Next Article in Journal
Effect of Different Pre-Treatment on the Microstructure and Intumescent Properties of Rice Husk Ash-Based Geopolymer Hybrid Coating
Next Article in Special Issue
Experimental Study of the Dynamic and Static Compression Mechanical Properties of Closed-Cell PVC Foams
Previous Article in Journal
Silk Fibroin as Adjuvant in the Fabrication of Mechanically Stable Fibrin Biocomposites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

DMA Investigation of the Factors Influencing the Glass Transition in 3D Printed Specimens of Shape Memory Recycled PET

by
Bogdan Pricop
1,
Ștefan Dumitru Sava
2,
Nicoleta-Monica Lohan
1 and
Leandru-Gheorghe Bujoreanu
1,*
1
Faculty of Materials Science, “Gheorghe Asachi” Technical University of Iași, Blvd. Dimitrie Mangeron 71A, 700050 Iasi, Romania
2
Inotech Association, Plopii Fără Soț by Street 19A, 700281 Iasi, Romania
*
Author to whom correspondence should be addressed.
Polymers 2022, 14(11), 2248; https://doi.org/10.3390/polym14112248
Submission received: 26 April 2022 / Revised: 24 May 2022 / Accepted: 30 May 2022 / Published: 31 May 2022
(This article belongs to the Special Issue Dynamic Mechanical Analysis of Polymer Composites)

Abstract

:
Polyethylene terephthalate (PET) is used worldwide for packing, and for this reason, it is the main material in plastic waste. The paper uses granules of recycled PET (R-PET) as raw material for producing filaments for 3D printing, subsequently used for printing the test specimens in different ways: longitudinally and at angles between 10° and 40° in this direction. Both the filaments and the printed specimens experience thermally driven shape memory effect (SME) since they have been able to recover their straight shape during heating, after being bent to a certain angle, at room temperature (RT). SME could be reproduced three times, in the case of printed specimens, and was investigated by cinematographic analysis. Then, differential scanning calorimetry (DSC) was used, in R-PET granules, filaments and 3D printed specimens, to emphasize the existence of glass transition, which represents the governing mechanism of SME occurrence in thermoplastic polymers, as well as a recrystallization reaction. Subsequently, the paper investigated the 3D printed specimens by dynamic mechanical analysis (DMA) using a dual cantilever specimen holder. Temperature (DMA-TS) and isothermal scans (DMA-Izo) were performed, with the aim to discuss the variations of storage modulus and loss modulus with temperature and time, respectively.

Graphical Abstract

1. Introduction

Polyethylene terephthalate (PET) is the most commonly used material for food packing and fluid transportation purposes, with a production estimated at 70 million tons in 2020 [1]. Therefore, the huge number of plastic bags and bottles produced has largely contributed to the accumulation of the present 1.6 million square kilometers of floating “Great Pacific Garbage Patch” [2]. Despite recycling in sustainable ways, at least a part of the giant amount of PET waste amassed since the first synthesis, which succeeded in the midst of the 1940s [3], has become one of the present time’s most critical challenges [4]. Therefore, a large number of papers dedicated to PET recycling were published, being focused on physical (thermal extrusion and pelletization) or chemical processes (aiming to decompose PET into depolymerized oligomers) [5]. Since PET degradation naturally occurs after prolonged exposures (to temperature, humidity, radiation or bacteria) [6], various approaches aimed to accelerate these processes, such as depolymerization at 110 °C for 5 h [7], melting and plasticization under shear and tension flows [8], or gamma rays’ exposure [9].
Among various modalities of PET recycling, the production of filament for 3D printing—also valorized in the case of other thermoplastics [10,11]—has gained increasing interest, especially after the start of its commercialization in 2015 [12]. Thus, comprehensive studies were performed to ascertain the suitability of recycled PET (R-PET) for the production of powders [13] and filaments for 3D printing [14]. It has been reported that printed parts with virgin and R-PET filaments had comparable mechanical properties [15], especially when they were obtained by fused filament fabrication [16].
Nevertheless, besides the possibility of being recyclable, PET has chemical resistance and excellent mechanical, processing and thermal properties [17] associated with its structure, comprising a crystalline and two amorphous fractions with different mobilities [18]. The investigations performed by dynamic mechanical analysis (DMA) emphasized a marked storage modulus decrease during heating above the thermal range for glass transition [17,19].
On the other hand, glass transition is a potential mechanism for the shape memory effect (SME) occurrence in thermoplastic polymers, which recover their permanent shape during heating after being deformed to a temporary one [20]. Moreover, storage modulus decreases by up to two orders of magnitude and is a criterion for the identification of thermal memory behavior [21]. Considering that PET has comparable specific work outputs with certain shape memory alloys [22], concrete crack closure systems have been successfully developed based on PET knotted fibers [23] of tendon outer sleeves [24].
This ability of 3D printed objects to alter their shape and function after being subjected to an external stimulus, such as temperature, has added an additional dimension to the additive manufacturing process, which became 4D printing [25], and evolved from a concept to a manufacturing paradigm [26].
Nevertheless, as far as the knowledge of the present authors, no reports have been published on SME occurrence in R-PET. Therefore, the present paper aims to emphasize SME presence, both in R-PET 3D filaments and printings, and to corroborate it with the thermodynamic behavior observed by calorimetry and dynamic mechanical analysis.

2. Materials and Methods

R-PET grains, originating from recipients of carbonated drinks bottles, were purchased from the GreenTech SA company, Buzău, Romania. As compared to virgin grains that are injected and blown into chilled molds, the grains used in the present study are heated, extruded into a filament, deposited and chilled. The grains were processed by the Inotech Association by means of the experimental line for 3D filament production, as illustrated in Figure 1.
After water removal in the grain dryer, the grains fell into the central unit, where they were heated up to 270 °C. Then, they were extruded through a dye into a 1.75 mm-diameter filament which passed through the hot water (80 °C) vat and the cold water vat, being drawn by the roll tractor. The rotation speed of the roll tractor was controlled by a laser system that read the filament’s diameter. Since the process was entirely continuous, before being wound into rolls, the filament was deviated by means of an accumulation line.
Using R-PET filament, parallelepipedal specimens were printed with the dimensions 1 × 4 × 50 mm. Five different angles between specimens’ longitudinal axis and filament deposition direction were used to print specimens at 0°, 10°, 20°, 30° and 40°, respectively. The images of the R-PET grains, the filament and the five types of specimens, with optical microscopy (OM) details, are illustrated in Figure 2.
The presence of the shape memory effect (SME) was investigated by means of cinematographic analysis [27]. Both filament fragments and printed specimens were bent at room temperature (RT) and subsequently heated with a hot-air gun while having a multimeter’s thermocouple fixed in the deformed area. Cooling was performed in free air. The variations of the specimen’s free end and temperature were recorded and analyzed frame-by-frame.
The heating induced changes were investigated by thermal analysis, comprising differential scanning calorimetry (DSC) and dynamic mechanical analysis (DMA).
The former was performed on a NETZSCH DSC 200 F3 Maia device (Netzsch, Selb, Germany), calibrated with Bi, In, Sn, Zn and Hg standards. Grains and fragments weighing less than 50 mg were cut from the filament and printed specimens and were heated under an Ar protective atmosphere at 10 °C/min.
The latter was achieved using a NETZSCH DMA 242 Artemis device equipped with a dual cantilever specimen holder. Printed specimens were dynamically bent under an Ar protective atmosphere during heating or isothermal testing. The former used a heating rate of 5 °C/min and 1 Hz frequency. The latter was performed at three temperatures, at three frequencies: 1, 10 and 100 Hz, and in each case, using a bending amplitude of 100 µm. Both DSC and DMA records have been evaluated by Proteus software, v.6.1, Selb, Germany.

3. Results and Discussion

3.1. Shape Memory Effect

The typical images of the free-recovery SME analysis, corresponding to the cold and hot shapes of the filament, are illustrated in Figure 3.
It is obvious that the R-PET filament experienced free-recovery SME during the first heating. After applying a supplementary RT bending, SME was not observed in the second cycle.
Similar images are shown in Figure 4 for the evolution of a printed specimen; however, in this case, the phenomenon was reproducible for three cycles. It is noticeable that the free end’s displacement remains more and more behind the variation of temperature.
In order to illustrate the free end’s displacement delay with regard to temperature, Figure 5 displays the shift of displacement-temperature diagrams after three cycles.
Figure 5 displays both experimental values, with filled symbols and fitted values, with solid lines, as a result of a Boltzmann fitting function. The general equation of the Boltzmann function has the following form:
y = A 2 + ( A 1 A 2 ) / ( 1 + e x x 0 d x )
The values of the parameters of the Boltzmann function are listed in Table 1.
The standard errors, which do not exceed 1%, ascertain the validity of the mathematical model.
A possible cause for the SME’s disappearance in the filament after the first cycle might be the higher cooling rate of the filament during processing. The filament is extruded on its entire cross-section, drawn by the roll tractor and water-cooled while the specimens are printed layer-by-layer and air-cooled. Thus, a functionally-graded shrinkage along with the sample thickness was developed, which enhanced SME occurrence [28].

3.2. DSC Measurements

The representative DSC thermograms, recoded during heating, are summarized in Figure 6.
In most of the cases, the thermograms revealed three transformations: (i) glass transition, (ii) recrystallization and (iii) melting.
The grains did not reveal any recrystallization but seemed to experience two glass transitions (Tg1 and Tg2). The second transition might be an effect of ageing, underwent by original PET bottles before shredding. It has been reported that with the increasing ageing time [29], the degree of crystallinity increased and no recrystallization occurred [30]. It is noticeable, however, that both the recrystallization and melting became more intense in the printed specimens and even at the specimen printed at 40°, as compared to that printed at 0°. Figure 6b presents the thermograms of two specimens printed at 40°. The first was in an initial state and the second was subjected to three free-recovery SME cycles. It is obvious that the thermal range of glass transition moved to higher temperatures and the transition itself became less abrupt. Glass transition is directly related to the change of amorphous into crystalline phase and acts as a microstructural mechanism of SME [20]. During consecutive heating-cooling-bending cycles, when the temperature did not reach the recrystallization temperature, and cooling to RT was performed in air, one may suppose that the amount of amorphous phase decreased because low cooling rates do not enhance re-amorphization processes. Thus, it can be assumed that the glass transition underwent a degradation process caused by the decrease in an amorphous phase amount [18], which was reflected by the delay and final disappearance of the SME. This could sustain the displacement delay discussed in the previous section. A more comprehensive evaluation of the thermograms from Figure 6 is presented in Table 2.
The second glass transition was observed at grains, between 163.7 and 166.6 °C, and absorbed only 0.031 mJ/g °C. The grains, which were shredded from bottles cooled in water-chilled metallic molds, have a larger amount of amorphous matter, and this could be the reason why they absorb more energy during glass transition. It is obvious that the crystallization degree increased from the filament to the printed specimens and from 0 to 40° angle printing. In the last case, the crystallization degree decreased by 20%, from the first to the third free-recovery SME cycle.

3.3. DMA Measurements

The typical DMA diagrams recorded during heating are illustrated in Figure 7.
The sharp decrease in the storage modulus, seen in Figure 7a, is typical for the glass transition. Before the decrease, there is a local storage modulus increase, indicating the destabilization of the specimen. This increment has a minimum of 272 MPa for the specimen printed at 0° and a maximum of 839 MPa, for the specimen printed at 10°. The same two specimens had an extreme loss of modulus values of a maximum of 265 MPa at 0° and 417 MPa at 10°, as seen in Figure 7b. Figure 7c shows details of the storage modulus increase at the end of heating, which was previously reported in other articles, such as [8]. Considering the high mobility of the polymeric chains in the temperature range of 120–150 °C, the only possible explanation for a storage modulus increase can be associated with the recrystallization observed by DSC, as previously observed in a study on amorphous PET. In the same way, as in Figure 7c, the storage modulus began to rise at near 120 °C with a slower increasing rate and changed to a higher increasing rate near 130 °C [31].
The isothermal tests were performed at RT and at the temperature of storage modulus maximum. Figure 8 shows the storage modulus variation at RT for three 3D printed specimens.
As expected, the storage modulus values increased with test frequency and decreased with the augmentation of the deposition angle (raster) against the longitudinal direction of the specimen. The effect was explained, in the case of polylactic acid, by the change of the type and the number of deformed layers with increasing raster angles. Only individual layers were deformed at a 0° raster, while an increasing number of adjacent layers were deformed with an increasing raster angle [32]. According to the deposition-induced effect, the bonding area between the adjacent layers decreases with the increase of the raster angle [33].
In addition, at RT, the storage modulus remained almost constant in time. A simple calculation of the number of cycles at 100 Hz during 9 min gives 54,000 cycles.
A different situation can be observed for the values of storage modulus recorded isothermally, at the temperature corresponding to its minimum and maximum observed during heating, according to Figure 7. These variations are exemplified in Figure 9, for the specimen printed at 0°.
In this case, a strengthening effect can be observed for the storage modulus values recorded at 48 °C and 60 °C. At 48 °C, there was actually the start of the glass transition. It can be assumed, then, that the destabilization of the amorphous state just started and only a small part of the polymeric chains became crystalline. During 9 min, the storage modulus value increased by about 25%, probably because a part of the newly formed crystals became amorphous again. At 60 °C, there was actually a climax of glass transition. The amount of the crystalline part should be much larger than at 48 °C. Therefore, the material is softer than at RT when in the initial stage of the isothermal test. However, during the test, more and more became amorphous again and, for this reason, the storage modulus increases from approx. 1200 to 1600 MPa.

4. Conclusions

The following conclusions can be drawn:
  • Free-recovery SME was emphasized, both in the case of the filaments produced from the R-PET pellets and in the case of the 3D printed parts obtained with these filaments.
  • The printed parts experienced free-recovery SME for up to three consecutive cycles, during which a delay was noticed between the displacement and temperature variations, which were fitted with Boltzmann-type functions with standard errors below 1%. This delay was associated with glass transition degradation, probably caused by the decrease in the amorphous phase amount during free-air cooling.
  • The DSC measurements emphasized a glass transition, which is the mechanism of SME and recrystallization which produced a storage modulus increase between 125 and 150 °C.
  • After three SME cycles, degradations were observed on the DSC thermograms, both at the glass transitions and at recrystallization.
  • The DMA measurements, performed with dual cantilever dynamic bending, emphasized the storage modulus increases during heating, before the glass transition thermal range.
  • Increasing the angle between the specimen’s direction and layer deposition direction, from 0° to 30°, caused storage modulus decreases at RT due to the decrease in the bonding area between the adjacent layers, with an increased raster angle;
  • Isothermal DMA measurements, performed at temperatures in the beginning and the climax of glass transition, emphasized the storage modulus increases in time by about 25%, which can be ascribed to the amorphization of a part of the newly formed crystallites.

Author Contributions

Conceptualization, L.-G.B. and B.P.; methodology, N.-M.L.; software, B.P.; validation, B.P., N.-M.L. and L.-G.B.; formal analysis, B.P.; investigation, B.P. and N.-M.L.; resources, Ș.D.S.; data curation, B.P.; writing—original draft preparation, L.-G.B.; writing—review and editing, L.-G.B.; visualization, N.-M.L.; supervision, Ș.D.S. All authors have read and agreed to the published version of the manuscript.

Funding

The APC was funded by “Gheorghe Asachi” Technical University of Iași.

Acknowledgments

The authors acknowledge the voluntary contribution of MSc V. Sava for providing the experimental materials.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Choudhary, K.; Sangwan, K.S.; Goyal, D. Environment and economic impacts assessment of PET waste recycling with conventional and renewable sources of energy. Proced. CIRP 2019, 80, 422–427. [Google Scholar] [CrossRef]
  2. Great Pacific Garbage Patch. Available online: https://www.nationalgeographic.org/encyclopedia/great-pacific-garbage-patch/ (accessed on 14 April 2022).
  3. Cho, E.; Lee, S.Y.; Choi, J.-W.; Kim, S.-H.; Jung, K.-W. Direct upcycling of polyethylene terephthalate (PET) waste bottles into α-Fe2O3 incorporated MIL-53(Al) for the synthesis of Al2O3/Fe3O4-encapsulated magnetic carbon composite and efficient removal of non-steroidal anti-inflammatory drugs. Sep. Purif. Technol. 2021, 279, 119719. [Google Scholar] [CrossRef]
  4. Sharifian, S.; Asasian-Kolur, N. Polyethilene therephtale (PET) waste to carbon materials: Theory, method and applications. J. Anal. Appl. Pyrolysis 2022, 163, 105496. [Google Scholar] [CrossRef]
  5. Naguib, H.M.; Zhang, X.H. Advanced recycled polyester based on PET and oleic acid. Polym. Test. 2018, 69, 450–455. [Google Scholar] [CrossRef]
  6. Thachnatharen, N.; Shahabuddin, S.; Sridewi, N. The waste management of polyethylene terephthalate (PET) plastic waste: A review. IOP Conf. Ser. Mater. Sci. Eng. 2021, 1127, 012002. [Google Scholar] [CrossRef]
  7. Wang, Y.; Wang, H.; Chen, H.; Liu, H. Towards recycling purpose: Converting PET plastic waste back to terephthalic acid using pH-responsive phase transfer catalyst. Chin. J. Chem. Eng. 2021. [Google Scholar] [CrossRef]
  8. Wu, H.; Lv, S.; Qu, J.P. The study of the thermomechanical degradation and mechanical properties of PET recycled by industrial-scale elongational processing. Polym. Test. 2019, 77, 105882. [Google Scholar] [CrossRef]
  9. Khan, M.I.; Sutanto, M.H.; Khan, K.; Iqbal, M.; Bin Napiah, M.; Zoorob, S.E.; Klemes, J.J.; Bokhari, A.; Rafiq, W. Effective use of recycled waste PET in cementitious grouts for developing sustainable semi-flexible pavement surfacing using artificial neural network (ANN). J. Clean. Prod. 2022, 340, 130840. [Google Scholar] [CrossRef]
  10. Mikula, K.; Skrzypczak, D.; Izydorczyk, G.; Warchoł, J.; Moustakas, K.; Chojnacka, K.; Witek-Krowiak, A. 3D printing filament as a second life of waste plastics—a review. Env. Sci. Poll. Res. 2021, 28, 12321–12333. [Google Scholar] [CrossRef]
  11. Gomes, T.E.P.; Cadete, M.S.; Dias-de-Oliveira, J.; Neto, V. Controlling the properties of parts 3D printed from recycled thermoplastics: A review of current practices. Polym. Degrad. Stab. 2022, 196, 109850. [Google Scholar] [CrossRef]
  12. Pakkanen, J.; Manfredi, D.; Minetola, P.; Iuliano, L. About the use of recycled or biodegradable filaments for sustainability of 3D printing. In Sustainable Design and Manufacturing; Campana, G., Howlett, R.J., Setch, R., Cimati, B., Eds.; Springer: Berlin/Heidelberg, Germany, 2017; pp. 776–785. [Google Scholar]
  13. Nwogu, C.N.; Uche, R.; Igbokwe, J.O.; Okoronkwo, A.C. Characterization of recycled polyethylene terephthalate powder for 3D printing feedstock. Int. J. Adv. Res. Sci. Eng. Technol. 2019, 6, 8844–8851. [Google Scholar] [CrossRef]
  14. Exconde, M.K.J.E.; Co, J.A.A.; Manapat, J.Z.; Magdaluyo, E.R., Jr. Materials selection of 3D printing filament and utilization of recycled polyethylene terephthalate (PET) in a redesigned breadboard. Proced. CIRP 2019, 84, 28–32. [Google Scholar] [CrossRef]
  15. Oussai, A.; Bártfai, Z.; Kátai, L. Development of 3D printing raw materials from plastic waste. a case study on recycled polyethylene terephthalate. Appl. Sci. 2021, 11, 7338. [Google Scholar] [CrossRef]
  16. Zander, N.E.; Gillan, M.; Lambeth, R.H. Recycled polyethylene terephthalate as a new FFF feedstock material. Addit. Manuf. 2018, 21, 174–182. [Google Scholar] [CrossRef]
  17. Cristea, M.; Ionita, D.; Simionescu, B.C. A new insight in the dynamo-mechanical behavior of poly(ethylene terephthalate). A new insight in the dynamo-mechanical behavior of poly(ethylene terephthalate). Eur. Polym. J. 2010, 46, 2005–2012. [Google Scholar] [CrossRef]
  18. Badia, J.D.; Strömberg, E.; Karlsson, S.; Ribes-Greus, A. The role of crystalline, mobile amorphous and rigid amorphous fractions in the performance of recycled poly (ethylene terephthalate) (PET). Polym. Degrad. Stab. 2012, 97, 98–107. [Google Scholar] [CrossRef] [Green Version]
  19. Mazzuca, P.; Firmo, J.P.; Correia, J.R.; Castilho, E. Mechanical behaviour in shear and compression at elevated temperature of polyethylene terephthalate (PET) foam. J. Build. Eng. 2021, 42, 102526. [Google Scholar] [CrossRef]
  20. Irie, M. Shape memory polymers. In Shape Memory Materials; Otsuka, K., Wayman, C.M., Eds.; Cambridge University Press: Cambridge, UK, 1998; pp. 203–219. [Google Scholar]
  21. Behl, M.; Zotzmann, J.; Lendlein, A. Shape-memory polymers. In Shape Memory Polymers; Lendlein, A., Ed.; Springer: Berlin/Heidelberg, Germany, 2010; pp. 1–40. [Google Scholar]
  22. Campbell, T.A.; Tibbits, S.; Garrett, B. The Next Wave: 4D Printing Programming the Material World, Atlantic Council Report. Available online: https://www.atlanticcouncil.org/in-depth-research-reports/report/the-next-wave-4d-printing-and-programming-the-material-world/ (accessed on 21 April 2022).
  23. Lacatusu, D.; Baican, M.; Crivoi, F.; Miftode, A.M. Comparative studies of work-developing capacity of shape memory alloys (SMA) and polymers. Rev.Cem. 2019, 70, 4366–4371. [Google Scholar]
  24. Maddalena, R.; Bonanno, L.; Balzano, B.; Tuinea-Bobe, C.; Sweeney, J.; Mihai, I. A crack closure system for cementitious composite materials using knotted shape memory polymer (k-SMP) fibres. Cem. Concr. Comp. 2020, 114, 103757. [Google Scholar] [CrossRef]
  25. Balzano, B.; Sweeney, J.; Thompson, G.; Tuinea-Bobe, C.-L.; Jefferson, A. Enhanced concrete crack closure with hybrid shape memory polymer tendons. Eng. Struct. 2021, 226, 111330. [Google Scholar] [CrossRef]
  26. Akbar, I.; El Hadrouz, M.; El Mansori, M.; Lagoudas, D. Toward enabling manufacturing paradigm of 4D printing of shape memory materials: Open literature review. Eur. Polym. J. 2022, 168, 111106. [Google Scholar] [CrossRef]
  27. Pricop, B.; Soyler, U.; Ozkal, B.; Lohan, N.M.; Paraschiv, A.L.; Suru, M.G.; Bujoreanu, L.G. Influence of mechanical alloying on the behavior of Fe-Mn-Si-Cr-Ni shape memory alloys made by powder metallurgy. In Materials Science Forum; Prokoshkin, S., Resnina, N., Eds.; Trans Tech Publications Ltd.: Stafa-Zurich, Switzerland, 2013; Volume 738, pp. 237–241. [Google Scholar]
  28. Aberoumand, M.; Soltanmohammadi, K.; Soleyman, E.; Rahmatabadi, D.; Ghasemi, I.; Baniassadi, M.; Abrinia, K.; Baghani, M. A comprehensive experimental investigation on 4D printing of PET-G under bending. J. Mater. Res. Technol. 2022, 18, 2552–2569. [Google Scholar] [CrossRef]
  29. Panowicz, R.; Konarzewski, M.; Durejko, T.; Szala, M.; Lazinska, M.; Czerwinska, M.; Prasula, P. Properties of polyethylene terephthalate (PET) after thermo-oxidative aging. Materials 2021, 14, 3833. [Google Scholar] [CrossRef] [PubMed]
  30. Corrales, T.; Peinado, C.; Bosch, P.; Catalina, F. Study of secondary relaxations of poly(ethylene terephthalate) by photoluminescence technique. Polymer 2004, 45, 1545–1554. [Google Scholar] [CrossRef]
  31. Shieh, Y.-T.; Lin, Y.-S.; Twu, Y.-K.; Tsai, H.-B.; Lin, R.-H. Effect of crystallinity on enthalpy recovery peaks and cold-crystallization peaks in PET via TMDSC and DMA studies. J. Appl. Polym. Sci. 2010, 116, 1334–1341. [Google Scholar] [CrossRef]
  32. Zhang, X.; Chen, L.; Mulholland, T.; Osswald, T.A. Effects of raster angle on the mechanical properties of PLA and Al/PLA composite part produced by fused deposition modeling. Polym. Adv. Technol. 2019, 30, 2122–2135. [Google Scholar] [CrossRef]
  33. Zhou, Y.-G.; Zou, J.-R.; Wu, H.-H.; Xu, B.-P. Balance between bonding and deposition during fused deposition modeling of polycarbonate and acrylonitrile-butadiene-styrene composites. Polym. Comp. 2020, 41, 60–72. [Google Scholar] [CrossRef]
Figure 1. The experimental line for filament production from R-PET grains.
Figure 1. The experimental line for filament production from R-PET grains.
Polymers 14 02248 g001
Figure 2. Images of raw materials and specimens: (a) R-PET grains; (b) 3D filament; (c) 3D printed specimens with corresponding OM details of the five different angles between their longitudinal axes and filament deposition direction.
Figure 2. Images of raw materials and specimens: (a) R-PET grains; (b) 3D filament; (c) 3D printed specimens with corresponding OM details of the five different angles between their longitudinal axes and filament deposition direction.
Polymers 14 02248 g002
Figure 3. Typical images recorded during the occurrence of free-recovery SME at R-PET filament: (a) RT bent cold shape; (b) hot shape recovered during 23 s heating.
Figure 3. Typical images recorded during the occurrence of free-recovery SME at R-PET filament: (a) RT bent cold shape; (b) hot shape recovered during 23 s heating.
Polymers 14 02248 g003
Figure 4. Typical images recorded during the occurrence of free-recovery SME at a 3D printed R-PET specimen during three consecutive heating-cooling-bending cycles. Time duration details (s).
Figure 4. Typical images recorded during the occurrence of free-recovery SME at a 3D printed R-PET specimen during three consecutive heating-cooling-bending cycles. Time duration details (s).
Polymers 14 02248 g004
Figure 5. Free end’s displacement vs. temperature during free-recovery SME, according to Figure 4.
Figure 5. Free end’s displacement vs. temperature during free-recovery SME, according to Figure 4.
Polymers 14 02248 g005
Figure 6. DSC thermograms recorded during heating: (a) R-PET grain, filament and printed specimens at 0° and 40°; (b) printed specimen at 40° in an initial state and after three free-recovery SME cycles.
Figure 6. DSC thermograms recorded during heating: (a) R-PET grain, filament and printed specimens at 0° and 40°; (b) printed specimen at 40° in an initial state and after three free-recovery SME cycles.
Polymers 14 02248 g006
Figure 7. DMA diagrams recorded during the heating of 3D printed specimens: (a) variation in storage modulus; (b) variation in loss modulus; (c) details of the variation in storage modulus between 125 and 150 °C.
Figure 7. DMA diagrams recorded during the heating of 3D printed specimens: (a) variation in storage modulus; (b) variation in loss modulus; (c) details of the variation in storage modulus between 125 and 150 °C.
Polymers 14 02248 g007
Figure 8. Isothermal DMA diagrams recorded at RT, with 3D printed specimens at 0°, 10° and 20° deposition angle.
Figure 8. Isothermal DMA diagrams recorded at RT, with 3D printed specimens at 0°, 10° and 20° deposition angle.
Polymers 14 02248 g008
Figure 9. Isothermal DMA diagrams recorded at RT at 48 °C and at 60 °C with 3D printed specimens at 0°.
Figure 9. Isothermal DMA diagrams recorded at RT at 48 °C and at 60 °C with 3D printed specimens at 0°.
Polymers 14 02248 g009
Table 1. Values of Boltzmann function parameters, according to the diagrams listed in Figure 5.
Table 1. Values of Boltzmann function parameters, according to the diagrams listed in Figure 5.
Parameter1st Cycle3rd Cycle
ValueStandard ErrorValueStandard Error
A10.845320.693981.008640.23239
A224.810750.9328117.564720.43851
x076.204040.4951788.820310.32189
dx3.035170.454552.201050.31673
Table 2. Evaluation results of the thermograms from Figure 6.
Table 2. Evaluation results of the thermograms from Figure 6.
SpecimenGlass TransitionRecrystallization
Onset
°C
Mid
°C
Inflection
°C
End
°C
ΔCp
J/(g∙°C)
Δh
kJ/kg
grain80.482.683.184.40.279-
filament73.675.976.178.00.08615.2
printed 0°74.877.476.679.30.09316.44
printed 40°73.576.976.078.30.10621.81
printed 40°, 3 cycles74.476.877.279.30.10117.44
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Pricop, B.; Sava, Ș.D.; Lohan, N.-M.; Bujoreanu, L.-G. DMA Investigation of the Factors Influencing the Glass Transition in 3D Printed Specimens of Shape Memory Recycled PET. Polymers 2022, 14, 2248. https://doi.org/10.3390/polym14112248

AMA Style

Pricop B, Sava ȘD, Lohan N-M, Bujoreanu L-G. DMA Investigation of the Factors Influencing the Glass Transition in 3D Printed Specimens of Shape Memory Recycled PET. Polymers. 2022; 14(11):2248. https://doi.org/10.3390/polym14112248

Chicago/Turabian Style

Pricop, Bogdan, Ștefan Dumitru Sava, Nicoleta-Monica Lohan, and Leandru-Gheorghe Bujoreanu. 2022. "DMA Investigation of the Factors Influencing the Glass Transition in 3D Printed Specimens of Shape Memory Recycled PET" Polymers 14, no. 11: 2248. https://doi.org/10.3390/polym14112248

APA Style

Pricop, B., Sava, Ș. D., Lohan, N. -M., & Bujoreanu, L. -G. (2022). DMA Investigation of the Factors Influencing the Glass Transition in 3D Printed Specimens of Shape Memory Recycled PET. Polymers, 14(11), 2248. https://doi.org/10.3390/polym14112248

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop