
a Estimated from static light scattering (SLS) analysis of the aqueous solutions. b Obtained from DLS analysis of the aqueous solutions. c Estimated via TEM. d Aggregation number (Nagg) calculated from the Mw values of the polymer micelle in water and the individual polymer chains in methanol obtained from SLS measurements. e Critical aggregation concentration (CAC) estimated via the pyrene fluorescence method.

Share and Cite

MDPI and ACS Style

Nguyen, T.L.; Kawata, Y.; Ishihara, K.; Yusa, S.-i. Synthesis of Amphiphilic Statistical Copolymers Bearing Methoxyethyl and Phosphorylcholine Groups and Their Self-Association Behavior in Water. Polymers 2020, 12, 1808. https://doi.org/10.3390/polym12081808

AMA Style

Nguyen TL, Kawata Y, Ishihara K, Yusa S-i. Synthesis of Amphiphilic Statistical Copolymers Bearing Methoxyethyl and Phosphorylcholine Groups and Their Self-Association Behavior in Water. Polymers. 2020; 12(8):1808. https://doi.org/10.3390/polym12081808

Chicago/Turabian Style

Nguyen, Thi Lien, Yuuki Kawata, Kazuhiko Ishihara, and Shin-ichi Yusa. 2020. "Synthesis of Amphiphilic Statistical Copolymers Bearing Methoxyethyl and Phosphorylcholine Groups and Their Self-Association Behavior in Water" Polymers 12, no. 8: 1808. https://doi.org/10.3390/polym12081808

APA Style

Nguyen, T. L., Kawata, Y., Ishihara, K., & Yusa, S. -i. (2020). Synthesis of Amphiphilic Statistical Copolymers Bearing Methoxyethyl and Phosphorylcholine Groups and Their Self-Association Behavior in Water. Polymers, 12(8), 1808. https://doi.org/10.3390/polym12081808

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop