Next Article in Journal
Effect of the Welding Speed on the Macrostructure, Microstructure and Mechanical Properties of AA6061-T6 Friction Stir Butt Welds
Next Article in Special Issue
Improved Compressive, Damping and Coefficient of Thermal Expansion Response of Mg–3Al–2.5La Alloy Using Y2O3 Nano Reinforcement
Previous Article in Journal
Discussion on the Local Magnetic Force between Reversely Magnetized Micro Metal Particles in the Microwave Sintering Process
Previous Article in Special Issue
A Meso-Mechanical Constitutive Model of Particle-Reinforced Titanium Matrix Composites at High Temperatures
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Microstructures and Tensile Properties of Al–Cu Matrix Composites Reinforced with Nano-Sized SiCp Fabricated by Semisolid Stirring Process

1
Key Laboratory of Automobile Materials, Ministry of Education and Department of Materials Science and Engineering, Jilin University, Renmin Street NO. 5988, Changchun 130025, China
2
State Key Laboratory of Luminescence and Applications, Changchun Institute of Optics, Fine Mechanics and Physics, Chinese Academy of Sciences, Changchun 130012, China
3
Department of Mechanical Engineering, Oakland University, Rochester, MI 48309, USA
*
Author to whom correspondence should be addressed.
Metals 2017, 7(2), 49; https://doi.org/10.3390/met7020049
Submission received: 29 December 2016 / Accepted: 3 February 2017 / Published: 8 February 2017
(This article belongs to the Special Issue Metal Matrix Composites)

Abstract

:
The nano-sized SiCp/Al–Cu composites were successfully fabricated by combining semisolid stirring with ball milling technology. Microstructures were examined by an olympus optical microscope (OM), field emission scanning electron microscope (FESEM) and transmission electron microscope (TEM). Tensile properties were studied at room temperature. The results show that the α-Al dendrites of the composites were strongly refined, especially in the composite with 3 wt. % nano-sized SiCp, of which the morphology of the α-Al changes from 200 μm dendritic crystal to 90 μm much finer equiaxial grain. The strength and ductility of the composites are improved synchronously with the addition of nano-sized SiCp particles. The as-cast 3 wt. % nano-sized SiCp/Al–Cu composite displays the best tensile properties, i.e., the yield strength, ultimate tensile strength (UTS) and fracture strain increase from 175 MPa, 310 MPa and 4.1% of the as-cast Al–Cu alloy to 220 MPa, 410 MPa and 6.3%, respectively. The significant improvement in the tensile properties of the composites is mainly due to the refinement of the α-Al dendrites, nano-sized SiCp strengthening, and good interface combination between the SiCp and Al–Cu alloys.

1. Introduction

In the past decades, particulate reinforced aluminum matrix composites (AMCs) have attracted much attention in the field of structural and functional materials [1,2,3,4]. SiCp reinforced AMCs have been a hot research issue in recent years because of their excellent properties such as low density, high tensile strength, high elastic modulus and wear resistance, etc. [5,6,7]. For example, SiCp reinforced AMCs are used for engine piston, and heat sink [8,9]. Compared with traditional micron-sized SiCp/Al composites, the higher tensile strength and good ductility of the nano-sized SiCp/Al composites entitle them to have more competitive ability for advanced structural applications such as in automotive and aerospace industries and the military [10]. In the past decades, several processing techniques have been developed for fabricating Al matrix composites reinforced with nano-sized particles such as high-energy milling, powder metallurgy, and nano-sintering, and liquid-state solidification processing (e.g., stir casting) [11,12,13,14,15,16,17,18,19]. In these techniques, the semisolid stirring process has some important advantages such as low cost, capability of producing products with complex shapes, and processing simplicity [14].
Al–Si and Al–Mg alloys are the usually used matrix phase in nano-sized SiCp/Al composites [10,16,20,21]. Xiong et al. [10] fabricated 14 vol. % nano-sized SiCp/Al–Mg composites. They reported that the ultimate tensile strength increased from 223 MPa to 286 MPa, while the ductility decreased from 4.8% to 3.9%. Hamedan et al. [16] produced 1.0 wt. % nano-sized SiCp/Al356 composite and reported that the ultimate tensile strength of the composite increased from 140 MPa to173 MPa, while the ductility decreased slightly from 6.1% to 5.38%. Compared to the Al–Si and Al–Mg alloys, the Al–Cu alloys can offer some good mechanical properties. For instance, a previous study by us has shown that the tensile strength and elongation increased by 26% and 50% respectively, for the modified Al–Cu alloys compared with unmodified alloy [22]. Moreover, we also found that the corrosion resistance of modified Al–Cu alloy had an improvement compared with the unmodified one [23]. However, to the best of our knowledge, so far, because there is no chemical affinity between the Cu element and SiCp, and the Cu element can also not improve the wettability between the aluminum matrix and SiCp [24], the Al–Cu alloys were rarely used as a matrix in the nano-sized SiCp/Al composites in stir casting. It is believed that if the nano-sized SiCp/Al–Cu composites with uniform distribution SiCp and clean interface between the SiCp and Al–Cu alloys could be successfully fabricated, the composites will exhibit excellent mechanical properties, which are very important for application in the automotive and aircraft industries.
In this paper, the nano-sized SiCp/Al–Cu composites were fabricated by combining semisolid stirring with ball milling technology. Semisolid stirring can suppress the interfacial reaction due to the low stirring temperature [19]. The usage of precursor powders fabricated by the mix of the nano-sized SiCp and alloy powders using mechanical ball milling is of benefit to the dispersion of the nano-sized SiCp in the matrix due to the disruption of the agglomerate nano-sized SiCp clusters in advance. The microstructures and tensile properties of the synthesized composites were investigated, and the strengthening mechanism was discussed. We expect that such knowledge would provide guidance for the fabrication and application of the nano-sized SiCp/Al–Cu composites.

2. Experimental Procedure

The Al–Cu alloy with a composition of (wt. %): 5.0 Cu, 0.8 Mn, 0.7 Fe, 0.5 Mg, 0.5 Si, 0.25 Zn, 0.15 Ti, 0.1 Cr and Al (balance) was used as the matrix. The nano-sized SiCp, with a purity of 99.9 wt. % and ~60 nm in diameter, were used as the reinforced particles. The morphology of the raw nano-sized SiCp particles is shown in Figure 1a. If the agglomerate nano-sized SiCp clusters are added into the melt directly, it is difficult for semisolid stirring to break the clustering and disperse the nano-sized particles uniformly. Figure 1b shows the Al–Cu alloy powders (99% pure) with average sizes of about 10 μm, their composition is the same as the Al–Cu alloy matrix. Figure 1c,d shows the precursor powders which are fabricated by the mix of the calculated nano-sized SiCp and Al–Cu alloy powders using mechanical ball milling with ZrO2 balls at the speed of 150 r/min for 50 h. Figure 1d is the a high magnification of the rectangular area in Figure 1c. It could be found that most of the nano-sized SiCp display a relatively uniform distribution in each individual composite particle surface. The ball to powder weight ratio was 8:1. During melting, Al–Cu alloy was melted at 933 K in air using an electricity resistant furnace and then cooled to 873 K at which point the matrix alloy was in semi-solid condition. The temperature range for the Al–Cu alloy used in this study to be in the semi-solid condition is 813 K–903 K. Then, the precursor powder was added into the molten metal after stirring the molten metal with a graphite stirrer at the speed of 500 r/min. After that, the melt was poured into a preheated steel die. After the casting process, the Al–Cu alloy and the composites were homogenised for 10 h at 758 K in order to avoid segregation. The materials were extruded to the batten shaped samples with the help of a 200-ton hydraulic press at 773 K with the extrusion ratio of 16. Before the tensile test, all the extruded samples underwent the T6 heat treatment (solutionized at 773 K for 2 h and aged at 433 K for 18 h).
Microstructures of the composites were examined by an Optical Microscope (Axio Imager A2m, Zeiss, Oberkochen, Germany) equipped with image analysis software and a camera; a computer was used for the OM observation and the quantitative measurements of microstructural features. The size of Al dendrites in every composite was measured from forty images taken at two magnifications, such as 50×, and 100×. Five samples of every composite were used to obtain the standard deviations (the error bars) plotted in Figure 2. Microstructures of the composites and morphologies of the raw nano-sized SiC particles and Al–Cu alloy powders were observed by field emission SEM (FESEM, JSM6700F, Tokyo, Japan) and SEM (Evo18, Carl Zeiss, Oberkochen, Germany).
The extruded samples were machined into dog-bone shaped tensile samples with a gauge cross section of 5.0 mm × 2.5 mm and a gauge length of 30.0 mm. Tensile tests were conducted at room temperature by using a servo-hydraulic materials testing system (MTS, MTS 810, Minneapolis, MN, USA) at a constant strain rate of 3 × 10−4 s−1.

3. Results and Discussion

Figure 3 shows the as-cast microstructures of the Al–Cu alloy and nano-sized SiCp/Al–Cu composites with the nominal content of 1 wt. %, 3 wt. %, 5 wt. % SiCp. As shown in Figure 3a, the α-Al dendrites of the Al–Cu matrix alloy are coarse and their average size is about 200 μm. However, in the nano-sized SiCp/Al–Cu composites, the α-Al dendrites are significantly refined by the addition of nano-sized SiCp, as shown in Figure 3b–d. The refinement of the dendrite size is mainly due to some heterogeneous nucleation sties of the α-Al crystal provided by nano-sized particles during solidification, and the hindrance of the other added nano-sized SiCp to the growth of α-Al dendrites during the solidification process. Figure 2 shows the size of dendrite in the nano-sized SiCp/Al–Cu composites with different particle contents. In the 3 wt. % nano-sized SiCp/Al–Cu composite, the morphology of α-Al changes from coarse dendritic grain to equiaxial grain with finer sizes of about 90 μm, which increases the boundary concentration in the Al matrix. The increase in the boundary concentration could be helpful to improve the tensile strength of metals or alloys due to the grain boundary playing a role as a barrier to the transmission of the dislocations. The as-cast microstructure of the composite with 5 wt. % SiCp is similar to that with 3 wt. % SiCp, although the sizes of the α-Al dendrites were uneven sizes of 60–150 μm (Figure 3d). In the composite with 5 wt. % SiCp, the shape of Al dendrites became very non-uniform due to the agglomeration of nano-sized SiCp particles. The hindrance effect of the nano-sized SiCp on the α-Al dendrite growth is strong in the area of agglomeration of ceramic particles. On the contrary, the hindrance effect of the nano-sized SiCp on the α-Al dendrite growth is weakened in the area of less ceramic particles. Thus, the difference in the size of the α-Al dendrites was probably due to the nonuniform dispersion of SiCp when their contents reached 5 wt. %.
Figure 4 shows the engineering stress–strain curves of the cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites, and Table 1 lists the detailed data of the tensile properties. As indicated, the strength and ductility of the composites (1 wt. % and 3 wt. %) are improved synchronously which is quite rare for the composites reinforced with ceramic particles, because in most reported works [11,14,20,21], the composites had a higher strength and lower ductility than the matrix alloy. The yield strength (σ0.2), ultimate tensile strength (UTS) and fracture strain (ε) of the nano-sized SiCp/Al–Cu composites firstly increase and then decrease with the increase in the content of SiCp. The 3 wt. % nano-sized SiCp/Al–Cu composite possesses the best tensile properties. The yield strength, UTS and fracture strain of the 3 wt. % SiCp/Al–Cu composite are 220 MPa, 410 MPa and 6.3%, which increase by 45 MPa (25.7%), 100 MPa (32.2%) and 2.2% (53.6%), respectively, compared to those of the as-cast Al–Cu alloy (175 MPa, 310 MPa and 4.1%).
Figure 5a–d shows the FESEM images of the 3 wt. % and 5 wt. % nano–sized SiCp/Al–Cu composite, and TEM micrographs of the 3 wt. % SiCp/Al–Cu composite. As indicated in Figure 5a,b, more evenly distributed nano-sized SiCp particles in the 3 wt. % SiCp/Al–Cu composite are observed compared with the 5 wt. % SiCp/Al–Cu composite. However, in the 5 wt. % SiCp/Al–Cu composite as shown in Figure 5b, although there are some uniform distribution zones of nano-sized SiCp, the agglomeration of particles can still be easily found, as shown in Figure 5d. In other words, more and more particles aggregate to form the clusters with the increase in the content of SiCp, resulting in the quite uneven α-Al dendrites sizes and higher concentration of defects. As shown in Figure 5c, it is clearly seen that the nano-sized SiC particles dispersed inside the α-Al dendrite and the interface between the SiC particles and matrix are good and clean without any contaminations, indicating the superiority of this fabrication technology.
The significant improvement of the strength of the SiCp/Al–Cu composites is mainly due to the refinement of the α-Al dendrites and the hindrance of the nano-sized SiCp to the start and motion of dislocations in the matrix. Moreover, the significantly improved ductility of the nano-sized SiCp/Al–Cu composites with a simultaneously increased tensile strength is derived from three factors:
(i)
Nano-sized reinforcement. Compared with micron-sized ceramic particles, the nano-sized ceramic particles used as reinforcement can not only possess higher tensile strength but also maintain good ductility, especially in the low contents [21]. Large reinforcement particles could give rise to cleavage in the particle due to the fact that they are acting as concentrators of stress, and lead to the formation of pits or cavities due to the loss of interphase cohesion. However, the smallest reinforcement particles usually do not initiate pits or cavities at the particle and bond well to the metal matrix [11].
(ii)
Dendrite refinement. The refinement of the α-Al dendrites will result in the increase in matrix dendrite boundaries. The finer the dendrite is, the more tortuous the grain boundaries are. Therefore, the crack propagation becomes more and more difficult and thus the composites can endure the larger plastic deformation before fracture.
(iii)
Suppression of interfacial reaction. It is known that the reaction between molten Al and SiCp takes place easily in the temperature range from 675 °C to 900 °C, producing Al4C3 which is a brittle and unstable phase [12]. The presence of Al4C3 degrades the mechanical properties through crack propagation. In the present work, low stirring temperature (600 °C) during the semisolid stirring process can suppress the interfacial reaction effectively, which will be helpful to restrict the formation of the Al4C3 phase. The improved strength and cracking resistance of the interface bonding make the occurrence of the crack source cracking become more difficult.
Nano-sized particle strengthening, microstructure refinement, and good interface between reinforcement and matrix with no brittle intermetallics can be responsible for the significant improvement in the mechanical properties of the nano-sized SiCp/Al–Cu composites. Hence, the nano-sized SiCp/Al–Cu composites showed high plasticity and strength. However, the properties of the composite with high content nano-sized SiCp particles could be weakened because this composite resulted in more agglomeration of the SiCp and higher concentration of defects. More severe agglomeration of SiCp could not lead to the matrix being completely wrapped up by the particles and thus result in the debonding of the interface. Moreover, micro-porosity and other defects around the SiCp clusters presented in the composites become the cracking source during the plastic deformation. The above analyses imply that the embrittlement of the composites resulting from micro-porosity and detects results in the decrease in strength and ductility of the 5 wt. % SiCp/Al–Cu.

4. Conclusions

The nano-sized SiCp/Al–Cu composites with contents of 1 wt. %, 3 wt. %, 5 wt. % SiCp were successfully fabricated by combining semisolid stirring with ball milling technology. The α-Al dendrites are significantly refined due to the addition of nano-sized SiCp. The refinement of the dendrite size is mainly attributed to some nano-sized particles providing some heterogeneous nucleation sties of the α-Al crystal, and the hindrance of the other added nano-sized SiCp to the growth of α-Al dendrites during the solidification process. The strength and ductility of the composites are improved synchronously with the addition of nano-sized SiCp particles. The 3 wt. % nano-sized SiCp/Al–Cu composite displays the best comprehensive tensile properties, i.e., the yield strength, UTS and fracture strain increase from 175 MPa, 310 MPa and 4.1% of the as-cast Al–Cu alloy to 220 MPa, 410 MPa and 6.3%, respectively. Nano-sized particle strengthening, microstructure refinement, and a good interface between reinforcement and the matrix with no brittle intermetallics can be responsible for the significant improvement in the mechanical properties of the nano-sized SiCp/Al–Cu composites.

Acknowledgments

The National Natural Science Foundation of China (NNSFC, No. 51571101), the “Thirteenth Five-year Plan” Science & Technology Research Foundation of Education Bureau of Jilin Province, China (Grant No. 2015-479), NNSFC (No. 51501176) and the Project 985-High Properties Materials of Jilin University.

Author Contributions

Feng Qiu and Qi-Chuan Jiang conceived and designed the experiments; Feng Qiu, Xiang Gao, Jian Tang, Yu-Yang Gao and Qiang Li performed the experiments; Feng Qiu, Jian Tang, Shi-Li Shu, and Xue Han, analyzed the data; Feng Qiu wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Wang, L.; Qiu, F.; Ouyang, L.C.; Wang, H.Y.; Zha, M.; Shu, S.L.; Zhao, Q.L.; Jiang, Q.C. A novel approach of using ground CNTs as the carbon source to fabricate uniformly distributed nano-sized TiCx/2009Al composites. Materials 2015, 8, 8839–8849. [Google Scholar] [CrossRef]
  2. Zhao, Q.; Liang, Y.H.; Zhang, Z.H.; Li, X.J.; Ren, L.Q. Study on the impact resistance of bionic layered composite of TiC-TiB2/Al from Al-Ti-B4C System. Materials 2016, 9, 708. [Google Scholar] [CrossRef]
  3. Shu, S.L.; Yang, H.Y.; Tong, C.C.; Qiu, F. Fabrication of TiCx-TiB2/Al composites for application as a Heat Sink. Materials 2016, 9, 642. [Google Scholar] [CrossRef]
  4. Zhao, Q.; Liang, Y.H.; Zhang, Z.H.; Li, X.J.; Ren, L.Q. Microstructure and dry-Sliding wear behavior of B4C ceramic particulate reinforced Al 5083 matrix composite. Metals 2016, 6, 227. [Google Scholar] [CrossRef]
  5. Sajjadi, S.A.; Ezatpoura, H.R.; Torabi Parizi, M. Comparison of microstructure and mechanical properties of A356 aluminum alloy/Al2O3 composites fabricated by stir and compo-casting processes. Mater. Des. 2012, 34, 106–111. [Google Scholar] [CrossRef]
  6. Molina, J.M.; Prieto, R.; Narciso, J.; Louis, E. The effect of porosity on the thermal conductivity of Al–12 wt. % Si/SiC composites. Scr. Mater. 2009, 60, 582–585. [Google Scholar] [CrossRef]
  7. Kerti, I.; Toptan, F. Microstructural variations in cast B4C-reinforced aluminium matrix composites (AMCs). Mater. Lett. 2008, 62, 1215–1218. [Google Scholar] [CrossRef]
  8. Du, X.F.; Gao, T.; Liu, G.L.; Liu, X.F. In situ synthesizing SiC particles and its strengthening effect on an Al-Si-Cu-Ni-Mg piston alloy. J. Alloy. Compd. 2017, 695, 1–8. [Google Scholar] [CrossRef]
  9. Schöbel, M.; Altendorfer, W.; Degischer, H.P.; Vaucher, S.; Buslaps, T.; di Michiel, M.; Hofmann, M. Internal stresses and voids in SiC particle reinforced aluminum composites for heat sink applications. Compos. Sci. Technol. 2011, 71, 724–733. [Google Scholar] [CrossRef]
  10. Xiong, B.; Xu, Z.; Yan, Q.; Cai, C.; Zheng, Y.; Lu, B. Fabrication of SiC nanoparticulates reinforced Al matrix composites by combining pressureless infiltration with ball-milling and cold-pressing technology. J. Alloy. Compd. 2010, 497, L1–L4. [Google Scholar] [CrossRef]
  11. Kang, Y.C.; Chan, S.L.I. Tensile properties of nanometric Al2O3 particulate-reinforced aluminum matrix composites. Mater. Chem. Phys. 2004, 85, 438–443. [Google Scholar] [CrossRef]
  12. Xiong, B.; Xu, Z.; Yan, Q.; Lu, B.; Cai, C. Effects of SiC volume fraction and aluminum particulate size on interfacial reactions in SiC nanoparticulate reinforced aluminum matrix composites. J. Alloy. Compd. 2011, 509, 1187–1191. [Google Scholar] [CrossRef]
  13. Hsu, C.J.; Chang, C.Y.; Kao, P.W.; Ho, N.J.; Chang, C.P. Al–Al3Ti nanocomposites produced in situ by friction stir processing. Acta Mater. 2006, 54, 5241–5249. [Google Scholar] [CrossRef]
  14. Zhang, H.; Geng, L.; Guan, L.; Huang, L. Effects of SiC particle pretreatment and stirring parameters on the microstructure and mechanical properties of SiCp/Al–6.8Mg composites fabricated by semi-solid stirring technique. Mater. Sci. Eng. A 2010, 528, 513–518. [Google Scholar] [CrossRef]
  15. Mazahery, A.; Shabani, M.O. Characterization of cast A356 alloy reinforced with nano SiC composites. Trans. Nonferr. Met. Soc. China 2012, 22, 275–280. [Google Scholar] [CrossRef]
  16. Dehghan Hamedan, A.; Shahmiri, M. Production of A356–1 wt % SiC nanocomposite by the modified stir casting method. Mater. Sci. Eng. A 2012, 556, 921–926. [Google Scholar] [CrossRef]
  17. Nie, K.B.; Wang, X.J.; Wu, K.; Xu, L.; Zheng, M.Y.; Hu, X.S. Processing, microstructure and mechanical properties of magnesium matrix nanocomposites fabricated by semisolid stirring assisted ultrasonic vibration. J. Alloy. Compd. 2011, 509, 8664–8669. [Google Scholar] [CrossRef]
  18. Mazahery, A.; Abdizadeh, H.; Baharvandi, H.R. Development of high-performance A356/nano-Al2O3 composites. Mater. Sci. Eng. A 2009, 518, 61–64. [Google Scholar] [CrossRef]
  19. Tahamtan, S.; Halvaee, A.; Emamy, M.; Zabihi, M.S. Fabrication of Al/A206–Al2O3 nano/micro composite by combining ball milling and stir casting technology. Mater. Des. 2013, 49, 347–359. [Google Scholar] [CrossRef]
  20. Amirkhanlou, S.; Niroumand, B. Effects of reinforcement distribution on low and high temperature tensile properties of Al356/SiCp cast composites produced by a novel reinforcement dispersion technique. Mater. Sci. Eng. A 2011, 528, 7186–7195. [Google Scholar] [CrossRef]
  21. Yang, Y.; Lan, J.; Li, X. Study on bulk aluminum matrix nano-composite fabricated by ultrasonic dispersion of nano-sized SiC particles in molten aluminum alloy. Mater. Sci. Eng. A 2004, 380, 378–383. [Google Scholar] [CrossRef]
  22. Zhao, H.L.; Yao, D.M.; Qiu, F.; Xia, Y.M.; Jiang, Q.C. High strength and good ductility of casting Al-Cu alloy modified by PrxOy and LaxOy. J. Alloy. Compd. 2011, 509, L43–L46. [Google Scholar] [CrossRef]
  23. Xia, Y.M.; Bai, Z.H.; Qiu, F.; Jin, S.B.; Jiang, Q.C. Effects of multi-modification of rare earth oxides PrxOy and LaxOy on microstructure and tensile properties of casting Al-Cu alloy. Mater. Sci. Eng. A 2012, 558, 602–606. [Google Scholar] [CrossRef]
  24. Kobashi, M.; Choh, T. Effects of alloying elements on SiC dispersion in liquid aluminum. Mater. Trans. 1990, 12, 1101–1107. [Google Scholar] [CrossRef]
Figure 1. SEM images of morphologies of the raw (a) nano-sized SiC particles and (b) Al–Cu alloy powders; FESEM (field emission SEM) images of (c) nano-sized SiCp/Al–Cu composite powders after ball milling; (d) high magnification of the area marked in (c).
Figure 1. SEM images of morphologies of the raw (a) nano-sized SiC particles and (b) Al–Cu alloy powders; FESEM (field emission SEM) images of (c) nano-sized SiCp/Al–Cu composite powders after ball milling; (d) high magnification of the area marked in (c).
Metals 07 00049 g001
Figure 2. Grain sizes of α-Al in the cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
Figure 2. Grain sizes of α-Al in the cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
Metals 07 00049 g002
Figure 3. Cast microstructures of the nano-sized Al–Cu alloy and SiCp/Al–Cu composites with different SiCp contents; (a) Al–Cu alloy; (b) 1 wt. % SiCp; (c) 3 wt. % SiCp; (d) 5 wt. % SiCp.
Figure 3. Cast microstructures of the nano-sized Al–Cu alloy and SiCp/Al–Cu composites with different SiCp contents; (a) Al–Cu alloy; (b) 1 wt. % SiCp; (c) 3 wt. % SiCp; (d) 5 wt. % SiCp.
Metals 07 00049 g003
Figure 4. Tensile stress–strain curves of the cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
Figure 4. Tensile stress–strain curves of the cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
Metals 07 00049 g004
Figure 5. FESEM images of the (a) 3 wt. % and (b) 5 wt. % nano-sized SiCp/Al–Cu composite; (c) TEM micrographs of the 3 wt. % SiCp/Al–Cu composite; (d) the high magnification of area A in (b).
Figure 5. FESEM images of the (a) 3 wt. % and (b) 5 wt. % nano-sized SiCp/Al–Cu composite; (c) TEM micrographs of the 3 wt. % SiCp/Al–Cu composite; (d) the high magnification of area A in (b).
Metals 07 00049 g005
Table 1. Tensile properties of the as-cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
Table 1. Tensile properties of the as-cast Al–Cu alloy and nano-sized SiCp/Al–Cu composites with different SiCp contents.
SiCp (wt. %)σ0.2 (MPa)σb (MPa)ε (%)
0 175 6 + 8 310 10 + 11 4. 1 0. 5 + 1 . 2
1 185 8 + 7 358 11 + 12 5. 3 0. 7 + 0. 8
3 220 6 + 10 410 8 + 14 6. 3 0. 5 + 0. 7
5 190 8 + 5 362 13 + 5 5. 4 1 . 6 + 1 . 3

Share and Cite

MDPI and ACS Style

Qiu, F.; Gao, X.; Tang, J.; Gao, Y.-Y.; Shu, S.-L.; Han, X.; Li, Q.; Jiang, Q.-C. Microstructures and Tensile Properties of Al–Cu Matrix Composites Reinforced with Nano-Sized SiCp Fabricated by Semisolid Stirring Process. Metals 2017, 7, 49. https://doi.org/10.3390/met7020049

AMA Style

Qiu F, Gao X, Tang J, Gao Y-Y, Shu S-L, Han X, Li Q, Jiang Q-C. Microstructures and Tensile Properties of Al–Cu Matrix Composites Reinforced with Nano-Sized SiCp Fabricated by Semisolid Stirring Process. Metals. 2017; 7(2):49. https://doi.org/10.3390/met7020049

Chicago/Turabian Style

Qiu, Feng, Xiang Gao, Jian Tang, Yu-Yang Gao, Shi-Li Shu, Xue Han, Qiang Li, and Qi-Chuan Jiang. 2017. "Microstructures and Tensile Properties of Al–Cu Matrix Composites Reinforced with Nano-Sized SiCp Fabricated by Semisolid Stirring Process" Metals 7, no. 2: 49. https://doi.org/10.3390/met7020049

APA Style

Qiu, F., Gao, X., Tang, J., Gao, Y. -Y., Shu, S. -L., Han, X., Li, Q., & Jiang, Q. -C. (2017). Microstructures and Tensile Properties of Al–Cu Matrix Composites Reinforced with Nano-Sized SiCp Fabricated by Semisolid Stirring Process. Metals, 7(2), 49. https://doi.org/10.3390/met7020049

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop