Article

Effect of Stress-Induced Martensite Stabilization on Acoustic Emission Characteristics and the Entropy of Martensitic Transformation in Shape Memory Ni51Fe18Ga27Co4 Single Crystal

1
Department of Solid State Physics, University of Debrecen, P. O. Box 400, H-4002 Debrecen, Hungary
2
Siberian Physical Technical Institute, Tomsk State University, 634050 Tomsk, Russia
*
Author to whom correspondence should be addressed.
Metals 2020, 10(4), 534; https://doi.org/10.3390/met10040534
Submission received: 18 March 2020 / Revised: 15 April 2020 / Accepted: 16 April 2020 / Published: 21 April 2020

Abstract

:
Simultaneous differential scanning calorimetry, DSC, and acoustic emission, AE, measurements were carried out for single crystals of quenched and stress-induced martensite stabilized (SIM-aged) shape memory Ni51Fe18Ga27Co4 alloy. The transformation temperatures were shifted to higher values, the forward (from austenite to martensite) and reverse transitions became sharper and the width of the hysteresis increased in the SIM-aged sample. The energy distributions of acoustic hits showed similar behaviour to those of the quenched sample and the energy exponents, characterizing the power law behaviour, were also similar. For SIM-aged alloys at heating, in accordance with the sharper (burst-like) transition observed in the DSC run, few high-energy solitary hits were observed, and these hits did not fit to the energy distribution function fitted for smaller energies. Thus, these high-energy events were attributed to high sudden jumps in the phase transition during heating. The effect of long-range order (by applying a heat treatment at 573 K for 6 h to transform the B2 austenite to ordered L21 structure) and the SIM-aging on the transformation entropy was also investigated by DSC. It was found that the entropy was about 36% smaller after SIM-aging of the quenched sample and it was practically unchanged after austenite stabilization.

1. Introduction

It is known that martensite stabilization heat treatments, under uniaxial stress, large enough to produce a single variant martensite in shape memory alloys, by aging at temperatures allowing atomic diffusion (stress-induced martensite stabilization, SIM) result in stabilization of the martensite [1,2,3,4,5,6,7,8,9,10,11,12]. While this stabilization, which can be understood on the basis of the so-called symmetry conforming short-range ordering process [5,13,14], plausibly causes a shift of transformation temperatures to higher values, significant improvement of the shape memory functional properties was also achieved [1,2,3,4,5,6,7,8,9,10,11,12]. For instance, it was demonstrated in [1] that martensite aging offers a general concept for the production of high temperature actuator materials, and the authors of [1] introduced a new class of high-temperature ferromagnetic shape memory alloys by choosing Co49Ni21Ga30 alloy as a model material. In [6], it was shown that SIM aging can result in a large reversible two-way shape memory behaviour in Ni49Fe18Ga27Co4 single crystal, and similar results were published, e.g., on NiMnGa [9] and Co49Ni21Ga30 [15] and CoNiAl [8] alloys. Thus, in order to reach high-deformation strains (close to the theoretical limits), due to the shift of the transformation temperatures to higher values and the stabilization of the two-way shape memory properties, high-temperature, high-strength ferromagnetic shape memory alloys were developed [1,4,5,8,9]. In a very recent paper [10], it was shown that in Ni51Fe18Ga27Co4 single crystal not only a two-way shape memory behaviour (with a reversible tensile strain of 9%) was achieved by SIM-aging but giant rubber-like behaviour was also observed up to 15%, during reorientation of martensite variants. This exceeded by about a factor of two, the maximum compression transformation strain during the B2-L1o martensitic transformation, and thus, it is very attractive for applications in different actuators. In addition, it was also found that in NiFeGaCo alloys, depending on the content and on the stabilization thermal treatments, martensitic transformations between any magnetic state of austenite and martensite can be achieved (see e.g., as a review, [16]), which can be important in tailoring magnetocaloric properties. In these alloys, stabilization thermal treatments of the austenite and martensite phases can also result in a change of the transformation entropy.
It is clear that such SIM-aging, giving preference to a certain martensite variant, should have important effects on the details of the martensite/austenite transformation. It is already documented in papers on the SIM-aging effect (see e.g., [1,9]) that after SIM-aging not only the transition temperatures were shifted to higher values, but the transitions also became sharper: frequently burst-like sharp transitions were observed [9,10,11,17,18]), and the sample can even suffer a macroscopic jump upon heating. However, no systematic investigations, like those suggested by Kustov et al. [19], on the shift and change of the width of the transitions were carried out. Thus, in our paper, we report comparative investigations of the martensitic transformation in SIM-aged and quenched (not SIM-aged) single crystalline shape memory Ni51Fe18Ga27Co4 crystals carried out using differential scanning calorimetry, DSC, and acoustic emission, AE, measurements. Acoustic emission measurements provide interesting information about the details of the jerky character of the transformation and thus about the microscopic details of the structural changes [20].
Special emphasis was given to the question: does the transformation entropy change or not after SIM-aging. Although, based on the arguments published in [12,19,21], it is expected that the entropy does not change due to the stabilization of martensite or austenite. On the contrary, it was concluded in [22] (on the basis of results, obtained in Cu-Zn-Al shape memory alloys) that “it would be improper to assume in any model that the entropy of transformation remains unchanged after specific thermal treatments which lead to stabilization…”. Indeed, it was shown that the entropy increased in austenite stabilized sample (by about 4%) and decreased after martensite stabilization (by about 12%) [22]. This question, which was not investigated in recent high temperature, high-strength ferromagnetic shape memory alloys, is also addressed.

2. Materials and Methods

An ingot of the Ni51Fe18Ga27Co4 (at%) alloy was prepared using vacuum induction melting. The single crystals were grown by the Bridgman method in a helium atmosphere. The samples (with dimensions of 3 mm × 3 mm × 6 mm) were annealed at 1373 K for 1 h at temperatures above the order–disorder transition temperature (T = 923–973 K) and then water quenched to T = 293 K (quenched samples). The B2 high temperature phase of the quenched crystals undergoes to a martensitic transformation to the L10-martensite.
The SIM-aging was performed using Instron VHS 5969 testing machine (Instron, Norwood, MA, USA)), with a nominal 1 × 10−3 s−1 strain rate [10]. The sample was undergone to compressive stress-induced forward martensitic transformation at 423 K, and it was followed by a heat treatment at this temperature, under 400 MPa compressive stress, for 1 h along the [110]B2||[100]L10 direction (SIM-aged sample).
Heat treatments for stabilizing the austenite, by initiating a B2/ordered L21 transformation in the austenitic state below the order/disorder temperature (T = 923–973 K [23]), were performed at 573 K for 6 h, in order to reach a highly ordered L21 phase.
The calorimetric measurements and their evaluations were carried out, similar to the usual procedure described in Refs. [24,25,26,27]. The mass of the quenched and austenite-stabilized samples was 385 mg, while it was 18 mg for the SIM-aged sample. The DSC measurements were carried out with a Perkin Elmer DSC 7 device (PerkinElmer Inc., Waltham, MA, USA), using 10 K/min driving rate. The calibration was made with the melting point of ice as well as pure indium. The time constant of the device was found to be 6 s. This value was taken into account in the calculation of the contributions of the decay of the overlapping peaks in the DSC curves [24].
The acoustic emission measurements were carried out in a modified DSC device (the same equipment with a homemade accessory) (using the same 10 K/min driving rate) with Sensophone AED 404 Acoustic Emission Diagnostic Equipment (Geréb and Co., Ltd., Budapest, Hungary) with piezoelectric sensor (MICRO-100s from Physical Acoustics Corporation, Princeton Junction, NJ, USA). The microphone has good frequency response between 100 KHz and 1 MHz, which is nearly flat in the range between 0.2 and 1 MHz at −75 dB in average with a maximum ±10 dB deviation (1 V reference value). The sensor was coupled to the sample surface via a 15-mm long and of 1-mm diameter steel waveguide (made of 100Cr6 chromium alloyed steel of C: ~1%, Cr: ~1.5%, Mn: ~0.35% and Si: ~0.25% composition in hardened state), in order to provide a thermal isolation from the sample when its temperature was widely varied. The analog-to-digital converter sampling rate was 16 MHz, and the setup had a band-pass from 30 KHz to 1 MHz. A 30 dB preamplifier and a main amplifier (logarithmic gain) with 90 dB dynamic range were used. The threshold level was determined from a measurement carried out in a martensitic state without heating/cooling (i.e., when the low-level acoustic emission should not belong to the phase transformation). The threshold was set to the minimum and then increased until the threshold got up the background noise level. The threshold level determined in this way was then increased by 3 dB for safety and fixed at 38 dB. For the computation of the exponents, logarithmic data binning (the whole interval was split into 50 bins) was used.

3. Results

The results of the DSC measurements, as an illustration, are shown in Figure 1 and Figure 2 for heating and cooling of the quenched and SIM-aged samples, respectively. In the latter case, since the burst-like transformation was accompanied with a large, sudden shape change [10], silicon grease was used to fix the SIM-aged sample into the sample holder of the DSC. It is one of the reasons why the mass of the SIM-aged sample was about twenty times smaller: this helped us to fix the sample. The second reason was that after a few thermal cycles, the sample was broken into small pieces, because of the very large local stresses during transformation. On the smaller samples, no cracking was observed even after many cycles. Of course, the DSC and AE measurements were carried out on the same piece of sample. This size, we believe, did not introduce disturbing scale effects: according to [27] decreasing the size of the sample resulted only in a split of the DSC peaks, at the same cooling/heating rates, but, e.g., the energy distribution of AE events did not essentially change. This was also confirmed by measuring AE on another piece of the broken sample (with a mass of about three times larger, i.e., with m = 47 mg), and besides the increased AE activity, the same characteristic features were obtained. It can be seen (see also Figure 1, Figure 2 and Figure 3 and Table 1) that the transformation temperatures are shifted to higher temperatures and the transitions are indeed sharper in the SIM-aged sample. In addition, for the SIM-aged sample, the DSC curve split into separate peaks, illustrating a stepwise character of the transformation. Table 1 also shows that the start and finish temperatures, obtained from the DSC and AE data, are in a good agreement with each other, except some acoustic activity during cooling at temperatures higher than the DSC martensite start temperature shown in Table 1 for the SIM-aged sample; see Figure 2b and Figure 4d. This can be related to the higher sensitivity of the AE as compared to the DSC. The heat treatment for austenite stabilization had no detectable effect. In Figure 3, the hysteresis loops of the martensitic transformation were constructed from the measured DSC curves. The martensite volume fraction was calculated using the normalized partial integrals of the Q/T curves [25,26] (Q is the heat of transformation and T is the temperature), and the value of the entropy, used for normalization, was determined from the measured DSC according to the usual procedure [26].
Table 2 shows the calculated values of the transformation entropy. It can be seen that the entropy did not change after austenite stabilization heat treatment. On the other hand, the transformation entropy decreased by about 36% for the SIM-aged sample.
The measured acoustic signals (at 10 K/min rate) for the quenched and SIM-aged samples are shown in Figure 4 (the plots for the austenite stabilized samples are very similar to those obtained in the quenched sample and thus are not shown). It can be seen that the number of AE events for the quenched sample, in accordance with the about 20 times larger mass, is much higher than for the SIM-aged one (see also Table 3, where the numbers of hits, N, and the sum of the AE peak energies and the average peak energies for heating and cooling are also given). For the determination of the energy probability distribution functions, the energy of an individual acoustic event, Ei, can be determined from the integration of the amplitude (voltage, Ui) versus time signal (see Figure 5) [28,29,30]. Our experimental setup allows the calculation of the energy associated with each individual hit. In our evaluation programme, the E i = 1 R j U i j 2 2 τ i approximation is used, where R is a reference electrical resistance [28,29] (taken as 1 MΩ) and   τ i t i n i , which means that it is assumed that all small separate triangle-shaped peaks (indexed by j in Figure 5) have the same lengths (ti and ni denote the duration time and the number of oscillations, respectively, during ti). The estimated characteristic frequency of the oscillations (using the relation f = ni/2ti) was in the order of 100 kHz. It is worth noting that the physics behind the source of AE is still far from being fully understood [28,31], and thus from the information contained in a detected AE signal, it is difficult to recover the information about the source [30]. However, there is a commonly accepted wisdom in the literature that AE provides a suitable measure of the dissipated energy associated with the process from which it originates [29,30,32]. This is also confirmed by a very good agreement between the energy exponents calculated from calorimetric and AE measurements [20,32].
The statistical distribution functions of the parameters of AE signals (Ui, Ei and ti), emitted during martensitic transformations, usually follow general power law behaviour [20,28,29]
P ( E ) = C E ε
where E is the peak energy of an acoustic event and ε, is the characteristic exponent, and the C prefactor includes normalization and is chosen to be proportional to e x p ( E / E c ) , where Ec is the cut-off value [28,29]. Thus, Figure 6, Figure 7 and Figure 8 show the energy distribution functions during heating and cooling for the quenched, austenite stabilized and SIM-aged samples, respectively. It can be seen that these functions can be well approximated by a straight line over three to four orders of magnitude on the energy scale, i.e., we can take that e x p ( E / E c ) 1 in the prefactor C (Equation (1)). (In our measurements, the number of hits at higher energies became very low before the cut-off effect would become visible.) The values of the energy exponents are also included in Table 3. The most remarkable difference between the plots for the SIM-aged and quenched samples is that while the characteristic exponents are the same within the error bars in Table 3 (and their values were also the same for heating and cooling), the distribution function for heating in the SIM-aged sample contains high energy solitary AE hits and these points fall above the straight line fitted to the remaining part of the plot in Figure 8a. It is worth mentioning that the existence of such AE hits was checked by performing eight separate runs: in all cases similar results were obtained, and it was also detected that they appeared not randomly but at the same temperature (see the marked points in Figure 4c). In addition, the average peak energy, Eav, after the removal of the last three high energy points, is in the same order of magnitude as the values for the other three cases in Table 3 (compare the Eav values for heating in the SIM-aged sample before and after the removal of the above three points).
Figure 4. Acoustic emission signals during the transformation: heating and cooling for the quenched, (a,b) and SIM-aged (c,d) Ni51Fe18Ga27Co4 single crystals. (Each point corresponds to an acoustic emission (AE) event, and the continuous line, indicating the transition, is the cumulative number of them.) In Figure 4c, the three points, indicated by arrows, show the solitary high energy hits for the sample with m = 18 mg (see also below in Figure 8a), whereas Figure 4e shows the same plot for the SIM-aged sample for heating with m = 47 mg.
Figure 4. Acoustic emission signals during the transformation: heating and cooling for the quenched, (a,b) and SIM-aged (c,d) Ni51Fe18Ga27Co4 single crystals. (Each point corresponds to an acoustic emission (AE) event, and the continuous line, indicating the transition, is the cumulative number of them.) In Figure 4c, the three points, indicated by arrows, show the solitary high energy hits for the sample with m = 18 mg (see also below in Figure 8a), whereas Figure 4e shows the same plot for the SIM-aged sample for heating with m = 47 mg.
Metals 10 00534 g004
Figure 5. Typical measured signal belonging to one acoustic event with a medium energy. The insert shows one oscillation of the event. The index “ i ” refers to the number of the AE event, while index “ j ” refers to the number of oscillations in the i -th event, 1 j n i , where n i is the total number of oscillations for the i -th event. τ i t i / n i (see also the text).
Figure 5. Typical measured signal belonging to one acoustic event with a medium energy. The insert shows one oscillation of the event. The index “ i ” refers to the number of the AE event, while index “ j ” refers to the number of oscillations in the i -th event, 1 j n i , where n i is the total number of oscillations for the i -th event. τ i t i / n i (see also the text).
Metals 10 00534 g005
Figure 6. Energy distribution functions; Log P versus log E, obtained from acoustic measurements during heating (a) and cooling (b) in quenched Ni51Fe18Ga27Co4 single crystal.
Figure 6. Energy distribution functions; Log P versus log E, obtained from acoustic measurements during heating (a) and cooling (b) in quenched Ni51Fe18Ga27Co4 single crystal.
Metals 10 00534 g006
Figure 7. Energy distribution functions; Log P versus log E, obtained from acoustic measurements during heating (a) and cooling (b) in austenite stabilized Ni51Fe18Ga27Co4 single crystal.
Figure 7. Energy distribution functions; Log P versus log E, obtained from acoustic measurements during heating (a) and cooling (b) in austenite stabilized Ni51Fe18Ga27Co4 single crystal.
Metals 10 00534 g007
Figure 8. Energy distribution functions for heating (a) and cooling (b), obtained from acoustic measurements for SIM-aged (m = 18 mg) Ni51Fe18Ga27Co4 single crystals. (c) shows, for comparison, the distribution for heating on the SIM-aged sample with m = 47 mg (slopes of the lines, fitted to the first parts, are the same within the error bars).
Figure 8. Energy distribution functions for heating (a) and cooling (b), obtained from acoustic measurements for SIM-aged (m = 18 mg) Ni51Fe18Ga27Co4 single crystals. (c) shows, for comparison, the distribution for heating on the SIM-aged sample with m = 47 mg (slopes of the lines, fitted to the first parts, are the same within the error bars).
Metals 10 00534 g008aMetals 10 00534 g008b

4. Discussion

The results on the hysteresis loops should be compared to the start and finish temperatures (measured also by DSC) and the transformation strain versus temperature (εtr~T) plots, published in [11] on the same single crystal after the same heat treatments/SIM-aging. Although in [11] the details of the shape of the hysteresis loop was not determined, the agreement is reasonable; see Figure 9 which, for the illustration of the shift and increase of the width of the hysteresis, shows the schematic hysteresis loops constructed from the data of Table 1 in [11]. Thus, we can conclude that the start and finish temperatures were indeed shifted to higher values, as expected for the martensite stabilization. In addition, according to Figure 3 (and Figure 1b in [11]), the cooling transition is less sharp as compared to the heating one.
The value of the transformation entropy can be compared with the value estimated from the Clausius–Clapeyron relation for the temperature dependence of the critical stress, σcr:
σ c r T = ρ Δ s / ε tr .
(ρ is the density and εtr is the transformation strain). Figure 10 shows the σcr and εtr as the function of T for the quenched sample as calculated from the σ versus εtr loops, taken at different temperatures. It can be seen that Figure 10a can be well fitted by a linear function between 350 and 550 K. Although the transformation strain has temperature dependence in (2), since the linear fit is a good approximation in Figure 10a, we can use the average value of the transformation strain in this interval (Figure 10b). Thus, using the value of the slope, cr/dT = 3.27 MPa/K, and εtr ≅ 0.035, we get Δs = −0.88 J/mol∙K, which is in a good agreement with the values shown in Table 2.
It is clear that the width of the hysteresis increased for the SIM-aged sample. Taking into account that the transformation entropy decreased only by about 36%, the increase of the area of the hysteresis loop by about a factor of 3.5 cannot be attributed only to the entropy change (ΔT, the width of the hysteresis, is inversely proportional to −Δs). Thus, the change of the entropy cannot be fully responsible for the above increase, but some additional microscopic dissipative processes have a contribution to this. In [11], it was argued that the stabilization of the detwinned martensite resulted in a significant increase of the dissipated energy (i.e., of ΔT), but understanding the details calls for further microscopic investigations. It is worth noting that the increase of the area of the hysteresis cannot be solely interpreted by the increase of the dissipated energy only if the so-called thermoelastic balance is fulfilled. If this is violated, e.g., for the SIM-aged sample (i.e., the magnitude of the elastic energy stored during cooling is different from the relaxed elastic energy during heating), then the contribution of the elastic energies to the area of hysteresis is also not negligible [33]. The results of the AE measurements can give some additional hints in this respect.
Indeed, the results shown in Figure 6 and Figure 8 and Table 3 are very interesting. While the characteristic energy exponents are the same within the error bar, there are two striking features of the results belonging to the SIM-aged sample:
  • There are high amplitude/energy hits during heating and these fall above the points on the energy distribution function.
  • Removing these, the energy exponent agrees with the other three values in Table 3 and the average peak energy has similar value to the others.
These findings indicate that some microscopic details of the forward and reverse transformations are different in the SIM-aged sample, which should be related to the burst-like transition. For the sharper heating transition, interestingly, even a few solitary high amplitude/energy AE hits were observed. These belong to the same temperature: see the high, almost vertical jump in the cumulative numbers in Figure 4c. This temperature agrees well with the temperature of the second peak in Figure 2a. It is worth noting that the envelope type DSC curves can be split into small individual peaks using appropriate low heating/cooling rates and/or small investigated masses [27,32,34]. However, we rather attribute the large two peaks in Figure 2a to high velocity sudden jumps of the interface over relatively large distances, resulting in transformation of a considerable amount of martensite volume fraction to austenite.
The energies of the individual acoustic events are directly related to the relaxation (and dissipation) of the energy of elastic waves emitted during an individual jump of the moving austenite/martensite interface [20,28,30,32]. Thus, the few large energy events belong to jumps of high velocity, since it is generally accepted that the amplitude of an AE signal is proportional to the interface velocity [20,28,30,35] and Ei is proportional to square of the amplitude, Ui. Nevertheless, the fact that the characteristic exponents are almost the same for both types of samples and in both directions is a strong indication of the robustness of the power law behaviour and calls also for further measurements and microscopic modelling. The above results remind of the effect observed in [36], where stress drops and AE during mechanically induced motion of twin boundary motion (type I boundary in Ni2MnGa) were measured. It was obtained that the stress drop events were accompanied with single dominant AE signals, while 98% of the AE signals were emitted during the intervals where no stress drop was happening. The latter signals followed nice power law behaviour, while those associated with stress drops displayed a distribution with a peak (i.e., they did not fit to the curve corresponding to the power law).
The results on the effects of austenite stabilization indicate that the change of the long range order from B2 to ordered L21 of the austenite structure has no detectable effect: the shift of the hysteresis and the change of the transformation entropy was within the limits of experimental error and the energy exponents are also similar for austenite stabilized and quenched samples, although the exponents are a little bit larger for the austenite stabilized sample (Table 3). It can be noted that in [37] differential scanning calorimetric measurements in three polycrystalline ferromagnetic shape memory alloys with compositions Ni53.5+xFe19.5-xGa27.0 (x = 0, 0.5 and 1.5) were carried out, investigating the effect of the degree of L21 order by quenching from different temperatures. It was observed, as expected, that the transformation temperatures were increased/decreased with decreasing/increasing L21 order, but the transformation entropy was not determined.
Regarding the change of the transformation entropy, we can conclude that our results are in a good agreement with the results of [22], where a minor increase (about 4%, which was close to the error bar) for the austenite stabilization and about a 12% decrease for martensite stabilization was observed. Nevertheless, the observed increase of the width of the hysteresis indicates that the entropy change cannot be connected with this since it alone would cause a much smaller effect. It is worth adding that in ferromagnetic shape memory alloys, there is a magnetic contribution to Δs [16,34,37,38] and its possible change due to SIM-aging calls for further investigations. It can be added that since the transformation entropy can be sensitive to the changes in the atomic and magnetic order [16], it can be assumed that SIM-aging can have a similar effect as the change of the slope of free energy versus the temperature. Regarding the possible contribution of the change of the elastic energy to the entropy change, we remind that after a few thermal cycles, the SIM-aged sample was broken into small pieces because of the very large local stresses due to the large shape change accompanied with the transformation. If the material would not be brittle, this would lead to a small stress accumulation since in our case, the strain, accompanied with the shape change, is close to the expected maximal strain. Thus, in the broken sample, during cycling, this can also cause only a small, sudden change of the elastic energy. In the quenched sample, due to the presence of different twins, the elastic energy (accumulated during cooling and relaxed during heating) should be larger. On the other hand, since the temperature dependence of the elastic constants is usually weak, these different elastic energies represent a negligible contribution to the slopes of the free energies versus the temperature functions of the austenite and martensite, the difference of which is the measure of the entropy change. In addition, it seems to be less probable that defects introduced by the SIM aging would be responsible for the observed entropy change: the martensite stabilization results in more ideal martensite microstructure as compared to the one in the quenched state (e.g., by annealing out of the frozen-in vacancies by quenching). This assumption is also in accordance with the arguments used in [16]: “the only effect of such stabilization is a homogeneous decrease of the chemical free energy of the sample’s material”. On the other hand, the fact that the austenite stabilization has a minor effect is in accordance with arguments published in [12,19,22], i.e., the change of the long-range order in the austenite, after the heat treatments applied, has a moderate effect in this alloy too.

5. Conclusions

SIM-aging caused a shift of transformation temperatures to higher values, and the forward (from austenite to martensite) and reverse transitions became sharper, while the width of the hysteresis increased.
  • The energy distributions of acoustic hits in SIM-aged samples showed similar behaviour to those of the quenched sample, and the energy exponents characterizing the power law behaviour were also similar.
  • For heating, in accordance with the sharper transition observed in the DSC run, few high amplitude/energy solitary hits were observed, and these points did not fit to the energy distribution function fitted at smaller energies. Thus, these high-energy events were attributed to high sudden jumps in the phase transition during heating. These high, almost vertical jumps, in the cumulative numbers in Figure 4c, agreed well with the temperature of the second DSC peak in Figure 2a. Thus, we attributed the few large energy jumps to jumps of high austenite/martensite interface velocity; this velocity can be orders of magnitude larger than the other velocities with which the interface moves in the quenched sample.
  • It was found that the transformation entropy was about 36% smaller for the SIM-aged sample and was practically unchanged after austenite stabilization.

Author Contributions

Conceptualization, D.L.B., E.P. and Y.C.; methodology, L.D.; software, L.Z.T.; formal analysis, N.M.S.; investigation, N.M.S. and N.S.; writing—original and draft preparation, D.L.B., E.P. and Y.C.; supervision, D.L.B. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the GINOP-2.3.2-15-2016-00041 project. The project was co-financed by the European Union and the European Regional Development Fund. The described research was also supported through the National Research, Development and Innovation Office—NKFIH K119566 project.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript or in the decision to publish the results.

References

  1. Niendorf, T.; Krooß, P.; Somsen, C.; Eggeler, G.; Chumlyakov, Y.I.; Maier, H.J. Martensite aging - Avenue to new high temperature shape memory alloys. Acta Mater. 2015, 89, 298–304. [Google Scholar] [CrossRef]
  2. Picornell, C.; Pons, J.; Cesari, E. Stabilisation of martensite by applying compressive stress in Cu-Al-Ni single crystals. Acta Mater. 2001, 49, 4221–4230. [Google Scholar] [CrossRef]
  3. Chernenko, V.A.; Pons, J.; Cesari, E.; Zasimchuk, I.K. Transformation behaviour and martensite stabilization in the ferromagnetic Co-Ni-Ga Heusler alloy. Scr. Mater. 2004, 50, 225–229. [Google Scholar] [CrossRef]
  4. Kadletz, P.M.; Krooß, P.; Chumlyakov, Y.I.; Gutmann, M.J.; Schmahl, W.W.; Maier, H.J.; Niendorf, T. Martensite stabilization in shape memory alloys - Experimental evidence for short-range ordering. Mater. Lett. 2015, 159, 16–19. [Google Scholar] [CrossRef]
  5. Eftifeeva, A.; Panchenko, E.; Chumlyakov, Y.; Maier, H.J. Two-way shape memory effect in [001] B2-oriented Co-Ni-Al single crystals. Mater. Today Proc. 2017, 4, 4789–4796. [Google Scholar] [CrossRef]
  6. Panchenko, E.Y.; Timofeeva, E.E.; Larchenkova, N.G.; Chumlyakov, Y.I.; Tagiltsev, A.I.; Maier, H.J.; Gerstein, G. Two-way shape memory effect under multi-cycles in [001]-oriented Ni49Fe18Ga27Co6 single crystal. Mater. Sci. Eng. A 2017, 706, 95–103. [Google Scholar] [CrossRef]
  7. Gerstein, G.; L’vov, V.A.; Kosogor, A.; Maier, H.J. Internal pressure as a key thermodynamic factor to obtain high-temperature superelasticity of shape memory alloys. Mater. Lett. 2018, 210, 252–254. [Google Scholar] [CrossRef]
  8. Panchenko, E.; Eftifeeva, A.; Chumlyakov, Y.; Gerstein, G.; Maier, H.J. Two-way shape memory effect and thermal cycling stability in Co35Ni35Al30 single crystals by low-temperature martensite ageing. Scr. Mater. 2018, 150, 18–21. [Google Scholar] [CrossRef]
  9. Timofeeva, E.E.; Panchenko, E.Y.; Pichkaleva, M.V.; Tagiltsev, A.I.; Chumlyakov, Y.I. The effect of stress-induced martensite ageing on the two-way shape memory effect in Ni53Mn25Ga22 single crystals. Mater. Lett. 2018, 228, 490–492. [Google Scholar] [CrossRef]
  10. Panchenkoa, E.Y.; Timofeeva, E.E.; Chumlyakov, Y.I.; Osipovich, K.S.; Tagiltsev, A.I.; Gerstein, G.; Maier, H.J. Compressive shape memory actuation response of stress-induced martensite aged Ni51Fe18Ga27Co4 single crystals. Mater. Sci. Eng. A 2019, 746, 448–455. [Google Scholar] [CrossRef]
  11. Panchenko, E.; Timofeeva, E.; Eftifeeva, A.; Osipovich, K.; Surikov, N.; Chumljakov, Y.; Gerstein, G.; Maier, H.J. Giant rubber-like behavior induced by martensite aging in Ni51Fe18Ga27Co4 single crystals. Scr. Mater. 2019, 162, 387–390. [Google Scholar] [CrossRef]
  12. Ahlers, M.; Pelegrina, J.L. Ageing of martensite: Stabilisation and ferroelasticity in Cu-based shape memory alloys. Mater. Sci. Eng. A 2003, 356, 298–315. [Google Scholar] [CrossRef]
  13. Ren, X.; Otsuka, K. Origin of rubber-like behaviour in metal alloys. Nature 1997, 389, 579–582. [Google Scholar] [CrossRef]
  14. Otsuka, K.; Ren, X. Mechanism of martensite aging effects and new aspects. Mater. Sci. Eng. A 2001, 312, 207–218. [Google Scholar] [CrossRef]
  15. Lauhoff, C.; Krooß, P.; Langenkämper, D.; Somsen, C.; Eggeler, G.; Kireeva, I.; Chumlyakov, Y.I.; Niendorf, T. Martensite aging in 〈001〉 oriented Co49Ni21Ga30 single crystals in tension. Funct. Mater. Lett. 2018, 11, 1850024. [Google Scholar] [CrossRef]
  16. Segui, C.; Cesari, E. Contributions to the transformation entropy change and influencing factors in metamagnetic Ni-Co-Mn-Ga shape memory alloys. Entropy 2014, 16, 5560–5574. [Google Scholar] [CrossRef] [Green Version]
  17. Zhao, D.; Xiao, F.; Nie, Z.; Cong, D.; Sun, W.; Liu, J. Burst-like superelasticity and elastocaloric effect in [011] oriented Ni50Fe19Ga27Co4 single crystals. Scr. Mater. 2018, 149, 6–10. [Google Scholar] [CrossRef]
  18. Nikolaev, V.I.; Yakushev, P.N.; Malygin, G.A.; Averkin, A.I.; Pulnev, S.A.; Zograf, G.P.; Kustov, S.B.; Chumljakov, Y.I. Influence of partial shape memory deformation on the burst character of its recovery in heated Ni–Fe–Ga–Co alloy crystals. Tech. Phys. Lett. 2016, 42, 399–402. [Google Scholar] [CrossRef]
  19. Kustov, S.; Pons, J.; Cesari, E.; Van Humbeeck, J. Chemical and mechanical stabilization of martensite. Acta Mater. 2004, 52, 4547–4559. [Google Scholar] [CrossRef]
  20. Beke, D.L.; Daróczi, L.; Tóth, L.Z.; Bolgár, M.K.; Samy, N.M.; Hudák, A. Acoustic emissions during structural changes in shape memory Alloys. Metals 2019, 9, 58. [Google Scholar] [CrossRef] [Green Version]
  21. Pelegrina, J.L.; Ahlers, M. The martensitic phases and their stability in Cu-Zn and Cu-Zn-Al alloys-I. The transformation between the high temperature β phase and the 18R martensite. Acta Metall. Mater. 1992, 40, 3205–3211. [Google Scholar] [CrossRef]
  22. Chandrasekaran, M.; Cooreman, L.; Van Humbeeck, J.; Delaey, L. Martensitic transformation in Cu-Zn-Al: changes in transformation entropy due to post quench ageing in the β or martensitic condition. Scr. Metall. 1989, 23, 239–273. [Google Scholar] [CrossRef]
  23. Imano, Y.; Omori, T.; Oikawa, K.; Sutou, Y.; Kainuma, R.; Ishida, K. Martensitic and magnetic transformations of Ni-Ga-Fe-Co ferromagnetic shape memory alloys. Mater. Sci. Eng. A 2006, 438–440, 970–973. [Google Scholar] [CrossRef]
  24. Bolgár, M.K.; Tóth, L.Z.; Szabó, S.; Gyöngyösi, S.; Daróczi, L.; Panchenko, E.Y.; Chumlyakov, Y.I.; Beke, D.L. Thermal and acoustic noises generated by austenite/martensite transformation in NiFeGaCo single crystals. J. Alloys Compd. 2016, 658, 29–35. [Google Scholar] [CrossRef]
  25. Planes, A.; Macqueron, J.L.; Ortîn, J. Energy contributions in the martensitic transformation of shape-memory alloys. Philos. Mag. Lett. 1988, 57, 291–298. [Google Scholar] [CrossRef]
  26. Beke, D.L.; Daróczi, L.; Elrasasi, T.Y. Determination of elastic and dissipative energy contributions to martensitic phase transformation in shape memory alloys. In Shape Memory Alloys-Processing, Characterization and Applications; Fernandes, F., Ed.; InTech: London, UK, 2013; p. 167. ISBN 978-953-51-1084-2. [Google Scholar]
  27. Tóth, L.Z.; Daróczi, L.; Szabó, S.; Beke, D.L. Simultaneous investigation of thermal, acoustic, and magnetic emission during martensitic transformation in single-crystalline Ni2MnGa. Phys. Rev. B 2016, 93, 144108. [Google Scholar] [CrossRef] [Green Version]
  28. Rosinberg, M.L.; Vives, E. Metastability, Hysteresis, Avalanches, and Acoustic Emission: Martensitic Transitions in Functional Materials. In Disorder and Strain Induced Complexity in Functional Materials; Kakeshita, T., Fukuda, T., Saxena, A., Planes, A., Eds.; Springer Series in Materials Science; Springer: Berlin, Germany, 2012; Volume 148, pp. 249–272. ISBN 978-3-642-20943-7. [Google Scholar]
  29. Planes, A.; Mañosa, L.; Vives, E. Acoustic emission in martensitic transformations. J. Alloys Compd. 2013, 577, S699–S704. [Google Scholar] [CrossRef]
  30. Bonnot, E.; Vives, E.; Mañosa, L.; Planes, A.; Romero, R. Acoustic emission and energy dissipation during front propagation in a stress-driven martensitic transition. Phys. Rev. B 2008, 78, 094104. [Google Scholar] [CrossRef]
  31. Mañosa, L.; Planes, A.; Rouby, D.; Morin, M.; Fleischmann, P.; Macqueron, J.L. Acoustic emission field during thermoelastic martensitic transformations. Appl. Phys. Lett. 1989, 54, 2574–2576. [Google Scholar] [CrossRef]
  32. Gallardo, M.C.; Manchado, J.; Romero, F.J.; Del Cerro, J.; Salje, E.H.; Planes, A.; Vives, E.; Ricardo, R.; Marcelo, S. Avalanche criticality in the martensitic transition of Cu67.64 Zn16.71 Al15.65 shape-memory alloy: A calorimetric and acoustic emission study. Phys. Rev. B 2010, 81, 174102. [Google Scholar] [CrossRef] [Green Version]
  33. Beke, D.L.; Bolgár, M.K.; Tóth, L.Z.; Daróczi, L. On the asymmetry of the forward and reverse martensitic transformations in shape memory alloys. J. Alloys Compd. 2018, 741, 106–115. [Google Scholar] [CrossRef] [Green Version]
  34. Marcos, J.; Planes, A.; Manosa, L.; Casanova, F.; Battle, X.; Labarta, A.; Martinez, B. Magnetic field induced entropy change and magnetoelasticity in Ni-Mn-Ga alloys. Phys. Rev. B 2002, 66, 224413. [Google Scholar] [CrossRef] [Green Version]
  35. Scruby, C.B. Quantitative acoustic emission techniques. In Research Techniques in Non-Destructive Testing; Sharpe, R.S., Ed.; Academic Press: London, UK, 1985; Volume III, ISBN 0126390533. [Google Scholar]
  36. Zreihan, N.; Faran, E.; Vives, E.; Planes, A.; Shilo, D. Relations between stress drops and acoustic emission measured during mechanical loading. Phys. Rev. Mater. 2019, 3, 043603. [Google Scholar] [CrossRef]
  37. Santamarta, R.; Cesari, E.; Font, J.; Muntasell, J.; Pons, J.; Dutkiewicz, J. Effect of atomic order on the martensitic transformation of Ni-Fe-Ga alloys. Scr. Mater. 2006, 54, 1985–1989. [Google Scholar] [CrossRef]
  38. Khovailo, V.V.; Oikawa, K.; Abe, T.; Takagi, T. Entropy change at the martensitic transformation in ferromagnetic shape memory alloys Ni2+xMn1-xGa. J. Appl. Phys. 2003, 93, 8483–8485. [Google Scholar] [CrossRef] [Green Version]
Figure 1. DSC runs for heating (a) and cooling (b) for the quenched Ni51Fe18Ga27Co4 single crystals.
Figure 1. DSC runs for heating (a) and cooling (b) for the quenched Ni51Fe18Ga27Co4 single crystals.
Metals 10 00534 g001
Figure 2. DSC runs for heating (a) and cooling (b) of the stress-induced martensite stabilized (SIM-aged) Ni51Fe18Ga27Co4 single crystals.
Figure 2. DSC runs for heating (a) and cooling (b) of the stress-induced martensite stabilized (SIM-aged) Ni51Fe18Ga27Co4 single crystals.
Metals 10 00534 g002
Figure 3. Hysteresis loops calculated from the DSC curves for the quenched and SIM-aged Ni51Fe18Ga27Co4 single crystals (10 K/min).
Figure 3. Hysteresis loops calculated from the DSC curves for the quenched and SIM-aged Ni51Fe18Ga27Co4 single crystals (10 K/min).
Metals 10 00534 g003
Figure 9. Schematic hysteresis loops from the start and finish temperatures published in [11].
Figure 9. Schematic hysteresis loops from the start and finish temperatures published in [11].
Metals 10 00534 g009
Figure 10. Temperature dependence of the critical stress (a), the transformation strain (b) for the quenched sample. The solid line in (a) shows the region where the linear fit is a good approximation, while in (b), it is only to guide the eye.
Figure 10. Temperature dependence of the critical stress (a), the transformation strain (b) for the quenched sample. The solid line in (a) shows the region where the linear fit is a good approximation, while in (b), it is only to guide the eye.
Metals 10 00534 g010
Table 1. Transition temperatures for the quenched, austenite stabilized and stress-induced martensite stabilized (SIM)-aged Ni51Fe18Ga27Co4 single crystals, as obtained from DSC and acoustic emission (AE) measurements. The error bars are about ±3 K.
Table 1. Transition temperatures for the quenched, austenite stabilized and stress-induced martensite stabilized (SIM)-aged Ni51Fe18Ga27Co4 single crystals, as obtained from DSC and acoustic emission (AE) measurements. The error bars are about ±3 K.
Type of SampleASAfMsMf
Quenched, AE270337317254
Quenched, DSC276320308259
Austenite Stabilized, AE270337317254
SIM-aged, DSC377386343317
Table 2. Values of the transformation entropy, −Δs, calculated from the DSC curves for the quenched, austenite stabilized (annealed at 573 K for 6 h) and SIM-aged Ni51Fe18Ga27Co4 single crystals. The numbers are averaged values for heating and cooling and the error bars are about ±0.08 J/mol∙K, within which, the values for heating and cooling were also the same.
Table 2. Values of the transformation entropy, −Δs, calculated from the DSC curves for the quenched, austenite stabilized (annealed at 573 K for 6 h) and SIM-aged Ni51Fe18Ga27Co4 single crystals. The numbers are averaged values for heating and cooling and the error bars are about ±0.08 J/mol∙K, within which, the values for heating and cooling were also the same.
−ΔSQuenchedAustenite StabilizedSIM-Aged
(J/mol∙K)0.940.940.60
Table 3. Critical energy exponents, ε, and energies of hits in the acoustic noises for heating and cooling at 10 K/min for the quenched, austenite stabilized and SIM-aged Ni51Fe18Ga27Co4 single crystals. Et is the sum of peak energies ( i E i ) , Eav is the average peak energy ( E a v = i E i N and N is the number of hits). The energies are given in μ∙V2∙Ω−1s units.
Table 3. Critical energy exponents, ε, and energies of hits in the acoustic noises for heating and cooling at 10 K/min for the quenched, austenite stabilized and SIM-aged Ni51Fe18Ga27Co4 single crystals. Et is the sum of peak energies ( i E i ) , Eav is the average peak energy ( E a v = i E i N and N is the number of hits). The energies are given in μ∙V2∙Ω−1s units.
Type of SampleAE for HeatingAE for Cooling
NEtEavεNEtEavε
Quenched320776.1 × 1041.91.84 ± 0.06405001.4 × 1053.61.87 ± 0.06
Austenite Stabilized188919.2 × 1030.51.97 ± 0.06269304.0 × 1041.51.94 ± 0.12
SIM-aged9671.9 × 1061970-527810620.21.2 ± 0.1
SIM-aged, removing high energy events9647690.81.7 ± 0.3----

Share and Cite

MDPI and ACS Style

Samy, N.M.; Daróczi, L.; Tóth, L.Z.; Panchenko, E.; Chumlyakov, Y.; Surikov, N.; Beke, D.L. Effect of Stress-Induced Martensite Stabilization on Acoustic Emission Characteristics and the Entropy of Martensitic Transformation in Shape Memory Ni51Fe18Ga27Co4 Single Crystal. Metals 2020, 10, 534. https://doi.org/10.3390/met10040534

AMA Style

Samy NM, Daróczi L, Tóth LZ, Panchenko E, Chumlyakov Y, Surikov N, Beke DL. Effect of Stress-Induced Martensite Stabilization on Acoustic Emission Characteristics and the Entropy of Martensitic Transformation in Shape Memory Ni51Fe18Ga27Co4 Single Crystal. Metals. 2020; 10(4):534. https://doi.org/10.3390/met10040534

Chicago/Turabian Style

Samy, Nora Mohareb, Lajos Daróczi, László Zoltán Tóth, Elena Panchenko, Yury Chumlyakov, Nikita Surikov, and Dezső László Beke. 2020. "Effect of Stress-Induced Martensite Stabilization on Acoustic Emission Characteristics and the Entropy of Martensitic Transformation in Shape Memory Ni51Fe18Ga27Co4 Single Crystal" Metals 10, no. 4: 534. https://doi.org/10.3390/met10040534

APA Style

Samy, N. M., Daróczi, L., Tóth, L. Z., Panchenko, E., Chumlyakov, Y., Surikov, N., & Beke, D. L. (2020). Effect of Stress-Induced Martensite Stabilization on Acoustic Emission Characteristics and the Entropy of Martensitic Transformation in Shape Memory Ni51Fe18Ga27Co4 Single Crystal. Metals, 10(4), 534. https://doi.org/10.3390/met10040534

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop