Next Article in Journal
Effect of Welding Heat Input on Simulated HAZ Areas in S960QL High Strength Steel
Next Article in Special Issue
Production and Properties of Light Metal Matrix Nanocomposites
Previous Article in Journal
Effects of Temperature on Wear Properties and Mechanisms of HVOF Sprayed CoCrAlYTa-10%Al2O3 Coatings and H13 Steel
Previous Article in Special Issue
Quasi-Static and Plate Impact Loading of Cast Magnesium Alloy ML5 Reinforced with Aluminum Nitride Nanoparticles
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Fe3O4 Nanoparticle-Reinforced Magnesium Nanocomposites Processed via Disintegrated Melt Deposition and Turning-Induced Deformation Techniques

Department of Mechanical Engineering, National University of Singapore, Singapore 117 575, Singapore
*
Author to whom correspondence should be addressed.
Metals 2019, 9(11), 1225; https://doi.org/10.3390/met9111225
Submission received: 23 October 2019 / Revised: 12 November 2019 / Accepted: 12 November 2019 / Published: 16 November 2019
(This article belongs to the Special Issue Production and Properties of Light Metal Matrix Nanocomposites)

Abstract

:
Magnesium nanocomposites, with nano-scale ceramic reinforcements, have attracted a great deal of attention for several engineering and biomedical applications in the recent past. In this work, superparamagnetic iron oxide nanoparticles, Fe3O4, with their unique magnetic properties and the ability of being bio-compatible and non-toxic, are reinforced to magnesium to form Mg/(1, 2, and 3 wt %) Fe3O4 nanocomposites. These nanocomposites were fabricated using the conventional disintegrated melt deposition (DMD) technique followed by extrusion. Further, the materials were also processed using the novel turning-induced-deformation technique where the chips from turning process are collected, cold compacted, and hot extruded. The materials processed via the two techniques were compared in terms of microstructure and properties. Overall, the Mg/Fe3O4 nanocomposites, processed via both routes, exhibited a superior property profile. Further, the turning-induced deformation method showed promising results in terms of improved properties of the nanocomposites and serves as a great route for the recycling of metallic materials.

1. Introduction

An upsurge in the processing and fabrication of lightweight magnesium (Mg) and the associated alloys/nanocomposites, typically for weight-sensitive applications such as in the aerospace industry, has been observed in the recent past [1,2,3]. A number of components in the aircraft interiors, such as passenger seats, overhead compartments, folding tables and food trolleys, and transmission casings, have the potential to use magnesium [4]. Mg nanocomposites with nanometric length scale reinforcements such as ceramic, metallic, and other carbon-based reinforcements, i.e., CNTs (carbon nanotubes) have shown promising results in improving the mechanical, physical, and ignition properties of magnesium [2,5,6]. These nanoparticles were found to have properties that alleviate certain inherent weaknesses of Mg such as limited ductility, creep resistance, and strength but, more importantly, may also be used to incorporate new, desirable, and targeted properties. So far, several techniques have been reported for the synthesis of these nanocomposites. Some of them include (i) the disintegrated melt deposition (DMD) method whereby the melt is disintegrated and deposited onto a substrate using an inert shielding gas [2]; (ii) the ultrasound assisted casting technique, to break up particle clusters in the melt [7]; (iii) the in-situ synthesis technique utilizing the self-propagating high-temperature reactions based on the thermodynamic reactions between matrix and reinforcement [8,9]. Apart from the liquid state techniques, solid state processing techniques such as powder metallurgy followed by sintering [10] have also been popular in the production of these lightweight magnesium-based materials [11].
Conventional magnesium processing and machining, however, produces swarf/turnings, thus incurring wastage. While there have been studies on the recycling of such swarf, they were focused on re-melting for recovery of the magnesium which requires more energy than direct utilization [12]. Further studies on the recycling of magnesium turning/swarf commercially using industrial solutions are not readily available [13] while efforts on aluminum alloy machine swarf compaction methods were found, having been successfully hot-extruded into C-channels [14]. Thus, this provides a scope for a new magnesium recycling method that is more economical, via direct utilization of swarf. Such a method, named the turning-induced-deformation (TID) technique, has been recently introduced by some of the authors. This involves the consolidation of magnesium chips/turnings, followed by cold compaction and hot extrusion [15]. This technique produced extrudates with improved strength while directly utilizing machine swarf, resulting in better cost and energy efficiency owing to the fact that the chips are deformed during the turning process. The previous works dealt with the recycling of magnesium alloys. However, there has been no work on the recycling of the magnesium nanocomposites.
Hence, this work aimed to study the benefits of Fe3O4 nanoparticles, which have a unique combination of magnetic properties and the ability of being bio-compatible and non-toxic. Fe3O4 particles, being super paramagnetic in nature, have the ability to improve the electromagnetic interference (EMI) shielding effectiveness [16,17] of magnesium similar to that of iron particles, which were shown to be extremely promising [18]. These nanocomposites not only open up the possibility of applications in lightweight structural components with inherent shielding properties, but also applications in the biomedical field due to the bio-compatibility and non-toxic nature of the materials.
The focus of this work is two-fold: (i) to study and ascertain the effect of Fe3O4 nanoparticles on the overall properties of magnesium; (ii) to understand the properties of the magnesium nanocomposites processed using the TID technique in comparison to those processed using the conventional DMD-extrusion technique, so as to promote this technique to recycle the magnesium nanocomposites as well.

2. Materials and Methods

2.1. Materials and Processing

Magnesium turnings of 99.9% purity from Acros Organics (Morris Plains, NJ, USA) were used as the matrix material. Fe3O4 nanoparticles (15–30 nm) of 5.17 g/cm3 density were used in addition to the turnings to synthesize Mg/Fe3O4 nanocomposites for this study. The Mg/Fe3O4 (1%, 2%, and 3%) nanocomposites were casted using the DMD technique, followed by soaking for 1 h at 400 °C, and extrusion at 350 °C [19]. These materials were studied in this work to understand the effect of the presence of Fe3O4 nanocomposites. Further, in addition, these materials were also subjected to the turning-induced-deformation (TID) technique. In the TID technique, a conventional lathe is used to generate turnings from the cast ingots. A speed of 395 rpm, feed speed of 0.98 mm/s, and a depth of cut of 1 mm were used during the machining/turning of the ingots. The loose turnings (which are typically the industrial swarf) were collected and it was ensured that the turnings are free from contamination from foreign substances. Figure 1 below shows the cold compaction process of the turnings, from which the billets were extracted. The resulting billets were then homogenized at 400 °C for 1 h, followed by hot extrusion at 350 °C with an extrusion ratio of 20.25:1, resulting in rods of approximately 8 mm in diameter.
Table 1 below outlines the materials synthesized and the processing techniques and conditions used.

2.2. Physical Characterization

2.2.1. Density and Porosity

The theoretical density of the nanocomposites was calculated using the rule of mixtures. To calculate the experimental density, the gas displacement method was used to measure the density of the nanocomposite samples [20]. An AccuPyc II 1340 gas pycnometer (Norcross, GA, USA) was used to perform the measurements of the density of the nanocomposites from the two processing methods. The porosity of these samples was calculated using the assumption that the difference between the theoretical and experimental densities is due to the porosity in the materials. Average readings from 8 samples in each composition was considered as the final measurement.

2.2.2. Damping

Sample rods of ~7 mm diameter and ~55 mm length were subjected to impulse excitation by a resonance frequency damping analyzer (RFDA) acquired from IMCE, Genk, Belgium to obtain damping capacities and the elastic modulus of the nanocomposites. 10 measurements were taken for each composition to ensure consistency in the results.

2.3. Mechanical Characterization

Compression Testing

Samples of ~7 mm diameter, and a length/diameter ratio of ~1.5 were ground flat and subjected to a quasi-static compressive load in accordance with ASTM E9-09 using a MTS-810 servo-hydraulic testing system (Eden Prairie, MN, USA) with a crosshead speed of 0.07 mm/min and the samples were compressed until failure. Five samples were tested to ensure consistency in the readings obtained and the averages of the respective readings are presented in this work.

2.4. Thermogravimetric Analysis

Samples of approximately 2 mm x 2 mm x 1 mm were subjected to heating from 30 to 750 °C with a heating rate of 10 °C/min in purified air with a flow rate of 50 mL/min using a thermo gravimetric analyzer. The resultant temperature vs. time plots were then obtained for one sample from each composition and the point with a sharp increase in temperature is determined to be the ignition temperature of the nanocomposite [3,4,21].

2.5. Microstructure Characterization

2.5.1. Grain Size Analysis

Samples from each nanocomposite were ground flat and polished using alumina suspensions, starting from 5- to 0.05-micron size. The samples were etched using a solution of 20 mL acetic acid, 1 mL HNO3, 60 mL ethylene glycol, and 20 mL H2O and were viewed under a Leica DM2500 optical microscope (Leica Microsystems (SEA) Pte Ltd., Singapore, Singapore) to obtain images, following which the average grain sizes of each material were ascertained with the aid of MatLab software. The average grain size obtained was later used to understand the influence of grain size on the properties of the materials.

2.5.2. Microstructure

Samples from each nanocomposite were polished and etched for observation under a scanning electron microscope. A JEOL JSM-6010PLUS/LV scanning electron microscope (SEM) (Jeol USA Inc., Peabody, MA, USA) coupled with an energy dispersive spectroscope (EDS) was utilized to investigate the key features of the nanocomposite surfaces. In addition, a chip obtained from the machining process was also observed under the scanning electron microscope to observe the features on the chips. Fractured surfaces of the samples that failed in the compression testing were also examined using SEM.

2.6. Bio-Immersion Testing

Samples from each nanocomposite (height: 1 mm, diameter: 5 mm) and processing method were ground flat and subjected to a timed corrosion test by immersing them in HBSS (Hank’s balanced salt solution) at 37 °C in a temperature-controlled water bath. The samples were immersed for the durations of 1, 3, 6, 8, 15, 18, and 24 h (1 sample per duration). Once the durations elapsed, the samples were immersed in a solution consisting of 1.9 g of AgNO3 and 20 g of CrO3 in 100 mL of deionized water to remove the corrosion products formed on the surface, then rinsed, dried, and weighed to note down the mass loss from the corrosion-induced degradation.

3. Results

Properties of pure Mg processed using the DMD method (where included) were obtained from [21]. Pure Mg was used as a benchmark material for comparison with the Mg–Fe3O4 nanocomposites characterized in this study.

3.1. Microstructural Characterization

3.1.1. Grain Size Analysis

The grain characteristics of the nanocomposites processed via DMD and TID routes are given in Table 2. Figure 2 gives the representative micrographs of the samples. The Fe3O4 content addition lowers the mean grain diameter, i.e., the average grain size as compared to pure Mg regardless of the method of processing, highlighting the effect of reinforcement addition to magnesium matrix. For DMD materials, increasing Fe3O4 content generally results in smaller grains, and the least grain size was seen in Mg/2Fe3O4. Further addition of nanoparticles led to slight grain coarsening, as seen in the mean grain diameter values of Mg/3Fe3O4. For TID materials, the grain sizes are smaller than that of DMD materials, except for Mg/2Fe3O4. Thus, the TID method is favorable, resulting in materials with finer grain sizes.

3.1.2. General Microstructure

The morphology of a typical chip produced via turning is shown in Figure 3a. The chips/turnings have two distinct regions of plastic deformation, with high and low plastic deformation regions, as shown by the presence of shear bands and as given in one of our previous works [15]. Since this deformation is induced during the turning process, we call the process of obtaining these chips and compacting them the turning-induced-deformation process.
The general microstructure of the Mg/Fe3O4 nanocomposites processed by DMD and TID techniques is given in Figure 3b,c. Fe3O4 particles are seen to be well dispersed in the matrix and particularly seated at the grain boundaries throughout the samples. Agglomeration of Fe3O4 nanoparticles was found to be a natural tendency of such nanocomposites [22], and, as such, with an increase in the Fe3O4 content, the nanoparticles indeed further massed in agglomerates. However, in the TID nanocomposite, a finer dispersion of Fe3O4 nanoparticles was seen owing to the processing method which could have randomly scattered/broken the agglomeration of the nanoparticles during the turning process. The presence of the nanoparticles at the grain boundaries confirms the Zener pinning effects of the nanoparticles in the matrix during the dynamic recrystallization process (hot extrusion) [23,24]. This led to the reduction in the grain size due to the nanoparticles that assisted in pinning the grain boundaries, thereby increasing the grain boundary area, hindering grain growth and decreasing the grain size of the nanocomposites as compared to pure Mg. Coarsening of grain size with 3% Fe3O4 nanoparticles could be due to the agglomeration of the nanoparticles that reduced their pinning effects considerably.

3.2. Physical Properties

3.2.1. Density and Porosity

Table 3 gives the density and porosity results of the nanocomposites processed using both DMD and TID techniques. The addition of Fe3O4 results in the increase in density of nanocomposites due to the higher density of Fe3O4. Further, the porosity content also seemed to increase with increase in Fe3O4 content. Further, the TID samples showed marginally higher porosity levels. However, it is also observed that the experimental density of the nanocomposites remained largely the same relative to each other despite the higher theoretical density of those with higher Fe3O4 content, resulting in higher overall porosity levels as Fe3O4 content increases. The higher porosity of the TID nanocomposites is due to the presence of air gaps/voids during the compaction of turnings/chips to form a solid billet, inevitably resulting in voids and pores within the material. This is also observed in previous studies involving solid-state recycling of aluminum turnings [14], more so than the liquid phase processing, i.e., the DMD process.

3.2.2. Damping Capacity and Young’s Modulus

Table 4 and Figure 4 give the damping properties of the materials. The damping capacity and attenuation coefficient increase with the progressive increase in Fe3O4 content in the case of both the processing methods. The highest damping capacity is observed to be in Mg/3Fe3O4, which is the highest damping capacity for magnesium nanocomposites recorded thus far, to the authors’ best knowledge. The E-modulus is seen to decrease with increasing Fe3O4 content. Further, the time required to stop the vibration (Figure 4) also decreased with increasing Fe3O4, revealing the excellent improvement in the damping capacity of the materials with the addition of Fe3O4. It is to be highlighted that the TID processing of the materials showed a significant improvement in the damping capacities and no significant difference in the modulus values in comparison to the DMD samples. The highest recorded damping capacity is for the Mg/3Fe3O4 (TID) nanocomposite whose damping capacity was 33% higher than its DMD counterpart and 496% higher than pure Mg (DMD). This shows the TID technique as a viable route to process the materials, especially to achieve materials with excellent damping properties.
The increase in damping capacity for the TID samples were attributed to higher porosity levels (presence of air gaps in the materials) caused by compaction of turnings [25]. In addition, a prior study has shown that for processing methods resulting in high porosity, the damping capacity of the materials did indeed increase with porosity, as was done with spray-formed alloys [26] and porous magnesium [27]. The attenuation coefficient is a measure of the dampening of the curve with time, shown by the equation below ([28]):
A = Aoe−αt + C
where Ao and A are the initial and current amplitude, respectively; t is elapsed time after removal of external force; α is the apparent attenuation coefficient; and c is a fitting coefficient.
The attenuation coefficient is dependent on the resonant frequency and porosity of a material. The attenuation coefficient increased with Fe3O4 content, which implies that Fe3O4 nanoparticles can be used as dampening agents or reinforcements to magnesium and can find application in electronic, aerospace, and other engineering sectors [29].
Further, the elastic modulus of the nanocomposites, which is very critical for both engineering and biomedical applications, is seen to be marginally higher than that of Mg, i.e., ~46–49 GPa for all nanocomposites. Further, in engineering applications, stiffness is required at a minimum weight. With these materials exhibiting light weight and higher stiffness than Mg, they are well suited for engineering applications. Further, with densities and an elastic modulus fairly close to bone, the elastic mismatches between implants and bone can be eliminated with the use of these bio-compatible Mg nanocomposites [30].

3.3. Mechanical Properties (Compressive Properties)

Figure 5 show the results of the compressive tests. The addition of Fe3O4 increased the yield and ultimate strengths, and the highest was observed for the Mg/2Fe3O4 nanocomposite, processed using the DMD method. The stress–strain plots (Figure 5), however, showed that Fe3O4 presence lowers ductility and energy absorbed compared to pure Mg. Progressive addition of Fe3O4 increased strengths but at the cost of lowering maximum deformation and forces sustained. TID processing generally exhibited higher strengths over DMD counterparts, with the ultimate compressive strength not showing significant change. Overall, Figure 5 reveals that the TID method improved yield strengths in the nanocomposites. Further, the nanocomposites processed using the TID method were found to have increased ductility and fracture strain over DMD counterparts, indicating TID to be a favorable route for materials with superior strengths and ductility.
The significant change in properties corresponds to the microstructure, i.e., presence of grains and nanoparticles. As the grain sizes were still in the micron range, the Hall–Petch relationship stands true for these materials, whereby reduction in grain sizes results in improvement of mechanical strength without sacrificing ductility [31,32]. Effective grain hardening can be achieved by reducing grain size within the microstructure [33]. Smaller grains will have a larger chance of hindering the dislocations at the grain boundary due to the increase grain boundary area [34]. Further, the TID technique helped lower the grain size further, due to the prior induced deformation in the materials. Thus, the TID materials demonstrated improved strengths and ductilities due to the reduction in the grain size [35]. Previous studies on solid-state recycling of Al-based alloys showed resulting extrusions with high ductility [14], which aligns with the findings from this work where the materials with TID showed higher ductilities. The presence of nanoparticles also plays a significant role on the properties. With the increase in the content of nanoparticles, the strengths increased initially and dropped when the nanoparticles % was increased from 2% to 3%. This is due to the agglomeration of nanoparticles to form clusters of sub-micron to micron length scale which hampers the strength of the nanocomposite [7]. Thus, overall, the Mg/2Fe3O4 nanocomposite is seen to be the best in terms of the strength and ductility in both DMD and TID conditions.
Figure 6 shows the SEM images of all fracture surfaces showing the extent of plastic deformation undergone by the nanocomposites. All the nanocomposites are seen to undergo compressive failure by shear mode of deformation.

3.4. Ignition Properties

The results of ignition temperature measurement using thermogravimetric analysis is given in Table 5. The addition of Fe3O4 content increases the ignition temperature and the highest ignition temperature is recorded for the Mg/3Fe3O4 nanocomposite (DMD) with an ignition temperature of about 635.2 °C. There is no significant difference observed in the ignition temperatures recorded for the Mg/2Fe3O4 and Mg/3Fe3O4 processed via the DMD technique. A 2% addition of Fe3O4 can help in raising the ignition temperature by 45 °C. Although, the same trend of increase in ignition temperature with addition of Fe3O4 is observed in the materials processed by TID, the relative ignition temperatures values show a slight drop in ignition temperatures compared to their counterparts processed by DMD.
The nanocomposites used have already displayed a marked improvement in ignition temperature when compared to pure Mg which auto-ignites at 473 °C [36] and ignites in air under a constant heating rate of 590 °C. This is likely caused by the presence of the Fe3O4 nanoparticles which are thermally stable and provide insulating effects to the Mg matrix surfaces by hindering heat transfer at some points, much like other oxides such as Y2O3, as has been explored previously [37]. This results in elevating the ignition temperatures as Fe3O4 content increases. The TID nanocomposites were found to have relatively lower ignition temperatures due to the presence of higher porosity in the materials processed by the TID technique [15,38]. Better resistance to ignition is due to the formation of a relatively compact oxide layer (MgO) during oxidation that delays the further diffusion of oxygen towards Mg, prolonging the onset of ignition. With the presence of increasing porosity, the surface area exposed increases and the oxide layer is disrupted, thereby decreasing the ignition temperature. However, the TID method comes at the cost of lowering ignition temperature by only a marginal extent as compared to the DMD processing method.

3.5. Bio-Immersion Studies

The weight change in the nanocomposite samples due to immersion vs. the time of exposure of the samples (in hours) is depicted in Figure 7. The samples were immersed in HBSS solution which was maintained at normal body temperature of 37 °C. Mg/2Fe3O4 (DMD) displayed the least weight change and highest resistance to bio-corrosion among all the materials. TID processed materials show increasingly higher weight change due to immersion with higher Fe3O4 content. The significant weight loss in the materials subjected to immersion indicates that the materials exhibit lower corrosion resistance [39]. Due to the very high rate of weight change, TID materials failed to survive immersion tests past 8 h and completely dissolved in the solution.
The TID samples dissolved and disintegrated very quickly relative to DMD samples, despite the same composition due to presence of high porosity levels in the TID samples [40]. Materials with higher porosity corrode very rapidly, as a larger area of the material surface is exposed to the corrosive environment. Further, the residual strains in the TID materials due to the prior induced deformation could also be responsible for faster degradation of the nanocomposites in the corrosive media. The behavior of the samples processed using the same technique was different because of the difference in the content of Fe3O4 nanoparticles, which affected the microstructure of the nanocomposites. The Mg/Fe3O4 composites (DMD) however showed a similar trend of weight change compared to a significant weight change in Mg/ Fe3O4 (TID) composites. This was due to the porosity as well as residual strains induced during the TID process. Thus, TID materials result in quicker corrosion-induced-degradation when compared to DMD materials which is a drawback of this technique. However, porous Mg materials are desirable when used as implants due to the high biocompatibility and biodegradability of Mg [41]. Hence, further efforts need to be made in this direction to have a controlled degradability of the TID nanocomposites. Furthermore, future research in this field can involve experimentation with varying processing conditions, such as variation of turning parameters (depth of cut, feed rate, turning speed), comparison between materials produced by consolidation of turnings and consolidation of commercially-produced metal powders, as well as nanocomposite/nanoparticle variations to under the effects of the TID process.

4. Conclusions

This work aimed at synthesizing bio-compatible, superparamagnetic Fe3O4 nanoparticles to a magnesium matrix through the disintegrated melt deposition technique as well as turning-induced-deformation techniques. The following are the conclusions of this work.
  • The addition of Fe3O4 nanoparticles significantly enhances the damping capacity of the magnesium matrix and the highest ever damping capacity was recorded for the Mg/3Fe3O4 nanocomposite.
  • Further, Fe3O4 assists in improving the mechanical, ignition, and bio-corrosion response of magnesium and the best composition for the overall combination of properties was seen to be Mg/2Fe3O4 (DMD) which exhibited the lowest grain size.
  • The turning-induced-deformation (TID) method results in higher porosity as compared to the DMD method, due to which the TID nanocomposites display relatively poor ignition and bio-corrosion resistance.
  • In view of the physical and mechanical properties, the TID technique is not only economically viable and energy efficient, but also results in improvements of properties such as damping and strength.
  • Hence, the proposed TID method allows for the opportunity to directly utilize otherwise discarded metal swarf without a need for remelting, greatly reducing wastage as well as increasing the proportion of metal used overall towards finished products in large-scale industrial production.

Author Contributions

Conceptualization, S.T. and M.G.; methodology, M.J.; formal analysis and investigation, M.J. and S.T.; writing—original draft preparation, M.J. and S.T.; writing—review and editing, M.J., S.T. and M.G.; project administration, S.T.; funding acquisition, M.G.

Funding

This research was funded by SINGAPORE MINISTRY OF EDUCATION, grant number WBS. R 265 000 622 112.

Acknowledgments

The authors acknowledge Juraimi Bin Madon for assistance with extrusion and Ng Hong Wei for assistance with TGA.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Tekumalla, S.; Farhan, N.; Srivatsan, T.S.; Gupta, M. Nano-zno particles’ effect in improving the mechanical response of mg-3al-0.4ce alloy. Metals 2016, 6, 276. [Google Scholar] [CrossRef]
  2. Gupta, M.; Wong, W.L.E. Magnesium-based nanocomposites: Lightweight materials of the future. Mater. Charact. 2015, 105, 30–46. [Google Scholar] [CrossRef]
  3. Tekumalla, S.; Gupta, M. An insight into ignition factors and mechanisms of magnesium based materials: A review. Mater. Des. 2017, 113, 84–98. [Google Scholar] [CrossRef]
  4. Czerwinski, F. Controlling the ignition and flammability of magnesium for aerospace applications. Corros. Sci. 2014, 86, 1–16. [Google Scholar] [CrossRef]
  5. Goh, C.S.; Wei, J.; Lee, L.C.; Gupta, M. Development of novel carbon nanotube reinforced magnesium nanocomposites using the powder metallurgy technique. Nanotechnology 2006, 17, 7–12. [Google Scholar] [CrossRef]
  6. Sankaranarayanan, S.; Jayalakshmi, S.; Gupta, M. Effect of nano-Al2O3 addition and heat treatment on the microstructure and mechanical properties of mg-(5.6ti+3al) composite. Mater. Charact. 2013, 75, 150–164. [Google Scholar] [CrossRef]
  7. Dieringa, H. Processing of magnesium-based metal matrix nanocomposites by ultrasound-assisted particle dispersion: A review. Metals 2018, 8, 431. [Google Scholar] [CrossRef]
  8. Tekumalla, S.; Shabadi, R.; Yang, C.; Seetharaman, S.; Gupta, M. Strengthening due to the in-situ evolution of ß1’ Mg-Zn rich phase in a ZnO nanoparticles introduced mg-y alloy. Scr. Mater. 2017, 133, 29–32. [Google Scholar] [CrossRef]
  9. Tekumalla, S.; Bibhanshu, N.; Shabadi, R.; Suwas, S.; Ha, T.M.H.; Gupta, M. Evolution of texture and asymmetry and its impact on the fatigue behaviour of an in-situ magnesium nanocomposite. Mater. Sci. Eng. A 2018, 727, 61–69. [Google Scholar] [CrossRef]
  10. Gupta, M.; Seetharaman, S. Using energy efficient microwaves to synthesize high performance energy saving magnesium (nano) composites. In TMS 2015 144th Annual Meeting & Exhibition: Supplemental Proceedings; Springer International Publishing: Cham, Germany, 2015; pp. 187–193. [Google Scholar]
  11. Sankaranarayanan, S.; Gupta, M. Review on mechanical properties of magnesium (nano) composites developed using energy efficient microwaves. Powder Metall. 2015, 58, 183–192. [Google Scholar] [CrossRef]
  12. Lapovok, R.Y.; Thomson, P.F. Production of dense rod from magnesium swarf for re-melting. Magnes. Technol. 2004, 1, 149–154. [Google Scholar]
  13. Nakamura, K. Introduction of grinding swarf recycling. Ntn Technical Review No.71. 2014. Available online: https://www.ntnglobal.com/en/products/review/pdf/NTN_TR71_en_P080.pdf (accessed on 3 January 2019).
  14. Chiba, R.; Yoshimura, M. Solid-state recycling of aluminium alloy swarf into c-channel by hot extrusion. J. Manuf. Process. 2015, 17, 1–8. [Google Scholar] [CrossRef]
  15. Tekumalla, S.; Ajjarapu, M.; Gupta, M. A novel turning-induced-deformation based technique to process magnesium alloys. Metals 2019, 9, 841. [Google Scholar] [CrossRef]
  16. Pandey, R.; Tekumalla, S.; Gupta, M. Enhanced (X-band) microwave shielding properties of pure magnesium by addition of diamagnetic titanium micro-particulates. J. Alloy. Compd. 2019, 770, 473–482. [Google Scholar] [CrossRef]
  17. Pandey, R.; Tekumalla, S.; Gupta, M. Effect of defects on electromagnetic interference shielding effectiveness of magnesium. J. Mater. Sci. Mater. Electron. 2018, 29, 9728–9739. [Google Scholar] [CrossRef]
  18. Pandey, R.; Tekumalla, S.; Gupta, M. Magnesium-iron micro-composite for enhanced shielding of electromagnetic pollution. Compos. Part B Eng. 2019, 163, 150–157. [Google Scholar] [CrossRef]
  19. Jayalakshmi, S.; Singh, A.; Gupta, M. Synthesis of light metal nanocomposites: Challenges and opportunities. Indian J. Adv. Chem. Sci. S1 2016, 283–288. [Google Scholar]
  20. Micromeritics. Accupyc II 1340 Pycnometer. Available online: https://www.micromeritics.com/Product-Showcase/AccuPyc-II-1340.aspx (accessed on 3 January 2019).
  21. Tekumalla, S.; Yang, C.; Seetharaman, S.; Wong, W.L.E.; Goh, C.S.; Shabadi, R.; Gupta, M. Enhancing overall static/dynamic/damping/ignition response of magnesium through the addition of lower amounts (<2%) of yttrium. J. Alloy. Compd. 2016, 689, 350–358. [Google Scholar]
  22. NanoComposix. Useful Terminology. Available online: https://nanocomposix.com/pages/useful-terminology (accessed on 24 March 2019).
  23. Tekumalla, S.; Bibhanshu, N.; Suwas, S.; Gupta, M. Superior ductility in magnesium alloy-based nanocomposites: The crucial role of texture induced by nanoparticles. J. Mater. Sci. 2019, 54, 8711–8718. [Google Scholar] [CrossRef]
  24. Yang, W.; Tekumalla, S.; Gupta, M. Cumulative effect of strength enhancer—Lanthanum and ductility enhancer—Cerium on mechanical response of magnesium. Metals 2017, 7, 241. [Google Scholar] [CrossRef]
  25. Atlas Foundry Company. Mechanical Properties of Gray Iron—Damping Capacity. Available online: http://www.atlasfdry.com/grayiron-damping.htm (accessed on 3 January 2019).
  26. Li, B.; Lavernia, E.J. Damping capacity. In Comprehensive Composite Materials, 1st ed.; Kelly, A., Zweben, C., Eds.; Elsevier: Amsterdam, The Netherlands, 2000; Volume 3, pp. 617–653. [Google Scholar]
  27. Li, Q.; Jiang, G.; Dong, J.; Hou, J.; He, G. Damping behavior and energy absorption capability of porous magnesium. J. Alloy. Compd. 2016, 680, 522–530. [Google Scholar] [CrossRef]
  28. Xie, Z.-K.; Tane, M.; Hyun, S.-K.; Okuda, Y.; Nakajima, H. Vibration–damping capacity of lotus-type porous magnesium. Mater. Sci. Eng. A 2006, 417, 129–133. [Google Scholar] [CrossRef]
  29. Blaney, L. Magnetite (Fe3O4): Properties, synthesis, and applications. Lehigh Rev. 2007, 15, 33–81. [Google Scholar]
  30. Sezer, N.; Evis, Z.; Kayhan, S.M.; Tahmasebifar, A.; Koç, M. Review of magnesium-based biomaterials and their applications. J. Magnes. Alloy. 2018, 6, 23–43. [Google Scholar] [CrossRef]
  31. Whang, S.H. Introduction. In Nanostructured Metals and Alloys; Whang, S.H., Ed.; Woodhead Publishing: Oxford, UK, 2011; pp. xxi–xxxv. [Google Scholar]
  32. Chen, Y.; Tekumalla, S.; Guo, Y.B.; Shabadi, R.; Shim, V.P.W.; Gupta, M. The dynamic compressive response of a high-strength magnesium alloy and its nanocomposite. Mater. Sci. Eng. A 2017, 702, 65–72. [Google Scholar] [CrossRef]
  33. Yu, H.; Xin, Y.; Wang, M.; Liu, Q. Hall-petch relationship in mg alloys: A review. J. Mater. Sci. Technol. 2018, 34, 248–256. [Google Scholar] [CrossRef]
  34. Brush Wellman Inc. Grain size and material strength. In Technical Tidbits; Brush Wellman Inc.: Cleveland, OH, USA, 2010. [Google Scholar]
  35. Gao, W.; Liu, H. A highly ductile magnesium alloy system. IOP Conf. Ser. Mater. Sci. Eng. 2009, 4, 012003. [Google Scholar] [CrossRef]
  36. ToolBox, E. Fuels and Chemicals—Autoignition Temperatures. Available online: https://www.engineeringtoolbox.com/fuels-ignition-temperatures-d_171.html (accessed on 24 March 2019).
  37. Tekumalla, S.; Nandigam, Y.; Bibhanshu, N.; Rajashekara, S.; Yang, C.; Suwas, S.; Gupta, M. A strong and deformable in-situ magnesium nanocomposite igniting above 1000  °C. Sci. Rep. 2018, 8, 7038. [Google Scholar] [CrossRef]
  38. Tekumalla, S.; Si Chun, L.; Gupta, M. Preprocessing of powder to enhance mechanical and thermal response of bulk magnesium. Met. Powder Rep. 2019, 74, 137–140. [Google Scholar] [CrossRef]
  39. Singh, I.B.; Singh, M.; Das, S. A comparative corrosion behavior of Mg, AZ31 and AZ91 alloys in 3.5% NaCl solution. J. Magnes. Alloy. 2015, 3, 142–148. [Google Scholar] [CrossRef]
  40. Březina, M.; Minda, J.; Doležal, P.; Krystýnová, M.; Fintová, S.; Zapletal, J.; Wasserbauer, J.; Ptáček, P. Characterization of powder metallurgy processed pure magnesium materials for biomedical applications. Metals 2017, 7, 461. [Google Scholar] [CrossRef]
  41. Tan, L.; Yu, X.; Wan, P.; Yang, K. Biodegradable materials for bone repairs: A review. J. Mater. Sci. Technol. 2013, 29, 503–513. [Google Scholar] [CrossRef]
Figure 1. Schematic of the turning-induced deformation technique, showing compaction steps.
Figure 1. Schematic of the turning-induced deformation technique, showing compaction steps.
Metals 09 01225 g001
Figure 2. Optical micrographs with grains and grain boundaries of all Mg-Fe3O4 nanocomposites.
Figure 2. Optical micrographs with grains and grain boundaries of all Mg-Fe3O4 nanocomposites.
Metals 09 01225 g002
Figure 3. (a) A chip obtained via the turning of Mg/Fe3O4, showing low and high deformation regions; (b) the M/1Fe3O4 (DMD) nanocomposite; and (c) the Mg/1Fe3O4 (TID) with the presence of Fe3O4 particles seated at the grain boundaries.
Figure 3. (a) A chip obtained via the turning of Mg/Fe3O4, showing low and high deformation regions; (b) the M/1Fe3O4 (DMD) nanocomposite; and (c) the Mg/1Fe3O4 (TID) with the presence of Fe3O4 particles seated at the grain boundaries.
Metals 09 01225 g003
Figure 4. Damping characteristics of Mg-Fe3O4 nanocomposites in terms of amplitude vs. time. Note that the scale on the Y-axis is different in each case.
Figure 4. Damping characteristics of Mg-Fe3O4 nanocomposites in terms of amplitude vs. time. Note that the scale on the Y-axis is different in each case.
Metals 09 01225 g004
Figure 5. Stress vs strain plots of Mg–Fe3O4 nanocomposites under compressive loading.
Figure 5. Stress vs strain plots of Mg–Fe3O4 nanocomposites under compressive loading.
Metals 09 01225 g005
Figure 6. Compressive fractography images of all Mg-Fe3O4 nanocomposites.
Figure 6. Compressive fractography images of all Mg-Fe3O4 nanocomposites.
Metals 09 01225 g006
Figure 7. Wight change in the Mg–Fe3O4 nanocomposites with time in HBSS solution maintained at the normal body temperature of 37 °C.
Figure 7. Wight change in the Mg–Fe3O4 nanocomposites with time in HBSS solution maintained at the normal body temperature of 37 °C.
Metals 09 01225 g007
Table 1. Materials synthesized in this work and their processing conditions.
Table 1. Materials synthesized in this work and their processing conditions.
S. No.Material (wt %)Processing Technique and ConditionsRepresentation in This Work
1Mg/1Fe3O4DMD [19] + Extrusion at 350 °CDMD
2Mg/2Fe3O4DMD [19] + Extrusion at 350 °CDMD
3Mg/3Fe3O4DMD [19] + Extrusion at 350 °CDMD
4Mg/1Fe3O4DMD [19] + TID [15] + Extrusion at 350 °CTID
5Mg/2Fe3O4DMD [19] + TID [15] + Extrusion at 350 °CTID
6Mg/3Fe3O4DMD [19] + TID [15] + Extrusion at 350 °CTID
Table 2. Average grain size of Mg/Fe3O4 nanocomposites.
Table 2. Average grain size of Mg/Fe3O4 nanocomposites.
NanocompositeProcessing MethodMean Grain Diameter (µm)
Mg [21]
Mg/1Fe3O4
DMD25 ± 4
16 ± 6
Mg/2Fe3O48 ± 3
Mg/3Fe3O410 ± 4
Mg/1Fe3O4TID8 ± 2
Mg/2Fe3O48 ± 3
Mg/3Fe3O49 ± 3
Table 3. Density and porosity results of Mg/Fe3O4 nanocomposites obtained via both processing methods.
Table 3. Density and porosity results of Mg/Fe3O4 nanocomposites obtained via both processing methods.
NanocompositeProcessing MethodTheoretical Density (g/cm3)Average Experimental Density (g/cm3)Porosity (%)
MgDMD1.741.73 ± 0.010.65
Mg/1Fe3O41.771.76 ± 0.000.56
Mg/2Fe3O41.811.78 ± 0.011.66
Mg/3Fe3O41.841.79 ± 0.022.72
Mg/1Fe3O4TID1.771.75 ± 0.011.13
Mg/2Fe3O41.811.76 ± 0.022.76
Mg/3Fe3O41.841.77 ± 0.023.81
Table 4. Damping property results of Mg-Fe3O4 nanocomposites with respect to processing methods.
Table 4. Damping property results of Mg-Fe3O4 nanocomposites with respect to processing methods.
NanocompositeProcessing MethodAttenuation CoefficientDamping CapacityFrequency (Hz)E-Modulus (GPa)
MgDMD5.710.0002916567.9545.36
Mg/1Fe3O414.820.000410 ± 0.00004810528.449.58
Mg/2Fe3O419.930.000673 ± 0.00017910286.646.92
Mg/3Fe3O423.620.001303 ± 0.00014310131.546.05
Mg/1Fe3O4TID15.570.000453 ± 0.00002710409.348.70
Mg/2Fe3O418.810.000690 ± 0.00002210372.146.31
Mg/3Fe3O419.190.001735 ± 0.0002061019546.85
Table 5. Ignition test results of Mg–Fe3O4 nanocomposites with respect to processing methods.
Table 5. Ignition test results of Mg–Fe3O4 nanocomposites with respect to processing methods.
NanocompositeProcessing MethodIgnition Temperature (°C)
MgDMD590
Mg/1Fe3O4630.6
Mg/2Fe3O4635.0
Mg/3Fe3O4635.2
Mg/1Fe3O4TID625.4
Mg/2Fe3O4633.1
Mg/3Fe3O4632.2

Share and Cite

MDPI and ACS Style

Johanes, M.; Tekumalla, S.; Gupta, M. Fe3O4 Nanoparticle-Reinforced Magnesium Nanocomposites Processed via Disintegrated Melt Deposition and Turning-Induced Deformation Techniques. Metals 2019, 9, 1225. https://doi.org/10.3390/met9111225

AMA Style

Johanes M, Tekumalla S, Gupta M. Fe3O4 Nanoparticle-Reinforced Magnesium Nanocomposites Processed via Disintegrated Melt Deposition and Turning-Induced Deformation Techniques. Metals. 2019; 9(11):1225. https://doi.org/10.3390/met9111225

Chicago/Turabian Style

Johanes, Michael, Sravya Tekumalla, and Manoj Gupta. 2019. "Fe3O4 Nanoparticle-Reinforced Magnesium Nanocomposites Processed via Disintegrated Melt Deposition and Turning-Induced Deformation Techniques" Metals 9, no. 11: 1225. https://doi.org/10.3390/met9111225

APA Style

Johanes, M., Tekumalla, S., & Gupta, M. (2019). Fe3O4 Nanoparticle-Reinforced Magnesium Nanocomposites Processed via Disintegrated Melt Deposition and Turning-Induced Deformation Techniques. Metals, 9(11), 1225. https://doi.org/10.3390/met9111225

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop