Next Article in Journal
Ultrasonic Peening Treatment Used to Improve Stress Corrosion Resistance of AlSi10Mg Components Fabricated Using Selective Laser Melting
Next Article in Special Issue
Development of Low Silver AgCuZnSn Filler Metal for Cu/Steel Dissimilar Metal Joining
Previous Article in Journal
Experimental Determinations of Mixing Times in the IronArc Pilot Plant Process
Previous Article in Special Issue
Interfacial Characteristics of Dissimilar Ti6Al4V/AA6060 Lap Joint by Pulsed Nd:YAG Laser Welding
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Dissimilar Metals Laser Welding between DP1000 Steel and Aluminum Alloy 1050

by
António B. Pereira
1,*,
Ana Cabrinha
1,
Fábio Rocha
1,
Pedro Marques
1,2,
Fábio A. O. Fernandes
1 and
Ricardo J. Alves de Sousa
1
1
TEMA–Centre for Mechanical Technology and Automation, Department of Mechanical Engineering, University of Aveiro, Campus de Santiago, 3810-193 Aveiro, Portugal
2
Industrial Engineering and Management, Universidade Lusófona, Campo Grande 376, 1749 Lisbon, Portugal
*
Author to whom correspondence should be addressed.
Metals 2019, 9(1), 102; https://doi.org/10.3390/met9010102
Submission received: 16 December 2018 / Revised: 11 January 2019 / Accepted: 14 January 2019 / Published: 18 January 2019
(This article belongs to the Special Issue Dissimilar Metal Welding)

Abstract

:
The welding of dissimilar metals was carried out using a pulsed Nd: YAG laser to join DP1000 steel and an aluminum alloy 1050 H111. Two sheets of each metal, with 30 × 14 × 1 mm3, were lap welded, since butt welding proved to be nearly impossible due to the huge thermal conductivity differences and melting temperature differences of these materials. The aim of this research was to find the optimal laser welding parameters based on the mechanical and microstructure investigations. Thus, the welded samples were then subjected to tensile testing to evaluate the quality of the joining operation. The best set of welding parameters was replicated, and the welding joint obtained using these proper parameters was carefully analyzed using optical and scanning electron microscopes. Despite the predicted difficulties of welding two distinct metals, good quality welded joints were achieved. Additionally, some samples performed satisfactorily well in the mechanical tests, reaching tensile strengths close to the original 1050 aluminum alloy.

Graphical Abstract

1. Introduction

Currently, there is a growing interest across various industries to join different metals or alloys [1,2]. This interest is justified by the flexibility that such options would provide in terms of mechanical project and design, for instance, by utilizing high-quality alloys for critical structural points and low-quality ones for less significant areas. Additionally, considering for instance the automotive industry, this solution makes it possible to manufacture lighter components [3,4,5,6]. This would also significantly reduce fuel consumption, thereby reducing CO2 emissions, which is of the utmost importance in complying with environmental demands and policies, and also to improve manufacturers/brands in their green marketing campaigns.
Steel and aluminum are two materials that are extremely difficult to join by welding. They have different chemical compositions, as well as physical and mechanical properties, which translates into a homogeneity problem. These materials have completely different melting points. Aluminum can melt during the welding process, whereas steel can remain solid [2]. In other words, the laser power necessary to melt steel is excessive for aluminum. On the other hand, aluminum’s reflexivity and the high melting temperature of its surface oxides make its melting process quite difficult. Thus, specific welding strategies must be adopted in order to properly weld these materials.
Moreover, the thermal conductivities and thermal expansion coefficients of steel and aluminum alloys are also completely different, which makes welding of these materials a true challenge [4,5,6]. Therefore, during the welding process, thermal stresses and residual stresses develop on the welding joint [2]. Additionally, the occurrence of intermetallic compounds (IMCs) of Fe–Al on the welding joint during solidification is possible [7]. IMCs are very hard and fragile, decreasing the joint tenacity and plasticity of the joint, i.e., basically turning it brittle [2]. The IMC layers formation is highly dependent on the temperature and time [8], which must be controlled to successfully join steel and aluminum [9]. Consequently, there is a series of problems in joining these two materials, and some solutions have been proposed. Torkamany et al. [10] reported a successful welding of low-carbon steel ST14 (0.8 mm thick) and 5754 aluminum alloy (2.0 mm thick), using a pulsed Nd:YAG laser. It was found that parameters such as power and pulse duration had a significant influence on the overall welding process. Torkamany et al. [10] reported the expected formation of IMCs. An increase in both parameters meant an equal increase in the terms of the IMCs formation. Moreover, with the increase in laser power, the extent of spatter, cracks, and pores also increased. On the other hand, for low laser power values, penetration was insufficient. Sun et al. [11] studied weld butt joints between Q235 low-carbon steel and an AA6013 aluminum alloy, also using an Nd:YAG laser and adding the aluminum alloy 4043 as filler material. As in Reference [10], the formation of the IMCs: Fe2Al5 and FeAl3 occured. Failure analysis of the joints showed a typical cleavage-type fracture with crack initiation starting within the FeAl3 phase. The maximum registered tensile strength of the joint was 120 MPa.
These were the most recent and relevant studies found in the literature. Other authors have used fusion-brazing welding [12] or dual laser beam fusion welding [9] or even explosion welding [13,14,15], which are relatively if not widely different from the investigation at hand, especially the latter. Nevertheless, despite considering these techniques, we did not find any study relating to DP1000 steel and aluminum alloy 1050 welding. In fact, even in well performed literature reviews by Sun and Ion [1], Wang et al. [2], Shah and Ishak [4], and Katayama [3], no study was found regarding the laser welding of these metals. In this work, the authors aimed to determine the optimal set of laser welding parameters, based on mechanical testing and microstructure investigations.
Nowadays, laser technology is used in many applications. Concerning mechanical technology, this can be used to perform precise welding or even precise cutting of high strength steels [16,17]. Laser welding is a joining method that is still relatively recent and makes it possible to obtain better results compared to other welding technologies. This is the main reason behind the replacement of resistance spot welding in several industries. For instance, considering the automotive industry, laser welding has been extensively used, since it makes it possible to perform smaller welding joints (small heat-affected zone) with higher precisions, penetrations, and flexibility. Additionally, it only requires one side of the base metal to accomplish the joining process and it is a technique characterized by high welding speeds, making it an excellent alternative to the conventional welding processes [2,18]. Currently, laser welding is widely used in metals such as titanium alloys [19,20] and dual-phase steels [21].

2. Materials and Methods

2.1. Laser Welding Machine

The machine used was a SWA300 (SISMA, Vicenza, Italy), Figure 1a. The Nd:YAG laser uses, as an active medium, a crystalline solid made of Nd:YAG (neodymium-doped yttrium aluminum Garnet - Y3Al5O12). A parametric study was performed to find a set of welding parameters that made it possible to obtain quality welding joints between DP1000 steel and 1050 aluminum alloy. To evaluate the welded samples, the same methodology adopted in a previous study was also adopted [21], as well as performing tensile and microhardness tests.
The SISMA SWA300 was primarily designed to perform mold reparation and maintenance, with or without the use of a filler material. Since this machine was designed for mold reparation, it does not have an original fixation system. Thus, a simple and effective solution was designed as depicted in Figure 1b.
The support system has a hole for inserting the protection gas tube. From left to right, Figure 2 illustrates the procedure necessary to properly fix the samples. The first step was to insert the protection gas tube, ensuring that the protective gas was properly covering the samples. The second step consisted of putting the samples in their positions. In order to perform lap welds, a third metal sheet with the same thickness was placed under the top one, which meant it was under the steel sample. The third step was to ensure that both parts were properly placed, using screws at the sides. The last step was to guarantee the complete fixation by using the upper screws, thereby closing the gap between the metal sheets as much as possible.
In order to prevent oxidation, an isolating box was designed and placed on this device. This box was made of glass, due to its transparency and its better thermal resistance (compared to acrylic). Figure 3 shows the glass parts that were glued to create the referred to protective box, for use during the joining process. The protection gas used was Argon ARCAL TIG MIG, supplied by Air Liquide (Paris, France).

2.2. Materials and Samples

As described, the dissimilar metals chosen were the DP1000 steel and the AA1050 aluminum alloy H111. Both samples had a thickness of 1mm and dimensions of 30mm × 14 mm. The 1mm thick samples were cut using a guillotine (GUIFIL, Portugal).
These materials had completely different melting points. Table 1 presents a simple comparison between iron and aluminum. Aluminum can melt during the welding process, whereas steel can remain solid [2]. In other words, the laser power necessary to melt steel was overly excessive compared to the aluminum. Therefore, the welding was performed only on the steel part, whilst slightly penetrating the aluminum one, without destabilizing it. Table 2 and Table 3 present the chemical compositions of both materials.
The samples were lap welded with the steel on top (Figure 4). It was verified that as the welding progressed, naturally the samples would heat, and the penetration would increase longitudinally. Thus, for the second welding joint, the sample was rotated 180° and the welding process proceeded in the same direction. This way, less penetration achieved on the initial regions of the first welding joint would be compensated by the second, which would accomplish just that.

2.3. Laser Welding Parameters

Regarding the laser parameters that could be analyzed using the SISMA SWA300, the following parameters were considered: laser power (percentage of peak pulse); pulse duration; frequency/superposition; and laser beam diameter. Since there was no data in the literature regarding DP1000–AA1050 aluminum welding, the ideal welding parameters were found by trial and error, as well as taking into consideration the conclusions of other studies previously carried out using the same machine. From these conclusions, the following were considered:
  • Laser beam power: the penetration was proportional to the laser beam power. The ideal values were situated between 6 kW and 7.20 kW of the maximum peak power of 12 kW.
  • Pulse duration: the penetration was also proportional to higher pulse durations. Previous values were between 12–16 ms.
  • Superposition: It did not influence penetration until values around 80%.
  • Laser beam diameter: the penetration seemed to be inversely proportional to the welding spots diameter. A constant value of 1 mm was used.
  • Welding speed: a high welding speed meant high penetration. The speed was then limited by the amount of power/energy and pulse duration used. For higher values of pulse duration and/or power (and thus energy), smaller values of speed were allowed for a proper welding process.
Similar to Torkamany et al. [10], which evaluated the influence of power and pulse duration on the welding process, in the first stage, only power was varied to find its ideal value. Then, other parameters were changed based on visual analysis and tensile testing. This evolution regarding the welding parameter values is described thoroughly in the results section.
Table 4 shows the parameter values used for each welded sample. A square wave was defined as the pulse type for all the samples. The welding speed was the lowest possible concerning machine restrictions, because for higher values, the penetration on the aluminum sample would be excessively high, destroying any chance of a properly welded joint. Additionally, a constant laser beam diameter and superposition of 1 mm and 60% were used, respectively.

2.4. Tensile Testing

To determine the mechanical properties of the welded samples, mainly the tensile strength and respective deformation of each set of parameters, tensile testing was performed using an universal testing, 10 kN machine (Shimadzu, Kyoto, Japan), Figure 5.
Considering lap welding, deflection phenomena are expected to occur during tensile testing. We then used the following equation to compute stress:
S = F A 0 + M x   ×   y I x ,
where F is the magnitude of the forces applied, A0 is the initial cross section area of the joint, Mx and Ix are the torque and moment of inertia about the X-axis, respectively, and y is the maximum distance about the Y-axis considering a xOy plane as Figure 6:
Since the superposition of the welding spots had a value of 60%, the area of the joint was approximated to one of a 14 × 1 mm2 rectangle. However, the deflection stresses were negligible (<1.5 MPa on every test) due to the small dimensions of the samples. Thus, in order to determine the nominal stress, we used the following approximation:
S F A 0 ,
where S is the nominal stress, F is the magnitude of the applied force, and A0 is the cross-sectional area of the sample (since fracture should occur on the aluminum part). The normal strain was determined through:
e = Δ L L 0 ,
where e is the nominal deformation, ΔL is the change in length, and L0 is the original length considered for the sample at hand, in this case it was 30 mm for each test. The true stress was calculated by:
σ = S ( 1 + e ) ,
where σ is the true stress, whilst the true strain ε was determined as:
ε = l n ( 1 + e ) ,

2.5. Microstructure

For a deeper analysis of the welding, a new sample based on the optimum welding parameters found in the tensile testing was re-created to analyze its microstructure. Firstly, the sample was transversely cut for the observation of a substantial part of its welding joint, as well as longitudinally, to have a 25 mm length to fit the mold (Figure 7). Cutting was precisely performed using a Struers cutting machine.
After this, the sample was inserted on a cylindrical mold of 25 mm diameter and then epoxy resin was injected into it, as well as a hardener. Once solidified (Figure 8), the injected sample was removed from the mold and then polished for observation. Polishing diamond papers (3 μm) of 180, 320, 800, 1200, 2500, and 4000 grit were used. The machine used was a rotary polishing machine, the RotoPol-21 (Struers, Cleveland, OH, USA).
Then, the injected sample was subjected to chemical etching using nital (4%) (Ethanol + Nitric Acid), to help the microstructure observation. The nital etching was executed, lasting 20 seconds. At first, it was also subjected to a Keller’s reagent (HNO3 2.5 mL; HCl 1.5 mL; H2F2 1 mL, H2O 95 mL). However, it would cause oxidation due to the iron (Fe) present in the sample, complicating the observation. Thus, at the end, only the nital etching was considered. The microstructural observations were performed using an optical microscope and a scanning electron microscope TM4000Plus (SEM, Hitachi, Japan) with an integrated back-scattered electron detector (BSE). Elemental composition mapping was performed using an energy-dispersive X-ray spectroscopy (EDS, Hitachi, Japan).

3. Results

3.1. Laser Welding

Considering the values presented in Table 4 for each welded sample, after tensile testing, it was verified that considering the speed used, the ideal interval was from 6 kW to 7.20 kW. More specifically, the best performance on tensile testing was achieved at a laser power of 6.48 kW (sample eight from 12 samples, Table 4). It became clear that for welding powers higher than 7.20 kW, the laser would fully penetrate the aluminum part, resulting in brittle joints, which were easily breakable by hand. Then, the duration of the pulse was altered, and the laser power fixed (samples 13 to 16). On the final samples (17 to 20), these two parameters were slightly changed from the ideal values. Figure 9 presents the 20 welded samples.

3.2. Tensile Testing

Figure 10 presents the samples after tensile testing, as well as a reference sample made of aluminum (60 × 14 mm), since ideally, the fracture occurs on the aluminum part, due to its lower tensile strength. We considered the normalization of this reference sample. Nevertheless, it was not done for a better similarity with the welded samples. Additionally, it is worth mentioning that sample 20 was not subjected to tensile testing, since we noticed that the laser significantly penetrated the aluminum, with some wide penetrations in some regions. Therefore, the sample would fracture easily while testing, producing negligible data. Thus, this specific sample was removed from the experiment.
Figure 11a shows the stress–strain curve for the samples where fracture occurred partially or completely through the aluminum part (true stress/strain values). On the other hand, Figure 11b shows the samples where fracture occurred through the welding joint. In both, the reference sample stress–strain curve was included for comparison. Since Figure 11 plots the true stress vs. true strain, the curves were only presented up to maximum stress value.
An ideal welded sample would perform similarly to the original (weakest) material in terms of tensile strength and maximum elongation. Regarding tensile strength, the samples that performed better were samples 8 and 18 (Figure 11 and Figure 12). The latter had a slightly lower value but a higher strain value, thus being considered the best of this whole batch, reaching a 20 MPa lower tensile strength and a 1% strain difference compared the reference sample. It is also worth mentioning that for sample 19, although its maximum stress was significantly lower than samples 8 and 18, its maximum strain was closest to the reference sample. In this group, the worst sample was clearly sample 15 which had the lowest tensile strength. It could probably be justified by the excessive laser penetration on the aluminum part, causing its fragilization. Thus, an ideal laser power between 54 and 55, with a pulse duration between 13 and 15 ms can be herein stated.
For the samples where the welding joint did not remain intact after tensile testing, the maximum stress recorded was much lower than the one in the reference sample (at best, 80 MPa lower). However, it is important to highlight the sample 14 strain value, which came close to the value of the reference sample. It is worth mentioning that the curves of samples 3 and 16 are not plotted in Figure 11, since the results were irrelevant. For an exact reading of the tensile strength values, as well as their respective strain values, the following bar graphs are seen in Figure 12.
In terms of laser power (samples 2 to 12), the best results were obtained as this value decreased. Considering the pulse duration (samples 13 to 17), the contrary could be seen for the same value of the laser power. However, in terms of strain, the results were inconclusive without a linear behavior of any sort of pattern. Sample 18 could be considered the ideal sample, with a tensile strength and strain of only 20 MPa and 1.4%, respectively, which were lower than the reference sample. This ideal sample was repeated to evaluate its microstructure.

3.3. Microstructure

Figure 13 and Figure 14 show the observations using the optical microscope and SEM, respectively. In Figure 13, the welded joint is easily spotted, being observed in the way in which both metals melted and mixed in a successful way. This was also confirmed through the SEM observations in Figure 14, where it shows the interface between the two metals. In Figure 14b, it was possible to spot the Fe particles in the aluminum.
Figure 15 shows the BSE images collected, as well as the microstructural and compositional analysis of the welded zone. Compositions are detailed in Table 5 for a total of eight different points, six of them in the welded zone and the other two in the base materials used as the reference.

4. Conclusions

In this work, the welding of dissimilar metals was performed with success. A pulsed Nd: YAG laser welding machine, the SISMA SWA300, was used to join the DP1000 steel and the AA1050. The adopted strategy was based on the lap welding of two sheet samples of each metal, since butt welding was nearly impossible due to the great disparity in terms of the thermal properties of both materials.
Even if some predicted difficulties in welding these dissimilar metals were found, a good choice of welding parameters was studied resulting in good-quality welded joints. The quality was confirmed by the results obtained in the tensile tests and in the observations performed using the optical microscope and the SEM. It is worth highlighting the sample performance, which reached tensile strengths and maximum elongations close to the weakest base metal, the AA1050.
In conclusion, it was shown that even for highly dissimilar materials, with very distinct material properties (thermal and mechanical), one can declare the success of this work. The possibility to effectively join high strength dual-phase steels with a soft, ductile 1XXX aluminum alloy opens a new range of design possibilities and attests the versatility of laser-type welding operations. The authors hope that this study can serve as a sounding base for any other future work in this area.

Author Contributions

Conceptualization, A.C. and F.R.; Methodology, A.B.P.; Software and Validation, P.M.; Formal Analysis, P.M.; Investigation, A.C. and F.R.; Resources, A.B.P.; Data Curation, F.A.O.F.; Writing-Original Draft Preparation, F.A.O.F.; Writing-Review & Editing, R.J.A.d.S.; Supervision, P.M.; Project Administration, A.B.P.; Funding Acquisition, A.B.P. and R.J.A.d.S.

Funding

Programa Operacional Temático Factores de Competitividade: CENTRO-01-0145-FEDER-022083, Fundação para a Ciência e a Tecnologia, grant UID/EMS/00481/2013-FCT.

Acknowledgments

Center of Mechanical Technology and Automation, Fundação para a Ciência e a Tecnologia, grant CEECIND/01192/2017.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Sun, Z.; Ion, J.C. Laser welding of dissimilar metal combinations. J. Mater. Sci. 1995, 30, 4205–4214. [Google Scholar] [CrossRef]
  2. Wang, P.; Chen, X.; Pan, Q.; Madigan, B.; Long, J. Laser welding dissimilar materials of aluminum to steel: An overview. Int. J. Adv. Manuf. Technol. 2016, 87, 3081–3090. [Google Scholar] [CrossRef]
  3. Katayama, S. Laser welding of aluminium alloys and dissimilar metals. Weld. Int. 2004, 18, 618–625. [Google Scholar] [CrossRef]
  4. Shah, L.H.; Ishak, M. Review of research progress on aluminum-steel dissimilar welding. Mater. Manuf. Process. 2014, 29, 928–933. [Google Scholar] [CrossRef]
  5. Shao, L.; Shi, Y.; Huang, J.K.; Wu, S.J. Effect of joining parameters on microstructure of dissimilar metal joints between aluminum and galvanized steel. Mater. Des. 2015, 66, 453–458. [Google Scholar] [CrossRef]
  6. Song, J.L.; Lin, S.B.; Yang, C.L.; Ma, G.C.; Liu, H. Spreading behavior and microstructure characteristics of dissimilar metals TIG welding–brazing of aluminum alloy to stainless steel. Mater. Sci. Eng. A 2009, 509, 31–40. [Google Scholar] [CrossRef]
  7. Borrisutthekul, R.; Yachi, T.; Miyashita, Y.; Mutoh, Y. Suppression of intermetallic reaction layer formation by controlling heat flow in dissimilar joining of steel and aluminum alloy. Mater. Sci. Eng. A 2007, 467, 108–113. [Google Scholar] [CrossRef]
  8. Bouché, K.; Barbier, F.; Coulet, A. Intermetallic compound layer growth between solid iron and molten aluminium. Mater. Sci. Eng. A 1998, 249, 167–175. [Google Scholar] [CrossRef]
  9. Cui, L.; Chen, H.; Chen, B.; He, D. Welding of Dissimilar Steel/Al Joints Using Dual-Beam Lasers with Side-by-Side Configuration. Metals 2018, 8, 1017. [Google Scholar] [CrossRef]
  10. Torkamany, M.J.; Tahamtan, S.; Sabbaghzadeh, J. Dissimilar welding of carbon steel to 5754 aluminum alloy by Nd:YAG pulsed laser. Mater. Des. 2010, 31, 458–465. [Google Scholar] [CrossRef]
  11. Sun, J.; Yan, Q.; Gao, W.; Huang, J. Investigation of laser welding on butt joints of Al/steel dissimilar materials. Mater. Des. 2015, 83, 120–128. [Google Scholar] [CrossRef]
  12. Meco, S.; Pardal, G.; Ganguly, S.; Williams, S.; McPherson, N. Application of laser in seam welding of dissimilar steel to aluminium joints for thick structural components. Opt. Lasers Eng. 2015, 67, 22–30. [Google Scholar] [CrossRef] [Green Version]
  13. Corigliano, P.; Crupi, V.; Guglielmino, E. Non linear finite element simulation of explosive welded joints of dissimilar metals for shipbuilding applications. Ocean Eng. 2018, 160, 346–353. [Google Scholar] [CrossRef]
  14. Corigliano, P.; Crupi, V.; Guglielmino, E.; Mariano Sili, A. Full-field analysis of AL/FE explosive welded joints for shipbuilding applications. Mar. Struct. 2018, 57, 207–218. [Google Scholar] [CrossRef]
  15. Kaya, Y. Microstructural, Mechanical and Corrosion Investigations of Ship Steel-Aluminum Bimetal Composites Produced by Explosive Welding. Metals 2018, 8, 544. [Google Scholar] [CrossRef]
  16. Rana, R.S.; Chouksey, R.; Dhakad, K.; Paliwal, D. Optimization of process parameter of Laser beam machining of high strength steels: A review. Mater. Today Proc. 2018, 5, 19191–19199. [Google Scholar] [CrossRef]
  17. Patidar, D.; Rana, R.S. The effect of CO2 laser cutting parameter on Mechanical & Microstructural characteristics of high strength steel—A review. Mater. Today Proc. 2018, 5, 17753–17762. [Google Scholar] [CrossRef]
  18. Chen, S.; Huang, J.; Ma, K.; Zhao, X.; Vivek, A. Microstructures and Mechanical Properties of Laser Penetration Welding Joint With/Without Ni-Foil in an Overlap Steel-on-Aluminum Configuration. Metall. Mater. Trans. A 2014, 45, 3064–3073. [Google Scholar] [CrossRef]
  19. Zhan, Y.; Zhang, E.; Ge, Y.; Liu, C. Residual stress in laser welding of TC4 titanium alloy based on ultrasonic laser technology. Appl. Sci. 2018, 8, 1997. [Google Scholar] [CrossRef]
  20. Li, R.; Zhang, F.; Sun, T.; Liu, B.; Chen, S.; Tian, Y. Investigation of strengthening mechanism of commercially pure titanium joints fabricated by autogenously laser beam welding and laser-MIG hybrid welding processes. Int. J. Adv. Manuf. Technol. 2018. [Google Scholar] [CrossRef]
  21. Fernandes, F.A.O.; Oliveira, D.F.; Pereira, A.B. Optimal parameters for laser welding of advanced high-strength steels used in the automotive industry. Procedia Manuf. 2017, 13, 219–226. [Google Scholar] [CrossRef]
  22. Gale, W.F.; Totemeier, T.C. (Eds.) Smithells Metals Reference Book, 8th ed.; Elsevier Butterworth-Heinemann: Oxford, UK, 2004. [Google Scholar]
  23. Esmaeili, A.; Givi, M.K.B.; Rajani, H.R.Z. A metallurgical and mechanical study on dissimilar Friction Stir welding of aluminum 1050 to brass (CuZn30). Mater. Sci. Eng. A 2011, 528, 7093–7102. [Google Scholar] [CrossRef]
  24. Wang, J.; Yang, L.; Sun, M.; Liu, T.; Li, H. Effect of energy input on the microstructure and properties of butt joints in DP1000 steel laser welding. Mater. Des. 2016, 90, 642–649. [Google Scholar] [CrossRef]
Figure 1. (a) SISMA SWA300 Nd:YAG laser welding machine; (b) Fixation/support system.
Figure 1. (a) SISMA SWA300 Nd:YAG laser welding machine; (b) Fixation/support system.
Metals 09 00102 g001
Figure 2. Illustration of the support/fixation system operation.
Figure 2. Illustration of the support/fixation system operation.
Metals 09 00102 g002
Figure 3. Isolating glass box.
Figure 3. Isolating glass box.
Metals 09 00102 g003
Figure 4. Schematic of the welding performed on the samples.
Figure 4. Schematic of the welding performed on the samples.
Metals 09 00102 g004
Figure 5. Shimadzu 10 kN tensile testing machine.
Figure 5. Shimadzu 10 kN tensile testing machine.
Metals 09 00102 g005
Figure 6. Position of the Cartesian coordinate system plane on the sample.
Figure 6. Position of the Cartesian coordinate system plane on the sample.
Metals 09 00102 g006
Figure 7. Illustration of the sample for microstructural observation.
Figure 7. Illustration of the sample for microstructural observation.
Metals 09 00102 g007
Figure 8. Solidified sample after injection of epoxy resin + hardener.
Figure 8. Solidified sample after injection of epoxy resin + hardener.
Metals 09 00102 g008
Figure 9. Steel-aluminum welded samples.
Figure 9. Steel-aluminum welded samples.
Metals 09 00102 g009aMetals 09 00102 g009b
Figure 10. Samples after tensile testing.
Figure 10. Samples after tensile testing.
Metals 09 00102 g010aMetals 09 00102 g010b
Figure 11. True stress–strain curves for the samples where fracture occurred through: (a) the aluminum part; (b) the welding joint.
Figure 11. True stress–strain curves for the samples where fracture occurred through: (a) the aluminum part; (b) the welding joint.
Metals 09 00102 g011
Figure 12. Results from the tensile tests: (a) Ultimate tensile strength (samples 1 to 9); (b) Strain associated with the ultimate tensile strength (samples 1 to 9); (c) Ultimate tensile strength (samples 10 to 19); (d) Strain associated with the ultimate tensile strength (samples 10 to 19). (Note: RS means “reference sample” whereas S1 from S19 are the samples from 1 to 19).
Figure 12. Results from the tensile tests: (a) Ultimate tensile strength (samples 1 to 9); (b) Strain associated with the ultimate tensile strength (samples 1 to 9); (c) Ultimate tensile strength (samples 10 to 19); (d) Strain associated with the ultimate tensile strength (samples 10 to 19). (Note: RS means “reference sample” whereas S1 from S19 are the samples from 1 to 19).
Metals 09 00102 g012
Figure 13. Optical microscope observations of the welded zone.
Figure 13. Optical microscope observations of the welded zone.
Metals 09 00102 g013
Figure 14. Scanning electron microscope (SEM) observations: (a) Steel; (b) Aluminum; (c) Steel–aluminum joint interfaces.
Figure 14. Scanning electron microscope (SEM) observations: (a) Steel; (b) Aluminum; (c) Steel–aluminum joint interfaces.
Metals 09 00102 g014
Figure 15. Back-scattered electron detector (BSE) images with elemental composition mapping using Energy-dispersive X-ray spectroscopy (EDS).
Figure 15. Back-scattered electron detector (BSE) images with elemental composition mapping using Energy-dispersive X-ray spectroscopy (EDS).
Metals 09 00102 g015
Table 1. Properties of the Fe and Al at room temperature [22].
Table 1. Properties of the Fe and Al at room temperature [22].
MetalMelting Temperature [K]Density [kg·m−3]Thermal Conductivity [W·m−1·K−1]Specific Heat Capacity [J·kg−1·K−1]Thermal Expansion Coefficient [K−1]
Fe180978707845612.1 × 106
Al933270023891723.5 × 106
Table 2. Chemical composition of the AA1050 aluminum alloy [wt.%] [23].
Table 2. Chemical composition of the AA1050 aluminum alloy [wt.%] [23].
TiZnMnFeSiMgCu
0.050.070.050.40.250.050.05
Table 3. Chemical composition of DP1000 steel [wt.%] [24].
Table 3. Chemical composition of DP1000 steel [wt.%] [24].
CSiMnCuAlCrNiNbV
0.1410.491.470.020.0410.030.040.0160.01
Table 4. Parametric study for steel–aluminum welding.
Table 4. Parametric study for steel–aluminum welding.
SamplePower [kW]Pulse Duration [ms]
18.4014
27.2014
37.0814
46.9614
56.8414
66.7214
76.6014
86.4814
96.3614
106.2414
116.1214
126.0014
136.4816
146.4815
156.4813
166.4812
176.4811
186.6013
196.6015
206.6016
Table 5. Elemental composition mapping (normalized mass concentration [%]).
Table 5. Elemental composition mapping (normalized mass concentration [%]).
SpectrumCOAlSiFe
18.252.1012.17-77.48
28.302.8219.130.5969.15
313.0010.8762.779.373.99
48.182.374.73-84.72
59.393.3346.69-40.59
610.113.2223.85-62.82
77.832.119.53-80.53
87.702.138.86-81.31
Mean9.103.6223.474.9862.58
Sigma1.772.9720.666.2127.63
SigmaMean0.631.057.312.209.77

Share and Cite

MDPI and ACS Style

Pereira, A.B.; Cabrinha, A.; Rocha, F.; Marques, P.; Fernandes, F.A.O.; Alves de Sousa, R.J. Dissimilar Metals Laser Welding between DP1000 Steel and Aluminum Alloy 1050. Metals 2019, 9, 102. https://doi.org/10.3390/met9010102

AMA Style

Pereira AB, Cabrinha A, Rocha F, Marques P, Fernandes FAO, Alves de Sousa RJ. Dissimilar Metals Laser Welding between DP1000 Steel and Aluminum Alloy 1050. Metals. 2019; 9(1):102. https://doi.org/10.3390/met9010102

Chicago/Turabian Style

Pereira, António B., Ana Cabrinha, Fábio Rocha, Pedro Marques, Fábio A. O. Fernandes, and Ricardo J. Alves de Sousa. 2019. "Dissimilar Metals Laser Welding between DP1000 Steel and Aluminum Alloy 1050" Metals 9, no. 1: 102. https://doi.org/10.3390/met9010102

APA Style

Pereira, A. B., Cabrinha, A., Rocha, F., Marques, P., Fernandes, F. A. O., & Alves de Sousa, R. J. (2019). Dissimilar Metals Laser Welding between DP1000 Steel and Aluminum Alloy 1050. Metals, 9(1), 102. https://doi.org/10.3390/met9010102

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop